Nonaqueous electrolyte for lithium secondary battery and lithium secondary battery including same

A non-aqueous electrolyte with a compound represented by Chemical Formula 1 and a nitrile solvent addresses the performance deterioration in lithium secondary batteries by improving electrolyte impregnation and safety, thus enhancing battery stability and output characteristics.

JP7562214B2Active Publication Date: 2024-10-07LG ENERGY SOLUTION LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023518306
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-13
Filing Date
2021-10-13
Publication Date
2024-10-07
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

Existing lithium secondary batteries face issues with performance deterioration due to the use of high concentrations of lithium salt, leading to increased viscosity and surface tension, which affects the impregnation of electrolytes into electrodes and separation membranes, resulting in longer activation times and reduced output characteristics.

Method used

A non-aqueous electrolyte comprising a compound represented by Chemical Formula 1, a nitrile solvent, and a lithium salt, with specific ratios to maintain low viscosity and surface tension, enhancing electrolyte impregnation and ionic conductivity.

Benefits of technology

The solution improves electrolyte impregnation into electrodes and separation membranes, reduces activation times, and enhances the safety and stability of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562214000017
    Figure 0007562214000017
  • Figure 0007562214000018
    Figure 0007562214000018
  • Figure 0007562214000019
    Figure 0007562214000019
Patent Text Reader

Abstract

The present invention relates to a non-aqueous electrolyte for a lithium secondary battery, which comprises a compound represented by Chemical Formula 1; an organic solvent containing a nitrile-based solvent in a content of 90 vol % to 100 vol %; and a lithium salt, wherein the content of the compound represented by Chemical Formula 1 is 2 wt % to 50 wt % relative to the total weight of the non-aqueous electrolyte, and to a lithium secondary battery containing the non-aqueous electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2020-0132055, filed with the Korean Intellectual Property Office on October 13, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a non-aqueous electrolyte for a lithium secondary battery and a lithium secondary battery including the same. [Background technology]

[0003] Lithium secondary batteries are generally manufactured by forming an electrode assembly by providing a separator between a positive electrode including a positive electrode active material made of a lithium-containing transition metal oxide and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte as a medium for transferring lithium ions, and then sealing the battery case.

[0004] Such lithium secondary batteries are used in portable electronic devices such as mobile phones and notebook computers as well as electric vehicles, and the demand for them is rapidly increasing. As the demand for lithium secondary batteries increases and their applications become more diverse, the performance level required for lithium secondary batteries is gradually increasing. For example, lithium secondary batteries used in electric vehicles are required to have improved output characteristics.

[0005] The output characteristic of a battery is a measure of how much current can be passed at a given voltage. Generally, when the current increases, the output obtained from the battery increases initially and then decreases after reaching a maximum value. This is related to the polarization phenomenon, and when the current increases beyond a certain value, the voltage of the battery decreases, and the capacity obtained within a given voltage range also decreases. This polarization phenomenon is related to the diffusion rate of lithium ions and the internal resistance of the battery, so in order to improve the output characteristic of the battery, it is necessary to improve the diffusion rate of lithium ions and the electrical conductivity characteristics.

[0006] One method to improve the output characteristics of batteries is to increase the lithium ion transport number (Li + There is a proposal to increase the transference number and dissociation degree of lithium ions to improve the output characteristics of the battery, but in that case, there are problems such as a decrease in the electrolyte's affinity to the electrode and the separator, and an increase in viscosity and surface tension.

[0007] Therefore, there is a demand for the development of a lithium secondary battery that can overcome the above problems while still using a high-concentration lithium salt. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to solve the above problems, and provides a non-aqueous electrolyte for a lithium secondary battery and a lithium secondary battery including the same. [Means for solving the problem]

[0009] The present invention relates to a method for producing an organic solvent comprising: a compound represented by the following chemical formula 1; an organic solvent containing a nitrile-based solvent in an amount of 90 vol% to 100 vol%; and a lithium salt, The content of the compound represented by Chemical Formula 1 is 2 wt % to 50 wt % based on the total weight of the nonaqueous electrolyte.

[0010] [Chemical formula 1] R1-O-CH2-R2 In the above Chemical Formula 1, R1 and R2 are each an alkyl group having 1 to 8 carbon atoms substituted with one or more fluorine atoms.

[0011] The present invention also provides a lithium secondary battery comprising: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and the non-aqueous electrolyte for the lithium secondary battery. Effect of the Invention

[0012] The non-aqueous electrolyte for a lithium ion battery according to the present invention can improve the output characteristics by improving the problem of performance degradation caused by the use of a high-concentration lithium salt.

[0013] In addition, the non-aqueous electrolyte has excellent impregnation properties for electrodes and separators and excellent flame retardancy, so that a lithium secondary battery including the non-aqueous electrolyte has the effect of shortening the activation process time and improving stability. [Brief description of the drawings]

[0014] [Figure 1] 1 shows photographs for evaluating the ignition of the non-aqueous electrolyte produced in Example 5. [Diagram 2] 1 shows the results of thermal safety evaluation of the lithium secondary battery produced in Example B-3. [Diagram 3] 1 shows the results of thermal safety evaluation of the lithium secondary battery produced in Example B-5. [Figure 4] 1 shows the results of thermal safety evaluation of the lithium secondary battery produced in Comparative Example B-5. [Diagram 5] 1 shows voltage-capacity curves during the formation process of lithium secondary batteries produced in Examples A-1 to A-3 and Comparative Examples A-3 and A-6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will now be described in more detail.

[0016] In recent years, in order to improve the performance and safety of lithium secondary batteries, electrolytes with increased lithium salt concentrations or changed solvents have been developed, but such electrolytes have the disadvantage of being higher in viscosity and surface tension than electrolytes using commonly used carbonate-based solvents.

[0017] When the viscosity and surface tension of the electrolyte are increased, the impregnation of the electrodes containing polyolefin-based separators and PVdF binders, which are widely used in the industry, decreases, which leads to problems such as an increase in the activation process time during battery manufacturing and an increase in process costs due to the addition of a high-temperature aging step.

