Semiconductor Device

The semiconductor device addresses the issue of avalanche breakdown in the gate pad region by incorporating a trench structure with specific semiconductor regions to equalize the pn interface depth, enhancing reliability and breakdown voltage maintenance.

JP7563002B2Active Publication Date: 2024-10-08FUJI ELECTRIC CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020110963
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-26
Publication Date
2024-10-08
Estimated Expiration
2040-06-26

AI Technical Summary

Technical Problem

Conventional silicon carbide semiconductor devices face issues with avalanche breakdown and reliability in the gate pad region due to concentrated electric fields, as the trench structure does not allow for the provision of mold base regions, leading to poor breakdown voltage maintenance.

Method used

The semiconductor device incorporates a trench structure in the gate pad region with a first and second trench, a gate electrode, and specific semiconductor regions to equalize the pn interface depth, ensuring the mold base regions are present and distributed to prevent electric field concentration.

Benefits of technology

This design enhances the reliability of the gate pad region by preventing avalanche current concentration and maintaining breakdown voltage, improving the overall reliability of the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563002000001
    Figure 0007563002000001
  • Figure 0007563002000002
    Figure 0007563002000002
  • Figure 0007563002000003
    Figure 0007563002000003
Patent Text Reader

Abstract

To provide a semiconductor device capable of improving reliability of a gate pad region by eliminating concentration of an avalanche current in the gate pad region.SOLUTION: A semiconductor device comprises a semiconductor substrate 1 of a first conductivity type including an active part 40 and a gate pad part 50, a first semiconductor layer 2 of the first conductivity type, and a second semiconductor layer 6 of a second conductivity type. The active part 40 comprises a first semiconductor region 7 of the first conductivity type, a first trench 16a, a gate insulation film 9b, a first gate electrode 10, an interlayer insulation film 11, and a second semiconductor region 3 of the second conductivity type. The gate pad part 50 comprises a second trench 16b, an insulation film 9b, a second gate electrode 10b, a fourth semiconductor region 3b of the second conductivity type, and a gate electrode pad 14. A polycrystalline silicon film is provided between the gate electrode pad 14 and the semiconductor substrate 1.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device. [Background technology]

[0002] Silicon carbide (SiC) is expected to be a next-generation semiconductor material to replace silicon (Si). Compared to conventional semiconductor elements that use silicon carbide as a semiconductor material, semiconductor elements that use silicon carbide as a semiconductor material (hereinafter referred to as silicon carbide semiconductor devices) have various advantages, such as the ability to reduce the resistance of the element in the on-state to one-hundredth of that of conventional semiconductor elements that use silicon as a semiconductor material, and the ability to be used in higher temperature environments (200°C or higher). This is due to the characteristics of the material itself, namely, that the band gap of silicon is about three times larger than that of silicon, and that the dielectric breakdown field strength is nearly one order of magnitude larger than that of silicon.

[0003] Silicon carbide semiconductor devices that have been commercially available to date include Schottky barrier diodes (SBDs) and vertical MOSFETs (metal oxide semiconductor field effect transistors) having a planar gate structure or a trench gate structure.

[0004] The planar gate structure is a MOS gate structure in which a MOS gate is provided in a flat plate shape on the front surface of a semiconductor substrate. The trench gate structure is a MOS gate structure in which a MOS gate is embedded in a trench formed on the front surface of a semiconductor substrate (semiconductor chip), and a channel (inversion layer) is formed along the sidewall of the trench in a direction perpendicular to the front surface of the semiconductor substrate. Therefore, compared to a planar gate structure in which a channel is formed along the front surface of a semiconductor substrate, the unit cell (element constituent unit) density per unit area can be increased, and the current density per unit area can be increased, which is advantageous in terms of cost.

[0005] The structure of a conventional silicon carbide semiconductor device will be described by taking a trench MOSFET as an example. Fig. 15 is a cross-sectional view showing the structure of an active region of a conventional silicon carbide semiconductor device. Fig. 15 shows the structure of an active region 140 through which a current flows when the device is on. As shown in Fig. 15, in a trench MOSFET 170, n + The front surface of the silicon carbide substrate 101 is - A silicon carbide epitaxial layer 102 is deposited. - The n-type silicon carbide epitaxial layer 102 + An n-type high concentration region 105 is provided on the surface side opposite to the n-type silicon carbide substrate 101 side. - The first p-type silicon carbide epitaxial layer 102 is formed so as to cover the entire bottom surface of the trench 116. + A mold base region 103 is optionally provided.

[0006] In addition, as the MOS structure, a p-type silicon carbide epitaxial layer 106, a n + Type source region 107, p + The semiconductor device includes a contact region 108, a gate insulating film 109, a gate electrode 110, an interlayer insulating film 111, a source electrode 112, a back electrode 113, a trench 116, a source electrode pad (not shown), and a drain electrode pad (not shown). The source electrode 112 is an n + A p-type source region 107 is provided on the p-type silicon carbide epitaxial layer 106 , and a source electrode pad is provided on the source electrode 112 .

[0007] The bottom surface of the trench 116 is provided with a first p + By providing the base region 103, the electric field is prevented from concentrating on the bottom surface of the trench 116, and the gate insulating film 109 is protected. + The base region 103 is not floating, but is connected to the source electrode 112 and must be at the same potential. + A structure in which the second base region 104 is selectively provided is known. This prevents punch-through and maintains the breakdown voltage. +The second p-type base region 104 is provided on the sidewall of the m-plane of the trench 116, so that the a-plane having high mobility can be used as a channel. + By providing the p-type region in the base region 104, it is no longer necessary to provide a p-type region between the trenches 116, and the cell pitch can be reduced.

[0008] Also, a semiconductor device is known that can reduce the electric field applied to the bottom surface of the gate trench when the semiconductor device is in an off state by providing an electric field reduction region in contact with the bottom surface of the gate trench (see Patent Document 1 below).Also, a semiconductor device is known in which a second trench is provided in the non-element region, the bottom surface of which reaches the drift layer, and a low resistance region is provided in the second trench via an inner surface insulating film to form a capacitance, and during high-speed switching, a displacement current passing through the second reduction region below the second trench is branched off to the low resistance region, thereby suppressing the magnitude of the potential drop caused by the displacement current (see Patent Document 2 below). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2019-195081 A [Patent Document 2] International Publication No. 2019 / 159351 Summary of the Invention [Problem to be solved by the invention]

[0010] Fig. 16 is a cross-sectional view showing a first structure of a gate pad region of a conventional silicon carbide semiconductor device. Fig. 17 is a cross-sectional view showing a second structure of a gate pad region of a conventional silicon carbide semiconductor device. In the gate pad region 150, similar to the active region 140, n + On the front surface of the silicon carbide substrate 101, -A n-type silicon carbide epitaxial layer 102 and a p-type silicon carbide epitaxial layer 106 are provided. A gate electrode pad 114 is provided on the p-type silicon carbide epitaxial layer 106 via an interlayer insulating film 111. As shown in FIG. 17, a gate electrode wiring 115 may be provided in the interlayer insulating film 111. + A back surface electrode 113 is provided on the back surface of the silicon carbide substrate 101 .

