Electrolyte and lithium-ion secondary battery
The electrolyte solution with a combination of lithium salts and methyl propionate in lithium ion secondary batteries addresses viscosity and durability issues, enhancing structural and performance characteristics.
Patent Information
- Application Number
- JP2021056292
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-29
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-03-29
AI Technical Summary
Existing lithium ion secondary batteries face challenges in improving characteristics such as structural durability, charging and discharging performance, and capacity retention due to issues with electrolyte composition, particularly related to the use of LiPF6 and high viscosity of alkylene cyclic carbonates.
The electrolyte solution contains 30 mol% or more of lithium salts other than LiPF6 and 75% or more of methyl propionate in a non-aqueous solvent, combined with alkylene cyclic carbonate, to enhance ionic conductivity and reduce viscosity, along with a specific battery structure that includes a sealing part to improve durability.
The solution results in lithium ion secondary batteries with enhanced structural durability, improved charging and discharging performance, and increased capacity retention, particularly at high temperatures.
Smart Images

Figure 0007563273000012 
Figure 0007563273000013 
Figure 0007563273000014
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte solution that can be used in lithium ion secondary batteries, and to a lithium ion secondary battery that uses the electrolyte solution. [Background technology]
[0002] Lithium-ion secondary batteries, which have excellent capacity, are used as power sources for mobile terminals, personal computers, electric vehicles, etc. In recent years, the demand for decarbonization has increased, and efforts to electrify the driving sources of various devices have been actively carried out. Accordingly, further improvement in the characteristics of lithium-ion secondary batteries is desired.
[0003] The inventors of the present invention aimed to improve the characteristics of lithium ion secondary batteries by optimizing the electrolyte of the lithium ion secondary batteries.
[0004] Conventional electrolytes in lithium ion secondary batteries are generally prepared by dissolving LiPF6 at a concentration of about 1 mol / L in a mixed non-aqueous solvent prepared by mixing an alkylene cyclic carbonate such as ethylene carbonate and a chain carbonate such as dimethyl carbonate or ethyl methyl carbonate. For example, Patent Document 1 introduces an electrolyte prepared by dissolving LiPF6 at a concentration of 1 mol / L in a mixed non-aqueous solvent prepared by mixing ethylene carbonate and ethyl methyl carbonate at a volume ratio of 3:7. Patent Document 2 introduces an electrolyte prepared by dissolving LiPF6 at a concentration of 1 mol / L in a mixed non-aqueous solvent prepared by mixing ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate at a volume ratio of 3:2:5. Here, a chain carbonate is used as the main solvent of the electrolyte. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-123300 A [Patent Document 2] JP 2013-140734 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the process of improving the characteristics of lithium-ion secondary batteries, the inventors of the present invention discovered the use of alkylene cyclic carbonate and methyl propionate in combination as a non-aqueous solvent for an electrolyte, and have already filed an application for a lithium-ion secondary battery using this electrolyte (Patent Application No. 2020-026926).
[0007] The above-mentioned electrolyte solution can contribute to improving the characteristics of lithium ion secondary batteries. However, the present inventors were not satisfied with this and conducted extensive research to achieve further improvements in the characteristics. The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an electrolyte solution that can impart excellent characteristics to a lithium ion secondary battery, and a lithium ion secondary battery that exhibits excellent characteristics. [Means for solving the problem]
[0008] As a result of various experiments, the inventors of the present invention found that in an electrolyte solution using alkylene cyclic carbonate and methyl propionate in combination as a non-aqueous solvent, the characteristics of a lithium ion secondary battery can be further improved by further adjusting the non-aqueous solvent and lithium salt to a specific ratio. Based on this finding, the inventors of the present invention have completed the electrolyte solution of the present invention.
[0009] Furthermore, the applicant of the present invention has developed a structure of a storage cell and a storage device that can suppress the deterioration of the sealing property as part of an attempt to improve the durability of a storage device including a lithium ion secondary battery, and has already filed an application (Patent Application No. 2021-003409). In order to further improve the sealing property of the storage cell in a lithium ion secondary battery having the structure, the inventor of the present invention also conducted various studies on the electrolyte. In the process, it was found that the sealing property of the storage cell in the lithium ion secondary battery can be further improved by combining the structure with the above-mentioned electrolyte of the present invention, and the lithium ion secondary battery of the present invention was completed.
[0010] The electrolyte of the present invention that solves the above problems is The battery has an electrolyte containing a lithium salt and a non-aqueous solvent containing an alkylene cyclic carbonate and methyl propionate, The electrolyte contains a lithium salt other than LiPF6 in an amount of 30 mol % or more based on the total amount of lithium salts, The non-aqueous solvent is an electrolyte solution containing 75% by volume or more of the methyl propionate.
[0011] Further, the lithium ion secondary battery of the present invention which solves the above problems comprises: a positive electrode having a first current collector and a positive electrode active material layer provided on one surface of the first current collector; a negative electrode including a second current collector and a negative electrode active material layer provided on one surface of the second current collector, the negative electrode being overlapped on the positive electrode with the negative electrode active material layer facing the positive electrode active material layer; a separator disposed between the positive electrode active material layer and the negative electrode active material layer; a sealing portion that is disposed between the first current collector and the second current collector, that surrounds the positive electrode active material layer and the negative electrode active material layer, and that seals an electrolyte in a space between the first current collector and the second current collector; The lithium ion secondary battery uses the above-mentioned electrolytic solution of the present invention as the electrolytic solution. Effect of the Invention
[0012] The electrolyte of the present invention can impart excellent characteristics to a lithium ion secondary battery. The lithium ion secondary battery of the present invention also exhibits excellent characteristics, and is particularly excellent in structural durability. [Brief description of the drawings]
[0013] [Figure 1] 1 is a graph showing the change over time in CC discharge capacity in each of the lithium ion secondary batteries of Example 8 and Comparative Example 11. [Diagram 2] 1 is a graph showing the change over time in CC discharge capacity in each of the lithium ion secondary batteries of Example 8 and Comparative Examples 8 to 10. [Diagram 3] FIG. 13 is an explanatory diagram illustrating a lithium ion secondary battery according to a ninth embodiment. [Figure 4] FIG. 2 is an explanatory diagram illustrating a lithium ion secondary battery according to a tenth embodiment. [Diagram 5] FIG. 13 is an explanatory diagram illustrating the measurement positions of the natural peeling length in Evaluation Example 9. [Figure 6] 13 is a graph showing the natural peel length of each test piece in Evaluation Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiment of the present invention will be described. Unless otherwise specified, the numerical range "x to y" described in this specification includes the lower limit x and the upper limit y. These upper and lower limit values, as well as the numerical values listed in the examples, can be arbitrarily combined to form a new numerical range. Furthermore, any numerical value selected from any of the above numerical ranges can be used as the upper and lower limit numerical values of the new numerical range.
[0015] The electrolyte solution of the present invention can improve the characteristics of a lithium ion secondary battery by providing all of the following (1) to (3). (1) The electrolyte contains 30 mol% or more of a lithium salt other than LiPF6 based on the total amount of lithium salts. (2) The non-aqueous solvent contains an alkylene cyclic carbonate and methyl propionate. (3) The non-aqueous solvent contains 75% by volume or more of methyl propionate.
[0016] The above feature (1) can contribute to improving the properties of lithium ion secondary batteries, particularly the structural durability. The above (2) can contribute to the smooth charging and discharging of lithium-ion secondary batteries. Specifically, the alkylene cyclic carbonate facilitates the smooth generation of lithium ions and their insertion and desorption into and from the negative electrode, and the methyl propionate compensates for the shortcomings of the alkylene cyclic carbonate, such as high viscosity and high melting point. Furthermore, the above feature (3) can contribute to improving the capacity retention rate, output, and other characteristics of the lithium ion secondary battery. It can be said that the electrolyte solution of the present invention can improve the characteristics of lithium ion secondary batteries by utilizing these combined effects.
[0017] The structural durability of the lithium ion secondary battery of the present invention can be improved by providing both of the following (4) and (5). (4) a positive electrode having a first current collector and a positive electrode active material layer provided on one surface of the first current collector; a negative electrode including a second current collector and a negative electrode active material layer provided on one surface of the second current collector, the negative electrode being overlapped on the positive electrode with the negative electrode active material layer facing the positive electrode active material layer; a separator disposed between the positive electrode active material layer and the negative electrode active material layer; a sealing portion that is disposed between the first current collector and the second current collector, that surrounds the positive electrode active material layer and the negative electrode active material layer, and that seals an electrolyte in a space between the first current collector and the second current collector. (5) As the electrolyte, the above-mentioned electrolyte of the present invention is used.
[0018] As explained in detail in the aforementioned Patent Application No. 2021-003409, the above (4) can contribute to suppressing deterioration of the sealing property, which is one of the characteristics of lithium-ion secondary batteries. The above feature (5) can further contribute to improving the structural durability, specifically the sealing property, of the characteristics of the lithium ion secondary battery including the above feature (4). The lithium ion secondary battery of the present invention can achieve improved characteristics through the cooperation of these elements. Hereinafter, the electrolyte solution and the lithium ion secondary battery of the present invention will be described in detail with respect to each of their components.
[0019] First, the electrolyte of the present invention will be described.
[0020] The lithium ion concentration in the electrolyte solution of the present invention is preferably within the range of 0.8 to 1.8 mol / L, more preferably within the range of 0.9 to 1.5 mol / L, further preferably within the range of 1.0 to 1.4 mol / L, and particularly preferably within the range of 1.1 to 1.3 mol / L, from the viewpoint of ion conductivity.
[0021] The electrolyte used in the electrolytic solution of the present invention contains a lithium salt, and contains 30 mol % or more of a lithium salt other than LiPF6 based on the total amount of the lithium salts. The electrolytic solution of the present invention may or may not contain LiPF6 as a lithium salt.
[0022] Here, LiPF6 is widely used as an electrolyte in electrolytic solutions for lithium ion secondary batteries and is relatively inexpensive. The reason why the electrolytic solution of the present invention uses a lithium salt other than LiPF6 is as follows.
[0023] It is known that hydrogen fluoride is produced by the reaction of LiPF6 with water. Since a small amount of water is present in the electrolyte of a typical lithium-ion secondary battery, the electrolyte of a lithium-ion secondary battery containing LiPF6 may contain hydrogen fluoride. It is also known that LiPF6 is thermally unstable and produces PF5 at temperatures above 60° C., for example. The PF5 can react with water to produce hydrogen fluoride.
[0024] The inventors of the present invention have repeatedly studied the composition of the electrolyte in order to improve the characteristics of lithium-ion secondary batteries. In the process, they have found that hydrogen fluoride and PF5 present in the electrolyte may corrode the electrodes and containers of lithium-ion secondary batteries, and that corrosion of the electrodes and containers may impair the durability of the lithium-ion secondary battery. In particular, when a lithium-ion secondary battery has a structure having a sealing part between two current collectors as disclosed in Japanese Patent Application No. 2021-003409, if the surface of the metal part contained in the current collector is corroded (specifically, fluorinated), the bonding force between the sealing part and the current collector is weakened, the battery is structurally deteriorated, and the sealing property by the sealing part is likely to be reduced. This problem is particularly noticeable when the current collector contains aluminum.
[0025] The inventors of the present invention aimed to suppress the above-mentioned problems caused by LiPF6 in order to improve the structural durability of lithium ion secondary batteries, and found that the above-mentioned problems can be suppressed when the electrolyte contains 30 mol % or more of a lithium salt other than LiPF6 based on the total amount of lithium salts. As will be described in detail in the Examples section below, the inventors of the present invention conducted actual tests and found that in a lithium ion secondary battery having a sealing portion between two current collectors, when the electrolyte contains 30 mol % or more of a lithium salt other than LiPF6 relative to the total amount of lithium salts, the durability is improved compared to when the electrolyte contains only LiPF6.
[0026] Specific examples of lithium salts that can be used in the electrolyte of the present invention include LiPF6, LiClO4, LiAsF6, LiBF4, FSO3Li, CF3SO3Li, C2F5SO3Li, C3F7SO3Li, C4F9SO3Li, and C5F 11 SO3Li, C6F 13Examples of the lithium salt include SO3Li, CH3SO3Li, C2H5SO3Li, C3H7SO3Li, CF3CH2SO3Li, CF3C2H4SO3Li, (FSO2)2NLi, (CF3SO2)2NLi, (C2F5SO2)2NLi, FSO2(CF3SO2)NLi, FSO2(C2F5SO2)NLi, (SO2CF2CF2SO2)NLi, (SO2CF2CF2CF2SO2)NLi, FSO2(CH3SO2)NLi, FSO2(C2H5SO2)NLi, LiPO2F2, LiBF2(C2O4), and LiB(C2O4)2. Only one type of lithium salt other than LiPF6 may be used, or two or more types may be used in combination.
