Copper paste for forming a conductor, article having a conductor film, and method for producing the same
A copper paste with specific particle sizes and additives forms thick conductive films with low resistivity, addressing the issue of increased resistivity in screen printing methods, suitable for electronic components and flexible materials.
Patent Information
- Application Number
- JP2020115539
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-03
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-07-03
AI Technical Summary
Existing screen printing methods for forming copper conductors result in thick films with increased volume resistivity due to the use of additives, which hinders the formation of conductive films with low resistivity.
A copper paste composition comprising spherical copper-containing particles with specific diameter ranges and a dispersion medium, along with optional thixotropic agents, is used to form a thick conductive film with low volume resistivity through screen printing.
The copper paste enables the formation of thick conductive films with low volume resistivity, maintaining shape integrity and promoting fusion at lower temperatures, suitable for applications in electronic components and flexible materials.
Smart Images

Figure 0007563007000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a copper paste for forming a conductor, an article having a conductor film, and a method for producing the same. [Background technology]
[0002] As a method for forming a metal pattern, a so-called printed electronics method is known, which includes a step of applying a conductive material such as an ink or paste containing metal particles such as copper onto a substrate by inkjet printing, screen printing, etc., and a conductorization step of heating the conductive material to fuse the metal particles and develop conductivity. In recent years, with the aim of simplifying the process and achieving mass production, a method of producing wiring on a rigid or flexible substrate by a screen printing method has been attracting attention.
[0003] In the screen printing method, printing is performed using a screen plate consisting of a mesh-like structure called a screen mesh and an emulsion on which patterns of wiring, terminals, etc. are formed. As conductive materials used in the screen printing method, for example, Patent Document 1 discloses a conductive copper paste containing a thermosetting resin, a liquid fatty acid, and triethanolamine, and Patent Document 2 discloses a copper paste containing copper-containing particles with a median diameter of 10 nm to 100 nm, an organic solvent having a hydroxyl group, and an acrylic resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Re-tabled publication No. 2016 / 140185 [Patent Document 2] JP 2014-148732 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the screen printing method, the film thickness of the printed matter can be adjusted by changing the thickness of the emulsion. On the other hand, when a wiring pattern is formed by printing a copper paste by the screen printing method, the copper paste must pass through the screen mesh and the shape of the pattern must be maintained on the substrate. Therefore, when forming a thick film of, for example, 10 μm or more, it is important to adjust the composition of the copper paste in addition to adjusting the thickness of the emulsion. On the other hand, when forming a pattern with a thick film, additives such as thixotropic agents are usually used to maintain the pattern shape. However, the more the amount of additives is increased, the greater the volume resistivity of the conductor film (e.g., wiring) obtained by heating tends to be.
[0006] Therefore, an object of the present invention is to provide a copper paste that can form a thick conductor film with low volume resistivity even when using a screen printing method. [Means for solving the problem]
[0007] One aspect of the present invention relates to a copper paste for forming a conductor, comprising: spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm; spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm; flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm; and a dispersion medium.
[0008] According to the copper paste of the above aspect, a thick conductor film having a low volume resistivity can be formed by screen printing.
[0009] In the copper paste of the above aspect, the mass ratio of the content of the copper-containing particles (A) to the total content of the copper-containing particles (B) and the copper-containing particles (C) is preferably 0.5 to 5.0.
[0010] In the copper paste of the above aspect, the total content of the copper-containing particles (A), the copper-containing particles (B) and the copper-containing particles (C) is preferably 75 mass % or more based on the total mass of the copper paste.
[0011] The copper paste of the above aspect may further contain a thixotropic agent. In this case, the mass ratio of the content of the thixotropic agent to the content of the dispersion medium is preferably 0.001 to 0.050.
[0012] The copper paste on the side surface is preferably used in a screen printing method.
[0013] Another aspect of the present invention relates to a method for producing a copper paste for forming a conductor, comprising a step of dispersing spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm, spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm, and flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm in a dispersion medium.
[0014] According to the manufacturing method of the above aspect, it is possible to provide a copper paste capable of forming a thick conductor film with low volume resistivity even by screen printing.
[0015] In the manufacturing method of the above aspect, the mass ratio of the blending amount of the copper-containing particles (A) to the total blending amount of the copper-containing particles (B) and the copper-containing particles (C) is preferably 0.5 to 5.0.
[0016] In the manufacturing method of the above aspect, the total amount of the copper-containing particles (A), the copper-containing particles (B) and the copper-containing particles (C) is preferably 75 mass % or more based on the total mass of the copper paste.
[0017] The manufacturing method of the above aspect may include a step of adding a thixotropic agent to the dispersion medium. In this case, the mass ratio of the amount of the thixotropic agent to the amount of the dispersion medium is preferably 0.001 to 0.050.