[0011] As shown in Fig. 16 and Fig. 17, in the conventional trench structure, the trench structure is not provided in the gate pad region 150. + The base region 103 and the second p + Therefore, in the gate pad region 150, the p-type silicon carbide epitaxial layer 106 and the n-type silicon carbide epitaxial layer 107 cannot be provided. - The pn interface with the p-type silicon carbide epitaxial layer 102 is located shallower from the surface of the p-type silicon carbide epitaxial layer 106 than the active region 140, and an electric field is concentrated at the pn interface of the gate pad region 150. This causes avalanche breakdown in the gate pad region 150, making it impossible to maintain a breakdown voltage, and thus causing a problem of deteriorating reliability of the gate pad region 150.

[0012] SUMMARY OF THE PRESENT EMBODIMENT In order to solve the above-mentioned problems associated with the conventional techniques, an object of the present invention is to provide a semiconductor device capable of eliminating the concentration of avalanche current in the gate pad region and improving the reliability of the gate pad region. [Means for solving the problem]

[0013] In order to solve the above-mentioned problems and achieve the object of the present invention, the semiconductor device according to the present invention has the following features. The semiconductor device includes a semiconductor substrate of a first conductivity type having an active portion and a gate pad portion, a first semiconductor layer of a first conductivity type having a lower impurity concentration than the semiconductor substrate and provided on a front surface of the semiconductor substrate, and a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate side. The active portion includes a first semiconductor region of a first conductivity type selectively provided on a surface layer of the second semiconductor layer opposite to the semiconductor substrate side, a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer, a first gate electrode provided inside the first trench via a gate insulating film, an interlayer insulating film provided on the first gate electrode, a first electrode provided on the surfaces of the second semiconductor layer and the first semiconductor region, a second electrode provided on the back surface of the semiconductor substrate, and a second semiconductor region of a second conductivity type provided so as to contact a bottom of the first trench. The gate pad portion includes a second trench that penetrates the second semiconductor layer and reaches the first semiconductor layer, a second gate electrode provided inside the second trench via an insulating film, a fourth semiconductor region of a second conductivity type provided so as to contact a bottom of the second trench, and a gate electrode pad electrically connected to the second gate electrode. A polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate. The insulating film is also provided on the surface of the semiconductor substrate in a mesa region between adjacent second trenches, and the polycrystalline silicon film is a gate wiring electrode provided on the insulating film on the surface of the mesa region.

[0014] In order to solve the above-mentioned problems and achieve the object of the present invention, the semiconductor device according to the present invention has the following features. The semiconductor device includes a semiconductor substrate of a first conductivity type having an active portion and a gate pad portion, a first semiconductor layer of a first conductivity type having a lower impurity concentration than the semiconductor substrate and provided on a front surface of the semiconductor substrate, and a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate side. The active portion includes a first semiconductor region of a first conductivity type selectively provided on a surface layer of the second semiconductor layer opposite to the semiconductor substrate side, a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer, a first gate electrode provided inside the first trench via a gate insulating film, an interlayer insulating film provided on the first gate electrode, a first electrode provided on the surfaces of the second semiconductor layer and the first semiconductor region, a second electrode provided on the back surface of the semiconductor substrate, and a second semiconductor region of a second conductivity type provided so as to contact a bottom of the first trench. The gate pad portion includes a second trench that penetrates the second semiconductor layer and reaches the first semiconductor layer, a second gate electrode provided inside the second trench via an insulating film, a fourth semiconductor region of a second conductivity type provided so as to contact a bottom of the second trench, and a gate electrode pad electrically connected to the second gate electrode. A polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate. The extension direction of the second trench is parallel to a wire connected to the gate pad portion. In order to solve the above-mentioned problems and achieve the object of the present invention, the semiconductor device according to the present invention has the following features. The semiconductor device includes a semiconductor substrate of a first conductivity type having an active portion and a gate pad portion, a first semiconductor layer of a first conductivity type having a lower impurity concentration than the semiconductor substrate and provided on a front surface of the semiconductor substrate, and a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate.The active section includes a first semiconductor region of a first conductivity type selectively provided in a surface layer of the second semiconductor layer on the side opposite to the semiconductor substrate side, a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer, a first gate electrode provided in the first trench via a gate insulating film, an interlayer insulating film provided on the first gate electrode, a first electrode provided on the surface of the second semiconductor layer and the first semiconductor region, a second electrode provided on the back surface of the semiconductor substrate, and a second semiconductor region of a second conductivity type provided so as to contact the bottom of the first trench. The gate pad section includes a second trench penetrating the second semiconductor layer and reaching the first semiconductor layer, a second gate electrode provided in the second trench via an insulating film, a fourth semiconductor region of a second conductivity type provided so as to contact the bottom of the second trench, and a gate electrode pad electrically connected to the second gate electrode. A polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate. The polycrystalline silicon film is the second gate electrode, and the second gate electrode is provided on the entire surface between the gate electrode pad and the semiconductor substrate. In order to solve the above-mentioned problems and achieve the object of the present invention, the semiconductor device according to the present invention has the following features. The semiconductor device includes a semiconductor substrate of a first conductivity type having an active portion and a gate pad portion, a first semiconductor layer of the first conductivity type having a lower impurity concentration than the semiconductor substrate and provided on a front surface of the semiconductor substrate, and a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate. The active portion includes a first semiconductor region of a first conductivity type selectively provided in a surface layer of the second semiconductor layer opposite to the semiconductor substrate side, a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer, a first gate electrode provided inside the first trench via a gate insulating film, an interlayer insulating film provided on the first gate electrode, a first electrode provided on the surfaces of the second semiconductor layer and the first semiconductor region, a second electrode provided on the back surface of the semiconductor substrate, and a second semiconductor region of a second conductivity type provided so as to contact the bottom of the first trench.The gate pad portion includes a second trench that penetrates the second semiconductor layer and reaches the first semiconductor layer, a second gate electrode provided inside the second trench via an insulating film, a fourth semiconductor region of a second conductivity type provided so as to contact the bottom of the second trench, a gate electrode pad electrically connected to the second gate electrode, and a fifth semiconductor region of a second conductivity type provided in the first semiconductor layer so as to contact a sidewall of the second trench and electrically connecting the second semiconductor region and the fourth semiconductor region. A polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate. The fourth semiconductor region has a higher impurity concentration than the second semiconductor region.

[0015] In addition, the semiconductor device of the present invention is characterized in that, in the above-mentioned invention, it further comprises a third semiconductor region of a second conductivity type provided in the first semiconductor layer so as to contact at least one sidewall of the first trench in a second direction perpendicular to a first direction parallel to the extension direction of the first trench, electrically connecting the second semiconductor region and the second semiconductor layer.

[0016] In addition, in the semiconductor device according to the present invention, in the above-mentioned invention, the third semiconductor region is provided in plurality at intervals in the first semiconductor layer.

[0017] In addition, the semiconductor device of the present invention is characterized in that, in the above-mentioned invention, it further comprises a fifth semiconductor region of a second conductivity type provided in the first semiconductor layer so as to contact a side wall of the second trench and electrically connect the second semiconductor region and the fourth semiconductor region.

