SUBSTRATE PROCESSING METHOD, SEMICONDUCTOR DEVICE MANUFACTURING METHOD, SUBSTRATE PROCESSING APPARATUS AND PROGRAM
By alternating cycles of metal-containing, reducing, and oxygen-containing gas supply, the method addresses oxidation and impurity issues in metal films, resulting in improved film characteristics and productivity.
Patent Information
- Application Number
- JP2023556030
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The oxidation of base films and the presence of impurities in metal-containing films during the film forming process in semiconductor manufacturing pose challenges, leading to degraded film characteristics.
A method involving alternating cycles of supplying a metal-containing gas, reducing gas, and oxygen-containing gas to the substrate, followed by purging, to form and modify metal-containing films while minimizing oxidation and impurities.
This approach enhances the characteristics of the metal-containing films by suppressing oxidation and reducing impurities, improving film quality and productivity.
Smart Images

Figure 0007562013000001 
Figure 0007562013000002 
Figure 0007562013000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to Substrate processing method , a method for manufacturing a semiconductor device 、 Substrate processing apparatus and program Regarding. [Background technology]
[0002] 2. Description of the Related Art As one step in the manufacturing process of a semiconductor device, a film formation process is performed to form a film on a substrate accommodated in a processing chamber (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2006 / 134930 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when a metal-containing film containing a metal element is formed on an undercoat film, the undercoat film may be oxidized, resulting in impurities being contained in the metal-containing film.
[0005] An object of the present disclosure is to provide a technique capable of improving the properties of a metal-containing film formed on an underlayer while suppressing oxidation of the underlayer. [Means for solving the problem]
[0006] According to one aspect of the present disclosure, (a) supplying a metal-containing gas containing a metal element to a substrate on which a metal-containing film has been formed; (b) supplying a reducing gas to the substrate; (c) supplying an oxygen-containing gas containing oxygen atoms and the reducing gas to the substrate; (d) repeating a cycle comprising (a) and (b) a first number of times; (e) after (d), repeating the cycle comprising (a) and (c) a second number of times; The present invention provides a technique having the following features: Effect of the Invention
[0007] According to the present disclosure, it is possible to improve the properties of a metal-containing film formed on an undercoat film while suppressing oxidation of the undercoat film. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic vertical cross-sectional view of a vertical processing furnace of a substrate processing apparatus according to an embodiment of the present disclosure. [Diagram 2] 2 is a schematic cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. 2 is a schematic configuration diagram of a controller of the substrate processing apparatus according to an embodiment of the present disclosure, showing a control system of the controller in a block diagram. [Figure 4] 1A-1D are diagrams illustrating a substrate processing process according to an embodiment of the present disclosure. [Diagram 5] Figure 5(A) is a cross-sectional view of a substrate showing the state before a metal-containing film is formed in a recess on the substrate, Figure 5(B) is a cross-sectional view of the substrate showing the state after an oxide film formed in a recess on the substrate has been etched, Figure 5(C) is a cross-sectional view of the substrate showing the state after a first metal-containing film has been formed in a recess on the substrate, Figure 5(D) is a cross-sectional view of the substrate showing the state after a second metal-containing film has been formed in a recess on the substrate, and Figure 5(E) is a cross-sectional view of the substrate showing the state after a metal-containing film has been formed in a recess on the substrate. [Figure 6] 11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. [Figure 7] 11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. [Figure 8] 11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. [Figure 9]11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. [Figure 10] 11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. [Figure 11] 11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. [Figure 12] 11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. [Figure 13] 11A to 11C are diagrams illustrating a modified example of a substrate processing process according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The following description will be given with reference to Figures 1 to 4 and Figures 5(A) to 5(E). Note that all of the drawings used in the following description are schematic, and the dimensional relationships between elements, the ratios between elements, etc. shown in the drawings do not necessarily match those in reality. Furthermore, the dimensional relationships between elements, the ratios between elements, etc. between multiple drawings do not necessarily match.
[0010] (1) Configuration of the substrate processing device The substrate processing apparatus 10 includes a processing furnace 202 provided with a heater 207 as a heating means (heating mechanism, heating system). The heater 207 has a cylindrical shape and is installed vertically by being supported by a heater base (not shown) as a holding plate.
[0011] An outer tube 203 constituting a reaction vessel (processing vessel) is disposed inside the heater 207 concentrically with the heater 207. The outer tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC) and is formed in a cylindrical shape with a closed upper end and an open lower end. A manifold (inlet flange) 209 is disposed concentrically below the outer tube 203. The manifold 209 is made of a metal such as stainless steel (SUS) and is formed in a cylindrical shape with open upper and lower ends. An O-ring 220a is provided as a seal member between the upper end of the manifold 209 and the outer tube 203. The manifold 209 is supported by a heater base, so that the outer tube 203 is installed vertically.
[0012] An inner tube 204 constituting a reaction vessel is disposed inside the outer tube 203. The inner tube 204 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC) and is formed in a cylindrical shape with a closed upper end and an open lower end. A processing vessel (reaction vessel) is mainly constituted by the outer tube 203, the inner tube 204, and the manifold 209. A processing chamber 201 is formed in the cylindrical hollow portion of the processing vessel (inside the inner tube 204).
[0013] The processing chamber 201 is configured so as to be capable of accommodating wafers 200 as substrates in a boat 217 (described later) in a horizontal position and in a state in which the wafers are arranged in multiple stages in the vertical direction.
[0014] Nozzles 410, 420, 430, and 440 are provided in the processing chamber 201 so as to penetrate the sidewall of the manifold 209 and the inner tube 204. Gas supply pipes 310, 320, 330, and 340 are connected to the nozzles 410, 420, 430, and 440, respectively. However, the processing furnace 202 of this embodiment is not limited to the above-mentioned configuration.
[0015] Gas supply pipes 310, 320, 330, 340 are provided with mass flow controllers (MFCs) 312, 322, 332, 342, which are flow rate controllers (flow rate control parts), and valves 314, 324, 334, 344, which are on-off valves, in order from the upstream side. Gas supply pipes 510, 520, 530, 540, which supply inert gas, are connected to the downstream sides of the valves 314, 324, 334, 344 of the gas supply pipes 310, 320, 330, 340. Gas supply pipes 510, 520, 530, 540 are provided with MFCs 512, 522, 532, 542, which are flow rate controllers (flow rate control parts), and valves 514, 524, 534, 544, which are on-off valves, in order from the upstream side.
[0016] Nozzles 410, 420, 430, 440 are respectively connected to the tips of the gas supply pipes 310, 320, 330, 340. The nozzles 410, 420, 430, 440 are configured as L-shaped nozzles, and their horizontal parts are provided so as to penetrate the side wall of the manifold 209 and the inner tube 204. The vertical parts of the nozzles 410, 420, 430, 440 are provided inside the preliminary chamber 201a having a channel shape (groove shape) formed so as to protrude radially outward from the inner tube 204 and extend vertically, and are provided in the preliminary chamber 201a toward the upper side (upward in the arrangement direction of the wafers 200) along the inner wall of the inner tube 204.
[0017] The nozzles 410, 420, 430, 440 are provided so as to extend from the lower region of the processing chamber 201 to the upper region of the processing chamber 201, and a plurality of gas supply holes 410a, 420a, 430a, 440a are provided at positions facing the wafer 200. As a result, the gas supply holes 410a, 420a, 430a, 440a of the nozzles 410, 420, 430, 440 supply processing gas to the wafer 200. The gas supply holes 410a, 420a, 430a, 440a are provided from the lower part to the upper part of the inner tube 204, each having the same opening area, and further provided at the same opening pitch. However, the gas supply holes 410a, 420a, 430a, 440a are not limited to the above-mentioned form. For example, the opening area may be gradually increased from the lower part to the upper part of the inner tube 204. This makes it possible to make the flow rates of the gases supplied from the gas supply holes 410a, 420a, 430a, and 440a more uniform.
[0018] The gas supply holes 410a, 420a, 430a, 440a of the nozzles 410, 420, 430, 440 are provided at a height from the bottom to the top of the boat 217 described later. Therefore, the process gas supplied from the gas supply holes 410a, 420a, 430a, 440a of the nozzles 410, 420, 430, 440 into the process chamber 201 is supplied to the entire area of the wafers 200 accommodated from the bottom to the top of the boat 217. The nozzles 410, 420, 430, 440 may be provided so as to extend from the bottom region to the top region of the process chamber 201, but are preferably provided so as to extend to the vicinity of the ceiling of the boat 217.