[0027] As the lithium salt other than LiPF6, the one represented by the following general formula (1) is particularly preferable. This type of lithium salt is unlikely to produce hydrogen fluoride or PF5.
[0028] (R 1 X 1 )(R 2 SO2)NLi General formula (1) (R 1 is selected from hydrogen, halogen, an alkyl group which may be substituted with a substituent, a cycloalkyl group which may be substituted with a substituent, an unsaturated alkyl group which may be substituted with a substituent, an unsaturated cycloalkyl group which may be substituted with a substituent, an aromatic group which may be substituted with a substituent, a heterocyclic group which may be substituted with a substituent, an alkoxy group which may be substituted with a substituent, an unsaturated alkoxy group which may be substituted with a substituent, a thioalkoxy group which may be substituted with a substituent, an unsaturated thioalkoxy group which may be substituted with a substituent, CN, SCN, and OCN. R 2is selected from hydrogen, halogen, an alkyl group which may be substituted with a substituent, a cycloalkyl group which may be substituted with a substituent, an unsaturated alkyl group which may be substituted with a substituent, an unsaturated cycloalkyl group which may be substituted with a substituent, an aromatic group which may be substituted with a substituent, a heterocyclic group which may be substituted with a substituent, an alkoxy group which may be substituted with a substituent, an unsaturated alkoxy group which may be substituted with a substituent, a thioalkoxy group which may be substituted with a substituent, an unsaturated thioalkoxy group which may be substituted with a substituent, CN, SCN, and OCN. Also, R 1 and R 2 may be bonded to each other to form a ring. X 1 are SO2, C=O, C=S, R a P=O, R b P=S, S=O, Si=O. R a , R b are each independently selected from hydrogen, halogen, an alkyl group which may be substituted with a substituent, a cycloalkyl group which may be substituted with a substituent, an unsaturated alkyl group which may be substituted with a substituent, an unsaturated cycloalkyl group which may be substituted with a substituent, an aromatic group which may be substituted with a substituent, a heterocyclic group which may be substituted with a substituent, an alkoxy group which may be substituted with a substituent, an unsaturated alkoxy group which may be substituted with a substituent, a thioalkoxy group which may be substituted with a substituent, an unsaturated thioalkoxy group which may be substituted with a substituent, OH, SH, CN, SCN, and OCN. Also, R a , R b is R 1 or R 2 may be bonded to form a ring.)
[0029] The phrase "optionally substituted with a substituent" in the chemical structure represented by the above general formula (1) will be explained below. For example, "optionally substituted alkyl group" means an alkyl group in which one or more hydrogen atoms of the alkyl group are substituted with a substituent, or an alkyl group having no substituent.
[0030] Examples of the substituent in the phrase "may be substituted with a substituent" include an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, an unsaturated cycloalkyl group, an aromatic group, a heterocyclic group, a halogen, OH, SH, CN, SCN, OCN, a nitro group, an alkoxy group, an unsaturated alkoxy group, an amino group, an alkylamino group, a dialkylamino group, an aryloxy group, an acyl group, an alkoxycarbonyl group, an acyloxy group, an aryloxycarbonyl group, an acylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfonylamino group, a sulfamoyl group, a carbamoyl group, an alkylthio group, an arylthio group, a sulfonyl group, a sulfinyl group, a ureido group, a phosphoric acid amide group, a sulfo group, a carboxyl group, a hydroxamic acid group, a sulfino group, a hydrazino group, an imino group, and a silyl group. These substituents may be further substituted with a substituent. When there are two or more substituents, the substituents may be the same or different.
[0031] The lithium salt is preferably represented by the following general formula (1-1).
[0032] (R 13 X 2 )(R 14 SO2)NLi General formula (1-1) (R 13 , R 14 are each independently n H a F b Cl c Br d I e (CN) f (SCN) g (OCN) h It is. n, a, b, c, d, e, f, g, and h are each independently an integer of 0 or greater and satisfy 2n+1=a+b+c+d+e+f+g+h. Also, R 13 and R 14 may be bonded to each other to form a ring, in which case 2n=a+b+c+d+e+f+g+h is satisfied. X 2are SO2, C=O, C=S, R c P=O, R d P=S, S=O, Si=O. R c , R d are each independently selected from hydrogen, halogen, an alkyl group which may be substituted with a substituent, a cycloalkyl group which may be substituted with a substituent, an unsaturated alkyl group which may be substituted with a substituent, an unsaturated cycloalkyl group which may be substituted with a substituent, an aromatic group which may be substituted with a substituent, a heterocyclic group which may be substituted with a substituent, an alkoxy group which may be substituted with a substituent, an unsaturated alkoxy group which may be substituted with a substituent, a thioalkoxy group which may be substituted with a substituent, an unsaturated thioalkoxy group which may be substituted with a substituent, OH, SH, CN, SCN, and OCN. Also, R c , R d is R 13 or R 14 may be bonded to form a ring.)
[0033] In the chemical structure represented by the above general formula (1-1), the meaning of the phrase "optionally substituted with a substituent" is the same as that explained in the above general formula (1).
[0034] In the chemical structure represented by the above general formula (1-1), n is preferably an integer of 0 to 6, more preferably an integer of 0 to 4, and particularly preferably an integer of 0 to 2. In addition, in the chemical structure represented by the above general formula (1-1), R 13 and R 14 When they are bonded to form a ring, n is preferably an integer of 1 to 8, more preferably an integer of 1 to 7, and particularly preferably an integer of 1 to 3.
[0035] The lithium salt is more preferably one represented by the following general formula (1-2).
[0036] (R 15 SO2)(R 16 SO2)NLi General formula (1-2) (R 15 , R 16are each independently n H a F b Cl c Br d I e It is. n, a, b, c, d, and e are each independently an integer of 0 or greater and satisfy 2n+1=a+b+c+d+e. Also, R 15 and R 16 may be bonded to each other to form a ring, in which case 2n=a+b+c+d+e is satisfied.
[0037] In the chemical structure represented by the above general formula (1-2), n is preferably an integer of 0 to 6, more preferably an integer of 0 to 4, and particularly preferably an integer of 0 to 2. In addition, in the chemical structure represented by the above general formula (1-2), R 15 and R 16 When they are bonded to form a ring, n is preferably an integer of 1 to 8, more preferably an integer of 1 to 7, and particularly preferably an integer of 1 to 3.
[0038] In the chemical structure represented by the above general formula (1-2), a, c, d, and e are preferably 0.
[0039] Furthermore, the lithium salt represented by the above general formula (1), (1-1) or (1-2) is preferably at least one imide salt selected from (CF3SO2)2NLi, (FSO2)2NLi, (C2F5SO2)2NLi, FSO2(CF3SO2)NLi, (SO2CF2CF2SO2)NLi, or (SO2CF2CF2CF2SO2)NLi. When (FSO2)2NLi is used, the output and durability of the lithium-ion secondary battery improves. This is thought to be due to the fact that the use of (FSO2)2NLi reduces the viscosity of the electrolyte and forms a good coating on the surfaces of the negative and positive electrodes.
[0040] The amount of lithium salt other than LiPF6 contained in the electrolyte of the present invention may be 30 mol % or more based on the total amount of lithium salts, and preferable ranges thereof include 50 mol % or more, 75 mol % or more, and 90 mol % or more based on the total amount of lithium salts.
[0041] The electrolyte of the present invention contains an alkylene cyclic carbonate and methyl propionate in a non-aqueous solvent.
[0042] The alkylene cyclic carbonate is a non-aqueous solvent with a high dielectric constant, and is considered to contribute to the dissolution and ionic dissociation of the lithium salt. It is also known that alkylene cyclic carbonate is generally reductively decomposed during charging of a lithium ion secondary battery to form a solid electrolyte interphase (SEI) coating on the surface of the negative electrode. It is believed that the presence of such an SEI coating enables reversible insertion and extraction of lithium ions into and from a negative electrode containing graphite. The electrolyte of the present invention may contain only one type of alkylene cyclic carbonate or a combination of two or more types of alkylene cyclic carbonates. Examples of the alkylene cyclic carbonate include ethylene carbonate and propylene carbonate, and among these, ethylene carbonate is particularly preferred.
[0043] By the way, alkylene cyclic carbonate is useful as a non-aqueous solvent of electrolyte, but has high viscosity. Therefore, if the proportion of alkylene cyclic carbonate is too high, it may have a negative effect on the ionic conductivity of electrolyte and the diffusion of lithium ions in electrolyte. In addition, since alkylene cyclic carbonate has a relatively high melting point, if the proportion of alkylene cyclic carbonate is too high, electrolyte may solidify under low temperature conditions.
[0044] On the other hand, methyl propionate is a non-aqueous solvent with a low dielectric constant, low viscosity, and low melting point. In the electrolyte of the present invention, the alkylene cyclic carbonate and methyl propionate coexist, and the disadvantages of the alkylene cyclic carbonate are offset by the methyl propionate. That is, it is considered that the methyl propionate contributes to lowering the viscosity of the electrolyte, optimizing the ionic conductivity, optimizing the diffusion coefficient of lithium ions, and preventing solidification under low temperature conditions.
[0045] Esters having a chemical structure similar to that of methyl propionate include methyl acetate, ethyl acetate, ethyl propionate, methyl butyrate, and ethyl butyrate. Here, as disclosed in Japanese Patent Application No. 2020-026926, the inventors of the present invention have discovered that methyl esters are superior to ethyl esters in terms of electrolyte properties and battery characteristics. The melting points and boiling points of the methyl esters methyl propionate, methyl acetate, and methyl butyrate are as follows: Methyl propionate Melting point -88℃, boiling point 80℃ Methyl acetate Melting point -98℃, boiling point 57℃ Methyl butyrate Melting point -95℃, boiling point 102℃
[0046] Since the operating environment of a lithium ion secondary battery is expected to be about 60°C, the non-aqueous solvent contained in the electrolyte preferably has a boiling point of 60°C or higher. From the viewpoint of the manufacturing environment, it is preferable that the boiling point of the non-aqueous solvent used is high. In addition, the more carbon atoms in the ester, the more lipophilic the ester becomes, which is disadvantageous to the dissolution and dissociation of the lithium salt, so it is preferable that the number of carbon atoms in the ester is small.
[0047] Considering all the above, it can be said that methyl propionate is the most suitable ester. This is also supported by the results of Basic Study 2 described below.
[0048] The non-aqueous solvent in the electrolyte of the present invention contains 75% by volume or more of methyl propionate. By containing a sufficiently large amount of methyl propionate relative to the alkylene cyclic carbonate, the electrolyte of the present invention can improve both the charge / discharge capacity of the positive electrode and the charge / discharge capacity of the negative electrode in a lithium ion secondary battery.
[0049] There is no particular upper limit on the amount of methyl propionate, and it is sufficient that it is contained in the non-aqueous solvent at less than 100% by volume. In order to achieve high levels of charge / discharge capacity for the positive electrode and the negative electrode, the non-aqueous solvent preferably contains 85% by volume or less of methyl propionate, and more preferably contains 80% by volume or less of methyl propionate.
[0050] The non-aqueous solvent in the electrolytic solution of the present invention may contain other non-aqueous solvents in addition to the alkylene cyclic carbonate and methyl propionate, or may consist of the alkylene cyclic carbonate and methyl propionate. In either case, the electrolytic solution of the present invention may contain 75% by volume or more of methyl propionate when the total non-aqueous solvent is taken as 100% by volume. Note that the total non-aqueous solvent being taken as 100% by volume means the sum of the volumes of each non-aqueous solvent at normal temperature (25°C) and normal pressure before mixing.
[0051] In the electrolytic solution of the present invention, the ratio of methyl propionate to the total volume of the alkylene cyclic carbonate and methyl propionate is preferably within the range of 72 to 95 volume %, more preferably within the range of 75 to 90 volume %, and most preferably within the range of 75 to 85 volume %.
[0052] Similarly, the ratio of alkylene cyclic carbonate to the total volume of alkylene cyclic carbonate and methyl propionate is preferably within the range of 5 to 28 volume%, more preferably within the range of 10 to 25 volume%, and most preferably within the range of 15 to 25 volume%.
