Positive electrode, secondary battery, battery pack and vehicle

The positive electrode with coated lithium composite oxide particles and a conductive polymer stabilizes the battery, addressing metal elution and gas issues at high potentials, ensuring high capacity retention and low resistance.

JP7562488B2Active Publication Date: 2024-10-07KK TOSHIBA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021126657
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-02
Publication Date
2024-10-07
Estimated Expiration
2041-08-02

AI Technical Summary

Technical Problem

Non-aqueous electrolyte batteries face challenges with high positive electrode potentials, leading to metal elution and gas generation due to hydrogen and hydrofluoric acid formation, which degrade discharge capacity over cycles.

Method used

A positive electrode is developed with lithium composite oxide particles coated by a conductive polymer, where the mass ratio of conductive polymer to lithium composite oxide is between 0.5% to 5.0%, using a water-soluble polymer to stabilize the coating and prevent direct contact with the electrolyte.

Benefits of technology

The solution effectively suppresses metal elution and gas generation, maintaining high capacity retention rates and reducing resistance, thereby enhancing the battery's performance at high potentials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562488000002
    Figure 0007562488000002
  • Figure 0007562488000003
    Figure 0007562488000003
  • Figure 0007562488000004
    Figure 0007562488000004
Patent Text Reader

Abstract

To provide a positive electrode having low resistance and capable of achieving a high capacity retention rate.SOLUTION: According to one embodiment, a positive electrode is provided. The positive electrode includes a positive electrode active material-containing layer containing positive electrode active material particles and a water-soluble polymer. The positive electrode active material particles include lithium composite oxide particles exhibiting an operating potential of 4.4 V or higher on the basis of metallic lithium, and a conductive polymer covering at least part of surfaces of the lithium composite oxide particles. A ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is in a range of 0.5% by mass to 5.0% by mass.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to a positive electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]

[0002] Non-aqueous electrolyte batteries, such as lithium-ion batteries, in which lithium ions carry electric charge, are being widely used in a wide range of applications, from small applications such as portable electronic devices to large applications such as electric vehicles and power supply and demand adjustment, taking advantage of the advantages of being able to obtain high energy density and high output. To date, non-aqueous electrolyte batteries have used lithium transition metal composite oxides, such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and lithium manganese oxide (LiMn2O4), as the positive electrode active material. In addition, batteries using carbon materials as the negative electrode active material have been commercially available.

[0003] Non-aqueous electrolyte batteries using lithium titanium composite oxide, which has a high lithium absorption / release potential of about 1.55 V versus metallic lithium, instead of carbon materials as the negative electrode active material, have also been put to practical use. Lithium titanium composite oxide has excellent cycle characteristics because there is little volume change during charging and discharging. In addition, negative electrodes containing lithium titanium composite oxide do not precipitate lithium metal during lithium absorption / release, so secondary batteries equipped with this negative electrode can be charged at a large current.

[0004] As for the positive electrode active material, lithium manganese oxide (LiMn2O4) is abundant, inexpensive, has a low environmental impact, and is highly safe in an overcharged state. For this reason, lithium manganese oxide is being considered as an alternative material to lithium cobalt oxide (LiCoO2). However, the average operating potential of lithium manganese oxide is about 4.0 V based on metallic lithium. This makes it difficult to achieve a high battery voltage.

[0005] Therefore, attempts have been made to increase the battery voltage by using a positive electrode material that exhibits a high positive electrode potential of about 4.5 V to 5.0 V versus metallic lithium. However, a problem with positive electrodes that exhibit a high positive electrode potential is the elution of metals due to the generation of gas and hydrofluoric acid. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-263026 [Non-patent literature]

[0007] [Non-Patent Document 1] Hongyu Dong et al. "Improved High Temperature Performance of a Spinel LiNi0.5Mn1.5O4 Cathode for High-Voltage Lithium-Ion Batteries by Surface Modification of a Flexible Conductive Nanolayer" ACS Omega 2019, 4, 185-194 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a positive electrode that has low resistance and is capable of achieving a high capacity retention rate, a secondary battery including this positive electrode, a battery pack including this secondary battery, and a vehicle including this battery pack. [Means for solving the problem]

[0009] According to an embodiment, a positive electrode is provided. The positive electrode includes a positive electrode active material-containing layer containing positive electrode active material particles and a water-soluble polymer. The positive electrode active material particles include lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium, and a conductive polymer covering at least a part of the surface of the lithium composite oxide particles. The ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 0.5% by mass to 5.0% by mass. Water-soluble polymers include alginate polymers.

[0010] According to another embodiment, a secondary battery is provided, the secondary battery comprising a positive electrode according to the embodiment, a negative electrode, and an electrolyte.

[0011] According to another embodiment, a battery pack is provided, the battery pack including a secondary battery according to the embodiment.

[0012] According to another embodiment, a vehicle is provided, the vehicle including a battery pack according to an embodiment. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a cross-sectional view illustrating an example of a positive electrode according to an embodiment. [Diagram 2] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Diagram 3] 3 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 2. [Figure 4] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Diagram 5] 5 is an enlarged cross-sectional view of part B of the secondary battery shown in FIG. 4. [Figure 6] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 7] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 8] 8 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 7. [Figure 9] 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 10] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments will be described with reference to the drawings as appropriate. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Also, each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.

[0015] In secondary batteries, as a positive electrode active material, 4.4V (vs. Li / Li + ) or higher, gases mainly consisting of hydrogen gas are generated. Alternatively, when fluorine atoms are contained in the binder and electrolyte salt, hydrofluoric acid is generated. In the positive electrode active material, metals are dissolved with the generation of hydrogen gas and hydrofluoric acid, which causes a problem of a decrease in discharge capacity due to repeated charge-discharge cycles.

[0016] It has been reported that metal elution from the positive electrode active material can be suppressed by coating the positive electrode active material particles with a conductive polymer such as polyaniline. However, since the conductive polymer itself as a polymer is difficult to dissolve in water or an organic solvent, it is difficult to directly coat the positive electrode active material particles with the conductive polymer itself. In addition, a method has been reported in which the monomer constituting the conductive polymer is polymerized using a polymerization initiator while covering the active material particle surface. However, in this case, it is difficult to coat a sufficient amount of conductive polymer on the active material particle surface.

[0017] The inventors have +They have found that when coating the surfaces of lithium composite oxide particles having a high operating potential of 1000 kPa or more with a conductive polymer, the conductive polymer is easily retained on the surface of the active material particles by the presence of a water-soluble polymer between the particles.

[0018] (First embodiment) According to a first embodiment, a positive electrode is provided. The positive electrode includes a positive electrode active material-containing layer containing positive electrode active material particles and a water-soluble polymer. The positive electrode active material particles include lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium, and a conductive polymer covering at least a part of the surface of the lithium composite oxide particles. The ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 0.5% by mass to 5.0% by mass.

[0019] The lithium composite oxide particles contained in the positive electrode according to the embodiment are coated with a conductive polymer in an amount of 0.5% by mass to 5.0% by mass. The conductive polymer coats the lithium composite oxide particles, for example, in the form of a film. Since the ratio is 0.5% by mass or more, metal elution can be suppressed even in lithium composite oxide particles that exhibit a high operating potential. This is considered to be due in part to the fact that the lithium composite oxide particles are less likely to come into direct contact with the electrolyte. On the other hand, if the ratio exceeds 5.0% by mass, the battery resistance increases excessively and the weight energy density and / or volume energy density decrease, which is not preferable. The ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is preferably within the range of 1.0% by mass to 4.0% by mass.

[0020] The electrical conductivity of the conductive polymer is, for example, within the range of 1 S / cm to 200 S / cm, and preferably within the range of 10 S / cm to 200 S / cm. In order to suppress an increase in electrical resistance caused by coating the surface of the active material particles with the conductive polymer, it is preferable that the electrical conductivity of the conductive polymer is high. The conductive polymer is, for example, water-insoluble.

[0021] The conductive polymer is not particularly limited as long as it is a polymer having electronic conductivity, but is preferably at least one selected from the group consisting of polyanilines, polypyrroles, and polythiophenes. The electrical conductivity of polyanilines is, for example, within the range of 10 S / cm to 50 S / cm. The electrical conductivity of polypyrroles is, for example, within the range of 50 S / cm to 100 S / cm. The electrical conductivity of polythiophenes is, for example, within the range of 50 S / cm to 150 S / cm.

[0022] Examples of polyanilines include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid).

[0023] Examples of polypyrroles include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole).