[0019] A metal-containing gas, which is a source gas containing a metal element, is supplied as a processing gas from the gas supply pipe 310 into the processing chamber 201 via the MFC 312 , the valve 314 , and the nozzle 410 .
[0020] A reducing gas is supplied as a processing gas from the gas supply pipe 320 into the processing chamber 201 via the MFC 322 , the valve 324 , and the nozzle 420 .
[0021] From the gas supply pipe 330, an oxygen-containing gas, which is a gas containing oxygen atoms (O), is supplied as a processing gas into the processing chamber 201 via the MFC 332, the valve 334, and the nozzle 430.
[0022] A halogen-containing gas, which is a gas containing a halogen element, is supplied as a processing gas from the gas supply pipe 340 into the processing chamber 201 via the MFC 342 , the valve 344 , and the nozzle 440 .
[0023] Inert gas is supplied from gas supply pipes 510, 520, 530, and 540 into the processing chamber 201 via MFCs 512, 522, 532, and 542, valves 514, 524, 534, and 544, and nozzles 410, 420, 430, and 440, respectively.
[0024] As the inert gas, for example, nitrogen (N2) gas, argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas, or other rare gases can be used. As the inert gas, one or more of these can be used. This also applies to other inert gases described later.
[0025] The process gas supply system is mainly composed of the gas supply pipes 310, 320, 330, 340, the MFCs 312, 322, 332, 342, the valves 314, 324, 334, 344, and the nozzles 410, 420, 430, 440, but only the nozzles 410, 420, 430, 440 may be considered as the process gas supply system. The process gas supply system may be simply called a gas supply system. When a metal-containing gas is flowed from the gas supply pipe 310, the metal-containing gas supply system is mainly composed of the gas supply pipe 310, the MFC 312, and the valve 314, but the nozzle 410 may be included in the metal-containing gas supply system. When a reducing gas is flowed from the gas supply pipe 320, the reducing gas supply system is mainly composed of the gas supply pipe 320, the MFC 322, and the valve 324, but the nozzle 420 may be included in the reducing gas supply system. In addition, when oxygen-containing gas is caused to flow from the gas supply pipe 330, an oxygen-containing gas supply system is mainly composed of the gas supply pipe 330, the MFC 332, and the valve 334, but the nozzle 430 may be included in the oxygen-containing gas supply system. In addition, when halogen-containing gas is caused to flow from the gas supply pipe 340, a halogen-containing gas supply system is mainly composed of the gas supply pipe 340, the MFC 342, and the valve 344, but the nozzle 440 may be included in the halogen-containing gas supply system. In addition, an inert gas supply system is mainly composed of the gas supply pipes 510, 520, 530, and 540, the MFCs 512, 522, 532, and 542, and the valves 514, 524, 534, and 544. The inert gas supply system may be called a rare gas supply system.
[0026] In the method of supplying gas in this embodiment, gas is transported via nozzles 410, 420, 430, and 440 arranged in a preliminary chamber 201a in a vertically elongated space of an annular shape defined by the inner wall of the inner tube 204 and the ends of the multiple wafers 200. Then, gas is ejected into the inner tube 204 from multiple gas supply holes 410a, 420a, 430a, and 440a provided at positions of the nozzles 410, 420, 430, and 440 facing the wafer. More specifically, the process gas and the like are ejected in a direction parallel to the surface of the wafer 200 from the gas supply hole 410a of the nozzle 410, the gas supply hole 420a of the nozzle 420, the gas supply hole 430a of the nozzle 430, and the gas supply hole 440a of the nozzle 440.
[0027] The exhaust hole (exhaust port) 204a is a through hole formed in the side wall of the inner tube 204 at a position facing the nozzles 410, 420, 430, 440, and is, for example, a slit-shaped through hole elongated in the vertical direction. Gas is supplied from the gas supply holes 410a, 420a, 430a, 440a of the nozzles 410, 420, 430, 440 into the processing chamber 201 and flows over the surface of the wafer 200, and flows into the exhaust path 206 constituted by a gap formed between the inner tube 204 and the outer tube 203 through the exhaust hole 204a. The gas flowing into the exhaust path 206 then flows into the exhaust pipe 231 and is exhausted to the outside of the processing furnace 202.
[0028] The exhaust hole 204a is provided at a position facing the multiple wafers 200, and gas supplied from the gas supply holes 410a, 420a, 430a, and 440a to the vicinity of the wafers 200 in the processing chamber 201 flows in the horizontal direction and then flows into the exhaust path 206 via the exhaust hole 204a. The exhaust hole 204a is not limited to being configured as a slit-shaped through hole, and may be configured as a multiple hole.
[0029] The manifold 209 is provided with an exhaust pipe 231 for exhausting the atmosphere in the processing chamber 201. The exhaust pipe 231 is connected to a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201, an APC (Auto Pressure Controller) valve 243, and a vacuum pump 246 as a vacuum exhaust device, in this order from the upstream side. The APC valve 243 can evacuate and stop the evacuation of the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is in operation, and further, the pressure in the processing chamber 201 can be adjusted by adjusting the valve opening while the vacuum pump 246 is in operation. An exhaust system is mainly configured by the exhaust hole 204a, the exhaust path 206, the exhaust pipe 231, the APC valve 243, and the pressure sensor 245. The vacuum pump 246 may be included in the exhaust system.
[0030] Below the manifold 209, a seal cap 219 is provided as a furnace port cover capable of airtightly closing the lower end opening of the manifold 209. The seal cap 219 is configured to abut against the lower end of the manifold 209 from below in the vertical direction. The seal cap 219 is made of a metal such as SUS and is formed in a disk shape. An O-ring 220b is provided on the upper surface of the seal cap 219 as a seal member that abuts against the lower end of the manifold 209. On the opposite side of the seal cap 219 to the processing chamber 201, a rotation mechanism 267 is installed to rotate the boat 217 that accommodates the wafers 200. A rotation shaft 255 of the rotation mechanism 267 is connected to the boat 217 through the seal cap 219. The rotation mechanism 267 is configured to rotate the wafers 200 by rotating the boat 217. The seal cap 219 is configured to be raised and lowered in the vertical direction by a boat elevator 115 as a lifting mechanism that is vertically installed outside the outer tube 203. The boat elevator 115 is configured to be able to load and unload the boat 217 into and out of the processing chamber 201 by raising and lowering the seal cap 219. The boat elevator 115 is configured as a transfer device (transfer system) that transfers the boat 217 and the wafers 200 accommodated in the boat 217 into and out of the processing chamber 201.
[0031] The boat 217 as a substrate support is configured to arrange a plurality of wafers 200, for example, 25 to 200, in a horizontal position and with their centers aligned in a vertical direction at intervals. The boat 217 is made of a heat-resistant material such as quartz or SiC. The lower part of the boat 217 is supported by a heat insulating cylinder 218 configured as a cylindrical member made of a heat-resistant material such as quartz or SiC. This configuration makes it difficult for heat from the heater 207 to be transmitted to the seal cap 219. However, this embodiment is not limited to the above-mentioned form. For example, instead of providing the heat insulating cylinder 218, heat insulating plates made of a heat-resistant material such as quartz or SiC may be supported in multiple stages (not shown) in a horizontal position at the lower part of the boat 217.
[0032] 2, a temperature sensor 263 is installed in the inner tube 204 as a temperature detector, and the amount of electricity supplied to the heater 207 is adjusted based on temperature information detected by the temperature sensor 263 so that the temperature distribution in the processing chamber 201 is set to a desired value. The temperature sensor 263 is configured in an L-shape like the nozzles 410, 420, 430, and 440, and is provided along the inner wall of the inner tube 204.
[0033] 3, the controller 121, which is a control unit (control means), is configured as a computer including a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus. The controller 121 is connected to an input / output device 122 configured as, for example, a touch panel.
[0034] The storage device 121c is composed of, for example, a flash memory, an HDD (Hard Disk Drive), etc. A control program for controlling the operation of the substrate processing apparatus, a process recipe describing the procedure and conditions of a manufacturing method for a semiconductor device (substrate processing method) described later, and the like are readably stored in the storage device 121c. The process recipe is a combination of processes (steps) in a manufacturing method for a semiconductor device (substrate processing method) described later that is executed by the controller 121 to obtain a predetermined result, and functions as a program. Hereinafter, the process recipe, the control program, etc. are collectively referred to simply as a program. When the word program is used in this specification, it may include only a process recipe, only a control program, or a combination of a process recipe and a control program. The RAM 121b is configured as a memory area (work area) in which the programs and data read by the CPU 121a are temporarily stored.