[0053] Examples of the other non-aqueous solvents include fluorine-containing cyclic carbonates and unsaturated cyclic carbonates. These may be used alone or in combination. By using these non-aqueous solvents in combination with alkylene cyclic carbonate and methyl propionate, the performance of the lithium ion secondary battery can be improved.
[0054] Examples of fluorine-containing cyclic carbonates include fluoroethylene carbonate, 4-(trifluoromethyl)-1,3-dioxolan-2-one, 4,4-difluoro-1,3-dioxolan-2-one, 4-fluoro-4-methyl-1,3-dioxolan-2-one, 4-(fluoromethyl)-1,3-dioxolan-2-one, 4,5-difluoro-1,3-dioxolan-2-one, 4-fluoro-5-methyl-1,3-dioxolan-2-one, and 4,5-difluoro-4,5-dimethyl-1,3-dioxolan-2-one.
[0055] Examples of unsaturated cyclic carbonates include vinylene carbonate, fluorovinylene carbonate, methylvinylene carbonate, fluoromethylvinylene carbonate, ethylvinylene carbonate, propylvinylene carbonate, butylvinylene carbonate, dimethylvinylene carbonate, diethylvinylene carbonate, dipropylvinylene carbonate, trifluoromethylvinylene carbonate, and vinylethylene carbonate. It is particularly preferable that the electrolyte of the present invention contains vinylene carbonate.
[0056] The amount of the fluorine-containing cyclic carbonate and / or unsaturated cyclic carbonate added in the electrolytic solution of the present invention can be, for example, within the range of 0.1 to 5 mass %, 0.3 to 4 mass %, 0.5 to 3 mass %, or 1 to 2 mass % relative to the total mass of the other components.
[0057] The electrolyte solution of the present invention may contain an additive. It is preferable to select an additive that starts reductive decomposition at a potential higher than the potentials at which other components of the electrolyte solution, specifically, the alkylene cyclic carbonate and methyl propionate, start reductive decomposition. Specific examples of the additive include cyclic sulfate, oxalate borate, and dihalogenated phosphate. These additives may be used alone or in combination.
[0058] Cyclic sulfate esters are compounds represented by the following chemical formula: RO-SO2-OR (The two R's are alkyl groups that are bonded together to form a ring with -OSO-.) Examples of the cyclic sulfate ester include those having a 5- to 9-membered ring, a 5- to 8-membered ring, and a 5- to 7-membered ring. Examples of the cyclic sulfate ester include those having 2 to 6, 2 to 5, and 2 to 4 carbon atoms.
[0059] The oxalate borate is preferably a lithium salt. Specific examples of the oxalate borate include LiB(C2O4)2 and LiB(C2O4)X2 (X is a halogen selected from F, Cl, Br, and I). Preferably, the oxalato borate is LiB(C2O4)2, i.e., lithium bis(oxalato)borate, and / or LiB(C2O4)F2, i.e., lithium difluoro(oxalato)borate.
[0060] The dihalogenated phosphate is preferably a lithium salt. A specific example of the dihalogenated phosphate is LiPO2X2 (X is a halogen selected from F, Cl, Br, and I).
[0061] The amount of the above-mentioned additives added in the electrolyte solution of the present invention can be, for example, within a range of 0.1 to 5 mass %, a range of 0.3 to 4 mass %, a range of 0.5 to 3 mass %, or a range of 1 to 2 mass %, relative to the total mass of the components other than the additives. The lithium ion secondary battery of the present invention using the electrolyte of the present invention will be described below.
[0062] The lithium ion secondary battery of the present invention comprises a positive electrode, a negative electrode, a separator, a sealing portion, and an electrolyte, the electrolyte being as described above.
[0063] The positive electrode has a first current collector and a positive electrode active material layer provided on one surface of the first current collector. The negative electrode has a second current collector and a negative electrode active material layer provided on one surface of the second current collector, and is stacked on the positive electrode with the negative electrode active material layer facing the positive electrode active material layer of the positive electrode. In this specification, the term "current collector" refers to the first current collector and the second current collector, the term "electrode active material" refers to the positive electrode active material and the negative electrode active material, and the term "electrode active material layer" refers to the positive electrode active material. layer and negative electrode active material layer The above are collectively referred to as "
[0064] The current collector is a chemically inactive electronic conductor for continuing to pass current to the electrode during discharging or charging of the lithium ion secondary battery. Examples of the current collector include at least one selected from silver, copper, gold, aluminum, magnesium, tungsten, cobalt, zinc, nickel, iron, platinum, tin, indium, titanium, ruthenium, tantalum, chromium, and molybdenum, as well as metal materials such as stainless steel. The effect of improving durability, which is an effect of the lithium ion secondary battery of the present invention, is particularly remarkable when the first current collector, which is a current collector for the positive electrode, is made of aluminum. In other words, it is particularly preferable that the first current collector is made of aluminum.
[0065] The current collector may be coated with a known protective layer, or the surface of the current collector may be treated by a known method before use.
[0066] The current collector can be in the form of a foil, sheet, film, wire, rod, mesh, etc. Therefore, metal foils such as copper foil, nickel foil, aluminum foil, stainless steel foil, etc. can be suitably used as the current collector. In the case of a foil-shaped current collector (hereinafter referred to as a current collector foil), the thickness is preferably within the range of 1 μm to 100 μm.
[0067] The positive electrode active material may be any material capable of absorbing and releasing lithium ions. For example, the positive electrode active material may be a layered rock salt structure having the general formula: Li a Ni b Co c Mn d D e O f Examples of the positive electrode active material include a lithium composite metal oxide represented by the formula: (0.2≦a≦2, b+c+d+e=1, 0≦e<1, D is at least one element selected from W, Mo, Re, Pd, Ba, Cr, B, Sb, Sr, Pb, Ga, Al, Nb, Mg, Ta, Ti, La, Zr, Cu, Ca, Ir, Hf, Rh, Fe, Ge, Zn, Ru, Sc, Sn, In, Y, Bi, S, Si, Na, K, P, and V, 1.7≦f≦3), and Li2MnO3. Examples of the positive electrode active material include a metal oxide having a spinel structure such as LiMn2O4, a solid solution composed of a mixture of a metal oxide having a spinel structure and a layered compound, and a polyanion-based compound represented by LiMPO4, LiMVO4, or Li2MSiO4 (wherein M is selected from at least one of Co, Ni, Mn, and Fe). Further, examples of the positive electrode active material include taborite-based compounds represented by LiMPO4F (M is a transition metal) such as LiFePO4F, and borate-based compounds represented by LiMBO3 (M is a transition metal) such as LiFeBO3. Any metal oxide used as the positive electrode active material may have the above composition formula as the basic composition, and those in which the metal elements contained in the basic composition are replaced with other metal elements can also be used. Only one of these positive electrode active materials may be used, or multiple types may be used in combination.
[0068] Among these, the positive electrode active material having the olivine structure is suitable as a positive electrode active material for lithium ion secondary batteries because of its excellent thermal stability. To prepare a positive electrode active material having an olivine structure, a commercially available product may be purchased, or it may be manufactured with reference to the methods described in the following documents, etc. As the positive electrode active material having an olivine structure, those coated with carbon are preferred.
[0069] Japanese Patent Laid-Open No. 11-25983 Japanese Patent Laid-Open No. 2002-198050 Japanese Patent Publication No. 2005-522009 Japanese Patent Laid-Open No. 2012-79554
[0070] As an example of representing the positive electrode active material having an olivine structure by a chemical formula, Li a M b PO4 (M is at least one element selected from Mn, Fe, Co, Ni, Cu, Mg, Zn, V, Ca, Sr, Ba, Ti, Al, Si, B, Te, Mo. a satisfies 0.9 ≦ a ≦ 1.2, and b satisfies 0.6 ≦ b ≦ 1.1.) can be exemplified.
[0071] As the range of a, 0.95 ≦ a ≦ 1.1 and 0.97 ≦ a ≦ 1.05 can be exemplified.
[0072] Li a M b In LiMPO4, M is preferably at least one element selected from Mn, Fe, Co, Ni, Mg, V, Te, and more preferably M is composed of two or more elements. M is more preferably selected from Mn, Fe, and V. b preferably satisfies 0.95 ≦ b ≦ 1.05.
[0073] Li a M b As LiMPO4, LiMnFePO4 (x, y satisfy x + y = 1, 0 < x < 1, 0 < y < 1) in which Mn and Fe are essential constituent elements is more preferred. As the range of x and y, 0.5 ≦ x ≦ 0.9, 0.1 ≦ y ≦ 0.5, 0.6 ≦ x ≦ 0.8, 0.2 ≦ y ≦ 0.4, and further 0.7 ≦ x ≦ 0.8, 0.2 ≦ y ≦ 0.3 can be exemplified. x Fe y PO4 (x, y satisfy x + y = 1, 0 < x < 1, 0 < y < 1) is more preferably represented. As the range of x and y, 0.5 ≦ x ≦ 0.9, 0.1 ≦ y ≦ 0.5, 0.6 ≦ x ≦ 0.8, 0.2 ≦ y ≦ 0.4, and further 0.7 ≦ x ≦ 0.8, 0.2 ≦ y ≦ 0.3 can be exemplified.
[0074] LiFePO4 is widely used as a positive electrode active material with an olivine structure, but LiMn x Fe y PO4 is known to have a higher reaction potential than LiFePO4.
[0075] The positive electrode active material layer may contain additives such as a conductive assistant, a binder, and a dispersant in addition to the positive electrode active material. The proportion of the positive electrode active material in the positive electrode active material layer is, for example, in the range of 70 to 99 mass %, in the range of 80 to 98 mass %, or in the range of 90 to 97 mass %.
[0076] The conductive assistant is added to increase the electrical conductivity of the electrode. Therefore, the conductive assistant may be added optionally when the electrical conductivity of the electrode is insufficient, and may not be added when the electrical conductivity of the electrode is sufficiently excellent.
[0077] The conductive assistant may be any chemically inactive electron conductor, and examples thereof include carbonaceous fine particles such as carbon black, graphite, vapor grown carbon fiber, carbon nanotubes, and various metal particles. Examples of carbon black include acetylene black, Ketjen Black (registered trademark), furnace black, and channel black. These conductive assistants may be added to the positive electrode active material layer alone or in combination of two or more.
[0078] The amount of the conductive assistant to be added is not particularly limited. The proportion of the conductive assistant in the positive electrode active material layer is preferably within a range of 1 to 7 mass %, more preferably within a range of 2 to 6 mass %, and further preferably within a range of 3 to 5 mass %.
[0079] The binder serves to bind the positive electrode active material and the conductive assistant to the surface of the current collector. Examples of the binder include fluorine-containing resins such as polyvinylidene fluoride, polytetrafluoroethylene, and fluorine rubber, thermoplastic resins such as polypropylene and polyethylene, imide resins such as polyimide and polyamideimide, alkoxysilyl group-containing resins, poly(meth)acrylate resins, polyacrylic acid, polyvinyl alcohol, polyvinylpyrrolidone, carboxymethyl cellulose, and styrene butadiene rubber.
[0080] The amount of the binder to be added is not particularly limited. The ratio of the binder in the positive electrode active material layer is preferably within a range of 0.5 to 7 mass %, more preferably within a range of 1 to 5 mass %, and further preferably within a range of 2 to 4 mass %.
[0081] As additives such as a dispersant other than the conductive assistant and the binder, known ones can be used.
[0082] As the negative electrode active material, a material capable of absorbing and releasing charge carriers can be used. Therefore, there is no particular limitation as long as it is a simple substance, alloy, or compound capable of absorbing and releasing charge carriers such as lithium ions. For example, as the negative electrode active material, Li, group 14 elements such as carbon, silicon, germanium, and tin, group 13 elements such as aluminum and indium, group 12 elements such as zinc and cadmium, group 15 elements such as antimony and bismuth, alkaline earth metals such as magnesium and calcium, and group 11 elements such as silver and gold may be used as simple substances. Specific examples of alloys or compounds include tin-based materials such as Ag-Sn alloys, Cu-Sn alloys, and Co-Sn alloys, carbon-based materials such as various graphites, and SiO, which is disproportionated into silicon simple substance and silicon dioxide. x (0.3≦x≦1.6), silicon alone or a composite of a silicon-based material and a carbon-based material. and Nb2O5, TiO2, Li4Ti5O 12 , WO2, MoO2, Fe2O3, or other oxides, or Li 3-x M xAlternatively, a nitride represented by Mn(M=Co, Ni, Cu) may be used. As the negative electrode active material, one or more of these may be used.