[0024] Examples of polythiophenes include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene, poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), poly(3-iodothiophene), poly(3-cyanothiophene), poly(3- phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), phene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-didodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4 -butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), poly(3-methyl-4-carboxybutylthiophene), poly(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-propanesulfonate), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-propanesulfonate), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-propanesulfonic acid potassium salt), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-methyl-1-propanesulfonic acid sodium salt), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-ethyl-1-propanesulfonic acid sodium salt), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-propyl-1-propanesulfonic acid sodium salt) , poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-butyl-1-propanesulfonate sodium), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-pentyl-1-propanesulfonate sodium), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-hexyl-1-propanesulfonate sodium), poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-hexyl-1-propanesulfonate sodium), Poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-isopropyl-1-propanesulfonate), Poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-isobutyl-1-propanesulfonate), Poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-isopentyl-1-propanesulfonate), Poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-fluoro-1-propanesulfonate), sodium poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-methyl-1-propanesulfonate), potassium poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-methyl-1-propanesulfonate), ammonium poly(3-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-methyl-1-propanesulfonate),4]dioxepin-3-yloxy]-1-methyl-1-propanesulfonate triethylammonium), poly(4-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-butanesulfonate sodium), poly(4-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-butanesulfonate potassium), poly(4-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-methyl-1-butanesulfonate potassium), Poly(sodium 4-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-methyl-1-butanesulfonate), poly(sodium 4-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-fluoro-1-butanesulfonate), and poly(potassium 4-[(2,3-dihydrothieno[3,4-b]-[1,4]dioxepin-3-yloxy]-1-fluoro-1-butanesulfonate).

[0025] The water-soluble polymer contained in the positive electrode active material-containing layer is highly insoluble in the non-aqueous electrolyte. Therefore, even when the positive electrode is impregnated with the non-aqueous electrolyte, the structure of the positive electrode active material-containing layer can be stably maintained. As a result, the active material particles coated with the conductive polymer are unlikely to fall off from the positive electrode active material-containing layer even when the charge-discharge cycle is repeated. In addition, the surface of the coated lithium composite oxide particle or the conductive polymer coated surface can be prevented from being excessively exposed to the non-aqueous electrolyte, so that metal elution and gas generation can be suppressed to achieve an excellent capacity retention rate.

[0026] The HLB (Hydrophilic-Lipophilic Balance) value of the water-soluble polymer is, for example, in the range of 8 to 20, preferably in the range of 10 to 20. The HLB value of the water-soluble polymer can be in the range of 15 to 19. The HLB value is an index that represents the ratio of hydrophilicity and hydrophobicity of a surfactant. The HLB value ranges from 0 to 20, with the closer to 0 the more hydrophobic the surfactant is, and the closer to 20 the more hydrophilic the surfactant is.

[0027] In the present specification and claims, a polymer that dissolves in water is called a water-soluble polymer. Whether or not the positive electrode contains a water-soluble polymer is examined by the following procedure. First, the positive electrode is exposed to water to examine whether or not the positive electrode active material-containing layer dissolves. Next, if the positive electrode active material-containing layer dissolves in water, the solution is analyzed by GC-MS (Gas Chromatography-Mass Spectrometry), LC-MS (Liquid Chromatography-Mass Spectrometry), FT-IR (Fourier Transform-Infrared Spectroscopy), NMR (Nuclear Magnetic Resonance), or the like to identify the type of water-soluble polymer.

[0028] The HLB value of the water-soluble polymer is, for example, in the range of 8 to 20. The water-soluble polymer is a material used as an aqueous binder during the manufacture of a positive electrode, which will be described later. A method for measuring the HLB value of the water-soluble polymer contained in the positive electrode active material-containing layer will be described later. The HLB value of the water-soluble polymer is preferably 10 or more. In this case, even when the positive electrode active material-containing layer is impregnated with a non-aqueous electrolyte, the electrode material constituting the positive electrode active material-containing layer is likely to remain stable without being decomposed.

[0029] The water-soluble polymer is, for example, at least one selected from the group consisting of acrylic polymers, urethane polymers, carboxymethylcellulose (CMC), alginic acid polymers, polyethers, polyvinyl alcohols, water-soluble polyesters, and dicarboxylated polysaccharides. Among them, at least one selected from the group consisting of acrylic polymers, CMC, and alginic acid polymers is preferred from the viewpoint of maintaining high peel strength so that the positive electrode active material-containing layer does not peel off from the current collector.

[0030] The mass ratio of the water-soluble polymer in the positive electrode active material-containing layer is, for example, in the range of 1% by mass to 10% by mass, and preferably in the range of 2% by mass to 8% by mass. If the mass of the water-soluble polymer contained in the positive electrode active material-containing layer is excessively small, the binding force between the electrode materials constituting the layer may be insufficient, and the electrode strength may be insufficient. As a result, the positive electrode active material-containing layer may peel off from the current collector during charging and discharging, and the capacity may decrease. On the other hand, if the mass of the water-soluble polymer contained in the positive electrode active material-containing layer is excessively large, the internal resistance increases, which is not preferable.

[0031] The positive electrode according to the embodiment will be described in detail below.

[0032] The positive electrode may include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer may be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer contains at least the water-soluble polymer as a binder. The positive electrode active material-containing layer may optionally contain a conductive material.

[0033] The positive electrode according to the embodiment is, for example, a positive electrode for a battery, a positive electrode for a secondary battery, a positive electrode for a non-aqueous electrolyte secondary battery, or a positive electrode for a lithium secondary battery.

[0034] The positive electrode active material particles include, as the active material, lithium composite oxide particles that exhibit an operating potential of 4.4 V or more based on metallic lithium. The number of lithium composite oxide particles can be one or more. The positive electrode active material particles can be composed only of lithium composite oxide particles that exhibit an operating potential of 4.4 V or more based on metallic lithium. However, at least a part of the surface of one or more of the lithium composite oxide particles is coated with a conductive polymer. The positive electrode active material particles may contain only one type or a plurality of types of lithium composite oxide particles that exhibit an operating potential of 4.4 V or more based on metallic lithium.

[0035] As an example of a lithium composite oxide that exhibits an operating potential of 4.4 V or more based on metallic lithium, for example, an oxide represented by the following general formula (A) can be mentioned. Li u M1 x Mn 2-x O4···(A) In the general formula (A), M1 is at least one selected from the group consisting of Mn, Ni, Fe, Co, Cr, Mg, Zn, Al, and Cu, u satisfies 0 < u ≦ 1, and x satisfies 0 < x ≦ 1.

[0036] As a specific example of the lithium composite oxide represented by the general formula (A), for example, LiNi 0.5 Mn 1.5 O4 and LiCu 0.5 Mn 1.5 O4 can be mentioned.

[0037] The lithium composite oxide that exhibits an operating potential of 4.4 V or more based on metallic lithium includes, for example, at least one selected from the group consisting of lithium nickel manganate and lithium phosphate compounds. Among the above lithium composite oxides, since the electron conductivity is high and the structure is stable even when the voltage is increased up to around 5 V, it is preferable that the positive electrode active material particles contain lithium nickel manganate. Lithium nickel manganate has, for example, a crystal structure of a spinel structure.

[0038] Lithium nickel manganese oxide is represented by, for example, the following general formula (I). In this case, as described above, since the structure is stable even when the voltage is increased, excellent cycle life characteristics are easily obtained while maintaining a high operating voltage. Li u Ni x Mn 2-x O4···(I) In general formula (I), u satisfies 0 < u ≦ 1, and x satisfies 0 < x ≦ 1.

[0039] The lithium phosphate compound is represented by, for example, the following general formula (II).

[0040] Li w M2 y Co 1-y PO4···(II) In general formula (II), M2 is at least one selected from the group consisting of Ni and Cu, w satisfies 0 < w ≦ 1, and y satisfies 0 ≦ y ≦ 1. The lithium phosphate compound has, for example, a crystal structure of an olivine structure.

[0041] Specific examples of the lithium phosphate compound represented by general formula (II) include, for example, LiNiPO4 and LiCoPO4.

[0042] The positive electrode active material particles according to the embodiment may contain other active materials and exhibit an operating potential of less than 4.4 V based on metallic lithium. The proportion of other active materials in the entire positive electrode active material particles may be 20% by mass or less, may be 10% by mass or less, or may be 0% by mass.

[0043] Examples of other active materials include oxides or sulfides. Such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxides (for example, Li x Mn2O4 or Li x MnO2; 0 < x ≦ 1), lithium nickel composite oxides (for example, Li x NiO2; 0 < x ≦ 1), lithium cobalt composite oxides (for example, Li xCoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.

[0044] The primary particle size of the positive electrode active material is preferably 100 nm or more and 10 μm or less. The positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. The positive electrode active material with a primary particle size of 10 μm or less can smoothly progress the solid-state diffusion of lithium ions.