[0018] In addition, in the semiconductor device according to the present invention, in the above-mentioned invention, the fifth semiconductor region is provided in the first semiconductor layer so as to contact both trench sidewalls of the second trench.

[0020] In addition, in the semiconductor device according to the present invention, the second trench is wider than the first trench.

[0022] In addition, in the semiconductor device according to the present invention, the second trench is deeper than the first trench.

[0023] In addition, the semiconductor device of the present invention is characterized in that, in the above-mentioned invention, the first trench provided at the outermost periphery of the active portion does not have the first semiconductor region provided on the sidewall on the gate pad portion side in a second direction perpendicular to a first direction parallel to the extension direction of the first trench.

[0025] According to the above-mentioned invention, the first p-type semiconductor layer is formed in the gate pad region and covers the bottom surface of the trench. + A second conductive type base region (a second semiconductor region of a second conductive type) is provided. This allows the active region and the gate pad region to form an n - A first silicon carbide epitaxial layer (a first semiconductor layer of a first conductivity type) and a first p +The pn interface with the base region is at the same depth from the surface of the silicon carbide semiconductor substrate, which prevents avalanche current from concentrating in the gate pad region, making it possible to maintain the breakdown voltage of the gate pad region and improving the reliability of the gate insulating film. Effect of the Invention

[0026] The semiconductor device according to the present invention has an advantage that it is possible to eliminate the concentration of avalanche current in the gate pad region and improve the reliability of the gate pad region. [Brief description of the drawings]

[0027] [Figure 1] 1 is a cross-sectional view showing a structure of an active region of a silicon carbide semiconductor device in accordance with a first embodiment. [Diagram 2] 1 is a cross-sectional view showing a first structure of a gate pad region of the silicon carbide semiconductor device in accordance with the first embodiment. [Diagram 3] 4 is a cross-sectional view showing a second structure of the gate pad region of the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 4] 4 is a cross-sectional view showing a third structure of the gate pad region of the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Diagram 5] 10 is a cross-sectional view showing a fourth structure of the gate pad region of the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 6] 10 is a cross sectional view showing a fifth structure of the gate pad region of the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 7] 1 is a top view showing a structure of a silicon carbide semiconductor device in accordance with a first embodiment. [Figure 8] 1 is a cross-sectional view (part 1) showing a state during manufacture of a silicon carbide semiconductor device according to a first embodiment. [Figure 9] FIG. 2 is a cross-sectional view (part 2) showing a state during manufacture of the silicon carbide semiconductor device according to the first embodiment. [Figure 10] 5 is a cross-sectional view (part 3) showing a state during the manufacture of the silicon carbide semiconductor device according to the first embodiment. FIG. [Figure 11] FIG. 4 is a cross-sectional view showing a state during the manufacture of the silicon carbide semiconductor device according to the first embodiment (part 4). [Figure 12] FIG. 5 is a cross-sectional view showing a state during the manufacture of the silicon carbide semiconductor device according to the first embodiment (part 5). [Figure 13] 10 is a cross-sectional view showing a structure of an active region and a gate pad region of a silicon carbide semiconductor device according to a second embodiment. FIG. [Figure 14] FIG. 11 is a top view showing a structure of a silicon carbide semiconductor device according to a second embodiment. [Figure 15] 1 is a cross-sectional view showing a structure of an active region of a conventional silicon carbide semiconductor device. [Figure 16] FIG. 1 is a cross-sectional view showing a first structure of a gate pad region of a conventional silicon carbide semiconductor device. [Figure 17] FIG. 11 is a cross-sectional view showing a second structure of a gate pad region of a conventional silicon carbide semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] A preferred embodiment of the semiconductor device according to the present invention will be described in detail below with reference to the accompanying drawings. In this specification and the accompanying drawings, in a layer or region prefixed with n or p, electrons or holes are the majority carriers, respectively. In addition, + and - attached to n or p respectively mean that the impurity concentration is higher and lower than that of a layer or region not prefixed with n or p. Note that in the following description of the embodiment and the accompanying drawings, the same reference numerals are attached to similar configurations, and duplicated explanations are omitted. In addition, in this specification, in the notation of Miller indices, "-" means a bar attached to the index immediately following it, and adding "-" before the index represents a negative index. In addition, the description of "same" or "equivalent" should include up to 5% in consideration of manufacturing variations.

[0029] (Embodiment 1) The semiconductor device according to the present invention is configured using a wide band gap semiconductor. In the first embodiment, a trench-type MOSFET 70 will be taken as an example of a silicon carbide semiconductor device fabricated (manufactured) using silicon carbide (SiC) as a wide band gap semiconductor. Fig. 1 is a cross-sectional view showing a structure of an active region of the silicon carbide semiconductor device according to the first embodiment.

[0030] In the silicon carbide semiconductor device according to the first embodiment, an edge termination region that surrounds the active region 40 and maintains a withstand voltage, and a gate pad region 50 that is connected to a gate electrode are provided on the outer periphery of the active region 40 through which a main current flows. In FIG. 1, only the active region 40 of a trench MOSFET 70 is shown.

[0031] 1, the trench MOSFET 70 includes a MOS gate having a trench gate structure on the front surface (the surface on the side of a p-type silicon carbide epitaxial layer 6 described later) of a semiconductor substrate. + A silicon carbide substrate (a semiconductor substrate of a first conductivity type) 1 is formed on the n - The n-type silicon carbide epitaxial layer (first semiconductor layer of a first conductivity type) 2 is epitaxially grown in that order. An n-type high concentration region 5 may be epitaxially grown on the n-type silicon carbide epitaxial layer 2.

[0032] The MOS gate of the trench gate structure is a p-type silicon carbide epitaxial layer (a second semiconductor layer of a second conductivity type) 6, + A first conductive type source region (first semiconductor region) 7, p + The semiconductor device is composed of a contact region 8, a trench (first trench) 16a, a gate insulating film 9, and a gate electrode (first gate electrode) 10. + The mold contact region 8 may not be provided.

[0033] Specifically, the trench 16a penetrates the p-type silicon carbide epitaxial layer 6 in the depth direction y from the front surface of the semiconductor substrate, and defines the n-type high concentration region 5 (or the n-type high concentration region 5 in the case where the n-type high concentration region 5 is not provided). -The trenches 16a reach the silicon carbide epitaxial layer 2 (hereinafter referred to as (2)). The depth direction y is the direction from the front surface to the back surface of the semiconductor substrate. The trenches 16a are arranged in a stripe pattern (see FIG. 7).

[0034] Inside the trench 16a, a gate insulating film 9 is provided along the inner wall of the trench 16a, and a gate electrode 10 is provided on the gate insulating film 9 so as to be embedded inside the trench 16a. One unit cell of the main semiconductor element is composed of the gate electrode 10 in one trench 16a and adjacent mesa regions 17a (regions between adjacent trenches 16a) sandwiching the gate electrode 10. Although only three trench MOS structures are shown in FIG. 1, more trench-structured MOS gate (insulated gate made of metal-oxide film-semiconductor) structures may be arranged in parallel.

