Positive electrode active material and fluoride ion battery
The use of a Cu x La y M z alloy as a positive electrode active material enhances the capacity characteristics of fluoride ion batteries by improving ionic conductivity through defect introduction in the fluoride phase.
Patent Information
- Application Number
- JP2021032581
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-02
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-03-02
AI Technical Summary
The positive electrode active materials used in fluoride ion batteries have room for improvement in capacity characteristics at high rates.
A positive electrode active material composed of Cu x La y M z (where M is at least one of Ca, Sr, and Ba, with x, y, z satisfying specific atomic ratios) is used to enhance ionic conductivity and capacity characteristics.
The proposed alloy improves the capacity characteristics of fluoride ion batteries at high rates by facilitating better ion conduction through defect introduction in the fluoride phase.
Smart Images

Figure 0007563238000002 
Figure 0007563238000003 
Figure 0007563238000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to positive electrode active materials and fluoride ion batteries. [Background technology]
[0002] Li-ion batteries, for example, are known as high-voltage, high-energy density batteries. Li-ion batteries are cation-based batteries that utilize the reaction between Li ions and positive electrode active materials and the reaction between Li ions and negative electrode active materials. On the other hand, fluoride-ion batteries, which utilize the reaction of fluoride ions (fluoride anions), are known as anion-based batteries.
[0003] For example, Patent Document 1 discloses that a positive electrode active material containing one or more elements selected from Au, Pt, S, Ag, Co, Mo, Cu, W, V, Sb, Bi, Sn, Ni, Pb, Fe, and Cr is used in a fluoride ion battery, and that the positive electrode active material preferably contains Cu or CuF2. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-084506 A Summary of the Invention [Problem to be solved by the invention]
[0005] The positive electrode active material used in a fluoride ion battery has room for improvement in capacity characteristics at high rates. The present disclosure has been made in view of the above-mentioned circumstances, and has as its main object to provide a positive electrode active material having good capacity characteristics at high rates. [Means for solving the problem]
[0006] In order to solve the above problems, the present disclosure provides a positive electrode active material for use in a fluoride ion battery, the positive electrode active material comprising: Cux La y M z (M is at least one of Ca, Sr, and Ba, and x, y, z satisfy 0 < x, 0 < y, 0.01 ≤ z ≤ 0.1, x + y + z = 1.0, and x / y = 2.0 to 4.0), and provides a positive electrode active material characterized by having a composition represented by
[0007] According to the present disclosure, since the positive electrode active material is an alloy containing a predetermined metal element within a predetermined range, a positive electrode active material having good capacity characteristics at high rates can be obtained.
[0008] In the above disclosure, x / y may be 2.0.
[0009] According to the present disclosure, there is provided a fluoride ion battery having a positive electrode active material layer, a negative electrode active material layer, and an electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, wherein the positive electrode active material layer contains the above-described positive electrode active material.
[0010] According to the present disclosure, by using the above-described positive electrode active material, a fluoride ion battery having good capacity characteristics at high rates can be obtained.
Advantages of the Invention
[0011] In the present disclosure, there is an effect that a positive electrode active material having good capacity characteristics at high rates can be provided.
Brief Description of the Drawings
[0012] [Figure 1] It is a schematic cross-sectional view showing an example of a fluoride ion battery in the present disclosure. [Diagram 2] Results of the capacity retention rate in the evaluation batteries obtained in Examples 1 to 8 and the Comparative Example.
Modes for Carrying Out the Invention
[0013] Hereinafter, the positive electrode active material and the fluoride ion battery in the present disclosure will be described in detail.
[0014] A. Positive electrode active material The positive electrode active material in the present disclosure is a positive electrode active material used in a fluoride ion battery, Cu x La y M z (M is at least one of Ca, Sr, and Ba, and x, y, z satisfy 0 < x, 0 < y, 0.01 ≤ z ≤ 0.1, x + y + z = 1.0, and x / y = 2.0 to 4.0) and is an alloy having a composition represented by
[0015] According to the present disclosure, since the positive electrode active material is an alloy containing a predetermined metal element within a predetermined range, it is possible to obtain a positive electrode active material having good capacity characteristics at high rates.