[0018] Therefore, the present inventors have found that by incorporating the compound represented by Chemical Formula 1 into a nitrile-based electrolyte, which has significantly improved safety, the viscosity of the electrolyte is reduced without changing the dissociation structure of the lithium salt in the electrolyte, thereby improving the ionic conductivity of the electrolyte, and the surface tension of the electrolyte is reduced, thereby significantly improving the impregnation of the electrodes and the separator. In addition, it has been confirmed that the introduction of a nitrile-based solvent has the effect of improving the safety of the cell compared to the existing carbonate-based solvent.

[0019] Nonaqueous electrolyte The non-aqueous electrolyte for a lithium secondary battery of the present invention comprises a compound represented by the following chemical formula 1; an organic solvent containing a nitrile-based solvent in an amount of 90 vol % to 100 vol %; and a lithium salt, The content of the compound represented by the above Chemical Formula 1 is 2% by weight to 50% by weight based on the total weight of the non-aqueous electrolyte.

[0020] [Chemical formula 1] R1-O-CH2-R2 In the above Chemical Formula 1, R1 and R2 are each an alkyl group having 1 to 8 carbon atoms substituted with one or more fluorine atoms.

[0021] (a) A compound represented by chemical formula 1 In one embodiment of the present invention, R1 in the above Chemical Formula 1 may be an alkyl group having 1 to 5 carbon atoms substituted with one or more fluorine atoms, and R2 may be an alkyl group having 2 to 6 carbon atoms substituted with one or more fluorine atoms.

[0022] Specifically, R1 may be an alkyl group having 2 or 3 carbon atoms substituted with one or more fluorines, and R2 may be an alkyl group having 3 to 5 carbon atoms substituted with one or more fluorines, and more specifically, R1 may be an ethyl group substituted with one or more fluorines, and R2 may be a butyl group substituted with one or more fluorines.

[0023] In one embodiment of the present invention, R1 is -(CF2) n CHF2, and R2 is -(CF2) m The formula may be CHF2, in which n is an integer of 1 to 4, and m is an integer of 2 to 5.

[0024] Specifically, the n is 1 or 2, and the m is an integer of 2 to 4, and more specifically, the n may be 1 and the m may be 3.

[0025] In one embodiment of the present invention, the ratio of carbon atoms and fluorine atoms contained in R1 and R2, respectively, may be 1:2.

[0026] In one embodiment of the present invention, the compound represented by the above Chemical Formula 1 may be 1H,1H,5H-octafluoropentyl 1,1,2,2-tetrafluoroethyl ether represented by the following Chemical Formula 1A.

[0027] [ka]

[0028] The content of the compound represented by the above chemical formula 1 may be 2 wt % to 50 wt %, preferably 3 wt % to 30 wt %, and more preferably 3 wt % to 10 wt %, relative to the total weight of the non-aqueous electrolyte.

[0029] If the content of the compound represented by Formula 1 is less than 2 wt%, the effect of reducing the viscosity and surface tension of the electrolyte is weak, so that the impregnation of the electrode and the separator is not improved. If the content exceeds 50 wt%, the concentration of the lithium salt is low, so that the ionic conductivity of the electrolyte is reduced, so that the charging speed and output characteristics may be reduced when applied to a battery.

[0030] (b) Compound represented by chemical formula 2 The non-aqueous electrolyte for a lithium secondary battery of the present invention may further contain a compound represented by the following Chemical Formula 2, which is a fluorine-based acrylate / methacrylate compound.

[0031] [ka] In the above Chemical Formula 2, R3 is hydrogen or an alkyl group having 1 to 5 carbon atoms; R4 is an alkyl group having 1 to 10 carbon atoms and substituted with one or more fluorine atoms.

[0032] When the compound represented by Formula 2 is contained in the non-aqueous electrolyte, the compound having a positive polarity acts as a surfactant to further improve the impregnation of the electrodes and the separator, and the safety of the battery is improved due to the interface stabilization effect and the polymer hardening reaction.

[0033] In one embodiment of the present invention, R3 may be hydrogen or a methyl group.

[0034] In one embodiment of the present invention, R4 is -(CH2) p (CF2) q CHF2, where p is an integer of 1 to 3, and q is an integer of 2 to 6.

[0035] In one embodiment of the present invention, the compound represented by the above Chemical Formula 2 may be represented by the following Chemical Formula 2A or Chemical Formula 2B.

[0036] [ka]

[0037] [ka]

[0038] The content of the compound represented by the above chemical formula 2 may be 0.1 wt % to 10 wt %, preferably 0.1 wt % to 5 wt %, and more preferably 0.1 wt % to 3 wt %, relative to the total weight of the non-aqueous electrolyte.

[0039] If the content of the compound represented by the above formula 2 is less than 0.1 wt %, the improving effect on the electrode and the separator is weak, and if it exceeds 10 wt %, the ion conductivity may decrease.

[0040] (c) Organic Solvent The organic solvent of the present invention contains a nitrile solvent as an essential component. Here, the nitrile solvent means an organic solvent containing a -C≡N functional group.

[0041] In one embodiment of the present invention, the nitrile-based solvent may be one or more selected from succinonitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, and is preferably succinonitrile.

[0042] Succinonitrile is most suitable as a solvent for the non-aqueous electrolyte of the present invention because it exists in a solid form at room temperature and has low volatility, which can greatly improve the safety of the electrolyte.

[0043] The content of the nitrile solvent may be 90 vol % to 100 vol %, and preferably 92 vol % to 100 vol %, relative to 100 vol % of the total organic solvents.

[0044] The organic solvent may be a nitrile-based solvent alone or may further contain a carbonate-based solvent. When the organic solvent is a nitrile-based solvent alone, the volatility of the electrolyte is reduced, thereby improving the safety of the battery. When the organic solvent further contains a carbonate-based solvent, the impregnation of the electrodes and the separator is improved, thereby realizing a battery with a high energy density and ensuring safety.

[0045] When the organic solvent contains a carbonate-based solvent, the volume ratio of the nitrile-based solvent to the carbonate-based solvent may be 90:10 to 97:3, preferably 90:10 to 93:7, and more preferably 90:10 to 92:8. When the weight ratio of the two solvents is within the above range, it is preferable in that the safety of the battery is ensured and corrosion of the current collector is suppressed.