[0035] n - An n-type region (hereinafter referred to as n-type high concentration region) 5 may be provided in the surface layer on the source side (the source electrode 12 side described later) of the silicon carbide epitaxial layer 2 so as to be in contact with the p-type silicon carbide epitaxial layer 6. The n-type high concentration region 5 is a so-called current spreading layer (CSL) that reduces the spreading resistance of carriers. The n-type high concentration region 5 is provided uniformly in a direction parallel to the front surface of the substrate (front surface of the semiconductor substrate) so as to cover the inner wall of the trench 16a, for example. The n-type high concentration region 5 is provided from the interface with the p-type silicon carbide epitaxial layer 6 to a position not reaching the bottom surface of the trench 16a. The n-type high concentration region 5 is deeper than the bottom surface of the trench 16a and is located at a position corresponding to a first p-type high concentration region described later. + It may be provided to a position shallower than the bottom surface of the mold base region 3 .

[0036] n - The inside of the silicon carbide epitaxial layer 2 is a first p + A first base region (a second semiconductor region of a second conductivity type) 3 may be selectively provided. +The mold base region 3 covers at least the bottom surface of the trench 16a and the bottom corners thereof. The bottom corners of the trench 16a are the boundaries between the bottom surface and the sidewalls of the trench 16a.

[0037] 1st p. + Type base region 3 and n - The pn junction with the first silicon carbide epitaxial layer 2 is formed at a position deeper on the drain side than the bottom surface of the trench 16a. + The depth position of the drain side end of the base region 3 is the first p + Type base region 3 and n - It is sufficient that the pn junction with the first silicon carbide epitaxial layer 2 is located deeper on the drain side than the bottom surface of the trench 16a, and various changes can be made according to design conditions. + The mold base region 3 can prevent a high electric field from being applied to the gate insulating film 9 along the bottom surface of the trench 16a.

[0038] The n-type n-type semiconductor layer 16a is formed so as to contact at least one of the trench side walls in a second direction (x direction) perpendicular to a first direction (z direction) parallel to the extension direction of the trench 16a. - The n-type silicon carbide epitaxial layer 2 (when the n-type high concentration region 5 is provided, - A second p-type silicon carbide epitaxial layer 2 and an n-type high concentration region 5 (hereinafter referred to as (2, 5)) are formed in the n-type silicon carbide epitaxial layer 2 and the n-type high concentration region 5 (hereinafter referred to as (2, 5)). + A second conductive type base region (third semiconductor region of the second conductivity type) 4 may be provided. One of the trench side walls may be the m-plane or the a-plane.

[0039] 2nd p. + The base region (third semiconductor region of the second conductivity type) 4 is formed by a p-type silicon carbide epitaxial layer 6 and a first p + The second p is provided so as to contact the mold base region 3. + The mold base region 4 has a bottom surface which is a first p + At the same depth as the base region 3, - The upper surface of the epitaxial layer 2 is a n-type silicon carbide epitaxial layer 3. + The second p+ The first p + The base region 3 and the p-type silicon carbide epitaxial layer 6 are electrically connected to form a first p + The base region 3 is not floating, but is set to the same potential as the source electrode 12. This makes it possible to prevent punch-through and maintain the breakdown voltage.

[0040] 2nd p. + The base region 4 is an n - In the silicon carbide epitaxial layer 2 (2, 5), a plurality of trenches 16a may be provided at intervals in a first direction parallel to the extension direction of the trenches 16a. In this case, one side wall of the trench 16a in the first direction is a second p + Type base region 4 and n - The epitaxial layers 2 (2, 5) are alternately in contact with the silicon carbide epitaxial layer 2 (2, 5).

[0041] Also, page 2 + The mold base region 4 may be provided on one sidewall of the trench 16a without any space therebetween. In this case, the one sidewall of the trench 16a in the first direction is the second p + It comes into contact with the mold base region 4 .

[0042] Inside the p-type silicon carbide epitaxial layer 6, + Type source region 7 and p + A contact region 8 is optionally provided. + The source region 7 is in contact with the gate insulating film 9 on the sidewall of the trench 16a, and faces the gate electrode 10 via the gate insulating film 9 on the sidewall of the trench 16a.

[0043] The interlayer insulating film 11 is provided on the entire front surface of the semiconductor substrate so as to cover the gate electrode 10. The interlayer insulating film 11 has a contact hole that penetrates the interlayer insulating film 11 in the depth direction y and reaches the front surface of the substrate.

[0044] The source electrode (first electrode) 12 is disposed in a contact hole opened in the interlayer insulating film 11 and is connected to the semiconductor substrate (n +The source electrode 12 is in ohmic contact with the n-type source region 7 and is electrically insulated from the gate electrode 10 by an interlayer insulating film 11. A source electrode pad (not shown) is provided on the source electrode 12. The source electrode 12 is an n-type + Type source region 7 and p + The p-type contact region 8 is in ohmic contact with the p-type contact region 8. + If the contact region 8 is not provided, the source electrode 12 is + The p-type source region 7 is in ohmic contact with the p-type silicon carbide epitaxial layer 6 .

[0045] A back surface electrode (second electrode) 13 serving as a drain electrode is provided on the back surface of the semiconductor substrate. A drain electrode pad (not shown) is provided on the back surface electrode 13.

[0046] 2 is a cross-sectional view showing a first structure of a gate pad region of the silicon carbide semiconductor device according to the first embodiment. In the gate pad region 50, similarly to the active region 40, n + On the front surface of the silicon carbide substrate 1, - A n-type silicon carbide epitaxial layer 2 and a p-type silicon carbide epitaxial layer 6 are provided in the gate pad region 50. + Silicon carbide substrate 1, n - The thickness and impurity concentration of each of the p-type silicon carbide epitaxial layer 2 and the p-type silicon carbide epitaxial layer 6 are set to be equal to or larger than the n-type silicon carbide epitaxial layer 2 in the active region. + Silicon carbide substrate 1, n - The p-type silicon carbide epitaxial layer 2 in the gate pad region 50 is the same as the p-type silicon carbide epitaxial layer 6. The p-type silicon carbide epitaxial layer 6 in the gate pad region 50 is connected to the p-type silicon carbide epitaxial layer 6 in the active region 40.

[0047] In the first embodiment, a trench gate structure consisting of a trench (second trench) 16b, a gate insulating film (insulating film) 9b, and a gate electrode (second gate electrode) 10b is provided in the gate pad region 50. The width and depth of the trench 16b in the gate pad region 50 are the same as the width and depth of the trench 16a in the active region 40. In the gate pad region 50, the gate insulating film 16b is also provided on the surface of the semiconductor substrate in the mesa region 17b between adjacent trenches 16b.

[0048] Also, n - The inside of the silicon carbide epitaxial layer 2 is a first p + A first base region (fourth semiconductor region of the second conductivity type) 3b may be selectively provided. + The base region 3b covers at least the bottom surface and the bottom corners of the trench 16b, as well as the active region 40. + The width and depth of the base region 3b are the first p + The width and depth are the same as those of the mold base region 3 .

[0049] An interlayer insulating film 11 is provided on the entire front surface of the semiconductor substrate via a gate insulating film 9b, and a gate electrode pad 14 electrically connected to the gate electrode 10 is provided on the interlayer insulating film 11. A back surface electrode 13 serving as a drain electrode is provided on the back surface of the semiconductor substrate. A drain electrode pad (not shown) is provided on the back surface electrode 13. In addition, n - An n-type high concentration region 5 may be provided in the surface layer on the source side of the p-type silicon carbide epitaxial layer 2 so as to be in contact with the p-type silicon carbide epitaxial layer 6 .