[0035] The I / O port 121d is connected to the above-mentioned MFCs 312, 322, 332, 342, 512, 522, 532, 542, valves 314, 324, 334, 344, 514, 524, 534, 544, pressure sensor 245, APC valve 243, vacuum pump 246, heater 207, temperature sensor 263, rotation mechanism 267, boat elevator 115, etc.
[0036] The CPU 121a is configured to read and execute a control program from the storage device 121c, and to read a recipe or the like from the storage device 121c in response to an input of an operation command from the input / output device 122. The CPU 121a is configured to be capable of controlling the flow rate adjustment of various gases by the MFCs 312, 322, 332, 342, 512, 522, 532, and 542, the opening and closing of the valves 314, 324, 334, 344, 514, 524, 534, and 544, the opening and closing of the APC valve 243 and the pressure adjustment based on the pressure sensor 245 by the APC valve 243, the temperature adjustment of the heater 207 based on the temperature sensor 263, the start and stop of the vacuum pump 246, the rotation and rotation speed adjustment of the boat 217 by the rotation mechanism 267, the lifting and lowering of the boat 217 by the boat elevator 115, the accommodation of the wafers 200 in the boat 217, and the like, in accordance with the contents of the read recipe.
[0037] The controller 121 can be configured by installing the above-mentioned program stored in an external storage device (for example, a magnetic tape, a magnetic disk such as a flexible disk or a hard disk, an optical disk such as a CD or a DVD, a magneto-optical disk such as an MO, or a semiconductor memory such as a USB memory or a memory card) 123 into a computer. The storage device 121c and the external storage device 123 are configured as computer-readable recording media. Hereinafter, these are collectively referred to simply as recording media. In this specification, the recording medium may include only the storage device 121c alone, may include only the external storage device 123 alone, or may include both. The program may be provided to the computer using a communication means such as the Internet or a dedicated line, without using the external storage device 123.
[0038] (2) Substrate processing process (substrate processing method) As one step in the manufacturing process of a semiconductor device, an example of a step of forming a metal-containing film 600 containing a metal element on a wafer 200 on which a metal-containing film 300 containing a metal element has been formed as an undercoat film will be described with reference to Fig. 4. The step of forming the metal-containing film 600 on the wafer 200 on which the metal-containing film 300 has been formed is performed using the processing furnace 202 of the above-mentioned substrate processing apparatus 10. In the following description, the operation of each part constituting the substrate processing apparatus 10 is controlled by a controller 121.
[0039] In the substrate processing process (semiconductor device manufacturing process) according to this embodiment, (a) supplying a metal-containing gas containing a metal element to a wafer 200 on which a metal-containing film is formed; (b) supplying a reducing gas to the wafer 200; (c) supplying an oxygen-containing gas containing oxygen atoms and the reducing gas to the wafer 200; (d) repeating a cycle comprising (a) and (b) a first number of times; (e) after (d), repeating the cycle comprising (a) and (c) a second number of times; has.
[0040] In this specification, the term "wafer" may mean "the wafer itself" or "a laminate of a wafer and a specified layer, film, etc. formed on its surface." In this specification, the term "surface of a wafer" may mean "the surface of the wafer itself" or "the surface of a specified layer, film, etc. formed on the wafer." In this specification, the term "substrate" is synonymous with the term "wafer."
[0041] (Wafer loading) 1, when a plurality of wafers 200 are loaded into the boat 217 (wafer charge), the boat 217 supporting the plurality of wafers 200 is lifted by the boat elevator 115, carried into the processing chamber 201 (boat load), and accommodated in the processing vessel. In this state, the seal cap 219 closes the lower end opening of the outer tube 203 via the O-ring 220.
[0042] (Pressure and temperature regulation) The inside of the processing chamber 201, i.e., the space in which the wafer 200 exists, is evacuated by the vacuum pump 246 so as to reach a desired pressure (vacuum level). At this time, the pressure inside the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 243 is feedback-controlled (pressure adjustment) based on the measured pressure information. The vacuum pump 246 is kept in a constantly operating state at least until the processing of the wafer 200 is completed.
[0043] The inside of the processing chamber 201 is heated by the heater 207 so as to reach a desired temperature. At this time, the amount of electricity supplied to the heater 207 is feedback-controlled (temperature adjustment) based on temperature information detected by the temperature sensor 263 so as to achieve a desired temperature distribution in the processing chamber 201. Heating of the inside of the processing chamber 201 by the heater 207 continues at least until the processing of the wafer 200 is completed.
[0044] Here, the metal-containing film 300 serving as the undercoat film can be a film containing at least one of metal elements and transition metals (transition elements), such as tungsten (W), molybdenum (Mo), copper (Cu), and cobalt (Co). The metal-containing film 300 can be used as metal wiring, and may be metal wiring M1 in the bottom layer of a wiring layer, or metal wiring My in an intermediate layer (y is a natural number).
[0045] For example, as shown in FIG. 5(A), a metal-containing film 300 is formed on a wafer 200, an insulating film 400 is formed on the metal-containing film 300, and a recess 400a such as a trench or a hole is formed in the insulating film 400. When a metal-containing film 600 containing a metal element is embedded in the recess 400a on the wafer 200, a metal oxide film 500, which is a natural oxide film, may be formed on the surface of the metal-containing film 300 in the recess 400a. In particular, transition metals such as W, Mo, Cu, and Co are easily oxidized, and the metal oxide film 500 may be formed on the surface. If the metal oxide film 500 is formed and remains without being removed, the contact resistance between the metal-containing film 300 and the metal-containing film 600 embedded in the recess 400a may increase. When a ruthenium (Ru) film is formed as an example of the metal-containing film 600, it is essential to reduce the contact resistance in order to utilize the low resistance characteristic of the Ru film.
[0046] Therefore, in the substrate processing step (semiconductor device manufacturing step) according to this embodiment, before forming the metal-containing film 600 in the recess 400a, a pre-treatment step is performed in the same processing chamber 201 to supply a halogen-containing gas containing a halogen element to the wafer 200 and remove at least a part of the metal oxide film 500. That is, the pre-treatment step and the film formation step are performed consecutively in the same processing chamber (in-situ). That is, after removing the metal oxide film 500 by the pre-treatment step described later, the film formation step described later is performed in the same processing chamber 201 to form the metal-containing film 600.
[0047] A. Pre-treatment process (Halogen-containing gas supply, step S1) The valve 344 is opened to allow a halogen-containing gas to flow into the gas supply pipe 340. The halogen-containing gas is adjusted in flow rate by the MFC 342, supplied from the gas supply hole 440a of the nozzle 440 into the processing chamber 201, and exhausted from the exhaust pipe 231. At this time, the halogen-containing gas is supplied to the wafer 200. At this time, the valve 544 is opened at the same time to allow an inert gas to flow into the gas supply pipe 540. The inert gas flowing through the gas supply pipe 540 is adjusted in flow rate by the MFC 542, supplied together with the halogen-containing gas into the processing chamber 201, and exhausted from the exhaust pipe 231. At this time, in order to prevent the halogen-containing gas from entering the nozzles 410, 420, and 430, the valves 514, 524, and 534 are opened to allow an inert gas to flow into the gas supply pipes 510, 520, and 530. The inert gas is supplied into the processing chamber 201 via gas supply pipes 310 , 320 , and 330 and nozzles 410 , 420 , and 430 , and is exhausted from an exhaust pipe 231 .
[0048] At this time, the APC valve 243 is adjusted to set the pressure in the process chamber 201 to, for example, a pressure in the range of 1 to 3990 Pa. The supply flow rate of the halogen-containing gas controlled by the MFC 342 is, for example, a flow rate in the range of 0.05 to 20 slm. The supply flow rates of the inert gases controlled by the MFCs 512, 522, 532, and 542 are, for example, a flow rate in the range of 0.1 to 50 slm. Note that in this disclosure, the expression of a numerical range such as "1 to 3990 Pa" means that the lower limit and the upper limit are included in the range. Thus, for example, "1 to 3990 Pa" means "1 Pa or more and 3990 Pa or less". The same applies to other numerical ranges.