[0046] The carbonate solvent may be a non-fluorinated cyclic carbonate solvent, a non-fluorinated chain carbonate solvent, a fluorinated cyclic carbonate solvent, a fluorinated chain carbonate solvent, or a mixture thereof.

[0047] The non-fluorinated cyclic carbonate solvent is a high-viscosity organic solvent having a high dielectric constant, and therefore can easily dissociate the lithium salt in the electrolyte. The non-fluorinated cyclic carbonate solvent may be one or more selected from ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and specifically may be ethylene carbonate and propylene carbonate.

[0048] The non-fluorinated chain carbonate solvent is an organic solvent having low viscosity and low dielectric constant, and may be one or more selected from dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and specifically may be dimethyl carbonate, diethyl carbonate, or ethyl methyl carbonate.

[0049] The fluorine-based cyclic carbonate solvent may be one or more selected from fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoroethylene carbonate, tetrafluoroethylene carbonate, 3,3,3-trifluoropropylene carbonate, and 1-fluoropropylene carbonate, and specifically may be fluoroethylene carbonate (FEC).

[0050] The fluorine-based chain carbonate solvent may be at least one selected from fluoromethyl methyl carbonate (FMMC) and fluoroethyl methyl carbonate (FEMC), and specifically may be fluoroethyl methyl carbonate (FEMC).

[0051] The remainder of the total weight of the nonaqueous electrolyte, excluding the organic solvent, such as the compound represented by Chemical Formula 1, the compound represented by Chemical Formula 2, the lithium salt, and other additives described below, may be an organic solvent, unless otherwise specified.

[0052] (d) Lithium salt The lithium salt can be any salt that is commonly used in electrolytes for lithium secondary batteries. For example, the cation is Li + Contains F as an anion - , Cl - , Br - , I- , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , BF2C2O4CHF - , PF4C2O4 - , PF2C4O8 - , PO2F2 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - and SCN - Lithium salts containing one or more selected from the following can be used.

[0053] Specifically, the lithium salts include LiPF6, LiClO4, LiBF4, LiFSI (Lithium bis(fluorosulfonyl)imide), LiN(SO2CF3)2 (LiTFSI), LiSO3CF3, LiPO2F2, lithium bis(oxalate)borate (LiBOB), lithium difluoro(oxalate)borate (LiDFOB), lithium difluoro(bisoxalato)phosphate (LiDFBP), lithium tetrafluoro(oxalate)phosphate (LiTFOP), and lithium fluoromalonato(difluoro)borate (LiTFOP). The compound may be one or more selected from LiFMDFB), and is preferably one or more selected from LiFSI and lithium difluoro(oxalato)borate.

[0054] In one embodiment of the present invention, the concentration of the lithium salt in the organic solution consisting of the organic solvent and the lithium salt may be 1.0M to 6.0M, preferably 1.3M to 6.0M, and preferably 1.3M to 2.4M.

[0055] If the concentration of the lithium salt is less than 1.0M, the effect of improving the low-temperature output and cycle characteristics of the lithium secondary battery is weak, and if the concentration exceeds 6.0M, the viscosity and surface tension of the non-aqueous electrolyte may increase excessively, resulting in a decrease in the impregnation of the electrolyte.

[0056] In addition, the non-aqueous electrolyte of the present invention contains a high concentration of lithium salt and a nitrile-based solvent as described above, and can maintain a viscosity of 5 cP to 15 cP. When a high concentration of lithium salt and a nitrile-based solvent are contained as described above, the viscosity generally becomes as high as 15 cP or more, but in the case of the present invention, since the compound represented by Chemical Formula 1 is contained and a high concentration of lithium salt and a nitrile-based solvent are used, the viscosity of 5 cP to 15 cP can be maintained.

[0057] (e) Other additives The nonaqueous electrolyte for a lithium secondary battery of the present invention may selectively contain an additive in the nonaqueous electrolyte as necessary in order to prevent the nonaqueous electrolyte from being decomposed in a high voltage environment, which may induce electrode collapse, and to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and battery expansion suppression effects at high temperatures.

[0058] The additive in the non-aqueous electrolyte may be at least one selected from a cyclic carbonate-based compound, a halogen-substituted carbonate-based compound, a sultone-based compound, a sulfate-based compound, a phosphate-based or phosphite-based compound, a borate-based compound, a nitrile-based compound, an amine-based compound, a silane-based compound, a benzene-based compound, and a lithium salt-based compound.

[0059] The cyclic carbonate compound may be at least one selected from vinylene carbonate (VC) and vinyl ethylene carbonate, specifically vinylene carbonate. When the cyclic carbonate compound is contained as an additive, the content of the cyclic carbonate compound may be less than 4% by weight, preferably 0.1% to 3% by weight, based on the total weight of the non-aqueous electrolyte.

[0060] The halogen-substituted carbonate compound may be fluoroethylene carbonate (FEC).

[0061] The sultone-based compound is a material capable of forming a stable SEI film on the surface of the negative electrode through a reduction reaction, and may be one or more compounds selected from 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone, and specifically, may be 1,3-propane sultone (PS).

[0062] The sulfate-based compound is a material capable of forming a stable SEI film that is not cracked even during high-temperature storage by being electrically decomposed on the surface of the negative electrode, and may be at least one selected from ethylene sulfate (Esa), trimethylene sulfate (TMS), and methyl trimethylene sulfate (MTMS).

[0063] The phosphate or phosphite compound may be one or more selected from lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tetramethyltrimethylsilylphosphate, trimethylsilylphosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.

[0064] The borate-based compound may be lithium tetraphenylborate.

[0065] The nitrile compound may be one or more selected from succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, and specifically, may be one or more selected from 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, and trifluorobenzonitrile containing a fluorine component.

[0066] The amine compound may be at least one selected from triethanolamine and ethylenediamine, and the silane compound may be tetravinylsilane.

[0067] The benzene-based compound may be at least one selected from monofluorobenzene, difluorobenzene, trifluorobenzene, and tetrafluorobenzene.