[0083] The proportion of the negative electrode active material in the negative electrode active material layer can be, for example, in the range of 70 to 99 mass %, 80 to 98.5 mass %, 90 to 98 mass %, or 95 to 97.5 mass %.
[0084] The negative electrode active material layer may contain additives such as a binder and a dispersant in addition to the negative electrode active material. The binder may be any of those described for the positive electrode. The additives such as the dispersant may be any of those known in the art.
[0085] The amount of the binder to be added is not particularly limited. The ratio of the binder in the negative electrode active material layer is preferably within a range of 0.5 to 7 mass %, more preferably within a range of 1 to 5 mass %, and further preferably within a range of 2 to 4 mass %.
[0086] To form an active material layer on the surface of a current collector, the active material may be applied to the surface of the current collector using a conventionally known method such as roll coating, die coating, dip coating, doctor blade, spray coating, or curtain coating. Specifically, an active material, a solvent, and, if necessary, a binder and a conductive assistant are mixed to produce a slurry-like active material layer forming composition, which is then applied to the surface of a current collector and then dried. Examples of the solvent include N-methyl-2-pyrrolidone, methanol, methyl isobutyl ketone, and water. The dried product may be compressed to increase the electrode density.
[0087] In addition, the active material layer may be formed using the manufacturing method disclosed in JP-A-2015-201318 and the like. Specifically, a mixture containing an active material, a binder, and a solvent is granulated to obtain a wet granule. The granules are then placed in a predetermined mold to obtain a flat plate-like compact. The flat plate-like compact is then attached to the surface of a current collector using a transfer roll to form an active material layer.
[0088] In the lithium ion secondary battery of the present invention, the positive electrode active material can be selected to have an olivine structure, and the negative electrode active material can be selected to have graphite. A lithium ion secondary battery having a positive electrode with an olivine structure positive electrode active material and a negative electrode with graphite as the negative electrode active material can be said to have excellent thermal stability, but the capacity per unit volume of the electrode is low.
[0089] The industrial world demands high-capacity lithium-ion secondary batteries. One possible way to meet this demand is to increase the amount of positive and negative active materials per electrode, specifically, to increase the amount of positive and negative active material layers applied to the current collector foil. By increasing the amount of positive and negative active material layers applied to the current collector foil, the mass of the positive active material layer present on an area of 1 cm2 on one side of the positive current collector foil (hereinafter sometimes referred to as the "basis weight of the positive electrode") and the mass of the negative active material layer present on an area of 1 cm2 on one side of the negative current collector foil (hereinafter sometimes referred to as the "basis weight of the negative electrode") increase.
[0090] The weight of the positive electrode is 20 mg / cm 2 The preferred coating weight of the positive electrode is 30 to 200 mg / cm. 2 Within the range of 35-150mg / cm 2 Within the range of 40-120mg / cm 2 Within the range of 50-100mg / cm 2 Examples of the range are as follows.
[0091] The weight of the negative electrode is 10 mg / cm 2 The preferred coating weight of the negative electrode is 15 to 100 mg / cm. 2 Within the range of 17-75mg / cm 2 Within the range of 20-60mg / cm 2 Within the range of 25-50mg / cm 2 Examples of the range are as follows.
[0092] In general, in a lithium ion secondary battery having a thick electrode with a large basis weight and a thick active material layer, a rate characteristic deterioration phenomenon occurs in which the charge / discharge capacity at a high rate is insufficient compared to the charge / discharge capacity at a low rate. The rate characteristic deterioration phenomenon is thought to be related to the diffusion resistance of lithium ions in the lithium ion secondary battery, and the diffusion resistance of lithium ions is thought to be related to the viscosity of the electrolyte and the diffusion coefficient of lithium ions in the electrolyte.
[0093] The electrolyte of the present invention has a low viscosity due to the presence of methyl propionate, and is designed in consideration of the diffusion coefficient of lithium ions. Therefore, in the lithium ion secondary battery of the present invention, for example, the positive electrode has a diffusion coefficient of 30 to 200 mg / cm. 2 In the negative electrode range, 15 to 100 mg / cm 2 Even if the weight is within the range of 100%, the rate characteristic deterioration phenomenon is suppressed to some extent.
[0094] Furthermore, when the lithium ion secondary battery of the present invention is not a so-called wound type lithium ion secondary battery in which the electrodes are wound and housed in a container, but a so-called cell stack type lithium ion secondary battery in which the electrodes are not wound but are maintained in a stacked state, there is no need to consider damage to the electrode active material layer during winding. Therefore, the lithium ion secondary battery is suitable as a lithium ion secondary battery having thick electrodes.
[0095] In the lithium ion secondary battery of the present invention, a positive electrode active material layer is provided on one surface of the first current collector, and a negative electrode active material layer is provided on one surface of the second current collector. layeris provided. A positive electrode active material layer or a negative electrode active material layer may be provided on the other surface of the first current collector. Similarly, a positive electrode active material layer or a negative electrode active material layer may be provided on the other surface of the second current collector. Furthermore, the other surface of the first current collector having a positive electrode active material layer on one surface and the other surface of the second current collector having a negative electrode active material layer on one surface may be stacked and integrated. In this case, the first current collector and the second current collector can be regarded as a multi-layered current collector described later. In this case, a positive electrode active material layer is provided on one surface (or the other surface) of a two-layered current collector in which the first current collector and the second current collector are integrated, and a negative electrode active material layer is provided on the other surface (or the other surface).
[0096] That is, the electrode in the lithium ion secondary battery of the present invention may be an electrode in which the same kind of active material layers, i.e., a positive electrode active material layer and a positive electrode active material layer, or a negative electrode active material layer and a negative electrode active material layer, are provided on both sides of a current collector, or the electrode in the lithium ion secondary battery of the present invention may be a bipolar electrode in which different kinds of active material layers, i.e., a positive electrode active material layer and a negative electrode active material layer, are provided on both sides of a current collector. In either case, the positive electrode and the negative electrode are stacked with the negative electrode active material layer facing the positive electrode active material layer, and a separator is disposed between the positive electrode active material layer and the negative electrode active material layer in the direction in which the negative electrode active material layer and the positive electrode active material layer face each other (hereinafter referred to as the facing direction).
[0097] The first current collector and the second current collector may each be a single-layer structure made of a single metal, or a multi-layer structure made of a plurality of different metals. The first current collector and the second current collector may be laminated and integrated to form a multi-layer structure. When the first current collector and the second current collector form the multi-layer structure, for example, the second current collector (or the first current collector) may be plated on the first current collector (or the second current collector), or the second current collector (or the first current collector) may be roll-bonded to the first current collector (or the second current collector). Alternatively, the first current collector and the second current collector that are separately molded may be bonded to each other with a conductive adhesive or the like to be integrated. Specifically, a metal foil in which an aluminum foil is plated with copper or nickel may be used.
[0098] The separator has a function of isolating the positive electrode and the negative electrode, preventing a short circuit due to contact between the two electrodes, while allowing lithium ions to pass through. As the separator, any known separator may be used, and examples thereof include porous bodies, nonwoven fabrics, woven fabrics, etc., using one or more electrically insulating materials such as synthetic resins such as polytetrafluoroethylene, polypropylene, polyethylene, polyimide, polyamide, polyaramid (aromatic polyamide), polyester, polyacrylonitrile, etc., polysaccharides such as cellulose, amylose, etc., natural polymers such as fibroin, keratin, lignin, suberin, etc., and ceramics. The separator may also have a multi-layer structure. Specifically, examples thereof include an adhesive type separator in which an adhesive layer is provided on the separator to achieve high adhesion between the electrode and the separator, and a coating type separator in which a coating film containing an inorganic filler or the like is formed on the separator to improve high-temperature heat resistance.
[0099] As described above, in the lithium ion secondary battery of the present invention, the positive electrode active material layer and the negative electrode active material layer face each other. The positive electrode active material layer is formed on one side of the first current collector, and the negative electrode active material layer is formed on one side of the second current collector, so that the positive electrode active material layer and the negative electrode active material layer are disposed between the first current collector and the second current collector. The lithium ion secondary battery of the present invention includes a sealing portion between the first current collector and the second current collector in the facing direction. The sealing portion surrounds the periphery of the positive electrode active material layer and the negative electrode active material layer, and functions to seal the electrolyte in the space between the first current collector and the second current collector. In other words, in the lithium ion secondary battery of the present invention, a storage cell having a positive electrode active material layer, a separator, a negative electrode active material layer, and an electrolyte is formed between a pair of the first current collector and the second current collector, and the storage cell is separated from the outside by the sealing portion. The lithium ion secondary battery of the present invention may include only one storage cell, or may include a plurality of storage cells. The lithium ion secondary battery of the present invention has the above-mentioned structure, which allows the container to be made smaller and lighter, and also allows the wiring such as lead wires to be reduced. As a result, the energy density per volume and weight of the lithium ion secondary battery of the present invention having the above-mentioned structure is improved. Furthermore, the lithium ion secondary battery of the present invention having such a structure is suitable for realizing a cell stack type lithium ion secondary battery, and as described above, it can have thick electrodes.
[0100] The sealing portion functions as a sealant for enclosing the electrolyte inside the storage cell, and also functions as a spacer for electrically isolating the first and second current collectors constituting the same storage cell. The sealing portion that performs such functions may have a shape capable of accommodating the positive electrode active material layer and the negative electrode active material layer on its inner periphery, specifically, a ring-shaped or cylindrical shape.
[0101] The material of the sealing part may be any material capable of exhibiting the above-mentioned functions, and is preferably a resin material. The material of the sealing part is preferably an olefin or an acid-modified olefin, and specific examples thereof include polyethylene, polypropylene, acid-modified polyethylene, and acid-modified polypropylene.
[0102] The sealing portion is preferably fixed to the first current collector and the second current collector by a general method such as adhesion or welding. This is to reliably seal the electrolyte between the first current collector and the second current collector constituting the same cell, and to appropriately maintain the relative positions of the first current collector and the second current collector, and the relative positions of the positive electrode active material layer, the separator, and the negative electrode active material layer. Examples of the method for fixing the sealing portion to the first current collector and the second current collector include adhesion, welding, fusion, etc.
[0103] The sealing portion only needs to surround the periphery of the positive electrode active material layer and the negative electrode active material layer, and may be in contact with or separate from the outer edge of the positive electrode active material layer and the outer edge of the negative electrode active material layer. In order to improve the durability of the lithium ion secondary battery and to accommodate expansion and contraction of the cell during use of the lithium ion secondary battery, it is preferable that the sealing portion is separate from the outer edge of the positive electrode active material layer and the outer edge of the negative electrode active material layer.
[0104] A specific method for manufacturing a lithium ion secondary battery will be described. For example, a positive electrode having a positive electrode active material layer formed on one side of a first current collector and a negative electrode having a negative electrode active material layer formed on one side of a second current collector are arranged so that the positive electrode active material layer and the negative electrode active material layer face each other via a separator. At this time, a sealing portion is further disposed between the first current collector and the second current collector so as to surround the positive electrode active material layer and the negative electrode active material layer, and the sealing portion is fixed to the first current collector and the second current collector. At this time, an electrolyte is also sealed inside the sealing portion. This allows a lithium ion secondary battery to be manufactured. Depending on the structure of the separator, a first sealing portion may be disposed between the first current collector and the separator, and a second sealing portion may be disposed between the separator and the second current collector, and the first sealing portion and the second sealing portion may be integrated by a method such as adhesion.
[0105] The lithium ion secondary battery of the present invention may be mounted on a vehicle. The vehicle may be any vehicle that uses electric energy from a lithium ion secondary battery as all or part of its power source, and may be, for example, an electric vehicle or a hybrid vehicle. When a lithium ion secondary battery is mounted on a vehicle, a plurality of lithium ion secondary batteries may be connected in series to form a battery pack. In addition to vehicles, devices that mount a lithium ion secondary battery include various battery-driven home appliances, office equipment, industrial equipment, etc., such as personal computers and portable communication devices. Furthermore, the lithium ion secondary battery of the present invention may be used in a power storage device and power smoothing device for wind power generation, solar power generation, hydroelectric power generation, and other power systems, a power supply source for power and / or auxiliary equipment of ships, etc., a power supply source for power and / or auxiliary equipment of aircraft, spacecraft, etc., an auxiliary power source for vehicles that do not use electricity as a power source, a power source for mobile household robots, a power source for system backup, a power source for uninterruptible power supply systems, a power storage device that temporarily stores power required for charging in a charging station for electric vehicles, etc.