[0049] At this time, only the halogen-containing gas and the inert gas are flowing into the processing chamber 201. The halogen-containing gas undergoes a substitution reaction with at least a part of the metal oxide film 500 formed on the metal-containing film 300. That is, O in the metal oxide film 500 reacts with the halogen element, is desorbed from the metal oxide film 500, and is discharged from the processing chamber 201 as a reaction by-product. That is, at least a part of the metal oxide film 500 is removed (etched).
[0050] As the halogen-containing gas, for example, a gas capable of selectively etching only the metal oxide film 500 formed in the recess 400a on the wafer 200 can be used. As the halogen-containing gas, a gas containing, for example, one or more chlorine (Cl) atoms and one or more oxygen (O) atoms, which are halogen elements, can be used. In other words, as the halogen-containing gas, a gas having a molecular structure of MO x Cl y Here, M includes at least one of phosphorus (P), sulfur (S), and carbon (C). As the oxyhalide, for example, phosphorus oxychloride (POCl3), thionyl chloride (SOCl2), carbonyl dichloride (COCl2) gas, etc. can be used. As the halogen-containing gas, one or more of these can be used.
[0051] In this way, when an oxyhalide is used as the halogen-containing gas, O in the metal oxide film 500 reacts with Cl or O and is desorbed from the metal oxide film 500, so that only the metal oxide film 500 can be selectively etched as shown in Fig. 5(B). For example, only the metal oxide film 500 can be selectively etched without etching the insulating film 400 formed of a silicon oxide (SiO2) film. In other words, the halogen-containing gas can also be called an etching gas that etches the metal oxide film 500.
[0052] (Removal of residual gas (exhaust), step S2) After a predetermined time has elapsed since the supply of the halogen-containing gas was started, for example, 1 to 600 seconds, the valve 344 of the gas supply pipe 340 is closed to stop the supply of the halogen-containing gas. That is, the time for supplying the halogen-containing gas to the wafer 200 is, for example, 1 to 600 seconds. At this time, the APC valve 243 of the exhaust pipe 231 is left open, and the inside of the processing chamber 201 is evacuated by the vacuum pump 246, and the halogen-containing gas remaining in the processing chamber 201, unreacted or having contributed to etching the metal oxide film 500, is removed from the inside of the processing chamber 201 (the space in which the wafer 200 exists is evacuated). That is, the inside of the processing chamber 201 is purged. At this time, the valves 514, 524, 534, and 544 are left open to maintain the supply of the inert gas into the processing chamber 201. The inert gas acts as a purge gas, and can enhance the effect of removing the halogen-containing gas remaining in the processing chamber 201, unreacted or having contributed to etching, from the inside of the processing chamber 201.
[0053] The above-mentioned pretreatment step can also be called a metal oxide film removal step, a pre-etching step, or a pre-cleaning step.
[0054] B. Metal-containing film formation process (film formation process) [First metal-containing film forming step] (Metal-containing gas supply, step S11) The valve 314 is opened, and a metal-containing gas, which is a raw material gas, is flowed into the gas supply pipe 310. The flow rate of the metal-containing gas is adjusted by the MFC 312, and the metal-containing gas is supplied into the processing chamber 201 from the gas supply hole 410a of the nozzle 410, and is exhausted from the exhaust pipe 231. At this time, the valve 514 is opened at the same time, and an inert gas is flowed into the gas supply pipe 510. The inert gas flowing in the gas supply pipe 510 is adjusted in flow rate by the MFC 512, and is supplied into the processing chamber 201 together with the metal-containing gas, and is exhausted from the exhaust pipe 231. At this time, in order to prevent the metal-containing gas from entering the nozzles 420, 430, and 440, the valves 524, 534, and 544 are opened, and the inert gas is flowed into the gas supply pipes 520, 530, and 540. The inert gas is supplied into the processing chamber 201 via gas supply pipes 320 , 330 , and 340 and nozzles 420 , 430 , and 440 , and is exhausted from an exhaust pipe 231 .
[0055] At this time, the APC valve 243 is adjusted to set the pressure inside the processing chamber 201 within a range of, for example, 1 to 3990 Pa. The supply flow rate of the metal-containing gas controlled by the MFC 312 is set within a range of, for example, 0.05 to 1 slm. The supply flow rates of the inert gases controlled by the MFCs 512, 522, 532, and 542 are each set within a range of, for example, 0.1 to 50 slm.
[0056] At this time, only the metal-containing gas and the inert gas are flowing in the processing chamber 201. That is, as shown in Fig. 5(B), the metal-containing gas is supplied to the wafer 200 from which the metal oxide film 500 has been removed, and a metal-containing layer is formed on the wafer 200 (the insulating film 400 on the surface and in the recess 400a). The metal-containing layer may be a metal layer containing other elements, or may be an adsorption layer of the metal-containing gas.
[0057] As the metal-containing gas, a gas containing, for example, a transition metal (transition element) as the metal element can be used, and preferably, a gas containing a platinum group element and an element of group 8 can be used. As the metal-containing gas, for example, a Ru-containing gas containing ruthenium (Ru) can be used. In this way, by using a gas containing a transition metal, a platinum group element, and an element of group 8, it is possible to form a metal-containing film with low resistance. In addition, as the metal-containing gas, a gas containing a metal element and a carbonyl group can be used. This can improve the film formation rate.
[0058] Examples of the metal-containing gas include bisethylcyclopentadienyl ruthenium (Ru(C2H5C5H4)2), butylruthenocene (Ru(C5H5)(C4H9C5H4), tris-2,4-octanedionato ruthenium (Ru[CH3COCHCO(CH2)3CH3]3), 2,4-dimethylpentadienyl ethylcyclopentadienyl ruthenium (Ru(C2H5C5H4)((CH3)C5H5)), Ru(C7H8)(C7H 11 O2), dicarbonylbis(5-methyl-2,4-hexanediketonate)ruthenium(II)(C 16 H 22 O6Ru), triruthenium dodecacarbonyl (Ru3(CO) 12 ), η4-2,3-dimethylbutadiene ruthenium tricarbonyl ((DMBD)Ru(CO)3), η4-butadiene ruthenium tricarbonyl ((BD)Ru(CO3)), η4-1,3-cyclohexadiene ruthenium tricarbonyl ((CHD)Ru(CO)3), bis(cyclopentadienyl ruthenium dicarbonyl (C 14 H 10 For example, a gas obtained by vaporizing an organometallic material such as ruthenium(II) [Ru(CO)Cl], tricarbonyldichlororuthenium(II) [Ru(CO)Cl], etc. can be used. As the metal-containing gas, one or more of these can be used.
[0059] Here, when a Ru-containing gas, for example, is used as the metal-containing gas, a Ru-containing layer is formed in the recess 400a on the wafer 200. The Ru-containing layer may be a Ru layer containing other elements, an adsorption layer of the Ru-containing gas, or may contain both.
[0060] (Removal of residual gas, step S12) After a predetermined time has elapsed since the supply of the metal-containing gas was started, for example, 1 to 120 seconds, the valve 314 of the gas supply pipe 310 is closed to stop the supply of the metal-containing gas. That is, the time for supplying the metal-containing gas to the wafer 200 is, for example, 1 to 120 seconds. At this time, the APC valve 243 of the exhaust pipe 231 is kept open, and the inside of the processing chamber 201 is evacuated by the vacuum pump 246, and the metal-containing gas remaining in the processing chamber 201, which has not reacted or which has contributed to the formation of the metal-containing layer, is removed from the inside of the processing chamber 201. That is, the inside of the processing chamber 201 is purged. At this time, the valves 514, 524, 534, and 544 are kept open to maintain the supply of the inert gas into the processing chamber 201. The inert gas acts as a purge gas, and can enhance the effect of removing the metal-containing gas remaining in the processing chamber 201, which has not reacted or which has contributed to the formation of the metal-containing layer, from the inside of the processing chamber 201.