[0068] The lithium salt-based compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, and may be one or more compounds selected from LiPO2F2, LiBOB (lithium bis(oxalato)borate (LiB(C2O4)2), and lithium tetrafluoroborate (LiBF4).

[0069] On the other hand, the content of the additive may be 0.1% by weight to 10% by weight, preferably 1% by weight to 5% by weight, based on the total weight of the non-aqueous electrolyte. If the content of the additive is less than 0.1% by weight, the effect of improving the low-temperature capacity of the battery, as well as the high-temperature storage characteristics and high-temperature life characteristics is weak, and if the content of the additive is more than 10% by weight, excessive side reactions may occur in the electrolyte during charging and discharging of the battery. In particular, if the additive for forming the SEI film is added in an excessive amount, it may not be sufficiently decomposed at high temperatures, and may remain unreacted or precipitated in the electrolyte at room temperature. This may cause side reactions that reduce the life or resistance characteristics of the battery.

[0070] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.

[0071] The lithium secondary battery according to the present invention includes a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, where the non-aqueous electrolyte is the non-aqueous electrolyte for the lithium secondary battery according to the present invention. Since the non-aqueous electrolyte has been described above, a description thereof will be omitted and other components will be described below.

[0072] (a) Positive electrode The positive electrode may be prepared by coating a positive electrode current collector with a positive electrode mixture slurry including a positive electrode active material, a binder, a conductive material, and a solvent.

[0073] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like can be used.

[0074] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, including LCO (LiCoO2), LNO (LiNiO2), LMO (LiMnO2), LiMn2O4, LiCoPO4, LFP (LiFePO4), LiNiMnCoO2, and NMC (LiNiCoMnO2), etc., LiNi 1-x-y-z Co x M 1 y M 2 z O2 (M 1 and M 2 are each independently selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg, and Mo, and x, y, and z are each independently the atomic fraction of the oxide composition elements, where 0 ≦ x < 0.5, 0 ≦ y < 0.5, 0 ≦ z < 0.5, and x + y + z = 1), and one or more selected therefrom may be used.

[0075] Specifically, it may include a lithium metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium.

[0076] More specifically, the lithium metal oxide is a lithium-manganese-based oxide such as LiMnO2, LiMn2O4; a lithium-cobalt-based oxide such as LiCoO2; a lithium-nickel-based oxide such as LiNiO2; LiNi 1-Y Mn Y O2 (0 < Y < 1), LiMn 2-z Ni z O4 (0 < Z < 2), etc., lithium-nickel-manganese-based oxides; LiNi 1-Y1 Co Y1 O2 (0 < Y1 < 1), etc., lithium-nickel-cobalt-based oxides; LiCo 1-Y2 Mn Y2 O2 (0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (0 < Z1 < 2), etc., lithium-manganese-cobalt-based oxides; Li(Ni p Co q Mn r1)O2 (0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1), Li(Ni p1 Co q1 Mn r2 )O4 (0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc. lithium-nickel-manganese-cobalt oxides; and Li(Ni p2 Co q2 Mn r3 M S2 )O2 (M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, p2 + q2 + r3 + s2 = 1), etc. one or more selected from lithium-nickel-cobalt-transition metal (M) oxides may be used.

[0077] Among these, in terms of being able to enhance the capacity characteristics and stability of the battery, the lithium metal oxide is LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (for example, Li(Ni 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.); or lithium nickel cobalt aluminum oxide (for example, Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.) may be used. Considering the remarkable improvement effect by controlling the types and content ratios of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide is Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 ) O2.

[0078] The positive electrode active material may be contained in an amount of 60% to 99% by weight, preferably 70% to 99% by weight, and more preferably 80% to 98% by weight, based on the total weight of solid matters excluding the solvent in the positive electrode mixture slurry.

[0079] The binder is a component that assists in binding the active material and conductive material to the current collector.

[0080] Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof.

[0081] Generally, the binder may be contained in an amount of 1 wt % to 20 wt %, preferably 1 wt % to 15 wt %, and more preferably 1 wt % to 10 wt %, based on the total weight of solids excluding the solvent in the positive electrode mixture slurry.

[0082] The conductive material is a component for further improving the conductivity of the positive electrode active material.

[0083] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of conductive materials that can be used include graphite; carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0084] Generally, the conductive material may be contained in an amount of 1 wt % to 20 wt %, preferably 1 wt % to 15 wt %, and more preferably 1 wt % to 10 wt %, based on the total weight of solids excluding the solvent in the positive electrode mixture slurry.

[0085] The solvent may contain an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode active material and, optionally, a binder and a conductive material are contained. For example, the solvent may be contained so that the concentration of the solid content including the positive electrode active material and, optionally, a binder and a conductive material is 50% by weight to 95% by weight, preferably 50% by weight to 80% by weight, and more preferably 55% by weight to 70% by weight.

[0086] (b) Negative electrode The negative electrode may be prepared by, for example, coating a negative electrode current collector with a negative electrode mixture slurry containing a negative electrode active material, a binder, a conductive material, and a solvent, or a graphite electrode made of carbon (C) or a metal itself may be used as the negative electrode.

[0087] For example, when manufacturing a negative electrode by coating a negative electrode current collector with a negative electrode active material slurry, the negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, those with the surface of copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. Also, similar to the positive electrode current collector, fine irregularities can be formed on the surface to strengthen the bonding force of the negative electrode active material, and it can be used in various forms such as films, sheets, foils, nets, porous bodies, foams, non-woven bodies, etc.

[0088] The negative electrode active material of the present invention does not contain lithium metal. This is because when the nitrile-based solvent of the present invention comes into contact with lithium metal, a polymerization reaction occurs.

[0089] Also, the negative electrode active material of the present invention may be composed of one or more selected from carbon-based materials; silicon-based materials; one or more metals selected from Sn, Zn, Mg, Cd, Ce, Ni, and Fe; alloys composed of the above metals; oxides of the above metals; and composites of the above metals and carbon.

[0090] The carbon-based material may be one or more selected from crystalline carbon such as natural graphite and artificial graphite; and amorphous carbon such as soft carbon, hard carbon, mesophase pitch carbide, and fired coke.