[0106] Although the present invention has been described above, the present invention is not limited to the above-described embodiment. The present invention can be embodied in various forms including modifications and improvements that can be made by those skilled in the art without departing from the gist of the present invention. EXAMPLES
[0107] The present invention will be described in more detail below with reference to basic studies, examples, and comparative examples, although the present invention is not limited to these examples.
[0108] <Basic Study 1: Evaluation of electrolyte viscosity> In a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 30:70, (FSO2)2NLi and LiPF6 were dissolved in the ratios shown in Table 1 below to produce electrolytes 1 to 3. The viscosity of the electrolytes 1 to 3 was measured under the following conditions. The results are shown in Table 1. <Viscosity> The viscosity of each electrolyte solution was measured at 25° C. using a B-type viscometer (Brookfield, DV2T) with a cone-type spindle. The rotation speed of the cone-type spindle was set to 60 rpm.
[0109] [Table 1]
[0110] As shown in Table 1, if the amount of (FSO2)2NLi relative to the total amount of lithium salts is 30 mol % or more, the viscosity of the electrolyte decreases. This is thought to improve the ionic conductivity of the electrolyte. From the viewpoints of viscosity and ionic conductivity, when (FSO2)2NLi is used as the lithium salt, it is preferable that the amount of (FSO2)2NLi is 30 mol % or more relative to the total amount of lithium salts.
[0111] <Basic Study 2: Study of esters in electrolytes> Electrolytes were produced using propyl propionate, methyl butyrate, and ethyl butyrate, which are esters with a similar chemical structure to methyl propionate, and the effects of these esters on battery characteristics were examined. [Electrolyte solution 〕 · A mother liquor was prepared by dissolving LiPF6 at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85. Lithium difluoro(oxalato)borate (hereinafter sometimes abbreviated as LiDFOB. LiDFOB is one form of oxalato borate) in an amount equivalent to 1 mass% and vinylene carbonate in an amount equivalent to 1 mass% were added and dissolved in the mother liquor to obtain an electrolyte. 4 Manufactured 。 ·LiPF6 was dissolved at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and propyl propionate (hereinafter sometimes abbreviated as PP) in a volume ratio of 15:85 to prepare a mother solution. LiDFOB and vinylene carbonate were added to the mother solution in an amount equivalent to 1% by mass and dissolved therein to obtain an electrolyte. 5 Manufactured 。 · A mother solution was prepared by dissolving LiPF6 at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl butyrate (hereinafter sometimes abbreviated as MB) in a volume ratio of 15:85. An electrolyte solution was prepared by adding and dissolving LiDFOB and vinylene carbonate in an amount equivalent to 1% by mass to the mother solution. 6 Manufactured 。 · LiPF6 was dissolved at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and ethyl butyrate (hereinafter sometimes abbreviated as EB) in a volume ratio of 15:85 to prepare a mother solution. LiDFOB and vinylene carbonate were added to the mother solution in an amount equivalent to 1% by mass and dissolved therein to obtain an electrolyte. 7 Manufactured 。 · Ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate were mixed in a volume ratio of 30:30:40 to prepare a mixed solvent. LiPF6 was dissolved in the mixed solvent to prepare a mother liquid with a LiPF6 concentration of 1 mol / L. LiDFOB in an amount equivalent to 0.2 mol / L and vinylene carbonate in an amount equivalent to 1 mass% were added to the mother liquid and dissolved to prepare an electrolyte. 8 was manufactured.
[0112] [Lithium-ion secondary battery] electrolyte 4 ~ 8 A lithium ion secondary battery was manufactured as follows. LiFePO4 with an olivine structure coated with carbon as a positive electrode active material, acetylene black as a conductive assistant, and polyvinylidene fluoride as a binder were mixed so that the mass ratio of the positive electrode active material, conductive assistant, and binder was 90:5:5, and N-methyl-2-pyrrolidone was added as a solvent to prepare a slurry-like composition for forming a positive electrode active material layer. An aluminum foil was prepared as a positive electrode current collector. The composition for forming a positive electrode active material layer was applied to the surface of the aluminum foil in a film form, and then the solvent was removed to produce a positive electrode precursor. The positive electrode precursor was pressed in the thickness direction to produce a positive electrode in which a positive electrode active material layer was formed on the surface of the aluminum foil. In the manufacture of the positive electrode, the coating weight of the positive electrode was 13.9 mg / cm 2 The goal was to:
[0113] Graphite was used as the negative electrode active material, and carboxymethylcellulose and styrene butadiene rubber were used as the binder. The graphite, carboxymethylcellulose, and styrene butadiene rubber were mixed in a mass ratio of 97:0.8:2.2, and water was added as a solvent to prepare a slurry-like composition for forming a negative electrode active material layer. Copper foil was prepared as a negative electrode current collector. The negative electrode active material layer was applied to the surface of the copper foil in a film form, and the solvent was then removed to produce a negative electrode precursor. The negative electrode precursor was pressed in the thickness direction to produce a negative electrode having a negative electrode active material layer formed on the surface of the copper foil. In the manufacture of the negative electrode, the coating weight of the negative electrode was 6.3 mg / cm 2 The goal was to:
[0114] A porous polypropylene film was prepared as a separator. The separator was sandwiched between the positive and negative electrodes to form an electrode assembly. This electrode assembly was filled with an electrolyte solution. 4 At the same time, by sealing the battery in a bag-shaped laminate film, it becomes a lithium-ion secondary battery. 4 Similarly, the electrolyte was 5 ~ 8 Lithium-ion secondary battery 5 ~ 8 was manufactured.
[0115] [Storage test] Lithium-ion secondary battery 4 ~8 Each lithium-ion secondary battery was subjected to CC-CV charging at a rate of 0.4 C up to 4.0 V, and the charge capacity at this time was taken as the reference (SOC 100%). A storage test was performed by storing each lithium-ion secondary battery at 40° C. for 11 days in the SOC 100 state. The capacity was confirmed before and after the storage test. Specifically, CC-CV charging was performed at a rate of 0.4C to 4.0V. Then, CC-CV discharging was performed at a rate of 1C to 2.5V. This confirmed the discharge capacity of each lithium-ion secondary battery. The percentage of the discharge capacity after the storage test to the discharge capacity before the storage test was taken as the capacity retention rate of each lithium-ion secondary battery. In addition, after the storage test, the amount of voltage change was measured for each lithium ion secondary battery adjusted to SOC 60% when it was discharged at a constant current rate for 5 seconds under a condition of 25°C. The measurement was performed under a plurality of conditions with different current rates. From the obtained results, the constant current (mA) at which the discharge time to a voltage of 2.5V was 10 seconds was calculated for each lithium ion secondary battery with SOC 60%. The voltage change from SOC 60% to 2.5V was multiplied by the calculated constant current to obtain the output. The results of the above storage tests are shown in Table 2.
[0116] [Table 2]
[0117] As shown in Table 2, lithium-ion secondary batteries using methyl propionate as the non-aqueous solvent for the electrolyte 4 is a lithium ion secondary battery that uses a carbonate-based non-aqueous solvent and is excellent in both capacity retention and output, especially in terms of output. 8 This result supports the usefulness of selecting methyl propionate as the non-aqueous solvent.
[0118] Example 1 The electrolyte and the lithium ion secondary battery of Example 1 will be described below. The lithium ion secondary battery of Example 1 is As mentioned aboveUnlike the lithium ion secondary battery of the present invention, the battery has a general structure except that the electrodes are thickly packed.
[0119] [Electrolyte] A mother solution was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85. An electrolyte solution of Example 1 was produced by adding and dissolving vinylene carbonate in an amount equivalent to 1 mass % to the mother solution.
[0120] [Lithium-ion secondary battery] Graphite was used as the negative electrode active material, and carboxymethylcellulose and styrene butadiene rubber were used as the binder. The graphite, carboxymethylcellulose, and styrene butadiene rubber were mixed in a mass ratio of 94.8:0.8:4.4, and water was added as a solvent to prepare a slurry-like composition for forming a negative electrode active material layer. Copper foil was prepared as a negative electrode current collector. The negative electrode active material layer was applied to the surface of the copper foil in a film form, and the solvent was then removed to produce a negative electrode precursor. The negative electrode precursor was pressed in the thickness direction to produce a negative electrode having a negative electrode active material layer formed on the surface of the copper foil. The weight of the negative electrode is 26.5 mg / cm 2 It was.
[0121] positive electrode active material LiFePO4 with an olivine structure coated with carbon as a positive electrode active material, acetylene black as a conductive assistant, and polyvinylidene fluoride as a binder were mixed so that the mass ratio of the positive electrode active material, conductive assistant, and binder was 88.8:5.1:6.1, and N-methyl-2-pyrrolidone was added as a solvent to obtain a slurry-like positive electrode active material layer forming composition. Aluminum foil was prepared as a positive electrode current collector. The positive electrode precursor was produced by applying the positive electrode active material layer forming composition to the surface of the aluminum foil in a film form and then removing the solvent, and the resulting positive electrode precursor was pressed in the thickness direction to produce a positive electrode in which a positive electrode active material layer was formed on the surface of the aluminum foil. The weight of the positive electrode is 55.5 mg / cm 2 It was.
[0122] A polypropylene porous film was prepared as a separator. The separator was sandwiched between the positive electrode and the negative electrode to form an electrode body. This electrode body was placed in a bag-shaped laminate film together with the electrolyte solution of Example 1 and sealed to produce the lithium ion secondary battery of Example 1.
[0123] Example 2 The electrolyte of Example 2 was the same as that of Example 1 except for the volume ratio of ethylene carbonate and methyl propionate. Specifically, in Example 2, (FSO2)2NLi was dissolved at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 25:75 to prepare a mother solution. Vinylene carbonate was added to the mother solution in an amount equivalent to 1 mass % and dissolved therein to produce the electrolyte solution of Example 2. The lithium ion secondary battery of Example 2 is the same as the lithium ion secondary battery of Example 1, except that the electrolyte solution of Example 2 is used.
[0124] Comparative Example 1 The electrolyte of Comparative Example 1 was the same as that of Example 1 except for the volume ratio of ethylene carbonate and methyl propionate. Specifically, in Comparative Example 1, (FSO2)2NLi was dissolved at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 30:70 to prepare a mother solution. Vinylene carbonate was added to the mother solution in an amount equivalent to 1 mass % and dissolved therein to produce the electrolyte solution of Comparative Example 1. The lithium ion secondary battery of Comparative Example 1 is the same as the lithium ion secondary battery of Example 1, except that the electrolyte of Comparative Example 1 was used.
[0125] Comparative Example 2 The electrolyte of Comparative Example 2 was the same as that of Example 1 except for the volume ratio of ethylene carbonate and methyl propionate. Specifically, in Comparative Example 2, (FSO2)2NLi was dissolved at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 50:50 to prepare a mother solution. Vinylene carbonate was added to the mother solution in an amount equivalent to 1 mass % and dissolved therein to produce the electrolyte solution of Comparative Example 2. The lithium ion secondary battery of Comparative Example 2 is the same as the lithium ion secondary battery of Example 1, except that the electrolyte of Comparative Example 2 was used.
[0126] <Evaluation Example 1: Rate characteristic evaluation> For the lithium ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2, the following tests were performed: . 0C and 4.0 C Discharge was performed from SOC 95% to a voltage of 2.3 V at four discharge rates. The capacity at the end of discharge of each lithium ion secondary battery, i.e., the rate capacity, was compared for each discharge rate to evaluate the rate characteristics of the lithium ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2. The rate characteristic evaluation test was performed with n=2 for each C rate, and the average values were compared. For each lithium-ion secondary battery, the charge capacity when CC-CV charging was performed at a rate of 0.4 C up to 4.0 V was defined as SOC100%. The rate capacity was expressed as a percentage relative to the above SOC100%. The results are shown in Table 3.
[0127] [Table 3]
[0128] As shown in Table 3, the lithium ion secondary batteries of Examples 1 and 2 exhibit superior discharge characteristics at all C rates from 0.4 C to 4.0 C compared to the lithium ion secondary batteries of Comparative Examples 1 and 2. This is believed to be because the electrolytes in the lithium ion secondary batteries of Examples 1 and 2 contain 75% by volume or more of methyl propionate in the non-aqueous solvent. Although the lithium ion secondary battery of Example 1 has a different structure from the lithium ion secondary battery of the present invention described above, it goes without saying that the effect of the electrolyte of Example 1 is similarly exhibited in the lithium ion secondary battery of the present invention. The same applies to the following examples.