[0045] The specific surface area of the positive electrode active material is preferably 0.1 m 2 / g or more and 10 m 2 / g or less. The positive electrode active material having a specific surface area of 0.1 m 2 / g or more can sufficiently secure the Li ion storage and release sites. The positive electrode active material having a specific surface area of 10 m 2 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.

[0046] The water-soluble polymer is contained in the positive electrode active material-containing layer as a binder. The binder can fill the gaps between the dispersed positive electrode active material and can bind the positive electrode active material and the positive electrode current collector. As the positive electrode binder, any water-soluble polymer can be used without any restrictions. The positive electrode active material-containing layer may contain only the water-soluble polymer as a binder, or may further contain other binders. Examples of other binders include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, and imide compounds. The amount of the water-soluble polymer contained in the positive electrode binder may be 80% by mass or more, 90% by mass or more, or 100% by mass.

[0047] The conductive material is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive material include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanofibers, and carbonaceous materials such as carbon nanotubes. One of these may be used as the conductive material, or two or more may be combined and used as the conductive material. The conductive material may also be omitted.

[0048] In the positive electrode active material-containing layer, the positive electrode active material particles and the positive electrode binder are preferably mixed in an amount of 80% by mass to 98% by mass and 1% by mass to 20% by mass, respectively.

[0049] By making the amount of the binder 1% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of the binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.

[0050] When a conductive material is added, the positive electrode active material, binder, and conductive material are preferably mixed in proportions of 77% by mass to 95% by mass, 1% by mass to 20% by mass, and 3% by mass to 15% by mass, respectively.

[0051] By making the amount of the conductive material 3% by mass or more, the above-mentioned effects can be achieved. Also, by making the amount of the conductive material 15% by mass or less, the ratio of the conductive material in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.

[0052] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.

[0053] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.

[0054] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.

[0055] The electrode density of the positive electrode (excluding the current collector) is 2.0 g / cm 3 More than 4.0g / cm 3 A positive electrode having a positive electrode active material-containing layer with a density within this range is excellent in energy density and electrolyte retention. The electrode density of the positive electrode is preferably 2.5 g / cm or less. 3 More than 3.5g / cm 3 It is more preferable that:

[0056] An example of a positive electrode according to an embodiment will be described with reference to the drawings.

[0057] FIG. 1 is a cross-sectional view that shows a schematic diagram of a positive electrode according to an example. The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b provided on the positive electrode current collector 5a. Here, an example in which the positive electrode active material-containing layer 5b is provided on one side of the positive electrode current collector 5a is shown, but the positive electrode active material-containing layer 5b may be provided on both sides of the positive electrode current collector 5a. The thickness of the positive electrode active material-containing layer 5b is not particularly limited, but is, for example, within a range of 10 μm to 100 μm.

[0058] The positive electrode active material-containing layer 5b includes one or more positive electrode active material particles 5c and a water-soluble polymer 5d. The positive electrode active material particles 5c have a potential of 4.4 V (vs. Li / Li + ) or more, and a conductive polymer 52 that covers at least a part of the surface of the lithium composite oxide particle 51. Although the positive electrode active material-containing layer 5b includes a positive electrode conductive material 5e in Fig. 1, the positive electrode conductive material 5e does not necessarily have to be added.

[0059] The entire positive electrode active material-containing layer 5b is bound by a water-soluble polymer 5d that functions as a binder. This prevents the lithium composite oxide particles 51 from coming into direct contact with a non-aqueous electrolyte (not shown), thereby suppressing metal elution and / or gas generation from the lithium composite oxide particles 51. As a result, it is possible to suppress the deterioration of the positive electrode due to charge / discharge cycles. In addition, the ratio of the mass of the conductive polymer 52 to the mass of the lithium composite oxide particles 51 is within a range of 0.5% by mass to 5.0% by mass. Therefore, a secondary battery including the positive electrode according to the embodiment has low resistance and can achieve a high capacity retention rate.

[0060] <Measurement of the amount of conductive polymer coating> The ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium can be measured as follows.

[0061] The positive electrode is washed with propylene carbonate, dried, and the positive electrode active material-containing layer is peeled off from the current collector. The peeled positive electrode active material-containing layer is thoroughly washed with pure water to remove the water-soluble polymer. The residue after washing is centrifuged to remove the conductive material, and then vacuum dried. The mass of the solid obtained is then measured. The solid is, for example, a positive electrode active material particle containing lithium composite oxide particles exhibiting an operating potential of 4.4 V or more based on metallic lithium, and a conductive polymer covering at least a part of the surface of the particles. Next, the obtained solid is subjected to a combustion treatment at a temperature of 800 ° C. for 10 hours or more. The conductive polymer is decomposed by this combustion, and only the lithium composite oxide particles can be obtained. The mass of the obtained particles is then measured, and the mass of the conductive polymer is determined by subtracting the mass of the particles from the mass of the solid. In addition, the ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles can be calculated.

[0062] <Electrical conductivity measurement of conductive polymers> As described in the above coating amount measurement, the positive electrode active material-containing layer is thoroughly washed with pure water, and the conductive material is removed by centrifugation to obtain particles. The obtained particles are treated with acid to dissolve and remove the active material. The polymer component thus obtained is measured by an AC impedance method to determine the electrical conductivity of the conductive polymer that has coated at least a portion of the active material particle surface.

[0063] <Measurement of HLB value of water-soluble polymer> The HLB value of the water-soluble polymer can be determined by the Davis method. First, as described below, it is necessary to identify the type of water-soluble polymer contained in the positive electrode and specify the hydrophilic and hydrophobic groups.

[0064] The water-soluble polymer is dissolved and extracted from the positive electrode active material-containing layer using a solvent that dissolves only the water-soluble polymer, and the active material and conductive agent are removed by filtration. An example of a solvent that dissolves only the water-soluble polymer is pure water. The filtrate is then analyzed by GC-MS (Gas Chromatography-Mass Spectrometry), LC-MS (Liquid Chromatography-Mass Spectrometry), or FT-IR (Fourier Transform-Infrared Spectroscopy) to identify the type of water-soluble polymer. Alternatively, the type of water-soluble polymer may be identified by analyzing the positive electrode surface by infrared spectroscopy (ATR: Attenuated Total Reflectance).

[0065] In the Davis method, a predetermined number of groups is determined according to the hydrophilic and hydrophobic groups contained in a compound. For example, a hydroxyl group is a hydrophilic group, and its number of groups is 1.9. For example, a methyl group and a methylene group are hydrophobic groups, and their number of groups is -0.475. The HLB value of a target water-soluble polymer is calculated by the following formula (1). Formula (1): [HLB value]=7+SUM1-SUM2 In formula (1), SUM1 represents the sum of the numbers of hydrophilic groups, and SUM2 represents the sum of the numbers of hydrophobic groups.

[0066] <Measurement of the amount of water-soluble polymer> An active material-containing layer to be measured is prepared. For example, a certain amount of active material-containing layer is obtained from the positive electrode using a spatula or the like. The mass of the obtained active material-containing layer is measured. Then, similar to the pretreatment in the above-mentioned HLB value measurement, the water-soluble polymer is dissolved and extracted with pure water or the like, and filtered. The solvent in the obtained solution is evaporated to obtain a solidified water-soluble polymer. The mass of this water-soluble polymer is measured. Then, the mass of the water-soluble polymer is divided by the mass of the active material-containing layer previously measured, and the result is multiplied by 100 to calculate the mass ratio of the water-soluble polymer to the positive electrode active material-containing layer.

[0067] The crystal structure and elemental composition of the positive electrode active material can be confirmed by, for example, powder X-ray diffraction (XRD) measurement and inductively coupled plasma (ICP) emission spectroscopy, which will be described below. The crystal structure and elemental composition of the negative electrode active material, which will be described below, can also be analyzed by the method described below.

[0068] <Powder X-ray diffraction measurement of active materials> The powder X-ray diffraction measurement of the active material can be carried out, for example, as follows. First, the target sample is crushed until the average particle size is about 5 μm. The crushed sample is filled into the holder portion formed on the glass sample plate, with a depth of 0.2 mm. At this time, care is taken to ensure that the sample is filled sufficiently into the holder portion. Also, care is taken to fill the sample with just the right amount so that cracks, voids, etc. do not occur. Next, another glass plate is pressed from the outside to flatten the surface of the sample filled into the holder portion. Care is taken to ensure that the amount of filling is not too much or too little, resulting in unevenness compared to the reference surface of the holder.

[0069] Next, the glass plate filled with the sample is placed in a powder X-ray diffractometer, and a diffraction pattern (XRD pattern; X-Ray Diffraction pattern) is obtained using Cu-Kα radiation.