[0091] The silicon-based material is Si, SiO x (0 < x < 2), alloys composed of Si and the above metals; and composites of Si and carbon.

[0092] The negative electrode active material may be contained in an amount of 60% to 99% by weight, preferably 70% to 99% by weight, and more preferably 80% to 98% by weight, based on the total weight of solid matters excluding the solvent in the negative electrode mixture slurry.

[0093] The binder is a component that helps to bond the conductive material, active material, and current collector together. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof.

[0094] Generally, the binder may be contained in an amount of 1 wt % to 20 wt %, preferably 1 wt % to 15 wt %, and more preferably 1 wt % to 10 wt %, based on the total weight of solids excluding the solvent in the negative electrode mixture slurry.

[0095] The conductive material is a component for further improving the conductivity of the negative electrode active material. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples thereof include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0096] The conductive material may be contained in an amount of 1 wt % to 20 wt %, preferably 1 wt % to 15 wt %, and more preferably 1 wt % to 10 wt %, based on the total weight of solid matter excluding the solvent in the negative electrode mixture slurry.

[0097] The solvent may contain water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the negative electrode active material and, optionally, a binder and a conductive material are contained. For example, the solvent may be contained so that the concentration of the solid content including the negative electrode active material and, optionally, a binder and a conductive material is 50% by weight to 95% by weight, preferably 70% by weight to 90% by weight.

[0098] When a metal is used as the negative electrode, the negative electrode may be manufactured by physically bonding, rolling, or depositing a metal on a metal thin film or the negative electrode current collector. The deposition method may be an electrochemical deposition method or a chemical vapor deposition method.

[0099] For example, the metal thin film itself or the metal bonded / rolled / deposited onto the negative electrode current collector may include one metal or an alloy of two metals selected from the group consisting of nickel (Ni), tin (Sn), copper (Cu) and indium (In).

[0100] (c) Separation membrane The lithium secondary battery according to the present invention includes a separator between the positive electrode and the negative electrode.

[0101] The separator separates the negative electrode and the positive electrode to provide a path for lithium ion migration. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, it is preferable that the separator has low resistance to the migration of electrolyte ions and is excellent in electrolyte impregnation ability.

[0102] Specifically, the separation membrane may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer; or a laminate structure of two or more layers thereof. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting point glass fiber, polyethylene terephthalate fiber, or the like, may be used. Furthermore, in order to ensure heat resistance or mechanical strength, a separation membrane containing or coated with a ceramic component or a polymer substance in the form of a film, fiber, or powder may be used, and may be used as a single layer or multilayer structure.

[0103] The lithium secondary battery according to the present invention is useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0104] Therefore, according to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0105] The battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, including power tools; electric vehicles (Electric Vehicles, EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); and power storage systems.

[0106] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0107] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery for a medium- to large-sized battery module including a plurality of battery cells.

[0108] The present invention will now be described in more detail with reference to specific examples. EXAMPLES

[0109] <Example: Manufacture of lithium secondary battery> (1) Production of non-aqueous electrolyte [Table 1]

[0110] A mixed organic solvent was prepared according to the composition in Table 1, and a lithium salt was mixed therewith to obtain the concentration in Table 1 to prepare an organic solution. A nonaqueous electrolyte for a lithium secondary battery was prepared by mixing the compound represented by Chemical Formula 1A (content in Table 1), the compound represented by Chemical Formula 2A or 2B (content in Table 1), 3 wt % vinylene carbonate, 0.5 wt % 1,3-propane sultone (PS), and the remaining organic solution with respect to 100 wt % of the nonaqueous electrolyte.

[0111] (2) Manufacturing of general loading electrodes N-methyl-2-pyrrolidone (NMP) is used as the positive electrode active material (LiNi 0.8 Co 0.1 Mn 0.1 A positive electrode slurry was prepared by adding O2 (NCM811), a conductive material (carbon black) and a binder (polyvinylidene fluoride) in a weight ratio of 96.8:1.0:2.2. The positive electrode slurry was applied to a thickness of 45 μm on an aluminum (Al) thin film, which is a positive electrode current collector, having a thickness of 20 μm, and dried. Then, a roll press was performed to obtain a loading capacity of 2.8 mAh / cm. 2 A positive electrode having the formula:

[0112] A negative electrode slurry was prepared by adding a negative electrode active material (graphite), a binder (SBR-CMC), and a conductive material (carbon black) in a weight ratio of 95.3:4.0:0.7 to water as a solvent. The negative electrode slurry was applied to a thickness of 67 μm on a copper (Cu) thin film as a negative electrode current collector having a thickness of 8 μm, dried, and then roll pressed to obtain a loading capacity of 3.0 mAh / cm. 2 A negative electrode having the formula:

[0113] (3) Manufacturing of high-loading electrodes N-methyl-2-pyrrolidone (NMP) is used as the positive electrode active material (LiNi 0.8 Co 0.1 Mn 0.1 A positive electrode slurry was prepared by adding O2 (NCM811), a conductive material (carbon black) and a binder (polyvinylidene fluoride) in a weight ratio of 96.8:1.0:2.2. The positive electrode slurry was applied to a thickness of 76 μm on an aluminum (Al) thin film, which is a positive electrode current collector, having a thickness of 20 μm, and dried. Then, a roll press was performed to obtain a loading capacity of 4.8 mAh / cm. 2 A positive electrode having the formula:

[0114] A negative electrode slurry was prepared by adding a negative electrode active material (graphite), a binder (SBR-CMC), and a conductive material (carbon black) in a weight ratio of 95.3:4.0:0.7 to water as a solvent. The negative electrode slurry was applied to a thickness of 107 μm on a copper (Cu) thin film as a negative electrode current collector having a thickness of 8 μm, dried, and then roll pressed to obtain a loading capacity of 5.2 mAh / cm. 2 A negative electrode having the formula:

[0115] (4) Manufacture of lithium secondary batteries (Manufacturing batteries using standard loading electrodes) The general loading positive electrode, a polyolefin-based porous separator coated with inorganic particles (Al2O3), and the general loading negative electrode were sequentially stacked to prepare an electrode assembly.