[0016] As described above, it is known to use transition metals belonging to the fourth period such as Cu as the positive electrode active material of a fluoride ion battery. However, when using Cu or the like, an insulating transition metal fluoride is generated during the charging process. When this transition metal fluoride covers the surface of the active material, ion conduction is inhibited, making it difficult to supply ions to the center of the active material. As a result, the charging reaction may not be completed and the capacity may not be obtained as much as the theoretical capacity. In such a case, it is necessary to adjust (refine) the particle size of the active material to the nanosize. Further, when fabricating an electrode with a high ratio of refined active material, the electrolyte (solid electrolyte) also needs to be refined in the same way as the active material. This is because if the electrolyte is not refined, it becomes difficult to fabricate an electrode in which the electron conduction path and the ion conduction path are compatible, and it may be difficult to increase the energy density of the battery. However, when the electrolyte is refined, the ionic conductivity may deteriorate.
[0017] In contrast, the applicant of the present application has the metal element M 1 (The metal element M 1 is at least one of Cu, Fe, and Mn) and the metal element M 2 (The metal element M2 have found that if the positive electrode active material is an alloy containing at least one of the metal elements Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, and Yb as a main component, the positive electrode active material has good capacity characteristics. This is because if the positive electrode active material is such an alloy, the metal element M 2 is fluorinated, and a fluoride (e.g., LaF3) that can act as a solid electrolyte is formed inside the alloy, and this M 2 It is presumed that this is because the fluoride ions diffuse through the fluoride phase, and can be supplied to the center of the active material (the center of the alloy). 2 In simple fluorides (e.g., LaF3), the ionic conductivity is insufficient, and there is room for improvement in the capacity characteristics at high rates.
[0018] The positive electrode active material in the present disclosure is an alloy that contains, in addition to Cu, La (which can exhibit fluoride ion conductivity) and further contains M, which belongs to alkaline earth metals, in a predetermined range. 1 and metal element M 2 Compared to the case of using an alloy containing as its main component (e.g., Cu2La), this is a positive electrode active material with good capacity characteristics at high rates. This is because the inclusion of divalent M in addition to trivalent La results in the formation of a complex fluoride La that can act as a solid electrolyte during the initial charge. (1―z) M z F 3-z It is presumed that this is because La is formed inside the alloy. (1―z) M z F 3-z In comparison with the above-mentioned LaF3, defects have been introduced into the fluoride ions, and it is presumed that the fluoride ions conduct the defects, improving the ionic conductivity and resulting in good capacity characteristics.
[0019] 1.Alloy The alloy in this disclosure is Cu x La y M zAn alloy having a composition represented by (M is at least one of Ca, Sr, and Ba, and x, y, z satisfy 0 < x, 0 < y, 0.01 ≤ z ≤ 0.1, x + y + z = 1.0, and x / y is 2.0 to 4.0).
[0020] The above M is at least one of Ca, Sr, and Ba. The alloy in the present disclosure may contain only one kind or two or more kinds of the above M as M.
[0021] The above z represents the molar ratio (atomic ratio) of M to the total of Cu, La, and M in the alloy in the present disclosure, and is usually 0.01 or more, may be 0.02 or more, and may be 0.04 or more. On the other hand, the above z is usually 0.1 or less, may be 0.08 or less, and may be 0.05 or less. If there is too much metal element M, the alkaline earth element is likely to rust, which may make it difficult to handle the alloy. That is, the alloy in the present disclosure usually contains M in an amount of 1 at% or more and 10 at% or less.
[0022] The above x represents the molar ratio (atomic ratio) of Cu to the total of Cu, La, and M in the alloy in the present disclosure, and is usually greater than 0, may be 0.50 or more, may be 0.60 or more, and may be 0.63 or more. On the other hand, the above x is usually less than 1.0, may be 0.73 or less, and may be 0.66 or less.
[0023] The above y represents the molar ratio (atomic ratio) of La to the total of Cu, La, and M in the alloy in the present disclosure, and is usually greater than 0, may be 0.30 or more, and may be 0.31 or more. On the other hand, the above y is usually less than 1.0, may be 0.40 or less, and may be 0.33 or less.
[0024] Also, in the alloy in the present disclosure, the molar ratio of La to Cu (x / y) is usually 2.0 or more and 4.0 or less, may be 2.0 or more and 3.1 or less, and may be 2.0.
[0025] In the present disclosure, the composition of the positive electrode active material can be determined, for example, by dissolving the positive electrode active material in an acid and measuring it by inductively coupled plasma optical emission spectroscopy (ICP-OES).
[0026] 2.Cathode active material The positive electrode active material in the present disclosure is the alloy described above.