[0018] Another aspect of the present invention relates to a method for producing an article having a substrate and a conductive film provided on the substrate, the method comprising the steps of: forming a coating film of a copper paste for forming a conductor on the substrate; and sintering copper-containing particles in the coating film to form the conductive film. Step (A) in this method is, for example, printing the coating film of the copper paste for forming a conductor by a screen printing method.
[0019] According to the manufacturing method of the above aspect, an article having a thick conductor film with low volume resistivity can be obtained.
[0020] In the manufacturing method of the above aspect, the conductive film preferably has a thickness of 10.0 μm or more.
[0021] In the manufacturing method of the above aspect, the copper content in the conductor film is preferably 90 mass % or more.
[0022] In the manufacturing method of the above aspect, the conductive film is preferably a wiring pattern.
[0023] Another aspect of the present invention relates to an article having a substrate and a conductive film provided on the substrate, the conductive film including a sintered body of the conductor-forming copper paste of the above aspect.
[0024] In the article of the above aspect, the conductive film preferably has a thickness of 10.0 μm or more.
[0025] In the article of the above aspect, the copper content in the conductive film is preferably 90 mass % or more.
[0026] In the article of the above aspect, the conductive film is preferably a wiring pattern. Effect of the Invention
[0027] According to the present invention, it is possible to provide a copper paste capable of forming a thick conductor film having a low volume resistivity even when applied to a screen printing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, the embodiments for carrying out the present invention will be described in detail. However, the present invention is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified or considered to be obviously essential in principle. The same applies to the numerical values and their ranges, and they do not limit the present invention.
[0029] In this specification, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the purpose of the process is achieved. In addition, in this specification, a numerical range indicated using "to" indicates a range including the numerical values before and after "to" as the minimum and maximum values, respectively. In addition, in this specification, the content of each component in a composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified.
[0030] In this specification, "conducting" refers to fusing metal-containing particles to change them into conductors. "Conductor" refers to an object that has electrical conductivity, and more specifically, an object with a volume resistivity of 100 μΩ·cm or less. "Conductor film" refers to a film-like conductor (a film composed of a conductor).
[0031] In this specification, the term "film" encompasses a configuration of a shape formed on a part of a surface as well as a configuration of a shape formed over the entire surface when observed in a plan view.
[0032] In this specification, the term "median size" refers to the particle size when a particle aggregate is divided into two parts from a certain particle size such that the number of particles on the larger side is equal to the number of particles on the smaller side, and is also referred to as D50.
[0033] <Copper paste for conductor formation> A copper paste for forming a conductor in one embodiment contains copper-containing particles and a dispersion medium, and the copper-containing particles include spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm (hereinafter also simply referred to as "copper-containing particles (A)"), spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm (hereinafter also simply referred to as "copper-containing particles (B)"), and flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm (hereinafter also simply referred to as "copper-containing particles (C)"). Here, when the longest distance from the surface of a copper-containing particle through the center point of the particle to the opposite surface of the particle is defined as x and the shortest distance is defined as y, particles with a ratio (x / y) of less than 2 (x / y<2) are called "spherical copper-containing particles", and particles with a ratio (x / y) of 2 or more (x / y≧2) are called "flat copper-containing particles".
[0034] According to the copper paste having the above-mentioned configuration, even by a screen printing method, a thick conductor film (e.g., wiring) having a low volume resistivity, i.e., excellent conductivity, can be formed. Therefore, the copper paste of the present embodiment is suitably used for the screen printing method.
[0035] The reason why the above effect is obtained is not clear, but it is presumed that the copper-containing particles (B) and (C) penetrate into the gaps between the copper-containing particles (A), reducing the void ratio of the conductive film after firing, and that the copper-containing particles including the copper-containing particles (C) promote fusion between the copper particles more than when only spherical copper-containing particles are used, resulting in a lower conductive volume resistivity and making it easier to maintain the shape even in a thick film.
[0036] In addition, the copper paste having the above-mentioned configuration tends to have excellent fusion properties at low temperatures (for example, 250° C. or less) and can be made conductive at low temperatures, so it is useful for applications in which a conductor is formed at low temperatures (for example, applications in which a metal foil, wiring pattern, etc. is formed on a substrate having low heat resistance such as a resin). In addition, the copper paste of this embodiment is also suitable for applications such as decoration and printing that are not intended to conduct electricity.
[0037] The components that may be contained in the copper paste will be described in detail below.
[0038] (copper-containing particles) The copper-containing particles contain at least copper. From the viewpoint of thermal conductivity and sinterability, the copper-containing particles preferably contain copper as a main component. The element ratio of copper in the copper-containing particles may be 80 atomic % or more, 90 atomic % or more, or 95 atomic % or more based on all elements except hydrogen, carbon, and oxygen. When the element ratio of copper in the copper-containing particles is 80 atomic % or more, the thermal conductivity and sinterability derived from copper tend to be easily expressed.
[0039] The copper-containing particles include at least copper-containing particles (A), copper-containing particles (B) and copper-containing particles (C).
