Silicon carbide semiconductor device

The SiC semiconductor device with a recessed trench gate structure and protruding barrier metal design addresses electrode peeling issues, enhancing anchoring to prevent resistance and breakdown.

JP7563356B2Active Publication Date: 2024-10-08DENSO CORP +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021164344
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-05
Publication Date
2024-10-08
Estimated Expiration
2041-10-05

AI Technical Summary

Technical Problem

The peeling of the source electrode in SiC semiconductor devices with trench gate structures due to temperature fluctuations, leading to increased resistance and potential element breakdown, is addressed by enhancing the anchoring effect between the electrode and underlying layers.

Method used

A SiC semiconductor device with a trench gate structure that includes a recessed configuration between the interlayer insulating film and the electrode, featuring a protruding barrier metal and an electrode layer with uneven surfaces to enhance anchoring, reducing the likelihood of peeling.

Benefits of technology

The enhanced anchoring effect prevents electrode peeling, thereby reducing resistance and heat generation, and preventing element breakdown during temperature fluctuations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007563356000001
    Figure 0007563356000001
  • Figure 0007563356000002
    Figure 0007563356000002
  • Figure 0007563356000003
    Figure 0007563356000003
Patent Text Reader

Abstract

To suppress element breakdown due to the temperature rise by heat generation by suppressing separation of an electrode formed on a trench gate structure.SOLUTION: A step is formed between an upper surface of an interlayer insulating film 9 and an upper surface of an n+ type source region 4 to form a recess 12. The source electrode 10 comprises: a metal silicide layer 10a which is formed on the surface of the n+ type source region 4 or the like; a barrier metal 10b which is formed in the recess 12 on the metal silicide layer 10a; and an electrode layer 10c which is formed on the barrier metal 10b. Furthermore, a step is formed between a barrier metal 10ba formed in the recess 12 of the barrier metal 10b and a barrier metal 10bb formed on the metal silicide layer 10a, and a protrusion 10bc protruding to the inner side in the width direction of a gate trench 6 is provided on the barrier metal 10bb. A dimension W1 between the tips of the protrusion 10bc is made to be narrower than a dimension W2 of a portion which the electrode layer 10c enters on the lower side thereof.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicon carbide (hereinafter referred to as SiC) semiconductor device having a semiconductor element with a trench gate structure made of SiC. [Background technology]

[0002] Patent Document 1 proposes a trench-gate structure SiC semiconductor device that can reduce the cell pitch without increasing the on-resistance. In this SiC semiconductor device, an interlayer insulating film and a barrier metal are embedded on the gate electrode inside the gate trench to flatten the surface, and an electrode layer is formed on the gate electrode to form a source electrode including the barrier metal and the electrode layer. With this configuration, it is no longer necessary to expose the interlayer insulating film on the top surface of the SiC, so that contacts can be formed on the entire top surface of the SiC, and there is no misalignment of the mask when forming the contact holes, so there is no restriction on the cell pitch. This makes it possible to reduce the cell pitch. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-3967 A Summary of the Invention [Problem to be solved by the invention]

[0004] When semiconductor elements such as MOSFETs are operated, the temperature repeatedly rises and falls. Since the materials that make up the semiconductor element have different linear expansion coefficients, repeated stress is applied to the interfaces between the materials as the temperature rises and falls. This can cause the source electrode to peel off in a MOSFET with a trench gate structure.

[0005] In particular, in a structure in which an interlayer insulating film and a barrier metal are embedded on the gate electrode in the gate trench to flatten the surface and an electrode layer is formed on top of that, as in the SiC semiconductor device described in Patent Document 1, the anchor effect is small because of the small surface irregularities. In other words, if the surface is uneven, the electrode layer will be caught on the steps caused by the unevenness and the lateral displacement between the electrode layer and its base will be suppressed, but if the surface is less uneven, lateral displacement between the electrode layer and its base will be more likely to occur, making the source electrode more likely to peel off.

[0006] If the source electrode peels off, resistance increases when electricity is applied, which may cause a temperature rise due to heat generation, which may lead to destruction of the element.