[0061] (Supply of reduction gas, step S13) After removing the residual gas in the processing chamber 201, the valve 324 is opened to flow the reducing gas into the gas supply pipe 320. The reducing gas is adjusted in flow rate by the MFC 322, supplied into the processing chamber 201 from the gas supply hole 420a of the nozzle 420, and exhausted from the exhaust pipe 231. At this time, the reducing gas is supplied to the wafer 200. At the same time, the valve 524 is opened to flow the inert gas into the gas supply pipe 520. The inert gas flowing in the gas supply pipe 520 is adjusted in flow rate by the MFC 522. The inert gas is supplied into the processing chamber 201 together with the reducing gas, and exhausted from the exhaust pipe 231. At this time, in order to prevent the reducing gas from entering the nozzles 410, 430, and 440, the valves 514, 534, and 544 are opened to flow the inert gas into the gas supply pipes 510, 530, and 540. The inert gas is supplied into the processing chamber 201 via gas supply pipes 310 , 330 , and 340 and nozzles 410 , 430 , and 440 , and is exhausted from an exhaust pipe 231 .
[0062] At this time, the APC valve 243 is adjusted to set the pressure inside the processing chamber 201 within a range of, for example, 5 to 15,000 Pa. The supply flow rate of the reducing gas controlled by the MFC 322 is set within a range of, for example, 1 to 100 slm, preferably 15 to 50 slm. The supply flow rates of the inert gases controlled by the MFCs 512 to 542 are each set within a range of, for example, 0.1 to 50 slm.
[0063] Here, the pressure (total pressure) of the space in which the wafer 200 exists, which is the pressure inside the process chamber 201 in this step, is set to be higher than the pressure (total pressure) of the space in which the wafer 200 exists in step S23 described later. That is, the pressure inside the process chamber 201 in this step is set to be higher than the pressure inside the process chamber 201 in step S23 described later.
[0064] By increasing the pressure in the process chamber 201 when the reducing gas is supplied, the ligand in the film is easily removed. If purging is performed at high pressure when removing the residual gas in the above-mentioned step S12 in order to remove the ligand, it takes time to return the pressure in the process chamber 201 to the original pressure. By increasing the pressure in the process chamber 201 when the reducing gas is supplied in this step, the ligand can be removed (purged) in a shorter time than if the pressure in the process chamber 201 was increased during purging.
[0065] Furthermore, if the pressure in the process chamber 201 is made high during the supply of reducing gas in all steps of the substrate processing process, time is required for pressure adjustment from low pressure to high pressure between the supply of metal-containing gas and the supply of reducing gas. In the present disclosure, the pressure in the process chamber 201 is made high during the supply of reducing gas in the first metal-containing film formation step in the first half of the entire process, and the pressure in the process chamber 201 is made low during the supply of reducing gas in the second metal-containing film formation step in the second half, thereby shortening the pressure adjustment time between the supply of metal-containing gas and the supply of reducing gas. In other words, productivity can be improved.
[0066] The partial pressure of the reducing gas in this step may be set higher than the partial pressure of the reducing gas in step S23 described later. In addition, at least one of the pressure in the process chamber 201 and the partial pressure of the reducing gas in this step may be changed every predetermined cycle (first number of times). In other words, at least one of the pressure in the process chamber 201 and the partial pressure of the reducing gas when the reducing gas is supplied in this step may be changed every time the number of cycles (first number of times) of the first metal-containing film formation process is repeated. Specifically, at least one of the pressure in the process chamber 201 and the partial pressure of the reducing gas in this step may be decreased every predetermined cycle (first number of times).
[0067] At this time, the gases flowing inside the processing chamber 201 are only a reducing gas and an inert gas.
[0068] The reducing gas may be, for example, hydrogen (H2) gas, deuterium (D2) gas, activated hydrogen-containing gas, etc. One or more of these may be used as the reducing gas.
[0069] Here, when H2 gas is used as the reducing gas, the H2 gas undergoes a substitution reaction with at least a part of the metal-containing layer formed on the wafer 200 in step S11. For example, when a gas containing a metal element and a carbonyl group is used as the metal-containing gas, O and the like in the metal-containing layer react with H2, are desorbed from the metal-containing layer, and are exhausted from the process chamber 201 as reaction by-products such as water vapor (H2O). Then, a metal-containing layer containing a metal element and having reduced O is formed on the wafer 200.
[0070] (Removal of residual gas, step S14) After the metal-containing layer is formed, the valve 324 is closed to stop the supply of the reducing gas. Then, by a process similar to that of step S12 described above, the reducing gas and reaction by-products remaining in the process chamber 201 that have not reacted or that have contributed to the formation of the metal-containing layer are removed from the process chamber 201. In other words, the process chamber 201 is purged.
[0071] (Performed a set number of times) By performing the cycle of steps S11 to S14 in sequence at least once (a first number of times (predetermined number of times) (n times)), a first metal-containing film 600a of a predetermined thickness is formed on the wafer (insulating film 400 on the surface and metal-containing film 300 in recess 400a, i.e., in recess 400a), as shown in FIG. 5(C). The above-mentioned cycle is preferably repeated multiple times. This makes it possible to form first metal-containing film 600a in which the amount of the surface oxide layer of metal-containing film 300 is reduced and the growth of the oxide layer at the interface is suppressed.
[0072] [Second metal-containing film forming step] (Metal-containing gas supply, step S21) The valve 314 is opened to allow the metal-containing gas to flow into the gas supply pipe 310. The metal-containing gas used in this step may be the same as the metal-containing gas used in the first metal-containing film forming process described above, or may be a different type of metal-containing gas. The metal-containing gas is adjusted in flow rate by the MFC 312, supplied into the processing chamber 201 from the gas supply hole 410a of the nozzle 410, and exhausted from the exhaust pipe 231. At this time, the metal-containing gas is supplied to the wafer 200. At the same time, the valve 514 is opened to allow the inert gas to flow into the gas supply pipe 510. The inert gas flowing through the gas supply pipe 510 is adjusted in flow rate by the MFC 512, supplied into the processing chamber 201 together with the metal-containing gas, and exhausted from the exhaust pipe 231. At this time, in order to prevent the metal-containing gas from entering the nozzles 420, 430, 440, the valves 524, 523, 544 are opened to allow the inert gas to flow into the gas supply pipes 520, 530, 540. The inert gas is supplied into the processing chamber 201 via the gas supply pipes 320, 330, 340 and the nozzles 420, 430, 440, and is exhausted from the exhaust pipe 231.
[0073] At this time, the APC valve 243 is adjusted to set the pressure inside the processing chamber 201 within a range of, for example, 1 to 3990 Pa. The supply flow rate of the metal-containing gas controlled by the MFC 312 is set within a range of, for example, 0.05 to 1 slm. The supply flow rates of the inert gases controlled by the MFCs 512, 522, 532, and 542 are each set within a range of, for example, 0.1 to 50 slm.
[0074] At this time, only the metal-containing gas and the inert gas are flowing in the processing chamber 201. That is, the metal-containing gas is supplied to the first metal-containing film 600a as shown in Fig. 5(C), and a metal-containing layer is formed on the wafer 200 (first metal-containing film 600a on the surface). The metal-containing layer may be a metal layer containing other elements, or an adsorption layer of the metal-containing gas.
[0075] (Removal of residual gas, step S22) After a predetermined time has elapsed, for example, 1 to 120 seconds, from the start of the supply of the metal-containing gas, the valve 314 of the gas supply pipe 310 is closed to stop the supply of the metal-containing gas. Then, by a process procedure similar to that of step S12 described above, the metal-containing gas and reaction by-products remaining in the process chamber 201 that have not reacted or that have contributed to the formation of the metal-containing layer are removed from the process chamber 201. In other words, the process chamber 201 is purged.
[0076] (Supply of reducing gas and oxygen-containing gas simultaneously, step S23) After removing the residual gas in the processing chamber 201, the valves 324 and 334 are opened to flow the reducing gas into the gas supply pipe 320 and a small amount of oxygen-containing gas into the gas supply pipe 330. The reducing gas used in the second metal-containing film forming process may be the same as the reducing gas used in the first metal-containing film forming process described above, or may be a different type of reducing gas. The reducing gas is adjusted in flow rate by the MFC 322, supplied from the gas supply hole 420a of the nozzle 420 into the processing chamber 201, and exhausted from the exhaust pipe 231. The oxygen-containing gas is adjusted in flow rate by the MFC 332, supplied from the gas supply hole 430a of the nozzle 430 into the processing chamber 201, and exhausted from the exhaust pipe 231. At this time, the reducing gas and the oxygen-containing gas are simultaneously supplied to the wafer 200. That is, the supply of the oxygen-containing gas is started at the same time as the supply of the reducing gas is started. At this time, valves 524 and 534 are opened at the same time to allow inert gas to flow into the gas supply pipes 520 and 530, respectively. The flow rate of the inert gas flowing through the gas supply pipes 520 and 530 is adjusted by the MFCs 522 and 532. The inert gas is supplied into the processing chamber 201 together with the reducing gas and the oxygen-containing gas, respectively, and is exhausted from the exhaust pipe 231. At this time, in order to prevent the intrusion of the reducing gas and the oxygen-containing gas into the nozzles 410 and 440, the valves 514 and 544 are opened to allow the inert gas to flow into the gas supply pipes 510 and 540. The inert gas is supplied into the processing chamber 201 through the gas supply pipes 310 and 340 and the nozzles 410 and 440, and is exhausted from the exhaust pipe 231.