[0040] The copper-containing particles (A) are spherical copper-containing particles having a median diameter of 2.0 μm or more and less than 10.0 μm. When the copper-containing particles (A) have a median diameter of 10.0 μm or more, the voids in the conductor film after firing tend to become too large. When the copper-containing particles (A) have a median diameter of less than 2.0 μm, the conductor film after firing shrinks significantly as a whole, and cracks and dimensional changes in the conductor film tend to occur easily. From the viewpoint of further improving the fusion property at low temperatures and further reducing the voids in the conductor film after firing, the median diameter of the copper-containing particles (A) is preferably 9.0 μm or less, more preferably 8.0 μm or less. From the viewpoint of further suppressing cracks and dimensional changes in the conductor film, the median diameter of the copper-containing particles (A) may be 3.0 μm or more, or may be 3.5 μm or more.
[0041] The copper-containing particles (B) are spherical copper-containing particles having a median diameter of 0.1 μm or more and less than 2.0 μm. If the median diameter of the copper-containing particles (B) is outside the above range, the volume resistivity after firing tends to be too high. From the viewpoint of further improving the fusibility at low temperatures and further reducing the volume resistivity after firing, the median diameter of the copper-containing particles (B) is preferably 1.5 μm or less, more preferably 1.0 μm or less. From the viewpoint of further reducing the volume resistivity after firing, the median diameter of the copper-containing particles (B) may be 0.15 μm or more, or may be 0.2 μm or more.
[0042] The copper-containing particles (C) are flat copper-containing particles having a median diameter of 0.03 μm or more and less than 3.0 μm. When the copper-containing particles (C) have a median diameter of 3.0 μm or more, the void ratio of the conductor film after firing tends to be too large. When the copper-containing particles (C) have a median diameter of less than 0.03 μm, the volume resistivity after firing tends to be too large. From the viewpoint of further improving the fusion property at low temperatures and further reducing the voids of the conductor film after firing, the median diameter of the copper-containing particles (C) is preferably 2.5 μm or less, more preferably 2.3 μm or less, and even more preferably 2.0 μm or less. From the viewpoint of further reducing the volume resistivity after firing, the median diameter of the copper-containing particles (C) may be 0.1 μm or more, or may be 1.0 μm or more.
[0043] The median diameter of the copper-containing particles can be adjusted, for example, by adjusting conditions such as the type of raw materials, the temperature when mixing the raw materials, the reaction time, the reaction temperature, the washing process, and the washing solvent in the method for producing copper-containing particles described below.
[0044] The content of the copper-containing particles (A) may be 25% by mass or more, 30% by mass or more, or 35% by mass or more based on the total mass of the copper paste from the viewpoint of further suppressing cracks and dimensional changes in the conductor film. The content of the copper-containing particles (A) may be 90% by mass or less, 85% by mass or less, or 80% by mass or less based on the total mass of the copper paste from the viewpoint of further improving fusion properties at low temperatures and further reducing voids in the conductor film after firing.
[0045] The content of the copper-containing particles (B) may be 5% by mass or more, 10% by mass or more, or 12% by mass or more based on the total mass of the copper paste from the viewpoint of further improving the fusibility at low temperatures and further reducing the volume resistivity after firing. The content of the copper-containing particles (B) may be 80% by mass or less, 75% by mass or less, or 70% by mass or less based on the total mass of the copper paste from the viewpoint of further reducing the volume resistivity after firing.
[0046] The content of the copper-containing particles (C) may be 2% by mass or more, 3% by mass or more, or 5% by mass or more based on the total mass of the copper paste from the viewpoint of further improving the fusion property at low temperatures and further reducing the voids in the conductor film after firing. The content of the copper-containing particles (C) may be 50% by mass or less, 45% by mass or less, or 40% by mass or less based on the total mass of the copper paste from the viewpoint of further reducing the volume resistivity after firing.
[0047] The mass ratio of the content of the copper-containing particles (A) to the total content of the copper-containing particles (B) and the copper-containing particles (C) is preferably 0.5 to 5.0. With such a mass ratio, cracks in the conductor after sintering can be more easily suppressed, and the voids in the conductor after sintering can be more reduced. As a result, the volume resistivity can be more reduced, and a wiring with a larger current amount can be formed. The above mass ratio is preferably 1.0 or more, more preferably 1.2 or more, and even more preferably 1.4 or more, from the viewpoint of reducing the shrinkage of the conductor after sintering and more suppressing the occurrence of cracks in the conductor. The above mass ratio is preferably 3.5 or less, more preferably 2.5 or less, and even more preferably 2.0 or less, from the viewpoint of reducing the voids in the conductor after sintering and more reducing the volume resistivity.
[0048] The total content of the copper-containing particles (A), (B) and (C) is preferably 75% by mass or more, more preferably 80% by mass or more, based on the total mass of the copper paste, from the viewpoint of facilitating the formation of thicker wiring, i.e., wiring with a large current amount. The total content of the copper-containing particles (A), (B) and (C) may be 97% by mass or less, or may be 95% by mass or less, based on the total mass of the copper paste.