[0116] The assembled electrode assemblies were placed in a pouch-type battery case, and the non-aqueous electrolytes for the lithium secondary batteries of Examples 1 to 8 prepared in (1) were injected into the pouch-type battery case, respectively, to prepare lithium secondary batteries of Examples A-1 to A-8 using a general loading electrode.

[0117] (Manufacturing batteries using high loading electrodes) The lithium secondary batteries of Examples B-1 to B-8 were manufactured using high loading electrodes in the same manner as above, except that a high loading positive electrode was used instead of the normal loading positive electrode and a high loading negative electrode was used instead of the normal loading negative electrode.

[0118] <Comparative Example: Manufacture of Lithium Secondary Battery> (1) Production of non-aqueous electrolyte [Table 2] *MPPBFSI: 1-methyl-1-(3-methoxypropyl)pyrrolidinium bisfluorosulfonylimide

[0119] A mixed organic solvent was prepared according to the composition in Table 2, and a lithium salt was mixed therein to obtain the concentration in Table 2 to prepare an organic solution. A nonaqueous electrolyte for a lithium secondary battery was prepared by mixing the additive compound in Table 2, 3 wt% vinylene carbonate, 0.5 wt% 1,3-propane sultone (PS), and the remaining organic solution with respect to 100 wt% nonaqueous electrolyte.

[0120] (2) Manufacturing of general loading electrodes The positive and negative electrodes were manufactured in the same manner as in the manufacturing process of the general loading electrode of the above embodiment.

[0121] (3) Manufacturing of high-loading electrodes The positive and negative electrodes were manufactured in the same manner as in the manufacturing process of the high loading electrode of the above example.

[0122] (4) Manufacture of lithium secondary batteries (Manufacturing batteries using standard loading electrodes) The general loading positive electrode, a polyolefin-based porous separator coated with inorganic particles (Al2O3), and the general loading negative electrode were sequentially stacked to prepare an electrode assembly.

[0123] The assembled electrode assemblies were placed in a pouch-type battery case, and the non-aqueous electrolytes for the lithium secondary batteries of Comparative Examples 1 to 8 prepared in (1) were injected into the pouch-type battery case, respectively, to prepare lithium secondary batteries of Comparative Examples A-1 to A-8 using a general loading electrode.

[0124] (Manufacturing batteries using high loading electrodes) The lithium secondary batteries of Comparative Examples B-1 to B-8 were manufactured using high loading electrodes in the same manner as above, except that a high loading positive electrode was used instead of the normal loading positive electrode and a high loading negative electrode was used instead of the normal loading negative electrode.

[0125] <Experimental Example> Experimental Example 1: Evaluation of ionic conductivity of electrolyte The ionic conductivity of the nonaqueous electrolytes prepared in Examples 1 to 5, 7, and 8 and Comparative Examples 1 to 3 was measured at 25° C. using a METTLER TOLEDO Seven Excellence S700 device. Specifically, a bath was filled with the electrolytes of Examples 1 to 5, 7, and 8 and Comparative Examples 1 to 3 so that a probe for measuring ionic conductivity was immersed, and then the ionic conductivity was measured using the immersed probe. The measured ionic conductivity values ​​are shown in Table 3 below.

[0126] [Table 3]

[0127] From the results of Table 3, it is confirmed that the ionic conductivity of the nitrile-based electrolytes (Examples 1 to 5, 7, and 8) to which the additive of Formula 1A is added is higher than that of the nitrile-based electrolytes (Comparative Examples 1 and 3) to which the additive of Formula 1A is not added. Also, in the case of Comparative Example 2 in which an excessive amount (60 wt%) of the additive of Formula 1A is added, it is confirmed that the additive of Formula 1A is phase-separated and is difficult to use as an electrolyte.

[0128] Experimental Example 2: Evaluation of electrolyte impregnation into separation membrane The impregnation of the non-aqueous electrolytes into the separation membranes prepared in Examples 3 to 5, 7, and 8 and Comparative Examples 1, 3, and 5 to 8 was measured at 25°C using a 2032 coin cell with a diameter of 20 mm and a thickness of 3.2 mm. Specifically, a separation membrane made of polyethylene fabric coated on both sides with Al2O3 and PVdF was punched out to a diameter of 18 mm, and then impregnated with each electrolyte for 24 hours and inserted between the coin cells to assemble the cells. The assembled coin cell was subjected to measurement of AC impedance using an EIS device (biologic potentiostat) to measure the film ion conductivity of the electrolyte-impregnated separation membrane. The expression rate is calculated by dividing the film ion conductivity measured in this way by the ion conductivity of the electrolyte. The expression rate is an index showing how much the electrolyte is impregnated into the separation membrane, and a higher value indicates excellent electrolyte impregnation into the separation membrane. The measured expression rates are shown in Table 4 below.

[0129] [Table 4]

[0130] From the results of Table 4, it is confirmed that the expression rate of the nitrile-based electrolytes containing the additive of Chemical Formula 1A (Examples 3 to 5, 7, and 8) is higher than that of the nitrile-based electrolytes not containing the additive of Chemical Formula 1A (Comparative Examples 1 and 3). In particular, it is confirmed that the electrolyte using 100% nitrile-based solvent and not containing the additive of Chemical Formula 1A (Comparative Example 1) does not impregnate the separator at all.

[0131] However, it was confirmed from this experimental example that when the additive of Chemical Formula 1A was included, even if a 100% nitrile-based solvent was used (Example 3), it was possible to ensure a separator impregnation level higher than that of an electrolyte using a carbonate-based solvent (Comparative Example 5), which is mainly used in conventional lithium-ion batteries.

[0132] Also, when a pyrrolidinium compound is added to a carbonate-based solvent, it is confirmed that the impregnation property is reduced as in Comparative Example 6. Furthermore, in the cases of Comparative Examples 7 and 8, although a fluorine-based acrylate and methacrylate compound (Chemical Formula 2A or 2B) was used, Chemical Formula 1A was not used as an additive, so that the impregnation property was confirmed to be reduced.