[0077] At this time, the APC valve 243 is adjusted to set the pressure inside the processing chamber 201 to within a range of, for example, 1 to 13,000 Pa. The supply flow rate of the reducing gas controlled by the MFC 322 is set to within a range of, for example, 1 to 100 slm, preferably within a range of 5 to 50 slm. The supply flow rate of the oxygen-containing gas controlled by the MFC 332 is set to within a range of, for example, 0.01 to 10 slm, preferably within a range of 0.1 to 5 slm. The supply flow rates of the inert gases controlled by the MFCs 512, 522, 532, and 542 are each set to within a range of, for example, 0.1 to 50 slm.
[0078] At this time, the gases flowing into the processing chamber 201 are only the reducing gas, the oxygen-containing gas, and the inert gas. That is, the reducing gas and the oxygen-containing gas are supplied in parallel. The reducing gas and the oxygen-containing gas decompose the metal-containing gas and undergo a substitution reaction with at least a part of the first metal-containing film 600a formed on the wafer 200.
[0079] Here, by starting the supply of the oxygen-containing gas at the same time as starting the supply of the reducing gas, the decomposition effect of the metal-containing gas can be enhanced. That is, by performing this step, the organic ligand in the metal-containing gas can be removed. In addition, by stopping the supply of the oxygen-containing gas at the same time as stopping the supply of the reducing gas, it becomes possible to reduce and exhaust the oxygen atoms with the reducing gas, and the oxidation of the metal-containing film 300 can be suppressed. In addition, by supplying the oxygen-containing gas and the reducing gas in parallel, it is possible to obtain the effects of both decomposing the metal-containing gas and suppressing the oxidation of the metal-containing film.
[0080] The oxygen-containing gas is a gas containing oxygen (O) atoms, such as oxygen (O2) gas, ozone (O3) gas, plasma-excited O2 (O2 * ) gas, O2 gas + hydrogen (H2) gas, water vapor (H2O gas), hydrogen peroxide (H2O2) gas, nitrous oxide (N2O) gas, nitric oxide (NO) gas, nitrogen dioxide (NO2) gas, carbon monoxide (CO) gas, carbon dioxide (CO2) gas, etc. One or more of these can be used as the oxygen-containing gas.
[0081] For example, when a gas containing a metal element and a carbonyl group is used as the metal-containing gas, H2 gas is used as the reducing gas, and O2 gas is used as the oxygen-containing gas, the organic ligand in the first metal-containing film 600a reacts with H2 and O2, is desorbed from the first metal-containing film 600a, and is exhausted from the process chamber 201 as a reaction by-product such as water vapor (H2O). Then, a metal-containing layer containing a metal element and substantially no impurities is formed on the wafer 200.
[0082] (Removal of residual gas, step S24) Next, the valves 324 and 334 are closed to simultaneously stop the supply of the reducing gas and the oxygen-containing gas. That is, the timing of stopping the supply of the reducing gas and the supply of the oxygen-containing gas are set to be the same. By stopping the supply of the reducing gas and the supply of the oxygen-containing gas at the same time in this manner, it becomes possible to reduce and exhaust the oxygen atoms by the reducing gas, and it is possible to suppress the oxidation of the first metal-containing film 600a. Then, by a process procedure similar to that of step S12 described above, the reducing gas, the oxygen-containing gas, and the reaction by-products remaining in the process chamber 201 that have not reacted or that have contributed to the formation of the metal-containing layer are removed from the process chamber 201. That is, the process chamber 201 is purged.
[0083] (Performed a set number of times) That is, after the above-described first metal-containing film formation process, a cycle of sequentially performing steps S21 to S24 is performed at least once (second number (m times)), so that a second metal-containing film 600b of a predetermined thickness is formed on first metal-containing film 600a formed on wafer 200, as shown in FIG. 5(D), and the film is modified to metal-containing film 600. That is, as shown in FIG. 5(E), metal-containing film 600 can be formed on metal-containing film 300. The above-described cycle is preferably repeated multiple times.
[0084] (After purging and atmospheric pressure recovery) An inert gas is supplied into the processing chamber 201 from each of the gas supply pipes 510 to 540, and exhausted from the exhaust pipe 231. The inert gas acts as a purge gas, and the processing chamber 201 is purged with the inert gas, and residual gas and reaction by-products in the processing chamber 201 are removed from the processing chamber 201 (after-purge). Thereafter, the atmosphere in the processing chamber 201 is replaced with the inert gas (inert gas replacement), and the pressure in the processing chamber 201 is returned to normal pressure (return to atmospheric pressure).
[0085] (Wafer removal) Thereafter, the seal cap 219 is lowered by the boat elevator 115 to open the lower end of the outer tube 203. Then, the processed wafers 200 supported by the boat 217 are unloaded from the lower end of the outer tube 203 to the outside of the outer tube 203 (boat unloading). Thereafter, the processed wafers 200 are removed from the boat 217 (wafer discharging).
[0086] That is, in the substrate processing step of the present disclosure, a first metal-containing film 600a in which the growth of an oxidized layer at the interface on the metal-containing film 300 is suppressed is formed on the wafer 200 having the metal-containing film 300 formed on the surface thereof by the first metal-containing film formation step. Then, a second metal-containing film 600b in which impurities such as organic ligands in the first metal-containing film 600a are reduced is formed by continuously performing the second metal-containing film formation step thereafter. This makes it possible to form a metal-containing film 600 in which impurities in the film are removed while suppressing oxidation of the metal-containing film 300 on the metal-containing film 300 serving as the base film.
[0087] (3) Effects of this embodiment According to this embodiment, one or more of the following effects can be obtained. (a) By the first metal-containing film formation step, a metal-containing film in which the growth of an oxide layer at the interface on metal-containing film 300 is suppressed can be formed. (b) The second metal-containing film formation step can remove organic ligands in the metal-containing gas, and the metal-containing film can be formed with reduced impurities by promoting the decomposition of the metal-containing gas. In addition, the film formation speed can be improved by promoting the decomposition of the metal-containing gas, and the productivity can be improved. (c) Then, by optimizing the number of cycles in the first metal-containing film-forming step (thickness of first metal-containing film 600a) and the number of cycles in the second metal-containing film-forming step (thickness of second metal-containing film 600b), it is possible to form metal-containing film 600 in which both the inhibition of an oxidation layer and the reduction of impurities in the film are improved. (d) Furthermore, by performing a pretreatment step before the film formation step, the contact resistance between metal-containing film 300 and metal-containing film 600 embedded in recess 400a can be reduced.
[0088] (4) Other embodiments The above describes the embodiments of the present disclosure in detail. However, the present disclosure is not limited to the above-described embodiments, and various modifications are possible without departing from the spirit of the present disclosure. In the following modifications, only the differences from the above-described embodiments will be described in detail.
[0089] (Variation 1) FIG. 6 is a diagram showing a modification of the substrate processing process shown in FIG.
[0090] In this modification, the substrate processing step and the second metal-containing film forming step are different. That is, in this modification, the timing of starting the supply of the reducing gas in step S23 of the second metal-containing film forming step is made different from the timing of starting the supply of the oxygen-containing gas, and further, the timing of ending the supply of the reducing gas is made different from the timing of ending the supply of the oxygen-containing gas. Specifically, the supply of the oxygen-containing gas is started after the supply of the reducing gas is started, and the supply of the reducing gas is stopped after the supply of the oxygen-containing gas is stopped. That is, there is a timing for supplying the oxygen-containing gas and the reducing gas in parallel. And, the pressure in the processing chamber 201 at the timing of supplying the oxygen-containing gas and the reducing gas in parallel is made higher than the pressure in the processing chamber 201 at the timing of supplying only the reducing gas without supplying them in parallel.