[0049] The copper-containing particles (e.g., copper-containing particles (A) to (C)) may include a copper-containing core particle and an organic substance present on at least a portion of the surface of the core particle. The organic substance present on at least a portion of the surface of the copper-containing core particle may include a substance derived from an alkylamine. The presence of the organic substance is confirmed by heating the copper-containing particles in a nitrogen atmosphere at a temperature equal to or higher than the temperature at which the organic substance thermally decomposes, and comparing the weights before and after heating.
[0050] The proportion of the organic matter present on at least a portion of the surface of the core particle is preferably 0.1% by mass to 20% by mass based on the total of the core particle and the organic matter. When the proportion of the organic matter is 0.1% by mass or more, the oxidation resistance tends to be excellent. When the proportion of the organic matter is 20% by mass or less, the fusion property at low temperatures tends to be better. The proportion of the organic matter to the total of the core particle and the organic matter is more preferably 0.3% by mass to 10% by mass, and even more preferably 0.5% by mass to 5% by mass.
[0051] The core particle contains at least metallic copper, and may contain other substances as necessary. Examples of substances other than copper include metals such as gold, silver, platinum, tin, and nickel, or compounds containing these metal elements, fatty acid copper described below, organic substances derived from reducing compounds or alkylamines, copper oxide, and copper chloride. From the viewpoint of forming a conductor with excellent electrical conductivity, the content of metallic copper in the core particle is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more.
[0052] When the copper-containing particles contain a core particle containing copper and an organic substance present on at least a part of the surface of the core particle, oxidation of copper is suppressed even when the copper-containing particles are stored in the atmosphere, and the oxide content is reduced. For example, in one embodiment, the oxide content in the copper-containing particles is 5 mass% or less. The oxide content in the copper-containing particles can be measured, for example, by XRD (X-ray diffraction).
[0053] The copper-containing core particles and the copper-containing particles containing organic matter present on at least a part of the surface of the core particles can be manufactured by a conventional method.Specific manufacturing methods include, for example, the manufacturing method of copper-containing particles disclosed in JP 2016-037626 A. In the manufacturing method, the copper-containing particles are manufactured by a method having a step of heating a composition containing a metal salt of fatty acid and copper, a reducing compound, and an alkylamine.The method may have a step of centrifuging, washing, etc. after the heating step as necessary.
[0054] The copper-containing particles may contain copper-containing particles other than copper-containing particles (A), copper-containing particles (B) and copper-containing particles (C). However, the total content of copper-containing particles (A), copper-containing particles (B) and copper-containing particles (C) in the total mass of the copper-containing particles is preferably 90 mass% or more, more preferably 95 mass% or more, and even more preferably 100 mass%.
[0055] (dispersion medium) The dispersion medium is, for example, an organic solvent. The type of the dispersion medium is not particularly limited, and can be appropriately selected from organic solvents generally used depending on the application of the copper paste. The dispersion medium may be used alone or in combination of two or more. When the copper paste is applied to a screen printing method, it is preferable that the dispersion medium contains at least one selected from the group consisting of terpineol, isobornylcyclohexanol, dihydroterpineol, and dihydroterpineol acetate, from the viewpoint of easily adjusting the viscosity of the copper paste to a viscosity suitable for the screen printing method.
[0056] The content of the dispersion medium may be, for example, 3 to 25 mass % or 5 to 20 mass % based on the total mass of the copper paste.
[0057] The copper paste may further contain components other than the copper-containing particles and the dispersion medium as necessary. Such components include, but are not limited to, a thixotropic agent, a silane coupling agent, a polymer compound, a radical initiator, a reducing agent, etc. In particular, in the screen printing method, it is preferable that the composition contains a thixotropic agent.
[0058] The thixotropic agent is used for the purpose of suppressing the flow of the paste during screen printing and maintaining the shape of the conductor film (e.g., wiring). The thixotropic agent is preferably one that can be dispersed or dissolved in a dispersion medium. Specific examples of the thixotropic agent include polyvinylpyrrolidone, polyether, polyester, polyamide, polyvinyl alcohol, polyacrylic, modified urethane resin, epoxy resin, and cellulose derivatives (compounds in which the hydroxyl group in the cellulose molecule is replaced by a substituent (e.g., an alkyl group)). Among the thixotropic agents, cellulose derivatives are preferably used, and ethyl cellulose is more preferably used. The thixotropic agents may be used alone or in combination of two or more.