[0007] In view of the above, an object of the present invention is to provide a SiC semiconductor device that can suppress peeling of an electrode formed on a trench gate structure and suppress element destruction due to heat generation. [Means for solving the problem]

[0008] In order to achieve the above object, the invention described in claim 1 is a SiC semiconductor device having a semiconductor element with a trench gate structure, comprising: a substrate (1) of a first or second conductivity type made of SiC; a drift layer (2) of a first conductivity type formed on the substrate and having a lower impurity concentration than the substrate; a channel layer (3) of a second conductivity type formed on the drift layer and having a contact region (3a) formed in a surface layer portion; a first conductivity type region (4) formed at a position different from the contact region on the channel layer and having a higher first conductivity type impurity concentration than the drift layer; a gate insulating film (7) formed on an inner wall surface of a gate trench (6) penetrating the first conductivity type region and the channel layer, and a gate electrode (8) formed on the gate insulating film; an interlayer insulating film (9) covering the gate electrode in the gate trench; a first electrode (10) electrically connected to the contact region and the first conductivity type region; and a second electrode (11) formed on the back surface side of the substrate.

[0009] In such a configuration, a step is formed between the upper surface of the interlayer insulating film and the upper surface of the first conductivity type region, thereby forming a recess (12), and the first electrode has a metal layer (10a) formed on the surface of the contact region and the first conductivity type region, a barrier metal (10b) formed on the metal layer and within the recess, and an electrode layer (10c) formed on the barrier metal, and a step is formed between a first barrier metal (10ba) formed in the recess and a second barrier metal (10bb) formed on the metal layer, and a protrusion (10bc) is formed in the second barrier metal so as to protrude toward the inside in the width direction of the gate trench, and a part of the electrode layer extends below the protrusion, and the dimension (W1) between the tips of the protrusions on both sides of the width direction of the gate trench is narrower than the dimension (W2) of the portion where the electrode layer extends below the protrusion.

[0010] In this way, a step is formed between the first barrier metal and the second barrier metal. That is, the surface of the base of the electrode layer is uneven. In addition, the second barrier metal is provided with a protruding eaves-shaped protrusion on the inner side in the width direction of the gate trench, and the dimension between the tips of the protrusions on both sides in the width direction of the gate trench is narrower than the dimension of the part where the electrode layer enters below the protrusion. This allows the electrode layer to exert an anchor effect. Therefore, even if the temperature rises and falls repeatedly when the semiconductor element is operated, the electrode layer is less likely to peel off from the barrier metal that serves as the base, and peeling of the source electrode can be suppressed. This makes it possible to suppress an increase in resistance when electricity is applied and a rise in temperature due to heat generation, and to suppress element destruction.

[0011] The reference symbols in parentheses attached to each component indicate an example of the correspondence between the component and specific components described in the embodiments described below. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view of a SiC semiconductor device according to a first embodiment. [Diagram 2] FIG. 4 is a cross-sectional view showing a detailed structure of a source electrode. [Diagram 3] 11 is a cross-sectional view showing a detailed structure of a source electrode when the barrier metal has a laminated structure. FIG. [Figure 4] 4 is a flowchart showing a process for forming a trench gate structure and a source electrode in the SiC semiconductor device according to the first embodiment. [Figure 5A] 5 is a cross-sectional view showing a state after a gate trench forming step in FIG. 4. FIG. [Figure 5B] FIG. 5 is a cross-sectional view showing a state after the etch-back step in FIG. [Figure 5C] 5 is a cross-sectional view showing a state after a step of forming an interlayer insulating film in FIG. 4. [Figure 5D] 5 is a cross-sectional view showing a state after an etch-back process of the interlayer insulating film in FIG. 4. FIG. [Figure 5E] 5 is a cross-sectional view showing a state after a metal film forming step in FIG. 4. FIG. [Figure 5F] 5 is a cross-sectional view showing a state after a metal film removing step in FIG. 4. FIG. [Figure 5G] 5 is a cross-sectional view showing a state after a barrier metal forming step in FIG. 4. FIG. [Figure 5H] 5 is a cross-sectional view showing a state after a step of forming an electrode layer in FIG. 4. FIG. [Figure 6A] 1 is a cross-sectional view of a gate trench in which an interlayer insulating film and a barrier metal are embedded on a gate electrode to flatten the surface. [Figure 6B] FIG. 11 is a cross-sectional view showing the peeling of the source electrode. [Figure 7] 4 is a cross-sectional view showing a detailed structure of a source electrode in a SiC semiconductor device described in a modified example of the first embodiment. FIG. [Figure 8] 10 is a flowchart showing a process for forming a trench gate structure and a source electrode in a SiC semiconductor device according to a second embodiment. [Figure 9A] 9 is a cross-sectional view showing a state after a step of forming an interlayer insulating film in FIG. 8. FIG. [Figure 9B]9 is a cross-sectional view showing a state after an etch-back process of the interlayer insulating film in FIG. 8. FIG. [Figure 9C] 9 is a cross-sectional view showing a state after a metal film forming step in FIG. 8. FIG. [Figure 9D] 9 is a cross-sectional view showing a state after a metal film removing step in FIG. 8. FIG. [Figure 9E] 9 is a cross-sectional view showing a state after a gate contact hole forming step in FIG. 8. FIG. [Figure 9F] 9 is a cross-sectional view showing a state after a barrier metal forming step in FIG. 8. FIG. [Figure 9G] 9 is a cross-sectional view showing a state after a step of forming an electrode layer in FIG. 8. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In the following embodiments, parts that are the same or equivalent to each other will be denoted by the same reference numerals.