[0050] In this manner, in the first embodiment, the trench 16b is also provided in the gate pad region 50, and the first p + The active region 40 and the gate pad region 50 form an n-type base region 3b. - The first p-type silicon carbide epitaxial layer 2 +The pn interfaces with the type base regions 3, 3b are at the same depth from the surface of the silicon carbide semiconductor substrate. This prevents avalanche current from concentrating in the gate pad region 50, making it possible to maintain the breakdown voltage of the gate pad region 50 and improve the reliability of the gate insulating film 9.

[0051] Here, the trench 16b in the gate pad region 50 may or may not be connected to the trench 16a in the active region 40. When the trench 16b is connected to the trench 16a, + The base region 3b is the first p + By connecting it to the mold base region 3, the first p + The base region 3b can be set to the same potential as the source electrode 12. When the trench 16b is not connected to the trench 16a, the width and depth of the trench 16b can be made larger than those of the trench 16a. + The impurity concentration of the first p-type base region 3b in the active region 40 is + It can be made higher than the mold base region 3. This makes it easier for holes to be concentrated in the trench 16b, making it easier to control the holes.

[0052] FIG. 3 is a cross-sectional view showing a second structure of the gate pad region of the silicon carbide semiconductor device according to the first embodiment. As shown in FIG. 3, in the gate pad region 50, the interlayer insulating film 11A is provided on the entire front surface of the semiconductor substrate via the gate insulating film 9b so as to cover the p-type silicon carbide epitaxial layer 6. The interlayer insulating film 11A has a contact hole penetrating the interlayer insulating film 11A in the depth direction y to reach the front surface of the substrate. In the gate pad region 50, a gate electrode wiring (polycrystalline silicon film) 15 made of polycrystalline silicon (Poly-Si) is provided on the entire front surface of the semiconductor substrate. The gate electrode wiring 15 may be made of a high melting point metal such as titanium or tungsten, a silicide or nitride thereof, or a laminated film thereof, other than polycrystalline silicon. The gate electrode wiring 15 is in ohmic contact with the gate electrode 10 in the contact hole provided in the interlayer insulating film 11A, and is electrically insulated from the p-type silicon carbide epitaxial layer 6 by the interlayer insulating film 11A.

[0053] A gate electrode pad 14 is provided on the gate electrode wiring 15 via an interlayer insulating film 11B. + Between the gate electrode pad 1 and the silicon carbide substrate 1, a polycrystalline silicon film is provided as a gate electrode wiring 15 on the entire surface. The gate electrode wiring 15 and the gate electrode pad 14 are electrically connected. In FIG. 3, the interlayer insulating film 11B in the gate pad region 50 is not provided with a contact hole, and the gate electrode wiring 15 and the gate electrode pad 14 are connected in a portion other than the gate pad region 50. In this case, there is an advantage that the bonding area when bonding the wire to the gate electrode pad 14 is not reduced. Furthermore, since the interlayer insulating film 11B is always provided directly below the gate electrode pad 14, damage to the element structure below is small. In addition, it is also possible to provide a contact hole in the interlayer insulating film 11B in the gate pad region 50, and electrically connect the gate electrode wiring 15 and the gate electrode pad 14 through the contact hole. In this case, the interlayer insulating film 11B between the gate electrode pad 14 and the gate electrode wiring 15 can be opened widely, and the contact resistance between the gate electrode pad 14 and the gate electrode wiring 15 can be reduced.

[0054] In this way, by providing the gate electrode wiring 15 on the entire lower surface of the gate electrode pad 14 in the gate pad region 50, the surface of the gate electrode pad 15 can be made flat, and the bonding area can be increased when bonding a wire to the gate electrode pad 14. Furthermore, since the cross-sectional area of ​​the gate electrode wiring 15 under the gate electrode pad 14 is increased, the gate resistance (Rg) can be reduced.

[0055] 4 is a cross-sectional view showing a third structure of the gate pad region of the silicon carbide semiconductor device according to the first embodiment. As shown in FIG. 4, the second p + A second conductive type base region (a fifth semiconductor region of a second conductive type) 4b is selectively provided. + The base region 4b is formed by a p-type silicon carbide epitaxial layer 6 and a first p + The second p in the gate pad region 50 is provided so as to contact the base region 3b. + The width and depth of the base region 4b are the second p + The width and depth are the same as those of the mold base region 4 .

[0056] The p-type silicon carbide epitaxial layer 6 in the gate pad region 50 is continuously connected to the p-type silicon carbide epitaxial layer 6 in the active region 40 in the first direction (z direction) (see FIG. 7). + The first base region 4b + The first p-type base region 3b and the p-type silicon carbide epitaxial layer 6 are electrically connected to each other. + The base region 3b is not floating, but is set to the same potential as the source electrode 12. This makes it possible to prevent punch-through and maintain the breakdown voltage.

[0057] Similar to the active region 40, the second p + The base region 4b is an n -In the silicon carbide epitaxial layer 2, a plurality of trenches 16b may be provided at intervals in a first direction parallel to the extension direction of the trenches 16b. In this case, one side wall of the trench 16b in the first direction is a second p + Type base region 4b and n - The second p-type silicon carbide epitaxial layer 2 is in contact with the second p-type silicon carbide epitaxial layer 2. + The mold base region 4b may be provided on one sidewall of the trench 16b without any space therebetween. In this case, the one sidewall of the trench 16b in the first direction is the second p + It comes into contact with the mold base region 4b.

[0058] 5 is a cross-sectional view showing a fourth structure of the gate pad region of the silicon carbide semiconductor device according to the first embodiment. As shown in FIG. 5, in the gate pad region 50, the gate electrode wiring 15 is provided on the entire front surface of the semiconductor substrate, and the second p + The mold base region 4b is selectively provided. In this manner, the fourth structure has the features of the second and third structures, and has the effects of both the second and third structures.

[0059] 6 is a cross-sectional view showing a fifth structure of the gate pad region of the silicon carbide semiconductor device according to the first embodiment. As shown in FIG. 6, a second p + The trench 16b in the gate pad region 50 does not function as a MOS gate, does not need to form a channel, and has a second p-type base region 4b on both sides of the sidewall. + 6, a gate electrode wiring 15 can be provided over the entire front surface of the semiconductor substrate in the gate pad region 50, although this is not shown in the figure.

[0060] FIG. 7 is a top view showing the structure of the silicon carbide semiconductor device according to the first embodiment. In FIG. 7, the region below the source electrode 12 is the active region 40, and the region below the gate electrode pad 14 is the gate pad region 50. The p-type silicon carbide epitaxial layer 6 in the gate pad region 50 is connected to the p-type silicon carbide epitaxial layer 6 in the active region 40. As shown in FIG. 7, the extension direction (x direction) of the trench 16b in the gate pad region 50 is preferably provided in the same direction as the extension direction of the trench 16a in the active region 40. The extension direction of the trench 16b in the gate pad region 50 is preferably parallel to the wire connected to the gate electrode pad 14. For example, one end of the wire is at position A on the outer side in the x direction of the trench-type MOSFET 70, and position A and the gate electrode pad 14 are connected by the wire. This makes it possible to prevent shell cracks, such as the destruction of the interlayer insulating film 11, from occurring when the wire is bonded to the gate electrode pad 14.