[0059] The mass ratio of the content of the thixotropic agent to the content of the dispersion medium is preferably 0.001 or more, more preferably 0.003 or more, from the viewpoint of easily maintaining the shape of the conductor film. The mass ratio of the content of the thixotropic agent to the content of the dispersion medium may be 0.01 or more, 0.02 or more, or 0.03 or more. The mass ratio of the content of the thixotropic agent to the content of the dispersion medium is preferably 1 or less, more preferably 0.9 or less, even more preferably 0.8 or less, even more preferably 0.050 or less, particularly preferably 0.040 or less, and extremely preferably 0.030 or less, from the viewpoint of easily passing the copper paste through the screen mesh in the screen printing method and from the viewpoint of further reducing the volume resistance value of the conductor film after firing. In particular, when the mass ratio of the content of the thixotropic agent to the content of the dispersion medium is 0.001 to 0.050, the unevenness of the conductor film can be further reduced, and there is a tendency that the current can be passed more stably.
[0060] From the viewpoint of further reducing the volume resistivity, the content of the thixotropic agent is preferably 3.0 mass % or less, more preferably 2.5 mass % or less, and even more preferably 2.0 mass % or less, based on the total mass of the copper paste.
[0061] The viscosity of the copper paste is preferably 0.1 Pa·s to 30 Pa·s, and more preferably 1 Pa·s to 30 Pa·s. When the viscosity of the copper paste is in the above range, good printability is easily obtained in the screen printing method. The viscosity of the copper paste is a value measured at 25°C using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name: VISCOMETER-TV22, applicable cone-plate type rotor: 3°×R17.65).
[0062] <Method of manufacturing copper paste for forming conductor> A method for producing a copper paste for forming a conductor according to an embodiment includes a step of dispersing copper-containing particles in a dispersion medium. Specifically, for example, the above-mentioned copper-containing particles (A), copper-containing particles (B) and copper-containing particles (C) are mixed with a dispersion medium and other components (such as a thixotropic agent) that are added as necessary, and dispersed. When a thixotropic agent is used, the thixotropic agent may be dissolved or dispersed in the dispersion medium in advance. That is, when the method for producing a copper paste for forming a conductor includes a step of adding a thixotropic agent to the dispersion medium, the step may be performed before the step of dispersing copper-containing particles in the dispersion medium.
[0063] For the dispersion treatment, a media dispersing machine such as an Ishikawa type mixer, a planetary centrifugal mixer, an ultra-thin high-speed rotary dispersing machine, a roll mill, an ultrasonic dispersing machine, or a bead mill, a cavitation mixing machine such as a homomixer or a Silverson mixer, or a head-on collision method such as an Ultemizer can be used. These methods may also be used in appropriate combination.
[0064] The amount of the copper-containing particles may be appropriately adjusted so that the content of the copper-containing particles in the copper paste (for example, the content of the copper-containing particles (A), the copper-containing particles (B) and the copper-containing particles (C)) falls within the above-mentioned range. Specifically, for example, the mass ratio of the amount of the copper-containing particles (A) to the total amount of the copper-containing particles (B) and the copper-containing particles (C) may be 0.5 to 5.0. In addition, the total amount of the copper-containing particles (A), the copper-containing particles (B) and the copper-containing particles (C) may be 75 mass% or more based on the total mass of the copper paste.
[0065] The amount of the thixotropic agent may be appropriately adjusted so that the amount of the thixotropic agent in the copper paste falls within the above-mentioned range. Specifically, for example, the mass ratio of the amount of the thixotropic agent to the amount of the dispersion medium may be 0.001 to 0.05.
[0066] <Conductor film and method for forming same> The conductor film of one embodiment includes a sintered body of the conductor-forming copper paste of the above embodiment. First, a method for forming the conductor film will be described below.
[0067] The method for forming a conductor film includes a step (A) of forming a coating film of the copper paste for forming a conductor according to the above embodiment, and a step (B) of sintering the copper-containing particles in the coating film to form a conductor film. According to this method, a thick conductor film having a low volume resistivity can be formed.
[0068] In step (A), for example, a coating film of the copper paste for forming a conductor is formed on a substrate. The material of the substrate is not particularly limited. The substrate may or may not have electrical conductivity. Specifically, metals such as Cu, Au, Pt, Pd, Ag, Zn, Ni, Co, Fe, Al, Sn, etc., alloys of these metals, semiconductors such as ITO, ZnO, SnO, Si, etc., carbon materials such as glass, graphite, graphite, etc., resins, paper, and combinations thereof can be mentioned. Since the copper paste of the above embodiment can be sintered by heating at a low temperature, a substrate made of a material with relatively low heat resistance can also be used. Examples of materials with relatively low heat resistance include thermoplastic resins. Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, and polymethylpentene, polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polycarbonate, polyamide, polyimide, and polyamideimide. The shape of the substrate is not particularly limited, and may be a plate, a rod, a roll, a film, etc.
[0069] Step (A) may be a step of printing a coating of copper paste for forming a conductor by screen printing. In the screen printing method, for example, the copper paste for forming a conductor is supplied onto a screen plate using a tool such as a scraper, and then a squeegee is pressed against the plate and moved to form a pattern. In the screen printing method, a thick film of 20 μm or more can be easily formed depending on the thickness of the emulsion on the plate.