[0129] Example 3 The electrolyte and the lithium ion secondary battery of Example 3 will be described below. [Electrolyte] A mother solution was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85. An electrolyte solution of Example 3 was produced by adding and dissolving 1,3,2-dioxathiolane-2,2-dioxide (hereinafter sometimes abbreviated as DTD. DTD is one form of cyclic sulfate ester) in an amount equivalent to 0.5 mass % to the mother solution.
[0130] [Lithium-ion secondary battery] Graphite was used as the negative electrode active material, and carboxymethylcellulose and styrene butadiene rubber were used as the binder. The graphite, carboxymethylcellulose, and styrene butadiene rubber were mixed in a mass ratio of 97:0.8:2.2, and water was added as a solvent to prepare a slurry-like composition for forming a negative electrode active material layer. Copper foil was prepared as a negative electrode current collector. The negative electrode active material layer was applied to the surface of the copper foil in a film form, and the solvent was then removed to produce a negative electrode precursor. The negative electrode precursor was pressed in the thickness direction to produce a negative electrode having a negative electrode active material layer formed on the surface of the copper foil. The coating weight of the negative electrode is 6.7 mg / cm 2 It was.
[0131] positive electrode active materialLiFePO4 with an olivine structure coated with carbon as a positive electrode active material, acetylene black as a conductive assistant, and polyvinylidene fluoride as a binder were mixed so that the mass ratio of the positive electrode active material, conductive assistant, and binder was 94:3:3, and N-methyl-2-pyrrolidone was added as a solvent to obtain a slurry-like positive electrode active material layer forming composition. Aluminum foil was prepared as a positive electrode current collector. The positive electrode precursor was produced by applying the positive electrode active material layer forming composition to the surface of the aluminum foil in a film form and then removing the solvent, and the resulting positive electrode precursor was pressed in the thickness direction to produce a positive electrode in which a positive electrode active material layer was formed on the surface of the aluminum foil. The weight of the positive electrode is 13.9 mg / cm 2 It was.
[0132] A lithium ion secondary battery of Example 3 was produced in the same manner as in Example 1, using the above positive electrode and negative electrode.
[0133] Example 4 The electrolyte of Example 4 was the same as that of Example 3, except that (FSO2)2NLi and LiPF6 were used as the lithium salts. Specifically, in Example 4, (FSO2)2NLi and LiPF6 were dissolved at a concentration of 0.6 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution. DTD was added and dissolved in an amount equivalent to 0.5 mass % to the mother solution to produce the electrolyte solution of Example 4. The lithium ion secondary battery of Example 4 is the same as the lithium ion secondary battery of Example 3, except that the electrolyte of Example 4 is used.
[0134] Comparative Example 3 The electrolyte of Comparative Example 3 was the same as that of Example 3, except that (FSO2)2NLi and LiPF6 were used as the lithium salts. Specifically, in Comparative Example 3, LiPF6 was dissolved at a concentration of 1.2 mol / L in a mixed solvent in which ethylene carbonate and methyl propionate were mixed at a volume ratio of 15:85 to prepare a mother solution. An amount of (FSO2)2NLi equivalent to 0.5 mass% and an amount of DTD equivalent to 0.5 mass% were added to and dissolved in the mother solution to produce the electrolyte solution of Comparative Example 3. The amount of (FSO2)2NLi in the electrolyte solution of Comparative Example 3 was 0.03 mol / L, and the amount of (FSO2)2NLi was 2.4 mol% with respect to the total amount of (FSO2)2NLi and LiPF6. The lithium ion secondary battery of Comparative Example 3 is the same as the lithium ion secondary battery of Example 3, except that the electrolyte of Comparative Example 3 was used.
[0135] Comparative Example 4 Comparative Example 4 The electrolyte in Example 1 was the same as that in Example 3, except that only LiPF6 was used as the lithium salt. Specifically, the comparative example 4 In the comparative example 4, LiPF6 was dissolved at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution. DTD was added and dissolved in an amount equivalent to 0.5 mass % to the mother solution to produce the electrolyte solution of Comparative Example 4. The lithium ion secondary battery of Comparative Example 4 is the same as the lithium ion secondary battery of Example 3, except that the electrolyte of Comparative Example 4 was used.
[0136] <Evaluation Example 2: High-temperature charge-discharge cycle test> The lithium ion secondary batteries of Examples 3 and 4 and Comparative Examples 3 and 4 were subjected to a high-temperature charge-discharge cycle test.
[0137] [Check output] First, the amount of change in voltage was measured for each lithium ion secondary battery adjusted to SOC 60% when it was discharged at a constant current rate for 10 seconds under the condition of 25°C. The measurement was performed under a plurality of conditions with different current rates. From the obtained results, the constant current (mA) at which the discharge time to a voltage of 2.5V was 10 seconds was calculated for each lithium ion secondary battery with SOC 60%. The value obtained by multiplying the amount of voltage change from SOC 60% to 2.5V by the calculated constant current (mA) was determined as the initial output. The initial output test was also performed multiple times. The percentage of the output value of each lithium ion secondary battery relative to the output value of the lithium ion secondary battery of Comparative Example 4 was calculated, and the value obtained by subtracting 100(%) from the calculated percentage was determined as the initial output increase rate (%).
[0138] [High-temperature charge / discharge cycle] Then, at 60°C, CC-CV charge to 4V at 1C rate, and then charge to SO at 1C rate. C The high-temperature charge-discharge cycle, in which the battery was discharged in a CC manner until it was 90%, was repeated 100 times. Note that charging here means that lithium ions move from the negative electrode to the positive electrode, increasing the potential difference between the positive and negative electrodes. After the 100th charge / discharge cycle, the output of each lithium ion secondary battery was checked in the same manner as in the above output check. The percentage of the output value of each lithium ion secondary battery relative to the output value of the lithium ion secondary battery of Comparative Example 4 was calculated, and the value obtained by subtracting 100(%) from the percentage was determined as the output increase rate (%) after 100 cycles. The initial output of each lithium-ion secondary battery is shown in Table 4, and the output of each lithium-ion secondary battery after 100 cycles is shown in Table 5. Note that the output confirmation was performed with n=4, and the high-temperature charge / discharge cycle was performed with n=2, and the average values are shown in Tables 4 and 5.
[0139] [Table 4]
[0140] [Table 5]
[0141] As shown in Table 4, the lithium ion secondary batteries of Comparative Example 3, Example 3, and Example 4 containing (FSO2)2NLi as the lithium salt are superior in initial output compared to the lithium ion secondary battery of Comparative Example 4 using LiPF6 alone as the lithium salt. In particular, the lithium ion secondary batteries of Example 3 and Example 4, in which the content of (FSO2)2NLi is 30 mol % or more, have a significantly increased initial output even compared to the lithium ion secondary battery of Comparative Example 3, in which the content of (FSO2)2NLi is less than 30 mol %.
[0142] Furthermore, as shown in Table 5, the lithium ion secondary battery of Comparative Example 3 had the same charge-discharge cycle durability at high temperatures as Comparative Example 4, whereas the lithium ion secondary batteries of Examples 3 and 4 were superior in charge-discharge cycle durability at high temperatures as compared to the lithium ion secondary batteries of Comparative Example 3 and Comparative Example 4. These results support the idea that the use of an electrolyte containing (FSO2)2NLi, i.e., a lithium salt other than LiPF6, in an amount of 30 mol% or more relative to the total amount of lithium salts, improves the durability of lithium-ion secondary batteries, especially at high temperatures.
[0143] <Evaluation Example 3: Storage test> The lithium ion secondary batteries of Examples 3 and 4 and Comparative Examples 3 and 4 were subjected to CC-CV charging at a rate of 0.4 C up to 4.0 V, and the charge capacity at this time was taken as the reference (SOC 100%). In the SOC 100 state, each lithium ion secondary battery was stored at 40° C. for 12 days, whereby a storage test was performed. The output was confirmed before and after the storage test in the same manner as in Evaluation Example 2, and for the output value after the storage test, the percentage of the output value of each lithium ion secondary battery relative to the output value of the lithium ion secondary battery of Comparative Example 4 was calculated, and the value obtained by subtracting 100(%) from this percentage was used as the output increase rate (%) after storage. The output of each lithium ion secondary battery after 100 cycles of storage is shown in Table 6. The test was performed with n=2, and the average value is shown in Table 6.
[0144] [Table 6]
[0145] As shown in Table 6, the lithium ion secondary batteries of Example 3 and Example 4 were also superior in durability during storage at 40° C. compared to the lithium ion secondary batteries of Comparative Example 3 and Comparative Example 4. This result also supports that the use of an electrolyte solution containing 30 mol % or more of lithium salt other than LiPF6 relative to the total lithium salts improves the durability of the lithium ion secondary battery, particularly at high temperatures.
[0146] Example 5 A lithium ion secondary battery of Example 5 was manufactured as follows using the same electrolyte solution of Example 5 as that of Example 3. For reference, the electrolyte solution of Example 5 was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution, and then adding and dissolving DTD in an amount equivalent to 0.5 mass % to the mother solution.
[0147] [Lithium-ion secondary battery] Graphite was used as the negative electrode active material, and carboxymethylcellulose and styrene butadiene rubber were used as the binder. The graphite, carboxymethylcellulose, and styrene butadiene rubber were mixed in a mass ratio of 97:0.8:2.2, and water was added as a solvent to prepare a slurry-like composition for forming a negative electrode active material layer. Copper foil was prepared as a negative electrode current collector. The negative electrode active material layer was applied to the surface of the copper foil in a film form, and the solvent was then removed to produce a negative electrode precursor. The negative electrode precursor was pressed in the thickness direction to produce a negative electrode having a negative electrode active material layer formed on the surface of the copper foil. The weight of the negative electrode is 6.24 mg / cm 2 It was.
[0148] positive electrode active materialLiFePO4 with an olivine structure coated with carbon as a cathode active material, acetylene black as a conductive assistant, and polyvinylidene fluoride as a binder were mixed so that the mass ratio of the cathode active material, conductive assistant, and binder was 90:5:5, and N-methyl-2-pyrrolidone was added as a solvent to obtain a slurry-like cathode active material layer forming composition. Aluminum foil was prepared as a cathode current collector. The cathode active material layer forming composition was applied to the surface of the aluminum foil in a film form, and then the solvent was removed to produce a cathode precursor. The cathode precursor was pressed in the thickness direction to produce a cathode in which a cathode active material layer was formed on the surface of the aluminum foil. The weight of the positive electrode is 13.87 mg / cm 2 It was.
[0149] A lithium ion secondary battery of Example 5 was produced in the same manner as in Example 1, using the above positive electrode and negative electrode.
[0150] Comparative Example 5 A lithium ion secondary battery of Comparative Example 5 was produced in the same manner as in Example 5, using the same electrolyte solution of Comparative Example 5 as that of Comparative Example 4. For reference, the electrolyte solution of Comparative Example 5 was prepared by dissolving LiPF6 at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution, and then adding and dissolving DTD in an amount equivalent to 0.5 mass % to the mother solution.
[0151] <Evaluation Example 4: Gas Generation Evaluation> The lithium ion secondary batteries of Example 5 and Comparative Example 5 were activated by charging to 4.0 V at 0.05 C and holding at 60° C. for 20 hours. The volume of each lithium ion secondary battery before and after activation was measured by Archimedes' method, and the amount of gas (μL) generated by activation was calculated from the change in volume of each lithium ion secondary battery before and after activation. The amount of gas generated from each lithium ion secondary battery is shown in Table 7. The test was performed with n=3, and the average value is shown in Table 7.
[0152] [Table 7]
[0153] As shown in Table 7, the amount of gas generated in the lithium ion secondary battery of Example 5 is smaller than the amount of gas generated in the lithium ion secondary battery of Comparative Example 5. This result shows that the use of an electrolyte solution containing 30 mol % or more of lithium salts other than LiPF6 relative to the total amount of lithium salts makes it possible to suppress the generation of gas accompanying the charging and discharging of a lithium ion secondary battery. In addition, in lithium ion secondary batteries using graphite for the negative electrode, it is believed that gas is generated by decomposition of the electrolyte at the negative electrode. In the lithium ion secondary battery of Example 5, it is believed that a good coating is formed on the surface of the negative electrode by decomposing (FSO2)2NLi contained in the electrolyte, and the gas is generated by the coating. the law of nature It is presumed that decomposition of the electrolyte is suppressed. By suppressing gas generation, the amount of expansion of the lithium ion secondary battery accompanying charging and discharging can be reduced, and the stress acting on the lithium ion secondary battery can be reduced, which in turn makes it possible to improve the durability of the lithium ion secondary battery. This effect of suppressing gas generation is particularly useful for lithium ion secondary batteries that do not use a metal can as a container, and is also very useful in the lithium ion secondary battery of the present invention.