[0014] (First embodiment) A first embodiment will be described. A SiC semiconductor device according to this embodiment will be described. Here, a SiC semiconductor device in which a MOSFET is formed as a semiconductor element having a trench gate structure will be described as an example.

[0015] The SiC semiconductor device according to this embodiment includes a vertical MOSFET with a trench gate structure as shown in Fig. 1. The vertical MOSFET is formed in a cell region of the SiC semiconductor device, and the SiC semiconductor device is configured by forming a peripheral breakdown voltage structure so as to surround the cell region, but only the vertical MOSFET of the SiC semiconductor device is illustrated here. In the following description, the left-right direction of Fig. 1 is the width direction of the SiC semiconductor device, and the up-down direction is the thickness direction or depth direction of the SiC semiconductor device.

[0016] The SiC semiconductor device includes n + A mold substrate 1 is used as a semiconductor substrate.+ On the main surface of the substrate 1, a n-type semiconductor layer made of SiC is formed. - The n-type drift layer 2 is epitaxially grown. - On the first conductivity type drift layer 2, a p-type base region 3 corresponding to a channel layer and an n-type region corresponding to a first conductivity type region are provided. + A type source region 4 is in turn formed.

[0017] The p-type base region 3 is a region in which a channel region is formed, and + A p-type contact region 3a having a partially increased p-type impurity concentration is formed in a surface layer portion at a position different from the position where the n-type source region 4 is disposed. + The source region 4 is an n - The impurity concentration in the first layer is higher than that in the second layer.

[0018] In addition, the p-type base region 3 and the n + through the n-type source region 4 - A gate trench 6 is formed so as to reach the n-type drift layer 2. The p-type base region 3 and the n-type base region 4 are formed so as to contact the side surfaces of the gate trench 6. + A type source region 4 is arranged. The gate trenches 6 are formed in a line layout with the width direction being the left-right direction of the paper in FIG. 1, which is the width direction of the SiC semiconductor device, the length direction being the normal direction to the paper, and the depth direction being the up-down direction of the paper in FIG. 1, which is the thickness direction of the SiC semiconductor device. Although only one gate trench 6 is shown in FIG. 1, multiple gate trenches 6 are arranged at equal intervals in the left-right direction of the paper to form a stripe shape. The width of the gate trench 6 is arbitrary, but is preferably two or more times the thickness of a barrier metal 10b described later, and is 0.3 to 1 μm, for example 1 μm.

[0019] The portion of the p-type base region 3 located on the side of the gate trench 6 becomes an n + Type source region 4 and n -The gate trench 6 is a channel region connecting the gate electrode 8 and the gate drift layer 2. A gate insulating film 7 is formed on the inner wall surface of the gate trench 6 including the channel region. A gate electrode 8 made of doped polysilicon is formed on the surface of the gate insulating film 7. The gate electrode 8 is n-type doped or p-type doped. An interlayer insulating film 9 is formed on the gate insulating film 7 and the gate electrode 8 to form a trench gate structure. The gate trench 6 is not completely filled with the gate insulating film 7, the gate electrode 8, and the interlayer insulating film 9, but is completely filled with a barrier metal 10ba and a part of an electrode layer 10c shown in FIG. 2 to be described later.