[0070] The material of the mesh used in the screen is not particularly limited and is selected from stainless steel, polyester, nylon, etc., which are used in normal printing processes. The wire diameter of the mesh is preferably 5 to 80 μm. The opening ratio of the mesh is sufficient as long as printing is possible without bleeding or blurring, and is preferably 20 to 60%, more preferably 30 to 50%.
[0071] The thickness of the emulsion of the screen plate is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. When the thickness of the emulsion is 10 μm or more, a conductive film capable of passing a larger amount of current is easily obtained.
[0072] In screen printing, parameters such as the distance (clearance) between the screen and the substrate, the squeegee pressure, the squeegee angle, and the squeegee movement speed can be appropriately selected to optimally suit the shape of the coating film of the conductor-forming copper paste.
[0073] Step (B) is, for example, a step of heating the coating film formed in step (A) to sinter the copper-containing particles in the coating film. When the copper-containing particles have organic matter on their surfaces, the organic matter on the surfaces is thermally decomposed by heating, and the copper-containing particles are sintered (fused) together. This makes the coating film conductive, and a conductive film containing a sintered body of the conductor-forming copper paste is formed. Here, the sintered body is an object obtained by sintering the copper-containing particles in the copper paste, and has a structure in which the copper-containing particles are fused together.
[0074] The heating temperature may be a temperature at which the copper-containing particles can be sintered (when the copper-containing particles have organic matter on their surfaces, the organic matter can be thermally decomposed and the copper-containing particles can be sintered together). The copper paste for forming a conductor of the above embodiment tends to have excellent fusion properties at low temperatures, so the heating temperature can be 250°C or less. The heating temperature may be, for example, 130°C or more.
[0075] The components in the atmosphere in which the heating is performed in step (B) are not particularly limited, and can be selected from nitrogen, argon, and the like, which are used in normal conductor manufacturing processes. In addition, heating may be performed in an atmosphere saturated with nitrogen or the like containing reducing substances such as hydrogen and formic acid. From the viewpoint of improving the volume resistivity of the conductor, it is preferable to heat in a reducing atmosphere using hydrogen, formic acid, and the like. The pressure during heating is not particularly limited, but reducing the pressure tends to promote conductor formation at a lower temperature.
[0076] The heating step may be performed at a constant temperature rise rate or may be changed irregularly. The heating step time is not particularly limited and can be selected in consideration of the heating temperature, heating atmosphere, amount of copper-containing particles, etc. The heating method is not particularly limited and may include heating with a hot plate, heating with an infrared heater, heating with a pulse laser, etc.
[0077] The method for forming the conductor film may include other steps as necessary, such as a step of removing at least a part of the volatile components in the coating film of the copper paste by drying or the like before step (B), a step of reducing the copper oxide produced by heating in a reducing atmosphere after step (B), a step of removing the remaining components by performing light sintering after step (B), and a step of applying a load to the conductor film obtained after step (B).
[0078] According to the method described above, a thick conductor film having a low volume resistivity can be formed. The volume resistivity of the conductor film is, for example, less than 50 μΩ·cm, and can also be less than 30 μΩ·cm or less than 20 μΩ·cm. Since the volume resistivity of the conductor film obtained by the above formation method is less than 50 μΩ·cm, a large amount of current can be passed through the conductor film.
[0079] The shape of the conductive film is not particularly limited, and may be, for example, patterned or non-patterned. The thickness of the conductive film is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, in terms of allowing a large amount of current to flow. The thickness of the conductive film may be, for example, 100 μm or less.
[0080] The arithmetic mean roughness of the conductive film is preferably less than 3.0 μm, more preferably less than 2.5 μm, and even more preferably less than 2.0 μm. When the arithmetic mean roughness of the conductive film is less than 3.0 μm, a current can flow more stably.
[0081] The copper content in the conductor film is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass. When the copper content in the conductor film is 90% by mass or more, a sufficiently low volume resistivity is easily obtained.
[0082] The conductive film formed by the above method can be used for various applications. Specifically, it can be used as a member such as an electric wiring, a heat dissipation film, a surface coating film, etc., used in electronic components such as laminates, solar panels, displays, transistors, semiconductor packages, and laminated ceramic capacitors. In other words, the method for forming the conductive film of the above embodiment is suitable as a method for forming members such as an electric wiring, a heat dissipation film, a surface coating film, etc., used in electronic components such as laminates, solar panels, displays, transistors, semiconductor packages, and laminated ceramic capacitors. In particular, since the above method allows the conductive film to be formed on a substrate such as a resin, the above method is suitable as a method for forming members such as an electric wiring, a heat dissipation film, a surface coating film, etc., used in electronic components such as flexible laminates, solar panels, and displays.
[0083] <Article Having Conductive Film and Its Manufacturing Method> An article according to an embodiment includes, for example, a substrate and a conductive film provided on the substrate. The conductive film is formed by the conductive film forming method according to the embodiment. In other words, a method for manufacturing an article according to an embodiment includes a step of forming a conductive film on a substrate by the conductive film forming method.