[0154] Example 6 A lithium ion secondary battery of Example 6 was produced in the same manner as in Example 3, using the same electrolyte solution of Example 6 as that of Example 3. For reference, the electrolyte solution of Example 6 was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution, and then adding and dissolving DTD in an amount equivalent to 0.5 mass % to the mother solution.
[0155] Example 7 A lithium ion secondary battery of Example 7 was produced in the same manner as in Example 3, using the same electrolyte solution of Example 7 as that of Example 4. For reference, the electrolyte solution of Example 7 was prepared by dissolving (FSO2)2NLi at a concentration of 0.6 mol / L and LiPF6 at a concentration of 0.6 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution, and then adding and dissolving DTD in an amount equivalent to 0.5 mass % to the mother solution.
[0156] Comparative Example 6 A lithium ion secondary battery of Comparative Example 6 was manufactured in the same manner as in Example 3, using the same electrolyte of Comparative Example 6 as that of Comparative Example 3. For reference, the electrolyte of Comparative Example 6 was prepared by dissolving LiPF6 at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution, and adding and dissolving (FSO2)2NLi in an amount equivalent to 0.5 mass% and DTD in an amount equivalent to 0.5 mass% to the mother solution. The amount of (FSO2)2NLi in the electrolyte of Comparative Example 6 was 0.03 mol / L, and the amount of (FSO2)2NLi was 2.4 mol% with respect to the total of (FSO2)2NLi and LiPF6.
[0157] Comparative Example 7 A lithium ion secondary battery of Comparative Example 7 was produced in the same manner as in Example 3, using the same electrolyte solution of Comparative Example 7 as that of Comparative Example 4. For reference, the electrolyte solution of Comparative Example 7 was prepared by dissolving LiPF6 at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85 to prepare a mother solution, and then adding and dissolving DTD in an amount equivalent to 0.5 mass % to the mother solution.
[0158] <Evaluation Example 5 High-Temperature Charge-Discharge Cycle Test> Example 6, Example 7, Comparative Example 6, Comparative Example 7The lithium ion secondary battery was subjected to CC-CV charging at a rate of 0.4C to 4.0V. Then, CC-CV discharging was performed at a rate of 1C to 2.5V over 2 hours. The discharge capacity at this time was taken as the initial capacity. In addition, a high-temperature charge-discharge cycle test similar to that of Evaluation Example 2 was performed on each lithium ion secondary battery. Furthermore, the discharge capacity of each lithium ion secondary battery was confirmed after the 50th charge-discharge and after the 100th charge-discharge. The discharge capacity was confirmed in the same manner as the initial capacity described above. The percentage of the discharge capacity after the 50th charge-discharge and the percentage of the discharge capacity after the 100th charge-discharge relative to the initial capacity were calculated, and were taken as the capacity retention rate after 50 cycles and the capacity retention rate after 100 cycles, respectively. The capacity retention rate after 50 cycles and the capacity retention rate after 100 cycles for each lithium ion secondary battery are shown in Table 8. Each test was performed with n=2, and Table 8 shows the average value.
[0159] [Table 8]
[0160] As shown in Table 8, the lithium ion secondary batteries of Examples 6 and 7 were superior in capacity retention rate to the lithium ion secondary batteries of Comparative Examples 6 and 7. This result also supports that the use of an electrolyte solution containing 30 mol % or more of lithium salt other than LiPF6 relative to the total lithium salts improves the durability of the lithium ion secondary battery, particularly at high temperatures.
[0161] <Evaluation Example 6: Storage Test> For the lithium ion secondary batteries of Examples 6 and 7 and Comparative Examples 6 and 7, a storage test was carried out in the same manner as in Evaluation Example 3. Before the storage test, after 7 days had elapsed since the start of the storage test, and after 12 days had elapsed since the start of the storage test, the discharge capacity of each lithium ion secondary battery was confirmed in the same manner as in Evaluation Example 2. The discharge capacity before the storage test was defined as the initial capacity, and the percentage of the discharge capacity after 7 days had elapsed since the start of the storage test and the percentage of the discharge capacity after 12 days had elapsed since the start of the storage test were calculated to be the capacity maintenance rate after 7 days and the capacity maintenance rate after 12 days since the start of the storage test, respectively. The capacity retention rate after 7 days from the start of the storage test and the capacity retention rate after 12 days from the start of the storage test for each lithium ion secondary battery are shown in Table 9. Each test was performed with n=2, and the average value is shown in Table 9.
[0162] [Table 9]
[0163] As shown in Table 9, the lithium ion secondary batteries of Examples 6 and 7 were superior in capacity retention rate to the lithium ion secondary batteries of Comparative Examples 6 and 7, and the difference became more significant as the number of days elapsed after the start of the storage test increased. This result also supports the idea that the use of an electrolyte containing 30 mol % or more of a lithium salt other than LiPF6 relative to the total amount of lithium salts improves the durability of a lithium ion secondary battery, particularly at high temperatures.
[0164] Example 8 A mother solution was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85. An electrolyte solution of Example 8 was produced by adding and dissolving vinylene carbonate in an amount equivalent to 1.94 mass% to the mother solution. A lithium ion secondary battery of Example 8 was produced in the same manner as in Example 1, using the electrolyte of Example 8.
[0165] Comparative Example 8 A mother solution was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 15:85. An electrolyte solution of Comparative Example 8 was produced by adding and dissolving vinylene carbonate in an amount equivalent to 1.94 mass% to the mother solution. A lithium ion secondary battery of Comparative Example 8 was produced in the same manner as in Example 1, using the electrolyte of Comparative Example 8.
[0166] Comparative Example 9 A mother solution was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 15:65:20. An electrolyte solution of Comparative Example 9 was produced by adding and dissolving vinylene carbonate in an amount equivalent to 1.94 mass% to the mother solution. A lithium ion secondary battery of Comparative Example 9 was produced in the same manner as in Example 1, using the electrolyte solution of Comparative Example 9.
[0167] Comparative Example 10 A mother solution was prepared by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 15:45:40. An electrolyte solution of Comparative Example 10 was prepared by adding and dissolving vinylene carbonate in an amount equivalent to 1.94 mass% to the mother solution. A lithium ion secondary battery of Comparative Example 10 was produced in the same manner as in Example 1, using the electrolyte of Comparative Example 10.
[0168] Comparative Example 11 A mother solution was prepared by dissolving LiPF6 at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 15:85. An electrolyte solution of Comparative Example 11 was produced by adding and dissolving vinylene carbonate in an amount equivalent to 1 mass% and LiDFOB in an amount equivalent to 1 mass% to the mother solution. The electrolyte of Comparative Example 11 was used, and the same procedure as in Example 1 was carried out. 11 We manufactured lithium-ion secondary batteries.
[0169] <Evaluation Example 7 Long-term Discharge Test 1> The lithium ion secondary batteries of Example 8 and Comparative Example 11 were subjected to CC discharge at a discharge rate of 1.1 C from SOC 95% to a voltage of 2.2 V, and the change in discharge capacity was measured over time. Separately, CC-CV discharge was performed on each lithium ion secondary battery at a discharge rate of 0.33C from SOC 100% to 3.0V, and the capacity at this time was taken as the CC-CV capacity. The percentage of the capacity at the end of CC discharge relative to the above-mentioned CC-CV capacity was calculated for each lithium ion secondary battery to take the rate %. Note that the test was performed with n=2, and the average value was used as the capacity at the end of CC discharge. For each lithium-ion secondary battery, the charge capacity when CC-CV charging was performed at a rate of 0.2 C up to 3.75 V was defined as SOC100%. 1 is a graph showing the change over time in CC discharge capacity for each of the lithium ion secondary batteries of Example 8 and Comparative Example 11. In addition, Table 10 shows the rate % for each of the lithium ion secondary batteries of Example 8 and Comparative Example 11.
[0170] [Table 10]
[0171] As shown in FIG. 1, the lithium ion secondary battery of Example 8 has a similar structure to that of Comparative Example 11. lithium Compared to ion secondary batteries, the capacity at the end of discharge is significantly higher, and it can be said to have excellent long-term discharge characteristics. Furthermore, as shown in Table 10, the lithium ion secondary battery of Example 8 is also significantly superior in rate % at the end of discharge to the lithium ion secondary battery of Comparative Example 11. These results show that the use of (FSO2)2NLi as the lithium salt contributes to the improvement of long-term discharge characteristics. As shown in Basic Study 1, this result is believed to be due to the fact that when the amount of (FSO2)2NLi relative to the total amount of lithium salts is 30 mol % or more, the viscosity of the electrolyte is reduced and the ionic conductivity is improved.
[0172] <Evaluation Example 8 Long-term Discharge Test 2> For the lithium ion secondary batteries of Example 8 and Comparative Examples 8 to 10, the change in discharge capacity was measured over time in the same manner as in Evaluation Example 7. 2 is a graph showing the change over time in CC discharge capacity for each of the lithium ion secondary batteries of Example 8 and Comparative Examples 8 to 10. Moreover, Table 11 shows the rate % for each of the lithium ion secondary batteries of Example 8 and Comparative Examples 8 to 10.
[0173] [Table 11]
[0174] As shown in FIG. 2, the lithium ion secondary battery of Example 8 has a significantly higher capacity at the end of discharge than the lithium ion secondary batteries of Comparative Examples 8 to 10, and can be said to have excellent long-term discharge characteristics.
[0175] As shown in Table 11, the lithium ion secondary battery of Example 8 is also significantly superior in rate % at the end of discharge to the lithium ion secondary batteries of Comparative Examples 8 to 10. This result also makes it clear that the lithium ion secondary battery of Example 8 is superior in long-term discharge characteristics.
[0176] The reason why the lithium ion secondary battery of Example 8 is superior in long-term discharge characteristics to the lithium ion secondary batteries of Comparative Examples 8 to 10 is believed to be due to the composition of the non-aqueous electrolyte. From this result, the usefulness of using methyl propionate as the non-aqueous electrolyte becomes clearer. Furthermore, from the results of Evaluation Examples 7 and 8, it can be said that by using a combination of (FSO2)2NLi as the lithium salt and methyl propionate as the non-aqueous solvent, an electrolyte that can contribute to improving the battery characteristics of lithium ion secondary batteries can be obtained.
[0177] Example 9 The lithium ion secondary battery of Example 9 is a lithium ion secondary battery of the present invention. An explanatory diagram showing a schematic diagram of the lithium ion secondary battery of Example 9 is shown in Fig. 3. Hereinafter, the lithium ion secondary battery of Example 9 will be described with reference to Fig. 3.
[0178] 3, the lithium ion secondary battery 1 of Example 9 is formed by stacking two storage cells 10. Each storage cell 10 has a positive electrode 2, a negative electrode 3, a separator 4, a sealing portion 5 and an electrolyte 6.
[0179] The positive electrode 2 has a first current collector 20 and a positive electrode active material layer 21. The first current collector 20 is an aluminum foil having one surface 20a and the other surface 20b. of The one surface 20a and the other surface 20b are back-to-back with each other. The positive electrode active material layer 21 is the same as the positive electrode active material layer in the lithium ion secondary battery of Example 1, and is laminated in the central portion of one surface 20 a of the first current collector 20 .
[0180] The negative electrode 3 has a second current collector 30 and a negative electrode active material layer 31. The second current collector 30 is a copper foil having one surface 30a and the other surface 30b. of The one surface 30a and the other surface 30b are back-to-back with each other. The negative electrode active material layer 31 is the same as the negative electrode active material layer in the lithium ion secondary battery of Example 1, and is laminated in the central portion of one surface 30 a of the second current collector 30 . The negative electrode 3 is stacked on the positive electrode 2 with the negative electrode active material layer 31 facing the positive electrode active material layer 21 and with the separator 4 sandwiched between the negative electrode active material layer 31 and the positive electrode active material layer 21. In other words, in the above-mentioned facing direction, a laminate of the negative electrode active material layer 31, the separator 4, and the positive electrode active material layer 21 is sandwiched between the first current collector 20 and the second current collector 30 constituting the same storage cell 10. The separator 4 is the same as the separator in the lithium ion secondary battery of Example 1.