[0020] More specifically, the n-type GaN layer constituting the entrance of the gate trench 6 + The upper surface of the gate electrode 8 is lower than the upper surface of the type source region 4, and a step is formed between them to give the gate electrode 8 a recessed shape. Then, the interlayer insulating film 9, the barrier metal 10ba, and a part of the electrode layer 10c are arranged in the recessed shape so as to fill the step, thereby filling the inside of the gate trench 6. Even in a state where the interlayer insulating film 9 is formed on the gate electrode 8, the recessed shape remains, and a recess 12 having a depth of 40 to 300 nm, for example, about 200 nm, is formed. Therefore, the barrier metal 10ba and a part of the electrode layer 10c are formed so as to be embedded in the recess 12 that constitutes the recessed shape. In other words, the lower surface of the barrier metal 10ba is + The recess 12 is formed so that the upper surface of the barrier metal 10ba is located below the SiC surface, which is constituted by the p-type source region 4 and the p-type contact region 3a. The barrier metal 10ba is formed to fill the recess 12, and the upper surface of the barrier metal 10ba is located below the SiC surface. Part of the barrier metal 10ba and the electrode layer 10c are embedded in the recess 12.

[0021] A source electrode 10 corresponding to a first electrode, a gate wiring layer (not shown), and the like are formed on the interlayer insulating film 9. The source electrode 10 is connected to the n +The gate wiring portion is in contact with a gate electrode 8 in a cross section different from that in FIG.

[0022] As shown in FIG. 2, the source electrode 10 includes a metal silicide layer 10a, a barrier metal 10b, and an electrode layer 10c.

[0023] The metal silicide layer 10a is an ohmic contact layer formed by a silicidation reaction with SiC. The metal silicide layer 10a forms an ohmic contact with low contact resistance between the source electrode 10 and SiC. The metal silicide layer 10a is made of a refractory metal-based or noble metal-based silicide, such as Ni (nickel) silicide, Ti (titanium) silicide, Ta (tantalum) silicide, W (tungsten) silicide, or Mo (molybdenum). The metal silicide layer 10a may be made of one type of metal or may be made of multiple types of metal. For example, the metal silicide layer 10a may be made of different types of metal for n-type SiC and p-type SiC. Here, the metal silicide layer 10a is made of Ni silicide, for example. The thickness of the metal silicide layer 10a is arbitrary, but is set to 10 to 100 nm, for example, about 50 nm.

[0024] The barrier metal 10b has a barrier metal 10ba corresponding to the first barrier metal formed on the interlayer insulating film 9 and a barrier metal 10bb corresponding to the second barrier metal formed on the metal silicide layer 10a. The barrier metal 10ba suppresses the diffusion of metal elements from the source electrode 10 side to the interlayer insulating film 9 and the gate electrode 8. The barrier metal 10bb suppresses the diffusion of metal elements from the metal silicide layer 10a to the electrode layer 10c in the source electrode 10. If the metal silicide layer 10a is Ni silicide, the barrier metal 10ba suppresses the diffusion of Ni to the interlayer insulating film 9 and the gate electrode 8, and the barrier metal 10bb suppresses the diffusion of Ni to the electrode layer 10c. The barrier metal 10b is composed of a metal that fulfills these roles, such as Ti or TiN (titanium nitride). Although the barrier metal 10b is illustrated as a single-layer structure in FIG. 2, it may be a laminated structure of multiple metals, such as Ti and TiN, as shown in FIG. 3.

[0025] The barrier metal 10ba and the barrier metal 10bb are formed at the same time, but are not formed in a flat shape, and a step is formed between them, and the upper surface of the barrier metal 10bb is located higher than the upper surface of the barrier metal 10ba. Furthermore, the barrier metal 10ba and the barrier metal 10bb are separated from each other. The thickness of the barrier metal 10b is arbitrary, but is set to be equal to or smaller than the depth of the recess 12. When the barrier metal 10b is formed of a laminated structure of Ti and TiN, Ti is set to 30 to 100 nm, for example, 50 nm, and TiN is set to 50 to 100 nm, for example, 100 nm.