[0133] Experimental Example 3: Evaluation of electrolyte impregnation into positive electrode The impregnation of the non-aqueous electrolytes prepared in Examples 1 to 5, 7, and 8 and Comparative Examples 1 and 3 into the positive electrode was measured using a contact angle measuring device (Drop shape analysis system, DSA100) at 25°C. Specifically, 5 μl of each non-aqueous electrolyte was dropped onto the surface of the high loading positive electrode, and the angle between the surface of the positive electrode and the electrolyte droplet was then measured. The contact angle is an index of the electrolyte's affinity for the positive electrode, and a lower value indicates excellent impregnation of the electrolyte into the positive electrode. The measured contact angles are shown in Table 5 below.

[0134] [Table 5]

[0135] From the results of Table 5, it is confirmed that the contact angle of the positive electrode of the nitrile-based electrolytes (Examples 1 to 5, 7, and 8) to which the additive of Chemical Formula 1A is added is lower than the contact angle of the nitrile-based electrolytes (Comparative Examples 1 and 3) that do not contain the additive of Chemical Formula 1A. In particular, it is confirmed that the impregnation of the positive electrode of Examples 7 and 8 containing fluorine-based acrylate and methacrylate compounds (Chemical Formula 2A or Chemical Formula 2B) is further improved. This confirms that when the compound represented by Chemical Formula 1 is added to the nitrile-based electrolyte, the impregnation of the positive electrode is improved, and when the compound represented by Chemical Formula 2 is added, the effect is further enhanced.

[0136] Experimental Example 4: Evaluation of the flame retardancy of electrolytes The flame retardancy of the electrolyte was evaluated by contacting the electrolyte with a flame. Specifically, 1 mL of the nonaqueous electrolytes prepared in Examples 1 to 8 and Comparative Examples 4 to 6 were placed in separate Petri dishes and exposed to a lighter flame for 3 seconds, after which the electrolyte was checked for ignition. The results of ignition are shown in Table 6, and photographs of the ignition evaluation process of Example 5 taken in chronological order are shown in FIG. 1.

[0137] [Table 6]

[0138] From the results in Table 6 above, it is confirmed that the electrolytes containing 90 volume % or more of a nitrile-based solvent (Examples 1 to 8) have flame retardancy, but the electrolytes containing less than 50 volume % of a nitrile-based solvent (Comparative Examples 4 to 6) do not have flame retardancy and may ignite.

[0139] In FIG. 1, it is visually confirmed that the electrolyte of Example 5 does not ignite when exposed to a flame.

[0140] Experimental Example 5: Evaluation of cell resistance The lithium secondary batteries of Examples A-1 to A-5, A-7, and A-8 and Comparative Examples A-1, A-3, A-6 to A-8 were stored in an oven at 25° C. for 24 hours for impregnation, and then the cell resistance was measured using a 1 kHz resistance tester (Hioki). The results are shown in Table 7 below.

[0141] [Table 7]

[0142] From the results of Table 7 above, it is confirmed that the cell resistance of Examples A-1 to A-5, A-7, and A-8, which include an electrolyte containing an additive of Chemical Formula 1A (Examples 1 to 5, 7, and 8), is lower than the cell resistance of Comparative Examples A-1, A-3, A-7, and A-8, which include an electrolyte not containing an additive of Chemical Formula 1A (Comparative Examples 1, 3, 7, and 8), and Comparative Example A-6, which does not use a nitrile-based solvent and further includes a pyrrolidinium additive (Comparative Example 6).

[0143] In particular, in the case of Comparative Examples A-1, A-7, and A-8, which contain 100 vol% nitrile-based solvent and the electrolytes of Comparative Examples 1, 7, and 8, which do not contain the additive of Chemical Formula 1A, the cell resistance is so high that it is impossible to measure, and it is therefore impossible to operate the cell. This shows that when a nitrile-based solvent is used, the use of the compound represented by Chemical Formula 1 has a significant effect on reducing the cell resistance.

[0144] Experimental Example 6: Evaluation of the thermal stability of cells The lithium secondary batteries of Examples B-3, B-5 ​​and Comparative Example B-5 were each charged to SOC 30% at 25°C at 0.1C for 3 hours to perform a formation process, then aged for 24 hours, and then degassed. The lithium secondary batteries after degassing were charged to 4.2V at 0.1C at 25°C under CC-CV (constant current-constant voltage) conditions, and discharged to 3.0V at 0.1C under CC conditions. The above charge and discharge were counted as one cycle, and two cycles of initial charge and discharge were performed.

[0145] The thermal safety of the cells was evaluated by charging each of the initially charged and discharged lithium secondary batteries under CC-CV conditions at a rate of 0.1 C to 4.2 V, placing them in a high-temperature heat exposure chamber, heating them to 120° C. at a rate of 2° C. / min and holding them for 2 hours, and then heating them again to 150° C. at a rate of 2° C. / min and holding them for 2 hours.

[0146] The evaluation results of Example B-3 are shown in FIG. 2, the evaluation results of Example B-5 in FIG. 3, and the evaluation results of Comparative Example B-5 in FIG.

[0147] [Table 8]

[0148] 2, 3 and 4, it is confirmed that, even if the content of Chemical Formula 1A is the same, safety at high temperatures is improved compared to when a nitrile-based solvent is used (Example B-3) and when a carbonate-based solvent is used (Comparative Example B-5). In addition, it is confirmed that, even when mixed with a carbonate-based solvent, when the content of the nitrile-based solvent is 50 vol% or more, excellent high-temperature safety can be ensured as seen in Example B-5.

[0149] Experimental Example 7: Evaluation of life characteristics (general loading electrode) The lithium secondary batteries of Examples A-1 to A-3 and Comparative Examples A-3 and A-6 were each charged at 25°C at 0.1C for 3 hours to SOC 30% to carry out a formation process, then aged for 24 hours, and then degassed. The lithium secondary batteries after degassing were charged at 25°C at 0.1C to 4.2V under CC-CV (constant current-constant voltage) conditions, and discharged at 0.1C to 3.0V under CC conditions. The above charge and discharge constitute one cycle, and two cycles of initial charge and discharge were carried out.