[0181] The sealing portion 5 is made of an acid-modified olefin and has a substantially short cylindrical shape. The sealing portion 5 surrounds the periphery of the laminate of the negative electrode active material layer 31, the separator 4, and the positive electrode active material layer 21 between the first current collector 20 and the second current collector 30 over the entire circumferential direction of the laminate. The surface of the sealing portion 5 facing the first current collector 20 is heat-sealed to the first current collector 20, and the surface facing the second current collector 30 is heat-sealed to the second current collector 30. As a result, the sealing portion 5 liquid-tightly seals the gap between the first current collector 20 and the second current collector 30. The sealing portion 5 also functions as a spacer for maintaining the gap between the first current collector 20 and the second current collector 30 and interrupting direct electrical connection between them.
[0182] An electrolyte solution 6 is sealed in the space partitioned and formed by the sealing portion 5, the first current collector 20, and the second current collector 30. The electrolyte solution 6 is the same as the electrolyte solution in the first embodiment.
[0183] The lithium ion secondary battery 1 of Example 9 has two storage cells 10 connected in series. The first current collector 20x of one storage cell 10x and the second current collector 30y of the adjacent storage cell 10y are stacked on top of each other and directly electrically connected to each other. Therefore, the first current collector 20x and the second current collector 30y can be regarded as one current collector having a two-layer structure, and the current collector can be regarded as a bipolar electrode having a positive electrode active material layer 21x and a negative electrode active material layer 31y provided on each of both sides thereof.
[0184] A method for producing the lithium ion secondary battery 1 of Example 9 will be described below. First, the positive electrode 2 and the negative electrode 3 are produced by the method described in Example 1. Next, the sealing portion 5 is integrated with one of the positive electrode 2 and the negative electrode 3. Specifically, an impulse sealer is used to heat-seal the sealing portion 5 with one of the first current collector 20 and the second current collector 30. As a result, the sealing portion 5 is integrated into a box shape on the first current collector 20 or the second current collector 30, and the electrolyte 6 can be contained therein. Next, an electrolyte solution 6 is injected into the sealing portion 5, and the other of the positive electrode 2 and the negative electrode 3 is integrated therewith. Specifically, the positive electrode active material layer 21 and the negative electrode active material layer 31 are made to face each other, and are stacked with the separator 4 and the sealing portion 5 sandwiched therebetween. Then, the sealing portion 5 is heat-sealed to the other of the first current collector 20 and the second current collector 30 using an impulse sealer. In this way, the storage cell 10 of the lithium-ion secondary battery 1 of Example 9 was obtained. Two storage cells 10 are prepared, and a first current collector 20x of a first storage cell 10x, which is one of the storage cells 10, and a second current collector 30y of a second storage cell 10y, which is the other of the storage cells 10, are overlapped in a facing direction, and the first current collector 20x and the second current collector 30y are stacked. The two stacked storage cells 10 are restrained by a restraining member (not shown), and a predetermined restraining load is applied to each storage cell 10 in the facing direction. This allows the first storage cell 10x and the second storage cell 10y to be maintained in a state where they are stacked on each other. Furthermore, terminals (not shown) are fixed to the storage cells 10x and 10y. This resulted in the lithium ion secondary battery of Example 9 being obtained.
[0185] In the lithium ion secondary battery 1 of Example 9, the sealing portion 5 is fixed to the first current collector 20 and the second current collector 30. Therefore, each storage cell 10 can stably hold the electrolyte 6 therein.
[0186] Example 10 The lithium ion secondary battery of Example 10 is a lithium ion secondary battery of the present invention, and is generally the same as the lithium ion secondary battery of Example 9, except for the structures of the first current collector and the second current collector. An explanatory diagram that shows a schematic diagram of the lithium ion secondary battery of Example 10 is shown in Fig. 4. The lithium ion secondary battery of Example 10 will be described below with reference to Fig. 4.
[0187] 4, in the lithium-ion secondary battery of Example 10, the first current collector 20 of the positive electrode 2 and the second current collector 30 of the negative electrode 3 are integrally formed. Specifically, the first current collector 20 is an aluminum foil, and the second current collector 30 is a copper plating layer formed on the first current collector 20. The lithium ion secondary battery of Example 10 is also excellent in durability, similar to the lithium ion secondary battery of Example 9.
[0188] Example 11 An electrolyte solution of Example 11 was produced by dissolving (FSO2)2NLi at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 30:70.
[0189] Example 12 The electrolyte solution of Example 12 was produced by dissolving (FSO2)2NLi at a concentration of 1 mol / L and LiPF6 at a concentration of 0.2 mol / L in a mixed solvent in which ethylene carbonate and methyl propionate were mixed at a volume ratio of 30:70. In the electrolyte solution of Example 12, the amount of (FSO2)2NLi relative to the total amount of lithium salts was about 83.3 mol%.
[0190] (Example 13) Example 1: (FSO2)2NLi was dissolved at a concentration of 0.8 mol / L and LiPF6 was dissolved at a concentration of 0.4 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 30:70. 3 In the electrolyte of Example 13, the amount of (FSO2)2NLi relative to the total amount of lithium salts was about 66.7 mol %.
[0191] Example 14 In a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 30:70, (FSO2)2NLi was dissolved at a concentration of 0.6 mol / L and LiPF6 was dissolved at a concentration of 0.6 mol / L to produce the electrolyte solution of Example 14. In the electrolyte solution of Example 14, the amount of (FSO2)2NLi relative to the total amount of lithium salts was about 50 mol%.
[0192] Example 15 The electrolyte solution of Example 15 was produced by dissolving (FSO2)2NLi at a concentration of 0.4 mol / L and LiPF6 at a concentration of 0.8 mol / L in a mixed solvent in which ethylene carbonate and methyl propionate were mixed at a volume ratio of 30:70. In the electrolyte solution of Example 15, the amount of (FSO2)2NLi relative to the total amount of lithium salts was about 33.3 mol%.
[0193] Comparative Example 12 In a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 30:70, (FSO2)2NLi was dissolved at a concentration of 0.2 mol / L and LiPF6 was dissolved at a concentration of 1 mol / L to produce the electrolyte solution of Comparative Example 12. In the electrolyte solution of Comparative Example 12, the amount of (FSO2)2NLi relative to the total amount of lithium salts was about 16.7 mol%.
[0194] Comparative Example 13 An electrolyte solution of Comparative Example 13 was prepared by dissolving LiPF6 at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate and methyl propionate in a volume ratio of 30:70.
[0195] <Evaluation Example 9 Peeling Evaluation> A test piece was prepared by heat-sealing an aluminum foil and a copper foil with a sealant, and the test piece was immersed in each of the electrolytes of Examples 11 to 15 and Comparative Examples 12 and 13 to evaluate peeling. Specifically, the dimensions of each test piece were 15 mm × 65 mm, and the seal width was 18 mm. The sealant was an acid-modified olefin-based material, more specifically, it contained a low-melting point polyethylene resin. An impulse sealer was used for heat sealing, and the heating temperature was 110°C. The aluminum laminate film was made into a bag shape of 60 mm x 100 mm, 1 mL of electrolyte was poured into the bag, and the test piece was immersed in the bag. The opening of the bag was heat-sealed with an impulse sealer to seal the test piece and electrolyte inside the bag. This was stored at 60°C for 72 hours. After that, the test piece was taken out of the bag, washed with ethanol, and the natural peeling length of the test piece was measured. A groove micrometer was used for the measurement.
[0196] As shown in Fig. 5, the length from the peel start point between the resin 72 and the aluminum foil 70 to the end of the resin 72 was defined as the natural peel length L1 at the interface between the aluminum foil 70 and the resin 72. Similarly, the length from the peel start point between the resin 72 and the copper foil 71 to the end of the resin 72 was defined as the natural peel length L2 at the interface between the copper foil 71 and the resin 72. L1 and L2 were measured at multiple points and the average was calculated, which was defined as the natural peel length of the test piece for each electrolyte. The results are shown in Fig. 6.
[0197] 6, when the electrolyte solutions of Examples 11 to 15 and Comparative Example 12, which contained lithium salts other than LiPF6, were used, the spontaneous peeling length of the test pieces was shorter than that of Comparative Example 13, which contained only LiPF6 as the lithium salt. Moreover, the spontaneous peeling lengths of the test pieces using the electrolyte solutions of Examples 12 to 15 were almost the same. As mentioned above, LiPF6 reacts with water to produce hydrogen fluoride, and therefore, in the test piece using the electrolyte of Comparative Example 13, the aluminum foil is deteriorated by the hydrogen fluoride, and as a result, peeling at the interface between the resin and the aluminum foil is considered to have progressed. And, it can be said that the peeling is sufficiently suppressed when an electrolyte containing 30 mol% or more of lithium salt other than LiPF6 with respect to the total lithium salt is used as in Examples 11 to 15. Since the spontaneous peeling length of the test pieces using the electrolytes of Examples 12 to 15 was almost the same value, from the viewpoint of peeling suppression, it can be said that the amount of lithium salt other than LiPF6 contained in the electrolyte is sufficient if it is 30 mol% or more with respect to the total lithium salt.
[0198] In addition, when an electrolyte containing a large amount of LiPF6 is used as the electrolyte of the lithium ion secondary battery of the present invention, as in Comparative Examples 12 and 13, it is presumed that peeling will similarly occur at the interface between the first current collector and the sealing portion. In contrast, when an electrolyte solution containing 30 mol % or more of a lithium salt other than LiPF6 relative to the total amount of lithium salts is used as the electrolyte solution of the lithium ion secondary battery of the present invention, as in Examples 11 to 15, it can be said that peeling at the interface between the first current collector and the sealing portion is sufficiently suppressed.
Claims
1. a positive electrode having a first current collector and a positive electrode active material layer provided on one surface of the first current collector; a negative electrode including a second current collector and a negative electrode active material layer provided on one surface of the second current collector, the negative electrode being overlapped on the positive electrode with the negative electrode active material layer facing the positive electrode active material layer; a separator disposed between the positive electrode active material layer and the negative electrode active material layer; a sealing portion that is disposed between the first current collector and the second current collector, that surrounds the positive electrode active material layer and the negative electrode active material layer, and that seals an electrolyte in a space between the first current collector and the second current collector; The electrolyte solution may include The battery has an electrolyte containing a lithium salt and a non-aqueous solvent containing an alkylene cyclic carbonate and methyl propionate, The electrolyte is LiPF 6 The lithium salt other than the lithium salt is contained in an amount of 30 mol % or more based on the total amount of the lithium salts, The lithium ion secondary battery uses an electrolyte solution in which the non-aqueous solvent contains 75 volume % or more of the methyl propionate.
2. The battery has an electrolyte containing a lithium salt and a non-aqueous solvent containing an alkylene cyclic carbonate and methyl propionate, The electrolyte is LiPF 6 The lithium salt other than the lithium salt is contained in an amount of 30 mol % or more based on the total amount of the lithium salts, The non-aqueous solvent contains 75% by volume or more of the methyl propionate.
3. The LiPF 6 The lithium salt other than (CF 3 SO 2 ) 2 NLi, (FSO 2 ) 2 NLi, (C 2 F 5 SO 2 ) 2 NLi, FSO 2 (CF 3 SO 2 ) NLi, (SO 2 CF 2 CF 2 SO 2 ) NLi, or (SO 2 CF 2 CF 2 CF 2 SO 2 3. The electrolyte of claim 2, wherein NLi is 0.1 to 0.25 Mg.
4. The electrolyte solution according to claim 2 or 3, wherein the non-aqueous solvent contains 80% by volume or more of the methyl propionate.
5. The electrolyte is LiPF 6 The electrolyte solution according to any one of claims 2 to 4, wherein the electrolyte solution contains a lithium salt other than the lithium salt in an amount of 50 mol % or more based on the total amount of the lithium salts.
6. The lithium ion secondary battery according to claim 1 , wherein the negative electrode contains graphite in the negative electrode active material layer.
Citation Information
Patent Citations
Nonaqueous electrolyte for battery and nonaqueous electrolyte battery equipped with it
JP2008258022A
Lithium secondary battery and using method thereof
JP2010123300A
Nonaqueous electrolyte secondary battery
JP2013140734A
Electrolyte for lithium ion secondary battery and lithium ion secondary battery
JP2018092785A