[0084] The conductive film may be, for example, wiring (e.g., wiring pattern) or a coating of various electronic components. Specifically, it may be a member such as an electric wiring, a heat dissipation film, or a surface coating film used in the above-mentioned electronic components. The substrate may be the substrate exemplified as the substrate used for forming the above-mentioned conductive film.
[0085] The article may be, for example, an electronic component such as a laminate having wiring, a coating, etc., made of the above-mentioned conductor film, a solar cell panel, a display, a transistor, a ceramic capacitor, a semiconductor package, etc. Also included in the article of this embodiment are electronic devices, home appliances, industrial machines, transport machines, etc. that incorporate these electronic components. EXAMPLES
[0086] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.
[0087] <Copper-containing particles (A), (B), and (C) used in the preparation of copper paste for forming conductor> As copper-containing particles (A), copper-containing particles (B) and copper-containing particles (C), the copper-containing particles shown in Table 1 were prepared. Copper-containing particles (A): 1400YM (product name), manufactured by Mitsui Mining & Smelting Co., Ltd., shape = spherical, median diameter (D50) = 4.0 μm Copper-containing particles (B): CH0200 (product name), manufactured by Mitsui Mining & Smelting Co., Ltd., shape = spherical, median diameter (D50) = 0.2 μm Copper-containing particles (C): 1050YF (product name), manufactured by Mitsui Mining & Smelting Co., Ltd., shape = flat, median diameter (D50) = 1.4 μm The median diameter (D50) of copper-containing particles (A), (B), and (C) was measured using a submicron particle analyzer N5 PLUS (Beckman Coulter, Inc.).
[0088] <Examples 1 to 6 and Comparative Examples 1 to 9> Copper-containing particles were mixed in the combination and mixing ratio shown in Table 1, and a dispersion medium mixed with a thixotropic agent was added so that the mass of the copper-containing particles as a whole was 80 to 92% of the total copper paste, and mixed in a mortar. Here, terpineol was used as the dispersion medium, and ethyl cellulose (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the thixotropic agent. The amounts of the dispersion medium and the thixotropic agent were adjusted so that the mass ratio of the amount of ethyl cellulose to the amount of terpineol was 0.050 in Examples 1 to 4 and Comparative Examples 1 to 9, 0.026 in Example 5, and 0.029 in Example 6. Thereafter, the mixture was kneaded and defoamed using a planetary centrifugal mixer (product name: Awatori Rentaro, manufactured by Thinky Corporation), and copper pastes for forming a conductor of the Examples and Comparative Examples shown in Table 1 were obtained. In Table 1, "(A) / (B)+(C)" indicates the mass ratio of the amount (content) of copper-containing particles (A) to the total amount (content) of copper-containing particles (B) and copper-containing particles (C), and "(A)+(B)+(C)" indicates the total amount (content) of copper-containing particles (A), copper-containing particles (B), and copper-containing particles (C) based on the total mass of the copper paste.
[0089] <Evaluation> (Preparation of evaluation samples) The copper paste for forming a conductor of the examples and comparative examples prepared above was printed by a screen printing method (screen plate: Mino Group Co., Ltd., width = 0.5 mm, length = 1 cm, emulsion thickness = 20 μm) to form a coating film of the copper paste (a deposited layer of the copper paste) on the substrate. Here, a polyimide film was used as the substrate. Next, the substrate with the coating film formed was placed in a firing furnace and heated to sinter the copper-containing particles, thereby obtaining a structure with wiring (conductor film). An atmosphere-controlled heating device (RF-100B, manufactured by Ayumi Industry Co., Ltd.) was used for the heat treatment. The heat treatment conditions were a negative pressure (8.5 × 10 4 The mixture was heated to 225°C at a rate of 30°C / min under a pressure of 1.0 Pa, and then a mixture of nitrogen and formic acid was introduced to obtain a pressure of 9.0 × 10 4 The test was performed by using a mixed gas of 225 Pa and holding it at 225°C for 60 minutes.
[0090] (Appearance evaluation of wiring) The wiring surface was observed with a metallurgical microscope, and evaluation was performed as follows: if no cracks were found and the wiring width was uniform, it was marked as ◯; if cracks were found or the wiring width was not uniform, it was marked as ×. The results are shown in Table 1.
[0091] (Volume resistivity measurement) The volume resistivity of the obtained wiring (conductor film) was calculated from the resistance value of the wiring, the film thickness measured with a contact-type step gauge (product name: ET200, manufactured by Kosaka Laboratory Co., Ltd.), and the wiring width. The results are shown in Table 1.
[0092] (Surface roughness evaluation) The surface unevenness (arithmetic mean roughness: Ra) of the wiring was measured with a contact type step gauge (product name: ET200, Kosaka Laboratory Co., Ltd.) for Examples 5 and 6. The results are shown in Table 1.