[0061] (Method of Manufacturing Silicon Carbide Semiconductor Device According to First Embodiment) Next, a description will be given of a method for manufacturing the silicon carbide semiconductor device according to the first embodiment. Figures 8 to 12 are cross-sectional views showing states during the manufacturing process of the silicon carbide semiconductor device according to the first embodiment.

[0062] First, n-type silicon carbide + A type silicon carbide substrate 1 is prepared. + On the front surface of the silicon carbide substrate 1, a lower n-type silicon carbide layer is formed by doping n-type impurities, such as nitrogen atoms, on the front surface of the silicon carbide substrate 1. - The silicon carbide epitaxial layer 2a is then epitaxially grown. The state up to this point is shown in FIG.

[0063] Next, the bottom n - On the surface of the silicon carbide epitaxial layer 2a, a mask for ion implantation having predetermined openings is formed, for example, of an oxide film by photolithography. Then, p-type impurities such as aluminum are implanted into the openings of the oxide film to form a first p + The mold base regions 3, 3b are formed.

[0064] Next, the bottom n - On the surface of the silicon carbide epitaxial layer 2a, an upper n-type layer made of silicon carbide is formed while doping with n-type impurities such as nitrogen. - The lower n-type silicon carbide epitaxial layer 2b is epitaxially grown. - The silicon carbide epitaxial layer 2a and the upper n - The n-type silicon carbide epitaxial layer 2b is formed by combining the n-type silicon carbide epitaxial layer 2a and the n-type silicon carbide epitaxial layer 2b. - This results in a silicon carbide epitaxial layer 2 .

[0065] Next, a part of the ion implantation mask is removed, and n-type impurities such as nitrogen are ion-implanted into the opening. - An n-type high concentration region 5 may be formed in a part of the surface region of the silicon carbide epitaxial layer 2. However, this n-type high concentration region 5 may or may not be formed over the entire surface of the substrate. The state up to this point is shown in FIG.

[0066] Next, n - A p-type silicon carbide epitaxial layer 6 is formed by epitaxial growth on the surface of the p-type silicon carbide epitaxial layer 2. After the p-type silicon carbide epitaxial layer 6 is formed by epitaxial growth, a p-type impurity such as aluminum may be further ion-implanted into a channel region of the p-type silicon carbide epitaxial layer 6.

[0067] Next, an ion implantation mask having a predetermined opening is formed by photolithography on the surface of the p-type silicon carbide epitaxial layer 6. An n-type impurity such as nitrogen (N) or phosphorus (P) is ion-implanted into the opening to form an n-type impurity on a part of the surface of the p-type silicon carbide epitaxial layer 6. + The n-type source region 7 is formed. + The n-type source region 7 is formed only in the active region 40. + The ion implantation mask used for forming the p-type source region 7 is removed. A new ion implantation mask is formed, and p-type impurities such as aluminum (Al) or boron (B) are ion-implanted to implant adjacent n +Between the p type source regions 7 + A contact region 8 is formed. + The mold contact regions 8 are formed only in the active regions 40. The state up to this point is shown in FIG.

[0068] Next, a trench forming mask having a predetermined opening is formed by photolithography on the surface of the p-type silicon carbide epitaxial layer 6, for example, using an oxide film. Next, the p-type silicon carbide epitaxial layer 6 is penetrated by dry etching to form an n - The trenches 16a and 16b are formed so as to reach the silicon carbide epitaxial layer 2. The bottoms of the trenches 16a and 16b are n-type. - The first p-type silicon carbide epitaxial layer 2 + The trench 16a is formed in the active region 40, and the trench 16b is formed in the gate pad region 50. The trench forming mask is then removed.

[0069] Next, p-type impurities such as aluminum are ion-implanted obliquely from the opening of the trench 16a to form a second p-type impurity layer on a part of the side wall of the trench 16a. + The second p-type base region 4 is formed on the side wall of the trench 16b. + The mold base region 4b may be formed at the same time.

[0070] Next, heat treatment (annealing) is performed in an inert gas atmosphere at about 1700°C to form the first p + Mold base area 3, 3b, 2nd p + Type base region 4, p + Type contact region 8 and n + An activation process is then carried out for the source region 7. As described above, the ion implantation regions may be activated all at once by a single heat treatment, or each ion implantation may be activated by a heat treatment. The state up to this point is shown in FIG.

[0071] Next, n +A gate insulating film 9 is formed along the surface of the type source region 7 and the bottoms and sidewalls of the trenches 16a and 16b. This gate insulating film 9 may be formed by thermal oxidation at a temperature of about 1000° C. in an oxygen atmosphere. Alternatively, this gate insulating film 9 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).

[0072] Next, a polycrystalline silicon film doped with, for example, phosphorus atoms is provided on the gate insulating film 9. This polycrystalline silicon film may be formed so as to fill the trenches 16a and 16b. This polycrystalline silicon film is patterned by photolithography and left inside the trenches 16a and 16b to form the gate electrode 10. The state up to this point is shown in FIG.

[0073] Next, for example, phosphorus glass is deposited to a thickness of about 1 μm so as to cover the gate insulating film 9 and the gate electrode 10, forming an interlayer insulating film 11. The interlayer insulating film 11 and the gate insulating film 9 are patterned by photolithography. + A contact hole is formed exposing the p-type source region 7 and the p-type silicon carbide epitaxial layer 6. Then, a heat treatment (reflow) is performed to flatten the interlayer insulating film 11. After the contact hole is formed in the interlayer insulating film 11, a barrier metal made of titanium (Ti), titanium nitride (TiN), or a laminate of titanium and titanium nitride may be formed. In this case, the barrier metal may also be made of n-type silicon carbide. + A contact hole is provided to expose the type source region 7. When forming the gate wiring electrode 15, a process of forming, for example, a polycrystalline silicon film doped with phosphorus atoms and, for example, phosphorus glass as the interlayer insulating film 11B to a thickness of about 1 μm is added thereafter.

[0074] Next, a conductive film that becomes the source electrode 12 is formed in the contact hole provided in the interlayer insulating film 11 and on the interlayer insulating film 11. The conductive film is, for example, a nickel (Ni) film. Then, a heat treatment is performed at a temperature of, for example, about 970° C. to silicide the nickel film inside the contact hole to form the source electrode 12. Then, the unreacted nickel film is selectively removed, leaving the source electrode 12 only in the contact hole, for example.

[0075] Next, a source electrode pad (not shown) is formed so as to fill the contact hole. A part of the metal layer deposited to form the source electrode pad may be used as the gate electrode pad 14. + On the back surface of the silicon carbide substrate 1, a metal film such as a nickel (Ni) film or a titanium (Ti) film is formed on the contact portion of the back surface electrode 13 by sputter deposition or the like. This metal film may be a laminate of a combination of Ni films and Ti films. Then, annealing such as rapid thermal annealing (RTA) is performed so that the metal film is silicided to form an ohmic contact. Then, a thick film such as a laminate film in which a Ti film, a Ni film, and a gold (Au) are laminated in this order is formed by electron beam (EB) deposition or the like to form the back surface electrode 13.