[0026] Since the barrier metal 10b is set to be equal to or less than the depth of the recess 12, the barrier metal 10ba is located below the SiC surface, and the recess 12 remains even when the barrier metal 10ba is disposed. That is, the depth D1 of the recess 12 is greater than the thickness D2 of the barrier metal 10ba. Therefore, the electrode layer 10c is formed with the SiC surface having irregularities, and a part of the electrode layer 10c is embedded in the recess 12. In addition, in the present embodiment, the SiC is exposed at the upper end position on the side surface of the gate trench 6, and a part of the electrode layer 10c is in contact with the SiC.

[0027] Furthermore, the barrier metal 10bb has a protruding portion 10bc that protrudes further inward in the width direction of the gate trench 6 than the metal silicide layer 10a. A dimension W1 between the tips of the protruding portions 10bc on both sides in the width direction of the gate trench 6 is narrower than a dimension W2 of a portion below the protruding portion 10bc into which the electrode layer 10c enters. The dimension of the protruding portion 10bc can be adjusted by the deposition conditions of the barrier metal 10b, and can be made to protrude to the same extent as the thickness of the portion of the barrier metal 10ba formed on the metal silicide layer 10a, and is set to be at least half of that thickness here.

[0028] The electrode layer 10c is a portion that constitutes the pad portion of the source electrode 10. Here, the electrode layer 10c is made of a metal containing Al, such as AlSi. The electrode layer 10c is formed thicker than the metal silicide layer 10a and the barrier metal 10b. The electrode layer 10c is in a state of penetrating into the gate trench 6, including below the protruding portion 10bc, through a gap of dimension W1. In this way, the electrode layer 10c can penetrate below the protruding portion 10bc and exert an anchor effect.

[0029] Although the electrode layer 10c is described here as having a single-layer structure, it may have a multilayer structure by plating the surface with Ni (nickel) or Au (gold), for example.

[0030] Furthermore, n+ The back side of the mold substrate 1 is + A drain electrode 11 corresponding to a second electrode electrically connected to the type substrate 1 is formed. With this structure, an n-channel type inversion type trench gate structure vertical MOSFET is formed. A cell region is formed by arranging a plurality of such vertical MOSFETs. Then, a peripheral breakdown voltage structure using a guard ring (not shown) or the like is formed so as to surround the cell region in which such a vertical MOSFET is formed, thereby forming a SiC semiconductor device.

[0031] Next, the method for manufacturing the SiC semiconductor device of this embodiment will be described with reference to the flow chart shown in Fig. 4 and the cross-sectional views during the manufacturing process shown in Fig. 5A to Fig. 5H. However, since the steps other than the step of forming the gate electrode 8 in the method for manufacturing the SiC semiconductor device of this embodiment may be any steps, including publicly known steps, the step of forming the gate electrode 8 will be mainly described here, and the other steps will be briefly described.

[0032] First, a wafer-shaped n-type semiconductor substrate made of SiC was used. + After preparing the mold substrate 1, + On the main surface of the substrate 1, - The n-type drift layer 2 is then epitaxially grown. - A p-type base region 3 and an n-type drift layer 2 are disposed on the p-type drift layer 2. + The n-type source region 4 is formed by epitaxial growth or ion implantation. + A mask (not shown) is formed on the surface of the n-type source region 4, and p-type impurities are ion-implanted to form the p-type contact region 3a. + A mask (not shown) is placed on the surface of the source region 4, and an opening is made in the mask in a region where a trench gate structure is to be formed.

[0033] Thereafter, a process for forming a gate trench 6 shown in Fig. 4 is performed. For example, the above-mentioned mask is used to perform anisotropic etching such as RIE (Reactive Ion Etching) to form the gate trench 6 as shown in Fig. 5A. Then, after removing the mask, a process for forming a gate insulating film 7 shown in Fig. 4 is performed. For example, the gate insulating film 7 is formed by forming a silicon oxide film by CVD (chemical vapor deposition) or by forming a thermal oxide film by thermal oxidation.