[0070] In addition, the orientation of the particles may become large depending on the particle shape of the sample. When the orientation of the sample is high, the peak position may shift or the intensity ratio may change depending on how the sample is filled. Samples with extremely high orientation are measured using a glass capillary. Specifically, the sample is inserted into a capillary, and the capillary is placed on a rotating sample stage for measurement. This measurement method can reduce the orientation. As the glass capillary, it is preferable to use a Lindemann glass capillary with a diameter of 1 mm to 6 mmφ.

[0071] When performing powder X-ray diffraction measurement on the active material contained in a secondary battery or an electrode, it can be carried out, for example, as follows. First, in order to understand the crystal state of the active material, the lithium ions are completely removed from the active material. For example, when the active material is used in the negative electrode, the battery is brought into a fully discharged state. For example, the battery is repeatedly discharged at a current of 0.1C in a 25°C environment until the rated cut-off voltage or the battery voltage reaches 1.0V, and the battery can be put into a discharged state by making the current value during discharge 1 / 100 or less of the rated capacity. There may still be lithium ions remaining even in the discharged state.

[0072] Next, the battery is disassembled in a glove box filled with argon, the electrode is taken out and washed with an appropriate solvent. As an appropriate solvent, for example, ethyl methyl carbonate can be used. If the washing of the electrode is insufficient, impurity phases such as lithium carbonate and lithium fluoride may be mixed in due to the influence of the lithium ions remaining in the electrode. In that case, it is advisable to use an airtight container in which the measurement atmosphere can be in an inert gas. At this time, the peaks derived from the metal foil as the current collector, the conductive agent, the binder, etc. are measured and grasped in advance using EDX. Of course, if these can be grasped in advance, this operation can be omitted. When the peak of the current collector overlaps with the peak of the active material, it is desirable to peel off the active material-containing layer from the current collector for measurement. This is for separating the overlapping peaks when quantitatively measuring the peak intensity. The active material-containing layer may be physically peeled off. The active material-containing layer is easily peeled off by applying ultrasonic waves in an appropriate solvent. When ultrasonic treatment is performed to peel off the active material-containing layer from the current collector, the electrode body powder (including the active material, the conductive agent, and the binder) can be recovered by volatilizing the solvent. The powder X-ray diffraction measurement of the active material can be performed by filling the recovered electrode body powder into, for example, a Lindemann glass capillary, etc. for measurement. Incidentally, the electrode body powder recovered by ultrasonic treatment can also be used for various analyses other than powder X-ray diffraction measurement.

[0073] <ICP Emission Spectrometry> The composition of the active material can be analyzed, for example, by inductively coupled plasma (ICP) emission spectroscopy. At this time, the abundance ratio (molar ratio) of each element depends on the sensitivity of the analysis device used. Therefore, the measured molar ratio may deviate from the actual molar ratio by the error of the measurement device. However, even if the numerical value deviates within the error range of the analysis device, the performance of the active material according to the embodiment can be fully exhibited.

[0074] Specifically, the composition of the active material incorporated in the battery is measured by ICP emission spectroscopy according to the following procedure.

[0075] First, the electrode containing the active material to be measured is removed from the secondary battery and washed according to the procedure described in the section on powder X-ray diffraction measurement. The part containing the electrode active material, such as the active material-containing layer, is peeled off from the washed electrode. For example, the part containing the electrode active material can be peeled off by irradiating it with ultrasonic waves. As a specific example, the electrode can be placed in ethyl methyl carbonate in a glass beaker and vibrated in an ultrasonic cleaner to peel off the active material-containing layer containing the electrode active material from the electrode current collector.

[0076] Next, the peeled off part is heated in air for a short period of time (for example, at 500°C for about an hour) to burn off unnecessary components such as binder components and carbon. This residue is dissolved in acid to create a liquid sample containing the active material. The acid that can be used in this case is hydrochloric acid, nitric acid, sulfuric acid, hydrogen fluoride, etc. This liquid sample can be subjected to ICP analysis to determine the composition of the active material.

[0077] <Manufacturing method of positive electrode> The positive electrode according to the embodiment can be produced, for example, by the following method.

[0078] The manufacturing method of the positive electrode is as follows: Dissolving an electropolymerizable monomer of a conductive polymer in a solvent to prepare a monomer-containing solution; adding lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium to the monomer-containing solution, and then drying the solution to obtain the lithium composite oxide particles coated with the monomer; a step of mixing the lithium composite oxide particles coated with the monomer and an aqueous binder containing water to obtain a slurry; a step of applying the slurry to one or both sides of a current collector, followed by drying and pressing to obtain a positive electrode in an uncharged state; providing a negative electrode and an electrolyte; and performing an initial charge so that the positive electrode potential of the positive electrode in an uncharged state becomes 4.4 V or higher versus metallic lithium.

[0079] Prior to preparing the slurry for the positive electrode, 4.4 V (vs. Li / Li + ) or more, is coated in advance with an electropolymerizable conductive polymer monomer. The electropolymerizable conductive polymer monomer is a monomer that constitutes a conductive polymer by polymerization. Examples of the electropolymerizable conductive polymer monomer include anilines, pyrroles, and thiophenes. As the anilines, a monomer that constitutes at least one of the above-mentioned polyanilines can be used. As the pyrroles, a monomer that constitutes at least one of the above-mentioned polypyrroles can be used. As the thiophenes, a monomer that constitutes at least one of the above-mentioned polythiophenes can be used.

[0080] The type of the solvent contained in the monomer-containing solution is not particularly limited as long as it can dissolve the monomer used.However, from the viewpoint of evaporating the solvent after applying the monomer-containing solution on the surface of the lithium composite oxide particles, the solvent is preferably an organic solvent.For example, acetone can be used as the solvent contained in the monomer-containing solution.

[0081] The mass of the monomer coated on the lithium composite oxide particles can be adjusted by adjusting the mass of the electrolytically polymerizable monomer contained in the monomer-containing solution. The mass of the monomer in the monomer-containing solution can be appropriately changed according to the target coating amount, and is set within the range of, for example, 0.5% by mass to 5.0% by mass. All or almost all of the monomer contained in the monomer-containing solution is coated on the surface of the lithium composite oxide particles. In other words, the amount of monomer as the charged amount can be regarded as the amount of conductive polymer coated on the surface of the lithium composite oxide particles in the positive electrode active material to be produced.

[0082] The lithium composite oxide particles coated with the monomer-containing solution are dried, for example, on a hot plate. This drying is performed, for example, for 5 to 60 minutes on a hot plate set at a temperature of 80°C to 120°C. By drying the lithium composite oxide particles coated with the monomer-containing solution, the solvent is evaporated to obtain composite particles coated with the monomer. The drying method is not limited to heating, and vacuum drying, for example, may be performed.

[0083] Next, a water-based binder is prepared. The water-based binder contains water as a solvent and a water-soluble polymer. Since the water-soluble polymer is dissolved in water, the water-based binder can be in a state of, for example, an emulsion.

[0084] The lithium composite oxide particles coated with the monomer prepared above are added to the aqueous binder to obtain a slurry for preparing a positive electrode. A conductive material may be further dispersed in the slurry. The electrolytically polymerizable monomer is difficult to dissolve in the water constituting the aqueous binder. Therefore, the lithium composite oxide particles having the monomer coat can be present in the slurry in a coated state. In other words, the aqueous binder is excellent in the retention of the monomer coat of the lithium composite oxide particles having the monomer coat while appropriately binding the materials constituting the positive electrode active material-containing layer. If an organic solvent-based binder is used instead of the aqueous binder, the monomer coat will dissolve in the organic solvent. In that case, it is difficult to manufacture a positive electrode while retaining the monomer coat of the lithium composite oxide particles.

[0085] The amounts of the lithium composite oxide particles, conductive material, and aqueous binder (water-soluble polymer) contained in the positive electrode slurry are appropriately adjusted, for example, within the aforementioned numerical ranges for each material contained in the positive electrode active material-containing layer to be produced.

[0086] The prepared slurry is applied to one or both sides of the current collector. The applied slurry is then dried to obtain a laminate of the positive electrode active material-containing layer and the current collector. Then, the laminate is pressed. In this way, a positive electrode in an uncharged state is produced. Separately, a negative electrode and an electrolyte are prepared, for example, according to the method described below.

[0087] A battery is assembled using at least the above-mentioned positive electrode, negative electrode, and electrolyte in an uncharged state. Then, an initial charge is performed so that the positive electrode potential of the uncharged positive electrode is 4.4 V or more based on metallic lithium. This initial charge causes the monomer coated on the surface of the lithium composite oxide particles to be electrolytically polymerized to become a conductive polymer. In this way, the positive electrode according to the embodiment can be manufactured.