[0027] The shape of the positive electrode active material in the present disclosure is not particularly limited, but may be, for example, particulate. 50 ) is, for example, 0.1 μm or more, may be 0.3 μm or more, or may be 1 μm or more. On the other hand, the average particle diameter (D 50 ) is, for example, 20 μm or less, may be 15 μm or less, may be 10 μm or less, or may be 5 μm or less. If the average particle size is too small, when the ratio of the positive electrode active material in the positive electrode active material layer is increased, there is a possibility that an ion conduction path between the electrolytes is not sufficiently formed. On the other hand, if the average particle size is too large, there is a possibility that ions and electrons are difficult to diffuse into the active material. Note that the average particle size (D 50 ) can be determined, for example, from the results of particle size distribution measurement by a laser diffraction scattering method.
[0028] The method for producing the positive electrode active material in the present disclosure is not particularly limited as long as it is a method by which the desired positive electrode active material can be obtained, and examples thereof include an arc melting method, a sintering method, and a mechanical alloying method.
[0029] B. Fluoride-ion battery FIG. 1 is a schematic cross-sectional view showing an example of a fluoride ion battery according to the present disclosure. The fluoride ion battery 10 shown in FIG. 1 includes a positive electrode active material layer 1, a negative electrode active material layer 2, an electrolyte layer 3 formed between the positive electrode active material layer 1 and the negative electrode active material layer 2, a positive electrode current collector 4 that collects the current of the positive electrode active material layer 1, a negative electrode current collector 5 that collects the current of the negative electrode active material layer 2, and a battery case 6 that houses these members. In the present disclosure, a major feature is that the positive electrode active material layer 1 contains the positive electrode active material described in "A. Positive electrode active material" above. According to the present disclosure, the use of the above-mentioned positive electrode active material can provide a fluoride ion battery with good capacity characteristics.
[0030] 1.Cathode active material layer The positive electrode active material layer in the present disclosure is a layer containing at least the positive electrode active material described above. The positive electrode active material is the same as that described in "A. Positive electrode active material" above. The positive electrode active material layer may contain only the positive electrode active material described above, or may also contain other active materials. In the latter case, the ratio of the positive electrode active material described above in the entire active material is, for example, 85% by weight or more, may be 90% by weight or more, may be 95% by weight or more, or may be 99% by weight or more.
[0031] The content of the positive electrode active material in the positive electrode active material layer is, for example, 10% by weight or more and 90% by weight or less, and may be 20% by weight or more and 80% by weight or less.
[0032] The positive electrode active material layer may further contain at least one of a conductive material, a binder, and an electrolyte, if necessary. The conductive material is not particularly limited as long as it has the desired electronic conductivity, and may be, for example, a carbon material. The carbon material may be, for example, carbon black such as acetylene black, ketjen black, furnace black, thermal black, graphene, fullerene, carbon nanotube, etc. The content of the conductive material in the positive electrode active material layer is, for example, 1% by weight or more, may be 5% by weight or more, or may be 10% by weight or more. On the other hand, the content of the conductive material may be, for example, 20% by weight or less, may be 15% by weight or less. If the proportion of the conductive material is too small, a good electronic conduction path may not be formed, and if the proportion of the conductive material is too large, the proportion of the active material may be relatively small, and the energy density may be reduced.
[0033] There are no particular limitations on the binder as long as it is chemically and electrically stable, and examples of the binder include fluorine-based binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE).
[0034] The electrolyte is the same as that described later in “3. Electrolyte layer.” The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.
[0035] 2.Negative electrode active material layer The negative electrode active material layer in the present disclosure is a layer containing at least a negative electrode active material. The negative electrode active material layer may further contain at least one of a conductive material, an electrolyte, and a binder, as necessary.
[0036] As the negative electrode active material, any active material having a lower potential than the positive electrode active material can be selected. As the negative electrode active material, for example, a metal element, an alloy, a metal oxide, and a fluoride thereof can be mentioned. As the metal element contained in the negative electrode active material, for example, La, Ca, Al, Eu, Li, Si, Ge, Sn, In, V, Cd, Cr, Fe, Zn, Ga, Ti, Nb, Mn, Yb, Zr, Sm, Ce, Mg, Pb, etc. can be mentioned. Among them, the negative electrode active material is preferably Mg, MgFx, Al, AlFx, La, LaFx, Ce, CeFx, Ca, CaFx, Pb, or PbFx. Note that the above x is a real number greater than 0.