[0091] In this manner, by supplying the reducing gas before the oxygen-containing gas, oxidation of the metal-containing film 300 is suppressed. Furthermore, by stopping the supply of the reducing gas after stopping the supply of the oxygen-containing gas, it is possible to suppress oxygen atoms from remaining in the processing chamber 201. Furthermore, by having a timing for supplying the oxygen-containing gas and the reducing gas in parallel, it is possible to obtain both the effects of decomposing the metal-containing gas and suppressing the oxidation of the metal-containing film. Furthermore, even in this case, the same effects as those of the substrate processing process shown in FIG. 4 described above can be obtained.
[0092] (Variation 2) FIG. 7 is a diagram showing a modification of the substrate processing process shown in FIG.
[0093] In this modification, the substrate processing step and the second metal-containing film forming step are different. That is, in this modification, the timing of starting the supply of the reducing gas in step S23 of the second metal-containing film forming step is made different from the timing of starting the supply of the oxygen-containing gas. Specifically, the supply of the reducing gas is started after the supply of the reducing gas is started, and the supply of the reducing gas is stopped at the same time as the supply of the oxygen-containing gas is stopped. That is, there is a timing for supplying the oxygen-containing gas and the reducing gas in parallel. And, the pressure in the processing chamber 201 at the timing of supplying the oxygen-containing gas and the reducing gas in parallel is made higher than the pressure in the processing chamber 201 at the timing of supplying only the reducing gas without supplying them in parallel.
[0094] In this way, by supplying the reducing gas before the oxygen-containing gas, oxidation of the metal-containing film 300 is suppressed. Furthermore, by stopping the supply of the oxygen-containing gas at the same time as stopping the supply of the reducing gas, it becomes possible to reduce and exhaust oxygen atoms with the reducing gas, and oxidation of the metal-containing film 300 can be suppressed. Furthermore, by having a timing for supplying the oxygen-containing gas and the reducing gas in parallel, it is possible to obtain both effects of decomposing the metal-containing gas and suppressing oxidation of the metal-containing film. Furthermore, even in this case, the same effects as those of the substrate processing process shown in FIG. 4 described above can be obtained.
[0095] (Variation 3) FIG. 8 is a diagram showing a modification of the substrate processing process shown in FIG.
[0096] In this modification, the second metal-containing film forming process is different from the substrate processing process described above. That is, in this modification, the supply of the oxygen-containing gas is started at the same time as the supply of the reducing gas is started in step S23 of the second metal-containing film forming process described above, and the timing of the end of the supply of the reducing gas is made different from the timing of the end of the supply of the oxygen-containing gas. That is, the supply of the oxygen-containing gas is started at the same time as the supply of the reducing gas is started, and the supply of the reducing gas is stopped after the supply of the oxygen-containing gas is stopped. That is, there is a timing for supplying the oxygen-containing gas and the reducing gas in parallel. And, the pressure in the process chamber 201 at the timing of supplying the oxygen-containing gas and the reducing gas in parallel is made higher than the pressure in the process chamber 201 at the timing of supplying only the reducing gas without supplying them in parallel.
[0097] In this way, by starting the supply of the oxygen-containing gas at the same time as starting the supply of the reducing gas, the decomposition effect of the metal-containing gas can be enhanced. In addition, by stopping the supply of the reducing gas after stopping the supply of the oxygen-containing gas, it is possible to suppress oxygen atoms from remaining in the processing chamber 201. In addition, by having a timing for supplying the oxygen-containing gas and the reducing gas in parallel, it is possible to obtain both the effects of decomposing the metal-containing gas and suppressing the oxidation of the metal-containing film. Furthermore, even in this case, the same effects as those of the substrate processing process shown in FIG. 4 described above can be obtained.
[0098] (Variation 4) FIG. 9 is a diagram showing a modification of the substrate processing process shown in FIG.
[0099] In this modification, the substrate processing step and the second metal-containing film forming step are different. That is, in this modification, the timing of starting the supply of the reducing gas in step S23 of the second metal-containing film forming step is made different from the timing of starting the supply of the oxygen-containing gas, and further, the timing of ending the supply of the reducing gas is made different from the timing of ending the supply of the oxygen-containing gas. Specifically, the supply of the oxygen-containing gas is started after the supply of the reducing gas is started, and the supply of the oxygen-containing gas is stopped after the supply of the reducing gas is stopped. That is, there is a timing for supplying the oxygen-containing gas and the reducing gas in parallel. And, the pressure in the processing chamber 201 at the timing of supplying the oxygen-containing gas and the reducing gas in parallel is made higher than the pressure in the processing chamber 201 at the timing of supplying only the reducing gas or only the oxygen-containing gas without supplying them in parallel.
[0100] In this way, by supplying the reducing gas before the oxygen-containing gas, oxidation of the metal-containing film 300 is suppressed. In addition, by stopping the supply of the oxygen-containing gas after stopping the supply of the reducing gas, a metal-containing film having an oxide film formed on the surface can be formed. In addition, by having a timing for supplying the oxygen-containing gas and the reducing gas in parallel, it is possible to obtain both effects of decomposing the metal-containing gas and suppressing oxidation of the metal-containing film. Furthermore, even in this case, the same effects as those of the substrate processing process shown in FIG. 4 described above can be obtained.
[0101] (Variation 5) FIG. 10 is a diagram showing a modification of the substrate processing process shown in FIG.
[0102] In this modification, the second metal-containing film forming process is different from the substrate processing process described above. That is, in this modification, the timing of starting the supply of the reducing gas in step S23 of the second metal-containing film forming process is made different from the timing of starting the supply of the oxygen-containing gas, and further, the timing of ending the supply of the reducing gas is made different from the timing of ending the supply of the oxygen-containing gas. Specifically, the supply of the reducing gas is started after the supply of the oxygen-containing gas is started, and the supply of the reducing gas is stopped after the supply of the oxygen-containing gas is stopped. That is, there is a timing for supplying the oxygen-containing gas and the reducing gas in parallel. And, the pressure in the process chamber 201 at the timing of supplying the oxygen-containing gas and the reducing gas in parallel is made higher than the pressure in the process chamber 201 at the timing of supplying only the reducing gas or only the oxygen-containing gas without supplying them in parallel.
[0103] In this way, by supplying the oxygen-containing gas before the reducing gas, the decomposition effect of the metal-containing gas can be enhanced. In addition, by stopping the supply of the reducing gas after stopping the supply of the oxygen-containing gas, it is possible to suppress oxygen atoms from remaining in the processing chamber 201. In addition, by having a timing for supplying the oxygen-containing gas and the reducing gas in parallel, it is possible to obtain both the effects of decomposing the metal-containing gas and suppressing the oxidation of the metal-containing film. Furthermore, even in this case, the same effects as those of the substrate processing process shown in FIG. 4 described above can be obtained.
[0104] (Variation 6) FIG. 11 is a diagram showing a modification of the substrate processing process shown in FIG.
[0105] In this modification, the order of gas supply in the above-mentioned substrate processing step and the first metal-containing film formation step is different. That is, the first metal-containing film formation step starts with the supply of reducing gas in the above-mentioned step S13. That is, the supply of reducing gas in step S13 is performed before the supply of metal-containing gas in step S11.
[0106] After the pretreatment process, there is a possibility that a halogen-containing gas is adsorbed onto the wafer 200. As in this modification, by starting the first metal-containing film formation process with the supply of a reducing gas after the pretreatment process, it is possible to remove the halogen element adsorbed onto the wafer 200. For example, when a gas containing Cl is used as the halogen-containing gas and H2 gas is used as the reducing gas, the H2 gas reacts with Cl adsorbed onto the wafer 200, desorbs Cl from the wafer 200, and is discharged from the processing chamber 201 as reaction by-products such as hydrogen chloride (HCl) and chlorine (Cl2).
[0107] In addition, when H-containing gas is used as the reducing gas, the surface of the metal-containing film 300 can be terminated with H by starting the supply of the reducing gas after the pretreatment process, and the oxidation of the metal-containing film 300 can be suppressed. This is also effective when the pretreatment process is not performed. Specifically, when H2 gas is used as the reducing gas, H2 gas reacts with O adsorbed on the wafer 200, desorbs O from the wafer 200, and is discharged from the processing chamber 201 as a reaction by-product such as water vapor (H2O), and the O adsorbed on the wafer 200 can be removed, and the oxidation of the metal-containing film 300 as the base film can be suppressed. Furthermore, even in this case, the same effect as that of the substrate processing process shown in FIG. 4 described above can be obtained.