[0088] In order to properly polymerize the electropolymerizable monomer to produce a conductive polymer coating, the positive electrode must be charged to at least 4.0 V (vs. Li / Li) during the initial charging of the secondary battery. +) or higher, preferably 4.4V (vs. Li / Li + ) or higher. The positive electrode operating potential at the time of initial charging is 4.4V (vs. Li / Li + ), it may not be possible to produce a uniform conductive polymer coating. + ) is used, the lithium composite oxide particles cannot withstand the battery voltage required to polymerize the monomer, and their crystal structure is destroyed, changing to a structure that cannot be charged or discharged.

[0089] The initial charging conditions were: positive electrode operating potential 4.4V (vs. Li / Li + ), but for example, the following conditions are used: The secondary battery is charged at a current value of 0.1C to 2.0C at 25°C until the battery voltage reaches 2.5V to 4.0V. The current value during charging is expressed in units of 1C, which is the current value at which the SOC becomes 0% in 1 hour when the secondary battery is discharged from a state where the SOC is 100%.

[0090] According to a first embodiment, a positive electrode is provided. The positive electrode includes a positive electrode active material-containing layer containing positive electrode active material particles and a water-soluble polymer. The positive electrode active material particles include lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium, and a conductive polymer covering at least a part of the surface of the lithium composite oxide particles. The ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 0.5% by mass to 5.0% by mass. This positive electrode has low resistance and can achieve a high capacity retention rate.

[0091] Second embodiment According to the second embodiment, a secondary battery is provided that includes the positive electrode according to the first embodiment, a negative electrode, and an electrolyte. The secondary battery may be, for example, a lithium secondary battery. The secondary battery may also be a non-aqueous electrolyte secondary battery that includes a non-aqueous electrolyte.

[0092] The secondary battery may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.

[0093] Moreover, the secondary battery may further include an exterior member that contains the electrode group and the electrolyte.

[0094] Furthermore, the secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.

[0095] The positive electrode, the negative electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.

[0096] (1) Positive electrode As the positive electrode of the secondary battery according to the second embodiment, the positive electrode according to the first embodiment can be used.

[0097] (2) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode active material-containing layer may be formed on one or both sides of the negative electrode current collector. The negative electrode active material-containing layer may include a negative electrode active material, and optionally a conductive material and a binder.

[0098] The negative electrode active material contains at least one titanium-containing oxide selected from the group consisting of titanium oxide, lithium titanium composite oxide, niobium titanium composite oxide, and sodium niobium titanium composite oxide. Specific examples of the titanium-containing oxide include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12, 0≦x≦3), monoclinic titanium dioxide (TiO2), anatase titanium dioxide, rutile titanium dioxide, hollandite titanium composite oxide, monoclinic niobium titanium composite oxide, and orthorhombic titanium-containing composite oxide. Among them, from the viewpoint of achieving both high capacity and high rate performance, it is preferable that the negative electrode active material contains at least one selected from the group consisting of lithium titanium composite oxide and niobium titanium composite oxide. The lithium titanium composite oxide may have a spinel type crystal structure. The niobium titanium composite oxide may have a monoclinic type crystal structure.

[0099] As an example of the monoclinic niobium titanium composite oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium composite oxides include Li x Examples include Nb2TiO7 (0≦x≦5).

[0100] Another example of monoclinic niobium titanium composite oxide is Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦y<1, 0≦z≦2, and -0.3≦δ≦0.3.

[0101] As an example of an orthorhombic titanium-containing composite oxide, Li 2+a M(I) 2-b Ti 6-c M(II) d O 14+σHere, M(I) is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb, and K. M(II) is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).

[0102] The conductive material is blended to improve current collection performance and reduce contact resistance between the active material and the current collector. Examples of the conductive material include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive material, or two or more may be combined and used as the conductive material. Alternatively, instead of using a conductive material, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.

[0103] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the negative electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.

[0104] The mixing ratio of the negative electrode active material, the conductive material, and the binder in the negative electrode active material-containing layer can be appropriately changed depending on the application of the negative electrode. For example, it is preferable to mix the negative electrode active material, the conductive material, and the binder at a ratio of 70% by mass or more and 96% by mass or less, 2% by mass or more and 28% by mass or less, and 2% by mass or more and 28% by mass or less, respectively. By making the amount of the conductive material 2% by mass or more, the current collection performance of the negative electrode active material-containing layer can be improved. In addition, by making the amount of the binder 2% by mass or more, the binding property between the negative electrode active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive material and the binder 28% by mass or less, respectively, in order to achieve high capacity.

[0105] The negative electrode current collector is provided with a potential at which lithium (Li) is inserted and extracted from the active material, for example, 1.0 V (vs. Li / Li + ) is used. For example, the current collector is preferably made of copper, nickel, stainless steel, aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.

[0106] The negative electrode current collector may also include a portion on the surface of which the negative electrode active material-containing layer is not formed, and this portion can function as a negative electrode current collecting tab.

[0107] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 More than 2.8g / cm 3 A negative electrode having a density of the negative electrode active material-containing layer within this range is excellent in energy density and electrolyte retention. The density of the negative electrode active material-containing layer is preferably 2.1 g / cm or less. 3 More than 2.6g / cm 3 It is more preferable that:

[0108] The negative electrode can be produced, for example, by the following method. First, an active material, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, this laminate is pressed. In this manner, the negative electrode is produced.

[0109] Alternatively, the negative electrode may be prepared by the following method: first, the active material, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain the negative electrode.

[0110] (3) Electrolyte The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.

[0111] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.

[0112] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.

[0113] The gelled non-aqueous electrolyte is prepared by compounding a liquid non-aqueous electrolyte with a polymeric material. As the polymeric material, for example, at least one selected from the group consisting of polyvinylidene fluoride, polyacrylonitrile, polyethylene oxide, acrylic polymer, polyamide, and polyvinyl alcohol can be used. By using a gelled electrolyte as the electrolyte, it is possible to suppress the elution of metal from the positive electrode and the generation of gas such as hydrogen. As a result, excellent cycle life characteristics can be obtained.

[0114] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.

[0115] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.

[0116] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.

[0117] The inorganic solid electrolyte is a solid material that has Li-ion conductivity.

[0118] (4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.

[0119] A solid electrolyte layer containing solid electrolyte particles can also be used as the separator. The solid electrolyte layer may contain one type of solid electrolyte particles or may contain multiple types of solid electrolyte particles. The solid electrolyte layer may be a solid electrolyte composite membrane containing solid electrolyte particles. The solid electrolyte composite membrane is, for example, a membrane formed from solid electrolyte particles using a polymer material. The solid electrolyte layer may contain at least one selected from the group consisting of a plasticizer and an electrolyte salt. When the solid electrolyte layer contains an electrolyte salt, for example, the alkali metal ion conductivity of the solid electrolyte layer can be further increased.

[0120] Examples of the polymeric material include polyethers, polyesters, polyamines, polyethylenes, silicones, and polysulfides.

[0121] The lithium ion conductivity of the solid electrolyte is 1×10 at 25°C. -10 It is preferable that the lithium ion conductivity of the solid electrolyte at 25° C. is 1×10 -10 By having a lithium ion conductivity of 1×10 S / cm or more, the lithium ion concentration near the surface of the solid electrolyte is likely to be high, which can improve the rate performance and life characteristics. The lithium ion conductivity of the solid electrolyte at 25°C is 1×10 -6 The upper limit of the lithium ion conductivity of the solid electrolyte is, for example, 2×10 -2 S / cm.

[0122] Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes. Specific examples of the solid electrolyte include sulfide-based Li2SeP2S5-based glass ceramics and lithium lanthanum titanium composite oxides (e.g., Li 0.5 La 0.5 TiO3), inorganic compounds with LISICON structure (e.g., Li 3.6 S 0.6 P 0.4 O4), an inorganic compound with a NASICON structure, and amorphous LIPON (Li 2.9 PO 3.3 N 0.46 ), lithium calcium zirconium oxide (Li 1.2 Zr 1.9 Ca 0.1 (PO4)3) and at least one selected from the group consisting of inorganic compounds having a garnet structure. The coating layer may contain one type of solid electrolyte or may contain two or more types of solid electrolytes.

[0123] The inorganic compound having a NASICON skeleton is preferably an inorganic compound represented by the general formula LiM2(PO4)3 (wherein M is at least one selected from Ti, Ge, Sr, Zr, Sn, and Al). 1+x Al x Ge 2-x (PO4)3, Li 1+x Al x Zr 2-x (PO4)3, Li 1+x Al x Ti 2-x (PO4)3(LATP) is preferred because it has high ionic conductivity and high electrochemical stability against water. In the above, x preferably satisfies 0≦x≦0.5.