[0037] The conductive material and binder may be the same as those described in "1. Positive electrode active material layer" above. The electrolyte is the same as that described in "3. Electrolyte layer", so the description here is omitted.
[0038] The content of the negative electrode active material in the negative electrode active material layer is preferably as high as possible from the viewpoint of capacity, for example, 30% by weight or more, preferably 50% by weight or more, and more preferably 70% by weight or more. The thickness of the negative electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.
[0039] 3. Electrolyte layer The electrolyte layer in the present disclosure is a layer formed between a positive electrode active material layer and a negative electrode active material layer. The electrolyte constituting the electrolyte layer may be a liquid electrolyte (electrolytic solution), a polymer electrolyte, or an inorganic solid electrolyte.
[0040] The electrolyte contains, for example, a fluoride salt and a solvent. Examples of the fluoride salt include inorganic fluoride salts, organic fluoride salts, and ionic liquids. Examples of the inorganic fluoride salt include XF (X is Li, Na, K, Rb, or Cs). Examples of the cation of the organic fluoride salt include alkyl ammonium cations such as tetramethylammonium cations. The concentration of the fluoride salt in the electrolyte is, for example, 0.1 mol / L or more, may be 0.3 mol / L or more, or may be 0.5 mol / L or more. On the other hand, the concentration of the fluoride salt is, for example, 6 mol / L or less, and may be 3 mol / L or less.
[0041] Examples of the solvent include cyclic carbonates such as ethylene carbonate (EC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), propylene carbonate (PC), and butylene carbonate (BC), chain carbonates such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), chain ethers such as diethyl ether, 1,2-dimethoxymethane, and 1,3-dimethoxypropane, cyclic ethers such as tetrahydrofuran and 2-methyltetrahydrofuran, cyclic sulfones such as sulfolane, chain sulfones such as dimethyl sulfoxide (DMSO), cyclic esters such as γ-butyrolactone, nitriles such as acetonitrile, and any mixtures thereof. The polymer electrolyte can be obtained, for example, by adding a polymer to a liquid electrolyte and gelling it.
[0042] On the other hand, examples of inorganic solid electrolytes include fluorides of lanthanoid elements such as La and Ce, fluorides of alkali metal elements such as Li, Na, K, Rb, and Cs, and fluorides of alkaline earth elements such as Ca, Sr, and Ba. The inorganic solid electrolyte is preferably a fluoride containing at least one metal element selected from La, Ba, Pb, Sn, Ca, and Ce. The inorganic solid electrolyte may contain only one of the above metal elements, or may contain two or more of them. Specific examples of inorganic solid electrolytes include La, 1-x Ba xF 3-x (0≦x≦1), Pb 2-x Sn x F4(0≦x≦2), Ca 2-x Ba x F4(0≦x≦2) and Ce 1-x Ba x F 3-x (0≦x≦1). Each of the x's may be greater than 0, 0.3 or greater, 0.5 or greater, or 0.9 or greater. Each of the x's may be smaller than 1, 0.9 or less, 0.5 or less, or 0.3 or less. The shape of the inorganic solid electrolyte is not particularly limited, but may be, for example, particulate.
[0043] 4.Other configurations The fluoride ion battery in the present disclosure has at least the above-mentioned positive electrode active material layer, negative electrode active material layer, and electrolyte layer. In addition, it usually has a positive electrode current collector that collects the current of the positive electrode active material layer, a negative electrode current collector that collects the current of the negative electrode active material layer, and a battery case that houses the above-mentioned members. The materials of the positive electrode current collector, the negative electrode current collector, and the battery case can be conventionally known materials. The shape of the current collector can be, for example, a foil shape, a mesh shape, or a porous shape. The fluoride ion battery may also have a separator between the positive electrode active material layer and the negative electrode active material layer. By providing a separator, a safer battery can be obtained.
[0044] 5. Fluoride-ion batteries The fluoride ion battery in the present disclosure may be a liquid battery or an all-solid-state battery, but is preferably an all-solid-state battery. The fluoride ion battery in the present disclosure may be a primary battery or a secondary battery, but is preferably a secondary battery. This is because the battery can be repeatedly charged and discharged, and is useful, for example, as an in-vehicle battery. The shape of the fluoride ion battery in the present disclosure may be, for example, a coin type, a laminate type, a cylindrical type, or a square type.