[0108] (Variation 7) FIG. 12 is a diagram showing a modification of the substrate processing process shown in FIG.
[0109] In this modification, the pretreatment process is different from the substrate processing process shown in Fig. 4 described above. In the pretreatment process in this modification, the supply of a halogen-containing gas in step S1 and the removal (exhaust) of residual gas in step S2 are repeated a predetermined number of times. That is, a cyclic process is performed. This provides the same effects as the substrate processing process shown in Fig. 4 described above, while suppressing the residue of reaction by-products and facilitating the discharge of reaction by-products.
[0110] (Variation 8) FIG. 13 is a diagram showing a modification of the substrate processing process shown in FIG.
[0111] In this modification, between the first metal-containing film formation process and the second metal-containing film formation process shown in Fig. 4 described above, a process of supplying an inert gas as a purge gas into the processing chamber 201 and a process of exhausting the atmosphere in the processing chamber 201 are repeated a predetermined number of times. This provides the same effects as the substrate processing process shown in Fig. 4 described above, while suppressing the residue of reaction by-products and facilitating the discharge of the reaction by-products.
[0112] In the above embodiment, an example has been described in which a predetermined film is formed on the wafer 200, but the present disclosure is not particularly limited to the type of film.
[0113] In addition, in the above embodiment, an example of film formation using a substrate processing apparatus that is a batch-type vertical apparatus that processes multiple substrates at a time has been described, but the present disclosure is not limited to this and can also be suitably applied to film formation using a single-wafer type substrate processing apparatus that processes one or several substrates at a time.
[0114] It is preferable that the recipes (programs describing the processing procedure, processing conditions, etc.) used in the substrate processing are individually prepared according to the processing contents (film type, composition ratio, film quality, film thickness, processing procedure, processing conditions, etc. of the film to be formed) and stored in the storage device 121c via an electric communication line or an external storage device 123. Then, when starting the substrate processing, it is preferable that the CPU 121a appropriately selects an appropriate recipe according to the processing contents from among the multiple recipes stored in the storage device 121c. This makes it possible to form films of various film types, composition ratios, film qualities, and film thicknesses with good reproducibility using one substrate processing device. In addition, it is possible to reduce the burden on the operator (such as the burden of inputting the processing procedure, processing conditions, etc.), and to promptly start the substrate processing while avoiding operational errors.
[0115] The above-mentioned process recipe may not only be created anew, but may also be prepared by modifying an existing recipe already installed in the substrate processing apparatus. When modifying a recipe, the modified recipe may be installed in the substrate processing apparatus via an electric communication line or a recording medium on which the recipe is recorded. Also, an existing recipe already installed in the substrate processing apparatus may be directly modified by operating the input / output device 122 provided in the existing substrate processing apparatus. [Explanation of symbols]
[0116] 10 Substrate processing equipment 121 Controller 200 wafers (substrates) 201 Processing Room
Claims
1. (a) supplying a metal-containing gas containing a metal element to a substrate on which a metal-containing film has been formed; (b) supplying a reducing gas to the substrate; (c) supplying an oxygen-containing gas containing oxygen atoms and the reducing gas to the substrate; (d) repeating a cycle comprising (a) and (b) a first number of times; (e) after (d), repeating the cycle comprising (a) and (c) a second number of times; (d) increasing the partial pressure of the reducing gas in (b) to be higher than the partial pressure of the reducing gas in (c) in (e); A substrate processing method comprising the steps of:
2. 2. The substrate processing method according to claim 1, wherein in (c), a timing at which the supply of the reducing gas is started is made to differ from a timing at which the supply of the oxygen-containing gas is started.
3. 3. The substrate processing method according to claim 1, wherein in (c), the supply of the oxygen-containing gas is started after or simultaneously with the start of the supply of the reducing gas.
4. 3. The substrate processing method according to claim 1, wherein in (c), the supply of the reducing gas is started after the supply of the oxygen-containing gas is started.
5. 5. The substrate processing method according to claim 1, wherein in (c), a timing for terminating the supply of the reducing gas and a timing for terminating the supply of the oxygen-containing gas are differentiated from each other.
6. 6. The substrate processing method according to claim 1, wherein in (c), the supply of the reducing gas is stopped after or simultaneously with the supply of the oxygen-containing gas is stopped.
7. 7. The substrate processing method according to claim 1, wherein in (c), the supply of the oxygen-containing gas is stopped after the supply of the reducing gas is stopped.
8. 8. The substrate processing method according to claim 1, wherein in (c), the oxygen-containing gas and the reducing gas are supplied in parallel at a timing.
9. The pressure in the space in which the substrate is present in (b) is adjusted in (d), 9. The method of claim 1, wherein the pressure in step (e) is set to be higher than the pressure in the space in which the substrate exists in step (c).
10. 10. The substrate processing method according to claim 1, wherein in (b) performed in (d), at least one of the pressure of the space in which the substrate is present and the partial pressure of the reducing gas is changed for each of the first number of times.
11. The method of claim 1 , wherein in (d), starting with (b),
12. an oxide film is formed on the metal-containing film; (f) before (d), supplying a halogen-containing gas containing a halogen element to the substrate to remove at least a portion of the oxide film. The substrate processing method according to claim 1 .
13. 13. The substrate processing method according to claim 12, wherein in (f), the supply of the halogen-containing gas and the evacuation of the space in which the substrate exists are repeated.
14. 14. The substrate processing method according to claim 12, wherein the halogen element contained in the halogen-containing gas is chlorine.
15. 15. The substrate processing method according to claim 12, wherein the halogen-containing gas further contains oxygen.
16. The halogen-containing gas is POCl 3 , SOCl 2 , COCl 2 16. The method for processing a substrate according to claim 12, wherein the gas contains at least one of the following:
17. The substrate processing method according to claim 1 , wherein the metal-containing gas is a gas containing a carbonyl group.
18. (a) supplying a metal-containing gas containing a metal element to a substrate on which a metal-containing film has been formed; (b) supplying a reducing gas to the substrate; (c) supplying an oxygen-containing gas containing oxygen atoms and the reducing gas to the substrate; (d) repeating a cycle comprising (a) and (b) a first number of times; (e) after (d), repeating the cycle comprising (a) and (c) a second number of times; (d) increasing the partial pressure of the reducing gas in (b) to be higher than the partial pressure of the reducing gas in (c) in (e); A method for manufacturing a semiconductor device having the above structure.
19. A processing vessel; a metal-containing gas supply system for supplying a metal-containing gas containing a metal element into the processing vessel; a reducing gas supply system for supplying a reducing gas into the processing vessel; an oxygen-containing gas supply system for supplying an oxygen-containing gas containing oxygen atoms into the processing vessel; (a) supplying the metal-containing gas to a substrate on which a metal-containing film is formed in the processing vessel; (b) supplying the reducing gas to the substrate; (c) supplying the oxygen-containing gas and the reducing gas to the substrate; (d) repeating a cycle including (a) and (b) a first number of times; (e) after (d), repeating the cycle including (a) and (c) a second number of times; (d) a process of increasing the partial pressure of the reducing gas in (b) to be higher than the partial pressure of the reducing gas in (c) in (e); a control unit configured to be able to control the metal-containing gas supply system, the reducing gas supply system, and the oxygen-containing gas supply system so as to perform the above-mentioned steps; A substrate processing apparatus comprising:
20. (a) supplying a metal-containing gas containing a metal element to a substrate on which a metal-containing film has been formed; (b) supplying a reducing gas to the substrate; (c) supplying an oxygen-containing gas containing oxygen atoms and the reducing gas to the substrate; (d) repeating a cycle comprising (a) and (b) a first number of times; (e) after (d), repeating the cycle comprising (a) and (c) a second number of times; (d) making the partial pressure of the reducing gas in (b) higher than the partial pressure of the reducing gas in (c) in (e); A program for causing a computer to execute the above in a substrate processing apparatus.
Citation Information
Patent Citations
Method for producing noble metal electrode and process for fabricating semiconductor capacitor
JP2006060231A
Surface treatment method and treatment system
JP2020059916A
Deposition of ruthenium layers in interconnect metallization.
JP2020522618A
Methods for depositing tungsten or molybdenum films
US20200115798A1
Process for production of semiconductor device and apparatus for treatment of substrate
WO2006134930A1