[0124] Examples of inorganic compounds having a garnet structure include Li 5+x A y La 3-y M2O 12 (A is at least one selected from the group consisting of Ca, Sr and Ba, and M is at least one selected from the group consisting of Nb and Ta), Li3M 2-x ZrO 12 (M is at least one selected from the group consisting of Ta and Nb), Li 7-3x Al x La3Zr3O 12 , and Li7La3Zr2O 12 In the above, x is, for example, 0≦x<0.8, and preferably 0≦x≦0.5. y is, for example, 0≦y<2. The oxide having a garnet structure may be composed of one of these compounds, or may contain a mixture of two or more of these compounds. Among these, Li 6.25 Al 0.25 La3Zr3O 12 and Li7La3Zr2O 12 Since it has high ionic conductivity and is electrochemically stable, it has excellent discharge performance and cycle life performance.

[0125] It is not preferable for the solid electrolyte to contain elemental sulfur, since the sulfur component dissolves in the organic electrolyte described below.It is preferable for the solid electrolyte to not contain elemental sulfur.

[0126] A preferred solid electrolyte is LATP (Li 1+x Al x Ti 2-x (PO4)3), amorphous LIPON, garnet-type lithium lanthanum zirconium oxides (e.g., Li7La3Zr2O 12 :LLZ) and other oxides.

[0127] The lithium ion conductivity of the inorganic compound represented by LiM2(PO4)3 having a NASICON structure at 25°C is, for example, 1×10 -3 S / cm~1×10 -5 S / cm range. 2.9 PO 3.3 N 0.46 ) at 25°C has a lithium ion conductivity of 3×10 -6 S / cm. Garnet-type LLZ (Li7La3Zr2O 12 ) at 25°C has a lithium ion conductivity of 3×10 -4 S / cm.

[0128] Among these, the solid electrolyte is preferably LATP having a NASICON-type skeleton. LATP has high lithium ion conductivity and is not decomposed by water, so it can exist stably even in air.

[0129] (5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.

[0130] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.

[0131] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.

[0132] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.

[0133] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.

[0134] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin-shaped, or button-shaped. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.

[0135] (6) Negative terminal The negative electrode terminal can be made of a material that is electrochemically stable at the Li absorption / release potential of the negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.

[0136] (7) Positive terminal The positive electrode terminal has a potential range of 3V to 5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.

[0137] Next, the secondary battery according to the second embodiment will be described more specifically with reference to the drawings.

[0138] Fig. 2 is a cross-sectional view showing an example of a secondary battery according to a second embodiment of the present invention, and Fig. 3 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 2.

[0139] The secondary battery 100 shown in Figures 2 and 3 includes a bag-shaped exterior member 2 shown in Figures 2 and 3, an electrode group 1 shown in Figure 3, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.

[0140] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0141] As shown in Fig. 2, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 3, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.

[0142] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 3. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.

[0143] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.

[0144] As shown in FIG. 2, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.

[0145] The secondary battery according to the second embodiment is not limited to the secondary battery having the configuration shown in FIGS. 2 and 3, but may be a battery having the configuration shown in FIGS.

[0146] Fig. 4 is a partially cutaway perspective view showing typically another example of the secondary battery according to the second embodiment, Fig. 5 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 4.

[0147] The secondary battery 100 shown in Figures 4 and 5 includes an electrode group 1 shown in Figures 4 and 5, an exterior member 2 shown in Figure 4, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.

[0148] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.

[0149] The electrode group 1 is a laminated type electrode group, as shown in Fig. 5. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.

[0150] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.

[0151] The negative electrode current collector 3a of each negative electrode 3 includes a portion 3c on one side of which the negative electrode active material-containing layer 3b is not supported on any surface. This portion 3c serves as a negative electrode current collector tab. As shown in FIG. 5, the portion 3c serving as the negative electrode current collector tab does not overlap with the positive electrode 5. In addition, the multiple negative electrode current collector tabs (portions 3c) are electrically connected to a strip-shaped negative electrode terminal 6. The tip of the strip-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.

[0152] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6, and is drawn out to the outside of the exterior member 2.

[0153] The secondary battery according to the second embodiment includes the positive electrode according to the first embodiment, and therefore this secondary battery has low resistance and can achieve a high capacity retention rate.

[0154] Third embodiment According to a third embodiment, there is provided a battery pack. The battery pack according to the third embodiment includes a plurality of secondary batteries according to the second embodiment.

[0155] In the battery pack according to the third embodiment, the individual cells may be electrically connected in series or in parallel, or may be connected in a combination of series and parallel.

[0156] Next, an example of a battery pack according to a third embodiment will be described with reference to the drawings.

[0157] Fig. 6 is a perspective view showing an example of a battery pack according to the third embodiment. The battery pack 200 shown in Fig. 6 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the second embodiment.

[0158] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 6 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, thereby electrically connecting the plurality of cells.

[0159] The positive terminal 7 of at least one of the five cells 100a-100e is electrically connected to a positive lead 22 for external connection. Also, the negative terminal 6 of at least one of the five cells 100a-100e is electrically connected to a negative lead 23 for external connection.

[0160] The battery pack according to the third embodiment includes the secondary battery according to the second embodiment, and therefore this battery pack has low resistance and can achieve a high capacity retention rate.

[0161] (Fourth embodiment) According to a fourth embodiment, a battery pack is provided. The battery pack includes the battery assembly according to the third embodiment. The battery pack may include a single secondary battery according to the second embodiment, instead of the battery assembly according to the third embodiment.

[0162] The battery pack according to the fourth embodiment may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.

[0163] The battery pack according to the fourth embodiment may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or for inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.

[0164] Next, an example of a battery pack according to a fourth embodiment will be described with reference to the drawings.

[0165] Fig. 7 is an exploded perspective view showing an example of a battery pack according to a fourth embodiment of the present invention, and Fig. 8 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 7.

[0166] The battery pack 300 shown in Figs. 7 and 8 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).

[0167] 7 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.

[0168] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.

[0169] At least one of the plurality of unit cells 100 is a secondary battery according to the second embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 8. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.

[0170] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.

[0171] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.

[0172] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.

[0173] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.

[0174] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.

[0175] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.

[0176] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.

[0177] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.

[0178] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.

[0179] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.

[0180] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.

[0181] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.

[0182] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the plurality of assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal and a negative terminal, respectively, of the external terminals for current supply.

[0183] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.

[0184] The battery pack according to the fourth embodiment includes the secondary battery according to the second embodiment or the battery pack according to the third embodiment. Therefore, this battery pack has low resistance and can achieve a high capacity retention rate.

[0185] Fifth embodiment According to a fifth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fourth embodiment.

[0186] In the vehicle according to the fifth embodiment, the battery pack recovers, for example, regenerative energy of the vehicle's motive power. The vehicle may include a mechanism for converting the kinetic energy of the vehicle into regenerative energy.

[0187] Examples of the vehicle according to the fifth embodiment include a two-wheeled to four-wheeled hybrid electric vehicle, a two-wheeled to four-wheeled electric vehicle, an electric-assisted bicycle, and a railroad car.

[0188] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.

[0189] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.

[0190] Next, an example of a vehicle according to a fifth embodiment will be described with reference to the drawings.

[0191] FIG. 9 is a partial perspective view that illustrates an example of a vehicle according to the embodiment.

[0192] A vehicle 400 shown in Fig. 9 includes a vehicle body 40 and a battery pack 300 according to the embodiment. In the example shown in Fig. 9, the vehicle 400 is a four-wheeled automobile.

[0193] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.

[0194] 9 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.

[0195] Next, an embodiment of a vehicle according to the fifth embodiment will be described with reference to FIG.

[0196] Fig. 10 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to embodiment 5. A vehicle 400 illustrated in Fig. 10 is an electric vehicle.

[0197] The vehicle 400 shown in FIG. 10 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.

[0198] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 10, the mounting location of the vehicle power supply 41 is shown diagrammatically.

[0199] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.

[0200] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (e.g., VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a-300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a-200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a-200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.

[0201] Each of the assembled batteries 200a-200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the second embodiment. The assembled batteries 200a-200c are charged and discharged via a positive terminal 413 and a negative terminal 414, respectively.

[0202] The battery management device 411 communicates with the assembled battery monitoring devices 301a-301c and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a-200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.

[0203] The battery management unit 411 and the assembled battery monitoring units 301a-301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a-301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.