[0150] Next, each of the initially charged and discharged lithium secondary batteries was charged under CC-CV conditions at a rate of 0.1 C to 4.2 V, and discharged under CC conditions at a rate of 0.5 C to 3.0 V. The above charge and discharge constituted one cycle, and 100 cycles were performed at 25°C.

[0151] The voltage-capacity curve during the formation process is shown in Figure 5. In the case of charge-discharge cycles, the discharge capacity was measured for each cycle, and the measured value was substituted into the following formula 1 to calculate the capacity retention rate. The results are shown in Table 9.

[0152] [Formula 1] Capacity retention rate (%) = (discharge capacity for each cycle / discharge capacity after initial charge / discharge) x 100

[0153] [Table 9]

[0154] From FIG. 5, it is confirmed that in the cases of Comparative Examples A-3 and A-6, a very large overvoltage was applied during the activation process, causing the cell to not operate. This is believed to be because the battery of Comparative Example A-3 contains a nitrile-based electrolyte that does not contain the additive of Chemical Formula 1A, and therefore the impregnation of the separator and the positive electrode is low, causing the cell resistance to increase, which makes it impossible to operate the cell. In the case of Comparative Example A-6, it is confirmed that the impregnation of the separator is reduced due to the addition of a pyrrolidinium compound to the electrolyte, causing the cell resistance to increase, which makes it impossible to operate the cell. In contrast, it is confirmed that the activation process was smoothly performed in the case of the batteries (Examples A-1 to A-3) that use a nitrile-based electrolyte containing the additive of Chemical Formula 1A.

[0155] From Table 9, it can be seen that the cells of Examples A-1 to A-3 have excellent life performance. In the case of Comparative Examples A-3 and A-6, as described above, it was impossible to drive the cells, and it was impossible to measure the capacity retention rate.

[0156] Experimental Example 8: Evaluation of life characteristics (high loading electrode) The capacity retention rates of the lithium secondary batteries of Examples B-4 to B-8 and Comparative Examples B-3, B-4, and B-6 to B-8 were evaluated in the same manner as in Experimental Example 7. The capacity retention rates were also evaluated at 45° C. in the same manner, and the results are shown in Table 10 below.

[0157] [Table 10]

[0158] In the case of Comparative Examples B-3 and B-6, the cells could not be driven from the activation step as in Experimental Example 7, and the life characteristics could not be evaluated. In the case of Comparative Examples B-7 and B-8, although a fluorine-based acrylate and methacrylate compound (Chemical Formula 2A or 2B) was added, the additive of Chemical Formula 1A was not included, and therefore the impregnation of the electrodes and the separator was low, and the cells could not be driven. In the case of Comparative Example B-4, the activation step was performed, but as can be seen from Table 10, it is confirmed that the life performance is significantly inferior to that of Examples B-4 to B-6. It is confirmed that the performance decrease in Comparative Example B-4 is due to the increased aluminum corrosivity caused by the electrolyte containing less than 50 vol% of a nitrile-based solvent.

Claims

1. The present invention includes a compound represented by the following formula 1: an organic solvent containing a nitrile-based solvent in an amount of 90 vol % to 100 vol %; and a lithium salt, The content of the compound represented by Chemical Formula 1 is 2% by weight to 50% by weight based on the total weight of the non-aqueous electrolyte. [Chemical formula 1] R1-O-CH 2 -R2 In the above Chemical Formula 1, R1 is —(CF 2 ) n CHF 2 , R2 is —(CF 2 ) m CHF 2 ; n is an integer from 1 to 4, m is an integer from 2 to 5.

2. The nonaqueous electrolyte for a lithium secondary battery according to claim 1 , wherein the compound represented by Chemical Formula 1 is represented by Chemical Formula 1A below: 【Chemistry 1】

3. 3. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the content of the compound represented by Chemical Formula 1 is 3% by weight to 30% by weight based on the total weight of the non-aqueous electrolyte.

4. The nonaqueous electrolyte for a lithium secondary battery according to any one of claims 1 to 3, further comprising a compound represented by the following chemical formula 2: 【Chemistry 2】 In the above Chemical Formula 2, R3 is hydrogen; or an alkyl group having 1 to 5 carbon atoms; R4 is an alkyl group having 1 to 10 carbon atoms substituted with one or more fluorine atoms.

5. R3 is hydrogen or a methyl group; The R4 is -(CH 2 ) p (CF 2 ) q CHF 2 and The p is an integer of 1 to 3, 5. The nonaqueous electrolyte for a lithium secondary battery in accordance with claim 4, wherein the q is an integer of 2 to 6.

6. 6. The non-aqueous electrolyte for a lithium secondary battery according to claim 4, wherein the content of the compound represented by Chemical Formula 2 is 0.1% by weight to 10% by weight based on the total weight of the non-aqueous electrolyte.

7. The nonaqueous electrolyte for a lithium secondary battery according to claim 1 , wherein the nitrile-based solvent is succinonitrile.

8. The nonaqueous electrolyte for a lithium secondary battery according to claim 1 , wherein the organic solvent further comprises a carbonate-based solvent.

9. 9. The nonaqueous electrolyte for lithium secondary batteries according to claim 8, wherein a volume ratio of the nitrile-based solvent to the carbonate-based solvent is 90:10 to 97:

3.

10. 10. The nonaqueous electrolyte for a lithium secondary battery according to claim 1, wherein the concentration of the lithium salt in the organic solution consisting of the organic solvent and the lithium salt is 1.0 M to 6 M.

11. a positive electrode comprising a positive electrode active material; a negative electrode including a negative electrode active material; A separator interposed between the positive electrode and the negative electrode; and A lithium secondary battery comprising the nonaqueous electrolyte for lithium secondary batteries according to claim 1 .

12. The lithium secondary battery according to claim 11 , wherein the negative electrode active material does not contain lithium metal.

13. 13. The lithium secondary battery according to claim 11 or 12, wherein the negative electrode active material is at least one selected from the group consisting of a carbon-based material, a silicon-based material, one or more metals selected from Sn, Zn, Mg, Cd, Ce, Ni, and Fe, an alloy composed of the metal, an oxide of the metal, and a composite of the metal and carbon.

Citation Information

Patent Citations

  • Lithium-sulfur secondary battery

    WO2020085811A1