[0045] The present disclosure is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present disclosure and that exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0046] [Example 1] (Preparation of positive electrode active material) The composition is Cu 0.653 La 0.327 Ca 0.02 Cu, La, and Ca metals were weighed out so that the composition was (x=0.653, y=0.327, z=0.02, x / y=2.0, and the atomic ratio of the total of Cu2La to Ca was 98:2). In other words, the content of alkaline earth metal M (Ca) in the alloy was weighed out to be 2 at%. Then, all of the above elements were melted and alloyed by an arc melting method. After that, an alloy ribbon was produced by a liquid quenching method. The alloy ribbon was then pulverized in a mortar to obtain an alloy powder (positive electrode active material).
[0047] (Preparation of evaluation battery) The Cu 0.653 La 0.327 Ca 0.02 Powder and solid electrolyte (La 0.9 Ba 0.1 F 2.9 The positive electrode active material mixture was obtained by mixing the positive electrode active material (working electrode) and the conductive material (VGCF) in a weight ratio of 30:60:10 in a ball mill (rotation speed 100 rpm). 0.9 Ba 0.1 F 2.9 The electrode was made by powder compaction with Pb foil and a counter electrode made of a 95:5 mixture of PbF2 and a conductive material (acetylene black). This produced a battery for evaluation.
[0048] [Examples 2 to 9] Except for changing the alloy composition as shown in Table 1, a battery for evaluation was fabricated in the same manner as in Example 1.
[0049] [Comparative Example] A battery for evaluation was fabricated in the same manner as in Example 1, except that Cu2La was used as the positive electrode active material.
[0050] [evaluation] (Charge / discharge test) A charge-discharge test was carried out on the evaluation batteries obtained in Examples 1 to 9 and Comparative Example. The charge-discharge test was carried out at a temperature of 140° C., with the end potential of the working electrode ranging from −1.5 V (vs Pb / PbF2) to 3 V (vs Pb / PbF2), and with a current of 50 μA / cm 2 or 300μA / cm 2 The results are shown in Table 1. Capacity maintenance rate (%)=(300μA / cm 2 Discharge capacity when charged and discharged at 50μA / cm 2 (discharge capacity when charged and discharged at 100) x 100
[0051] [Table 1]
[0052] As shown in Table 1, in all of the positive electrode active materials of Examples 1 to 9, the capacity retention rate was increased compared to the Cu2La alloy of Comparative Example 1, and improvement in the battery characteristics at high rates was confirmed.
[0053] FIG. 2 shows the results of the capacity retention rate of the evaluation batteries obtained in Examples 1 to 8 and the Comparative Example. In Examples 1 to 8, the composition ratio of Cu:La is 2:1, the same as in the Comparative Example. In Examples 1 to 8, it was confirmed that the discharge capacity characteristics at high rates improve with an increase in the amount of added alkaline earth element, regardless of the type of element added. By adding divalent M to trivalent La, the complex fluoride La (1―z) M z F 3-z It is presumed that this is due to the formation of La (1―z) M z F 3-zIn comparison with the above-mentioned LaF3, since defects are introduced into the fluoride ions, it is presumed that the fluoride ions conduct the defects, improving the ionic conductivity and improving the capacity characteristics. In addition, it is presumed that the mechanism by which the ionic conductivity is improved by the amount of defects is the one that does not depend on the element type of M.
[0054] Example 9 differs from the comparative examples in that the composition ratio of Cu:La is not 2:1, but like Examples 1-8, the capacity characteristics at high rates were good. [Explanation of symbols]
[0055] 1...Cathode active material layer 2...Negative electrode active material layer 3...electrolyte layer 4...Positive electrode current collector 5...Negative electrode current collector 6. Battery case 10...Fluoride-ion battery
Claims
1. A positive electrode active material for use in a fluoride ion battery, comprising: The positive electrode active material is Cu x La y M z (M is at least one of Ca, Sr, and Ba, and x, y, and z satisfy 0<x, 0<y, 0.01≦z≦0.1, x+y+z=1.0, and x / y=2.0 to 4.0).
2. The positive electrode active material of claim 1 , wherein x / y is 2.
0.
3. A fluoride ion battery having a positive electrode active material layer, a negative electrode active material layer, and an electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, A fluoride ion battery, wherein the positive electrode active material layer contains the positive electrode active material according to claim 1 or 2.
Citation Information
Patent Citations
Fluoride ion secondary battery
JP2017084506A
Positive electrode active material for fluoride ion secondary batteries, positive electrode using said active material, fluoride ion secondary battery, and method for producing said active material
WO2019187942A1