[0204] The battery pack monitoring devices 301a-301c measure the voltage and temperature of each of the cells constituting the battery packs 200a-200c based on commands received through communication from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.

[0205] The vehicle power supply 41 may also have an electromagnetic contactor (e.g., a switch device 415 shown in FIG. 10) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a-200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a-200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed in the vicinity of the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.

[0206] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.

[0207] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.

[0208] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.

[0209] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.

[0210] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.

[0211] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.

[0212] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.

[0213] The vehicle according to the fifth embodiment includes the battery pack according to the fourth embodiment. Therefore, according to the present embodiment, it is possible to provide a vehicle equipped with a battery pack that has low resistance and can achieve a high capacity retention rate.

[0214] [Example] Examples will be described below, but the embodiments are not limited to the examples described below.

[0215] Example 1 A secondary battery was fabricated in the following manner.

[0216] <Preparation of positive electrode> The positive electrode active material is a spinel-type lithium nickel composite oxide (LiNi 0.5 Mn 1.5 O4:LNMO) powder was prepared. Aniline monomer was dissolved in acetone in an amount of 1% by mass relative to the mass of LNMO to prepare a monomer-containing solution. LNMO powder was added to the obtained monomer-containing solution to prepare a dispersion, which was stirred for 10 minutes and then dried by heating to remove the solvent. In this way, LNMO powder coated with aniline monomer was produced.

[0217] 100 parts by mass of the obtained powder, 5 parts by mass of acetylene black as a conductive material, and 5 parts by mass of alginic acid binder as a water-based binder were added to pure water and mixed to prepare a slurry. This slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 12 μm to obtain a laminate, which was then dried in a thermostatic chamber at 120° C. and pressed to obtain a positive electrode.

[0218] <Preparation of negative electrode> A slurry was prepared by adding 100 parts by mass of niobium titanium composite oxide (Nb2TiO7:NTO) powder as the negative electrode active material, 4 parts by mass of acetylene black as the conductive material, and 2 parts by mass of carboxymethyl cellulose (CMC) and 2 parts by mass of styrene butadiene copolymer (SBR) as the binder to pure water and mixing them. This slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 12 μm to obtain a laminate, and this laminate was dried in a thermostatic chamber at 120 ° C. and then pressed to obtain a negative electrode.

[0219] <Preparation of electrode groups> A positive electrode, a separator, a negative electrode, and a separator were laminated in this order to obtain a laminate. The laminate was then spirally wound. A flat electrode group was produced by hot pressing the laminate at 80°C. The obtained electrode group was housed in a pack made of a laminate film having a three-layer structure of a nylon layer, an aluminum layer, and a polyethylene layer and a thickness of 0.1 mm, and dried in a vacuum at 120°C for 16 hours.

[0220] <Preparation of non-aqueous electrolyte> A non-aqueous electrolyte was obtained by dissolving 1 mol / L of LiPF6 as an electrolyte in a mixed solvent of propylene carbonate (PC) and diethyl carbonate (DEC) (volume ratio 1:2). The electrolyte was prepared in an argon box.

[0221] <Preparation of secondary batteries, initial charging and charge / discharge cycle testing> A non-aqueous electrolyte was injected into the laminate film pack housing the electrode group, and the pack was then completely sealed by heat sealing to obtain a secondary battery in an uncharged state.

[0222] The secondary battery thus fabricated was subjected to a charge-discharge cycle test in an environment of 25°C. In the charge-discharge test, the battery was initially charged to 3.6 V at 20 mA, and then discharged to 2.3 V at 20 mA. The average operating potential of the positive electrode during the initial charge was 4.7 V (vs. Li / Li +). After that, charging and discharging were performed at 100 mA, the upper part of the laminate pack was opened under an Ar atmosphere, and the gas inside was discharged under vacuum. Then, the upper part of the laminate pack was completely sealed again by heat sealing. Furthermore, charging and discharging were performed at 20 mA up to 3.6 V, and the capacity of the battery was confirmed, and then charging and discharging were repeated 100 cycles at 100 mA. The capacity retention rate was calculated from the initial discharge capacity and the discharge capacity at the 100th cycle. In addition, the secondary battery after 100 cycles was sealed in a container with a vacuum inside, and then the exterior member was opened and the amount of gas that had flowed out was measured.

[0223] (Examples 2-5) A secondary battery was produced in the same manner as in Example 1, except that the amount of monomer contained in the monomer-containing solution was changed according to the column of "Conductive polymer coating amount (mass %)" in Table 1.

[0224] Example 6 A secondary battery was produced in the same manner as in Example 2, except that pyrrole was used as the electropolymerizable monomer.

[0225] Example 7 A secondary battery was produced in the same manner as in Example 2, except that thiophene was used as the electropolymerizable monomer.

[0226] Example 8 A secondary battery was produced in the same manner as in Example 2, except that a lithium phosphate compound (LiCoPO4:LCP) powder was used as the positive electrode active material.

[0227] Example 9 A secondary battery was produced in the same manner as in Example 6, except that LCP powder was used as the positive electrode active material.

[0228] Example 10 A secondary battery was produced in the same manner as in Example 7, except that LCP powder was used as the positive electrode active material.

[0229] Example 11 A secondary battery was produced in the same manner as in Example 2, except that the amount of alginic acid binder added was changed to 2 parts by mass when preparing the positive electrode slurry.

[0230] Example 12 A secondary battery was produced in the same manner as in Example 2, except that the amount of the alginic acid binder added was changed to 8 parts by mass when preparing the positive electrode slurry.

[0231] ( reference Example 13) A secondary battery was produced in the same manner as in Example 11, except that the type of the aqueous binder was changed to carboxymethyl cellulose (CMC).

[0232] ( reference Example 14) A secondary battery was produced in the same manner as in Example 2, except that the type of the aqueous binder was changed to carboxymethyl cellulose (CMC).

[0233] Example 15 The type of negative electrode active material was changed from niobium titanium composite oxide (NTO) to lithium titanium composite oxide (Li4Ti5O 12 A secondary battery was produced in the same manner as in Example 2, except that the PET film was changed to LTO.

[0234] Comparative Example 1 Except for not using an electrolytically polymerizable monomer, a secondary battery was produced in the same manner as in Example 1. That is, the positive electrode active material in Comparative Example 1 was an LNMO powder not having a conductive polymer coating.

[0235] Comparative Example 2 A secondary battery was produced in the same manner as in Example 1, except that the amount of the monomer contained in the monomer-containing solution was changed to 10 mass % relative to the mass of the LNMO powder used.

[0236] Comparative Example 3 A secondary battery was produced in the same manner as in Example 2, except that PVDF was used as an organic solvent binder instead of the aqueous binder, and the amount of PVDF added was changed to 3 parts by mass per 100 parts by mass of the positive electrode active material. PVDF, which is added as a binder when producing the positive electrode slurry, is added in a state dissolved in N-methyl-2-pyrrolidone (NMP) solvent. Therefore, when a positive electrode active material having a coating of aniline monomer is added to the slurry, at least a part of the coating of aniline monomer is dissolved in the slurry. The aniline monomer dissolved in the slurry dissolves in the electrolyte, becomes a by-reaction component, and generates a large amount of gas.

[0237] Comparative Example 4 Instead of LNMO, a cathode active material with an average operating potential of 4.0 V (vs. Li / Li + A secondary battery was fabricated in the same manner as in Example 2, except that LiMn2O4 (LMO) powder was used.

[0238] <Direct Current (DC) resistance measurement> For the secondary batteries produced in each example, DC resistance measurements were carried out as follows. The secondary battery was discharged at a constant current (CC) of 0.2 C until the voltage reached 2.5 V. Thereafter, the secondary battery was charged at a constant current (CC) of 0.2 C until the voltage reached 3.6 V. Next, the secondary battery was charged at a constant voltage (CV) of 3.11 V until the current value reached 1 / 20 C, thereby setting the state of charge of the secondary battery to SOC50%. The secondary battery adjusted to SOC50% was discharged at constant currents (CC) of 1 C and 10 C for 200 ms, respectively, and the DC resistance [mΩ] was calculated from the difference between the voltage value and the current value at this time.

[0239] The above results are summarized in Table 1. In Table 1, the column "Conductive polymer coating amount (mass %)" shows the mass ratio of the conductive polymer to the mass of the lithium composite oxide particles contained in the active material containing layer as the positive electrode active material. The column "Water-soluble polymer amount (mass %)" shows the mass ratio of the water-soluble polymer in the positive electrode active material containing layer.