[0093] [Table 1]
[0094] As shown in Table 1, in Examples 1 to 6, there were no cracks on the wiring surface, and the volume resistivity was low, less than 20 μΩ·cm. On the other hand, in Comparative Examples 1 to 4 and 7, many cracks were present on the wiring surface after firing, and the volume resistivity was 20 μΩ·cm or more. Moreover, in Comparative Examples 5 to 8, no cracks were observed on the wiring surface, but the volume resistivity was 20 μΩ·cm or more.
Claims
1. Spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm; Spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm; Flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm; A dispersion medium; A thixotropic agent is contained, a mass ratio of the content of the copper-containing particles (A) to the total content of the copper-containing particles (B) and the copper-containing particles (C) is 0.84 to 5.0; The copper paste for forming a conductor, wherein the mass ratio of the content of the thixotropic agent to the content of the dispersion medium is 0.001 to 0.
050.
2. 2. The copper paste for forming a conductor according to claim 1, wherein the total content of the copper-containing particles (A), the copper-containing particles (B) and the copper-containing particles (C) is 75 mass% or more based on the total mass of the copper paste.
3. A copper paste for forming a conductor as described in claim 1 or 2, wherein the thixotropic agent includes a cellulose derivative.
4. Spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm; Spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm; Flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm; A copper paste for forming a conductor, comprising: a dispersion medium (excluding copper pastes containing a gelling agent).
5. Spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm; Spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm; Flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm; A copper paste for forming a conductor, comprising: a dispersion medium (however, excluding a copper paste containing coated metal particles, which contain metal core particles and one or more molecules selected from aliphatic carboxylic acids and aliphatic aldehydes arranged on the surface of the metal core particles at a density of 2.5 to 5.2 molecules per nm 2 ).
6. The copper paste for forming a conductor according to any one of claims 1 to 5, which is used in a screen printing method.
7. The method includes the steps of dispersing spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm, spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm, and flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm in a dispersion medium, and adding a thixotropic agent to the dispersion medium, a mass ratio of the content of the copper-containing particles (A) to the total content of the copper-containing particles (B) and the copper-containing particles (C) is 0.84 to 5.0; A method for producing a copper paste for forming a conductor, wherein a mass ratio of the content of the thixotropic agent to the content of the dispersion medium is 0.001 to 0.
050.
8. 8. The method for producing a copper paste for forming a conductor according to claim 7, wherein the total amount of the copper-containing particles (A), the copper-containing particles (B) and the copper-containing particles (C) is 75 mass% or more based on the total mass of the copper paste.
9. A method for producing a copper paste for forming a conductor as described in claim 7 or 8, wherein the thixotropic agent includes a cellulose derivative.
10. A method for manufacturing a copper paste for forming a conductor (excluding a copper paste containing a gelling agent), comprising a step of dispersing spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm, spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm, and flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm in a dispersion medium.
11. A method for producing a copper paste for forming a conductor (excluding a copper paste containing coated metal particles including metal core particles and one or more molecules selected from aliphatic carboxylic acids and aliphatic aldehydes arranged on the surface of the metal core particles at a density of 2.5 to 5.2 molecules per nm2), comprising a step of dispersing spherical copper-containing particles (A) having a median diameter of 2.0 μm or more and less than 10.0 μm, spherical copper-containing particles (B) having a median diameter of 0.1 μm or more and less than 2.0 μm, and flat copper-containing particles (C) having a median diameter of 0.03 μm or more and less than 3.0 μm in a dispersion medium.
12. A method for manufacturing an article having a substrate and a conductive film provided on the substrate, comprising the steps of: A step (A) of forming a coating film of the copper paste for forming a conductor according to any one of claims 1 to 6 on the substrate; and (B) a step of sintering the copper-containing particles in the coating film to form the conductor film.
13. The method for producing an article according to claim 12, wherein the step (A) is a step of printing a coating film of the conductor-forming copper paste by a screen printing method.
14. The method for manufacturing an article according to claim 12 or 13, wherein the conductive film has a thickness of 10.0 μm or more.
15. The method for producing an article according to any one of claims 12 to 14, wherein the copper content in the conductor film is 90 mass % or more.
16. The method for manufacturing an article according to any one of claims 12 to 15, wherein the conductor film is a wiring pattern.
17. A substrate and a conductive film provided on the substrate, The conductor film comprises a sintered body of the conductor forming copper paste according to any one of claims 1 to 6.
18. The article of claim 17, wherein the conductive film has a thickness of 10.0 μm or more.
19. The article according to claim 17 or 18, wherein the copper content in the conductor film is 90 mass % or more.
20. The article according to any one of claims 17 to 19, wherein the conductor film is a wiring pattern.
Citation Information
Patent Citations
Conductive paste for multilayered substrate and multilayered substrate circuit using it
JP1994020517A
Ceramic electronic part and its manufacture
JP1996306580A
Conductive paste and ceramic capacitor
JP2011138704A
Conductive paste composition for low temperature firing
JP2013069654A
Novel coated copper fine particle and production method thereof
JP2014148732A