[0076] In the above-mentioned epitaxial growth and ion implantation, for example, nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), etc., which are n-type impurities (n-type dopants) with respect to silicon carbide, may be used. For example, boron (B), aluminum (Al), gallium (Ga), indium (In), thallium (Tl), etc., which are p-type impurities with respect to silicon carbide, may be used. In this manner, the trench-type MOSFET 70 shown in FIG. 1 is completed. Here, an example of the second structure is shown as the gate pad region 50, but other structures can be formed in the same manner.

[0077] As described above, according to the first embodiment, the first p-type semiconductor layer 100 that covers the trench and the bottom surface of the trench is also formed in the gate pad region.+ The n-type base region is provided. This allows the active region and the gate pad region to - Silicon carbide epitaxial layer and first p + The pn interface with the base region is at the same depth from the surface of the silicon carbide semiconductor substrate, which prevents avalanche current from concentrating in the gate pad region, making it possible to maintain the breakdown voltage of the gate pad region and improving the reliability of the gate insulating film.

[0078] (Embodiment 2) Fig. 13 is a cross-sectional view showing the structure of an active region and a gate pad region of a silicon carbide semiconductor device according to embodiment 2. Fig. 14 is a top view showing the structure of a silicon carbide semiconductor device according to embodiment 2. Fig. 13 is a cross-sectional view of the A-A' cross section of Fig. 14. The silicon carbide semiconductor device according to embodiment 2 differs from the silicon carbide semiconductor device according to embodiment 1 in that the width of trench 16b in gate pad region 50 is wider than the width of trench 16a in active region 40, and only one trench 16b is provided in gate pad region 50.

[0079] In the trench 16b in the gate pad region 50, the size of the trench 16b is slightly larger than that of the gate electrode pad 14. That is, the width of the trench 16b is slightly wider than that of the gate electrode pad 14, and the depth (length in the z direction) of the trench 16b is slightly longer than that of the gate electrode pad 14. A polycrystalline silicon film spreads over the entire surface of the back electrode 13 side of the gate electrode pad 14 as the gate electrode 10 in the trench 16b via the interlayer insulating film 11. The gate electrode 10 may be slightly smaller than the gate electrode pad 14. For example, if each side of the gate electrode 10 is about 10% smaller than the gate electrode pad 14, it can be considered that the polycrystalline silicon film spreads over the entire surface of the lower part of the gate electrode pad 14. In addition to polycrystalline silicon, the gate electrode 10 may be made of a high-melting point metal such as titanium or tungsten, its silicide, its nitride, or a laminated film of these. Here, a contact hole may be provided in the interlayer insulating film 11, and the gate electrode 10 in the trench 16b and the gate electrode pad 14 may be electrically connected. As a result, the first p + This facilitates contact with the base region 3, and the gate insulating film 9 in the gate pad region 50 is more highly protected than in the first embodiment. The trench 16b in the gate pad region 50 also has a second p-type insulating film on one side wall, as in the third structure in the first embodiment. + Alternatively, the second p-type base region 4 may be selectively provided on both side walls as in the fifth structure of the first embodiment. + A mold base region 4 may optionally be provided.

[0080] In addition, the trench 16a on the outermost periphery of the active region 40 is n-type on the gate pad region 40 side. + The first p-type source region 7 is not provided, and the first p-type source region 7 is in contact with the p-type silicon carbide epitaxial layer 6. + Holes can be easily extracted from the base region 3 .

[0081] The first p is formed on the entire bottom surface of the trench 16b. +Since the trench 16b is wide, the first p-type base region 3b formed under the trench 16b is formed. + The first p-type base region 3b is formed under the trench 16a of the active region 40. + The impurity concentration is higher than that of the first p-type base region 3. This is because, even if the trench 16b is formed by the same manufacturing method as the trench 16a, the impurities implanted by ion implantation are absorbed by the side walls of the mask at a low rate. Furthermore, the trench 16b is formed deeper than the trench 16a because it is wider. In this way, the first p-type base region 3, which has a high impurity concentration and a deep depth, + By providing the mold base region 3b, holes tend to concentrate in the trench 16b, making it easier to control the holes. For example, although there is only one wide trench 16b in FIG. 13, there may be two or more wide trenches 16b. In this case, a structure for extracting holes can be provided in the region between the trenches 16b, making it possible to control the holes.

[0082] (Method of Manufacturing Silicon Carbide Semiconductor Device According to Second Embodiment) The silicon carbide semiconductor device according to the second embodiment can be manufactured by forming one or more trenches 16b in the gate pad region 50, the width of which is wider than the width of the trenches 16a in the active region 40, in the method for manufacturing the silicon carbide semiconductor device according to the first embodiment. + Instead of the process of forming the base region 3b, ions are implanted into the bottom surfaces of the trenches 16a and 16b after the trenches 16a and 16b are formed, thereby forming a first p + It is possible to form a mold base region 3b.

[0083] As described above, according to the second embodiment, the same effects as those of the first embodiment can be obtained. Furthermore, in the second embodiment, the width of the trench in the gate pad region is set wider than the width of the trench in the active region. This reduces the first p +Contact with the mold base region is facilitated, and the protection capability of the gate insulating film in the gate pad region is improved compared to the first embodiment.

[0084] The present invention can be modified in various ways without departing from the spirit of the present invention, and in each of the above-mentioned embodiments, for example, the dimensions of each part and the impurity concentration are set in various ways according to the required specifications. In addition, in each of the above-mentioned embodiments, the case where silicon carbide is used as the wide band gap semiconductor is described as an example, but the present invention can also be applied to wide band gap semiconductors other than silicon carbide, such as gallium nitride (GaN). In addition, the present invention can also be applied to semiconductors other than wide band gap semiconductors, such as silicon (Si) and germanium (Ge). In addition, in each of the embodiments, the first conductivity type is n-type and the second conductivity type is p-type, but the present invention can be applied similarly even if the first conductivity type is p-type and the second conductivity type is n-type. [Industrial Applicability]

[0085] INDUSTRIAL APPLICABILITY As described above, the silicon carbide semiconductor device and the method for manufacturing a silicon carbide semiconductor device according to the present invention are useful for power semiconductor devices used in power conversion devices such as inverters, power supply devices for various industrial machines, and automobile igniters. [Explanation of symbols]

[0086] 1, 101 n + Silicon carbide substrate 2, 102 n - Silicon carbide epitaxial layer 2a bottom n - Silicon carbide epitaxial layer 2b Top n - Silicon carbide epitaxial layer 3, 3b, 103 1st p. + Type-based regions 4, 4b, 104 2nd p. + Type-based regions 5, 105 n-type high concentration region 6, 106 p-type silicon carbide epitaxial layer 7, 107 n+ Type Source Area 8, 108 p. + Mold Contact Area 9, 9b, 109 Gate insulating film 10, 10b, 110 Gate electrode 11, 111 Interlayer insulating film 12, 112 Source electrode 13, 113 Back electrode 14, 114 Gate electrode pad 15, 115 Gate electrode wiring 16a, 16b, 116 trenches 40 140 Active area 50 150 Gate pad area 70, 170 Trench MOSFET