[0240] [Table 1]

[0241] The following can be seen from Table 1: Example 1 12, The positive electrode active material-containing layer of each of Examples 1 to 5 contains one or more lithium composite oxide particles that exhibit an operating potential of 4.4 V or more versus metallic lithium. At least a portion of the surface of these lithium composite oxide particles is coated with a conductive polymer. The mass ratio of the conductive polymer to the mass of the one or more lithium composite oxide particles is within a range of 0.5% by mass to 5.0% by mass. In addition, the positive electrode active material-containing layer contains a water-soluble polymer. Therefore, in Examples 1 to 12, All of the 15 batteries achieved excellent capacity retention, low DC resistance, and low gas generation.

[0242] Examples 1-7 and 11-1 using lithium nickel manganese oxide (LNMO) as the positive electrode active material 12, When comparing Example 1-7 and Example 1-15 with Comparative Example 1-3, which also used LNMO, 12, It can be seen that, for Example 15, both a high capacity retention rate and low resistance were achieved. For Examples 8 to 10, which used the lithium phosphate compound LiCoPO4 (LCP), both a high capacity retention rate and low resistance were achieved.

[0243] In Comparative Example 1, since the LNMO particles were not coated with a conductive polymer, contact between the LNMO particles and the non-aqueous electrolyte could not be suppressed, and gas generation was increased. As a result, the capacity retention rate was poor. In Comparative Example 2, the LNMO particles as the active material were coated with an excessive amount of conductive polymer, and the DC resistance increased significantly. Comparative Example 3 is an example in which PVDF was used as an organic solvent-based binder as the positive electrode binder. In this case, the aniline monomer covering the surface of the positive electrode active material particles is dissolved into the organic solvent when the positive electrode slurry is prepared. Therefore, it is considered that the conductive polymer was not coated on the active material surface even when the initial charge was performed. As a result, it is considered that the side reaction on the surface of the LNMO particles as the positive electrode active material could not be suppressed, and gas generation increased and the capacity retention rate decreased.

[0244] In Comparative Example 4, the positive electrode active material (lithium composite oxide) had an average operating potential of 4.0 V (vs. Li / Li + This is an example in which lithium manganese oxide (LiMn2O4:LMO) of 10 ...

[0245] As shown in Examples 2 to 4, when the ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles as the positive electrode active material is within the range of 1.0 mass% to 4.0 mass%, the capacity retention rate and DC resistance are well-balanced and excellent, compared to when it is outside this range. 12, In No. 15, since the water-soluble polymer used had an HLB value in the range of 15 to 19, the positive electrode active material-containing layer was stable against the non-aqueous electrolyte.

[0246] According to at least one of the above-described embodiments and examples, a positive electrode is provided. The positive electrode includes a positive electrode active material-containing layer containing positive electrode active material particles and a water-soluble polymer. The positive electrode active material particles include lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium, and a conductive polymer covering at least a part of the surface of the lithium composite oxide particles. The ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 0.5% by mass to 5.0% by mass. This positive electrode has low resistance and can achieve a high capacity retention rate.

[0247] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are also included in the scope of the invention and its equivalents described in the claims. The invention as described in the claims of the present application as originally filed is set forth below. [1] A positive electrode active material-containing layer including positive electrode active material particles and a water-soluble polymer; The positive electrode active material particles are Lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium; and a conductive polymer that coats at least a part of the surface of the lithium composite oxide particles, A positive electrode in which the ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 0.5% by mass to 5.0% by mass. [2] The positive electrode according to [1], wherein the conductive polymer is at least one selected from the group consisting of polyanilines, polypyrroles, and polythiophenes. [3] The positive electrode according to [1] or [2], wherein the ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 1.0 mass % to 4.0 mass %. [4] The positive electrode according to any one of [1] to [3], wherein the water-soluble polymer has an HLB (hydrophilic-lipophilic balance) value in the range of 8 or more and 20 or less. [5] The positive electrode according to any one of [1] to [4], wherein the mass ratio of the water-soluble polymer in the positive electrode active material-containing layer is within a range of 1 mass % to 10 mass %. [6] The positive electrode according to any one of [1] to [5], wherein the water-soluble polymer is at least one selected from the group consisting of an acrylic polymer, a urethane polymer, carboxymethyl cellulose (CMC), an alginic acid polymer, a polyether, a polyvinyl alcohol, a water-soluble polyester, and a dicarboxylated polysaccharide. [7] The positive electrode according to any one of [1] to [6], wherein the lithium composite oxide includes at least one selected from the group consisting of lithium nickel manganese oxides and lithium phosphate compounds. [8] A positive electrode according to any one of [1] to [7], A negative electrode; and an electrolyte. [9] The negative electrode includes a negative electrode active material-containing layer containing a negative electrode active material, The secondary battery according to [8], wherein the negative electrode active material contains at least one titanium-containing oxide selected from the group consisting of titanium oxide, lithium titanium composite oxide, niobium titanium composite oxide, and sodium niobium titanium composite oxide.

[10] A battery pack comprising the secondary battery described in [9].

[11] An external terminal for supplying current; The battery pack according to

[10] , further comprising a protection circuit.

[12] A battery pack as described in

[10] or

[11] , comprising a plurality of the secondary batteries, the secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.

[13] A vehicle equipped with a battery pack described in any one of

[10] to

[12] .

[14] A vehicle as described in

[13] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy. [Explanation of symbols]

[0248] Reference Signs List 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b, 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 5c...positive electrode active material particles, 5d...water-soluble polymer, 5e...positive electrode conductive material, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 22a...other end, 23...negative electrode side lead, 23a...other end , 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 51...lithium composite oxide particles, 52...conductive polymer, 100...secondary battery, 200...assembled battery, 200a...assembled battery, 200b...assembled battery, 200c...assembled battery, 300...battery pack, 300a...battery pack, 300b...battery pack, 300c...battery pack, 301a...assembled battery monitoring device, 301b...assembled battery monitoring device, 301c...assembled battery monitoring device, 342...positive electrode connector, 343...negative electrode connector, 345...thermistor, 346...protective circuit, 342a...wiring, 343a...wiring, 350...for energizing External terminal, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.

Claims

1. a positive electrode active material-containing layer including positive electrode active material particles and a water-soluble polymer; The positive electrode active material particles are Lithium composite oxide particles exhibiting an operating potential of 4.4 V or more versus metallic lithium; and a conductive polymer that coats at least a part of the surface of the lithium composite oxide particles, a ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 0.5 mass% to 5.0 mass%; The positive electrode, wherein the water-soluble polymer comprises an alginate polymer.

2. 2. The positive electrode according to claim 1, wherein the conductive polymer is at least one selected from the group consisting of polyanilines, polypyrroles, and polythiophenes.

3. 3. The positive electrode according to claim 1, wherein the ratio of the mass of the conductive polymer to the mass of the lithium composite oxide particles is within a range of 1.0% by mass to 4.0% by mass.

4. The positive electrode according to any one of claims 1 to 3, wherein the water-soluble polymer has an HLB (hydrophilic-lipophilic balance) value in the range of 8 or more and 20 or less.

5. 5. The positive electrode according to claim 1, wherein the mass ratio of the water-soluble polymer in the positive electrode active material-containing layer is within a range of 1 mass % to 10 mass %.

6. The positive electrode according to any one of claims 1 to 5, wherein the lithium composite oxide comprises at least one selected from the group consisting of lithium nickel manganese oxide and lithium phosphate compound.

7. The positive electrode according to any one of claims 1 to 6, A negative electrode; and an electrolyte.

8. The negative electrode includes a negative electrode active material-containing layer that contains a negative electrode active material, 8. The secondary battery according to claim 7, wherein the negative electrode active material contains at least one titanium-containing oxide selected from the group consisting of titanium oxide, lithium titanium composite oxide, niobium titanium composite oxide, and sodium niobium titanium composite oxide.

9. A battery pack comprising the secondary battery according to claim 8.

10. An external terminal for supplying electricity; 10. The battery pack of claim 9, further comprising a protection circuit.

11. 11. The battery pack according to claim 9, comprising a plurality of the secondary batteries, the secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.

12. A vehicle equipped with the battery pack according to any one of claims 9 to 11.

13. The vehicle of claim 12, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.

Citation Information

Patent Citations

  • Battery

    JP1995263026A

  • Manufacturing method of electrode for lithium secondary battery and electrode for lithium secondary battery as well as lithium secondary battery

    JP2002008639A

  • Positive electrode active substance, its manufacturing method and paste, positive electrode and non-aqueous electrolyte secondary battery using the same

    JP2002358959A

  • Lithium ion secondary battery positive electrode and method for producing the same, and lithium ion secondary battery

    JP2016186854A

  • Method for manufacturing positive electrode for high-performance lithium ion secondary battery

    JP2017091697A