Claims

1. a first conductivity type semiconductor substrate having an active portion and a gate pad portion; a first semiconductor layer of a first conductivity type provided on a front surface of the semiconductor substrate and having a lower impurity concentration than the semiconductor substrate; a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate; Equipped with The active portion is a first semiconductor region of a first conductivity type selectively provided in a surface layer of the second semiconductor layer on a side opposite to the semiconductor substrate; a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer; a first gate electrode provided inside the first trench via a gate insulating film; an interlayer insulating film provided on the first gate electrode; a first electrode provided on a surface of the second semiconductor layer and the first semiconductor region; A second electrode provided on a rear surface of the semiconductor substrate; a second semiconductor region of a second conductivity type provided in contact with a bottom portion of the first trench; Equipped with The gate pad portion is a second trench penetrating the second semiconductor layer and reaching the first semiconductor layer; a second gate electrode provided inside the second trench via an insulating film; a fourth semiconductor region of a second conductivity type provided so as to be in contact with a bottom portion of the second trench; a gate electrode pad electrically connected to the second gate electrode; Equipped with a polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate; the insulating film is also provided on a surface of the semiconductor substrate in a mesa region between adjacent second trenches; a gate electrode formed on the insulating film on the surface of the mesa region;

2. A semiconductor substrate of a first conductivity type having an active portion and a gate pad portion; a first semiconductor layer of a first conductivity type provided on a front surface of the semiconductor substrate and having a lower impurity concentration than the semiconductor substrate; a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate; Equipped with The active portion is a first semiconductor region of a first conductivity type selectively provided in a surface layer of the second semiconductor layer on a side opposite to the semiconductor substrate; a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer; a first gate electrode provided inside the first trench via a gate insulating film; an interlayer insulating film provided on the first gate electrode; a first electrode provided on a surface of the second semiconductor layer and the first semiconductor region; A second electrode provided on a rear surface of the semiconductor substrate; a second semiconductor region of a second conductivity type provided in contact with a bottom portion of the first trench; Equipped with The gate pad portion is a second trench penetrating the second semiconductor layer and reaching the first semiconductor layer; a second gate electrode provided inside the second trench via an insulating film; a fourth semiconductor region of a second conductivity type provided so as to be in contact with a bottom portion of the second trench; a gate electrode pad electrically connected to the second gate electrode; Equipped with a polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate; The semiconductor device according to claim 1, wherein the second trench extends in a direction parallel to a wire connected to the gate pad portion.

3. A semiconductor substrate of a first conductivity type having an active portion and a gate pad portion; a first semiconductor layer of a first conductivity type provided on a front surface of the semiconductor substrate and having a lower impurity concentration than the semiconductor substrate; a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate; Equipped with The active portion is a first semiconductor region of a first conductivity type selectively provided in a surface layer of the second semiconductor layer on a side opposite to the semiconductor substrate; a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer; a first gate electrode provided inside the first trench via a gate insulating film; an interlayer insulating film provided on the first gate electrode; a first electrode provided on a surface of the second semiconductor layer and the first semiconductor region; A second electrode provided on a rear surface of the semiconductor substrate; a second semiconductor region of a second conductivity type provided in contact with a bottom portion of the first trench; Equipped with The gate pad portion is a second trench penetrating the second semiconductor layer and reaching the first semiconductor layer; a second gate electrode provided inside the second trench via an insulating film; a fourth semiconductor region of a second conductivity type provided so as to be in contact with a bottom portion of the second trench; a gate electrode pad electrically connected to the second gate electrode; Equipped with a polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate; a gate electrode formed on the semiconductor substrate and having a first insulating film and a second insulating film formed on the first insulating film;

4. A semiconductor substrate of a first conductivity type having an active portion and a gate pad portion; a first semiconductor layer of a first conductivity type provided on a front surface of the semiconductor substrate and having a lower impurity concentration than the semiconductor substrate; a second semiconductor layer of a second conductivity type selectively provided on a surface of the first semiconductor layer opposite to the semiconductor substrate; Equipped with The active portion is a first semiconductor region of a first conductivity type selectively provided in a surface layer of the second semiconductor layer on a side opposite to the semiconductor substrate; a first trench penetrating the first semiconductor region or the second semiconductor layer and reaching the first semiconductor layer; a first gate electrode provided inside the first trench via a gate insulating film; an interlayer insulating film provided on the first gate electrode; a first electrode provided on a surface of the second semiconductor layer and the first semiconductor region; A second electrode provided on a rear surface of the semiconductor substrate; a second semiconductor region of a second conductivity type provided in contact with a bottom portion of the first trench; Equipped with The gate pad portion is a second trench penetrating the second semiconductor layer and reaching the first semiconductor layer; a second gate electrode provided inside the second trench via an insulating film; a fourth semiconductor region of a second conductivity type provided so as to be in contact with a bottom portion of the second trench; a gate electrode pad electrically connected to the second gate electrode; a fifth semiconductor region of a second conductivity type provided in the first semiconductor layer so as to be in contact with a side wall of the second trench and electrically connecting the second semiconductor region and the fourth semiconductor region; Equipped with a polycrystalline silicon film is provided between the gate electrode pad and the semiconductor substrate; The fourth semiconductor region has a higher impurity concentration than the second semiconductor region.

5. A semiconductor device as described in any one of claims 1 to 4, characterized in that it comprises a third semiconductor region of a second conductivity type electrically connecting the second semiconductor region and the second semiconductor layer, the third semiconductor region being provided within the first semiconductor layer so as to contact at least one side wall of the first trench in a second direction perpendicular to a first direction parallel to the extension direction of the first trench.

6. A semiconductor device as described in claim 5, characterized in that the third semiconductor region is provided in a plurality of locations spaced apart within the first semiconductor layer.

7. A semiconductor device as described in any one of claims 1 to 4, characterized in that it comprises a fifth semiconductor region of a second conductivity type provided in the first semiconductor layer so as to contact the side wall of the second trench, electrically connecting the second semiconductor region and the fourth semiconductor region.

8. A semiconductor device as described in Claim 7, characterized in that the fifth semiconductor region is provided within the first semiconductor layer so as to contact both trench sidewalls of the second trench.

9. A semiconductor device described in any one of claims 1 to 8, characterized in that the second trench is wider than the first trench.

10. 5. The semiconductor device according to claim 1, wherein the second trench is deeper than the first trench.

11. The semiconductor device according to any one of claims 1 to 10, characterized in that the first trench provided at the outermost periphery of the active portion does not have the first semiconductor region provided on the sidewall facing the gate pad portion in a second direction perpendicular to a first direction parallel to the extension direction of the first trench.

Citation Information

Patent Citations

  • Semiconductor device

    JP2014135367A

  • Silicon carbide semiconductor device and manufacturing method of the same

    JP2019106507A

  • Semiconductor device and power conversion device

    JP2019195081A

  • Semiconductor device and method for producing semiconductor device

    WO2016006696A1

  • Silicon carbide semiconductor device

    WO2019159351A1