[0034] 4 is sequentially performed as a step of forming the gate electrode 8, thereby forming the gate electrode 8 in the gate trench 6 as shown in FIG. 5B. That is, a polysilicon film is formed on the surface of the gate insulating film 7 by CVD or the like so as to fill the inside of the gate trench 6, and then the polysilicon film is etched back by dry etching to remove the portion formed outside the gate trench 6. At this time, the polysilicon film is etched back until the inside of the gate trench 6 is recessed so that the inside of the gate trench 6 is not completely filled with the gate electrode 8.

[0035] Next, by performing the step of forming the interlayer insulating film 9 shown in FIG. 4, the interlayer insulating film 9 is formed on the gate electrode 8 so as to fill the inside of the gate trench 6 as shown in FIG. 5C. For example, the interlayer insulating film 9 can be formed by low-pressure CVD or the like. Then, the etch-back step of the interlayer insulating film 9 shown in FIG. 4 is performed. That is, as shown in FIG. 5D, the interlayer insulating film 9 is etched back by dry etching or the like so that the SiC surface is exposed while the interlayer insulating film 9 remains on the gate electrode 8, and a recess shape with the recess 12 remaining is formed. The depth of the recess 12 at this time is arbitrary, but for example, the depth of the recess 12 is set to about 200 nm.

[0036] Then, the metal film forming process and the silicide forming process by heat treatment shown in FIG. 4 are performed. Specifically, as shown in FIG. 5E, a metal film 20 for forming a metal silicide layer 10a is formed. Here, the Ni film is formed by Ni sputtering. At this time, since the recess 12 remains in the gate trench 6, when the metal film 20 is formed, a step is formed in the metal film 20 between the top of the gate trench 6 and the outside thereof.

[0037] Then, a heat treatment is performed at 600 to 800° C., for example, 700° C., to cause a silicidation reaction between the metal constituting the metal film 20 and the Si in the SiC. As a result, the silicidation reaction of the metal film 20 occurs on the SiC surface, and the metal film 20 remains on the interlayer insulating film 9 without undergoing the silicidation reaction.

[0038] Thereafter, the metal film 20 remaining on the interlayer insulating film 9 is removed as shown in FIG. 5F by performing the removal process of the metal film 20 shown in FIG. 4. For example, the metal film 20 is removed by wet etching. As a result, the metal silicide layer 10a remains only on the SiC surface. Even on the SiC surface, the metal film 20 is not necessarily silicided in its entirety, and the metal film 20 may remain on the metal silicide layer 10a. In this case, the metal film 20 remaining on the metal silicide layer 10a is also removed at the same time. Although the metal silicide layer 10a is formed by the above heat treatment, if the temperature of the heat treatment is increased, there is a possibility that the metal elements constituting the metal film 20 will diffuse into the interlayer insulating film 9. For this reason, the above heat treatment can be kept at a relatively low temperature of 800° C. or less, and after the removal process of the metal film 20, high-temperature annealing can be performed at a higher temperature of 900 to 1000° C., for example, 950° C. This makes it possible to further reduce the contact resistance between the metal silicide layer 10a and SiC.

[0039] Further, a process for forming the barrier metal 10b shown in FIG. 4 is performed. For example, by performing sputtering, the barrier metal 10b can be selectively deposited on the metal silicide layer 10a and the interlayer insulating film 9. Here, the barrier metal 10b is formed by sequentially sputtering Ti and TiN, but the barrier metal 10b may be formed by sputtering a single layer film such as Ti or TiN or other materials. As a result, as shown in FIG. 5G, the barrier metal 10b is formed on the metal silicide layer 10a and the interlayer insulating film 9. The barrier metal 10bb on the metal silicide layer 10a is formed to spread laterally and wrap around the inside of the gate trench 6, and the protruding portion 10bc is configured in an eaves shape. For example, the smaller the energy during sputtering, the more the barrier metal 10b can be deposited isotropically, so the size of the protruding portion 10bc can be adjusted by controlling the magnitude of the energy during sputtering.

[0040] At this time, since a step is formed between the interlayer insulating film 9 and the metal silicide layer 10a, the barrier metal 10b formed thereon also inherits the step. In the present embodiment, the depth D1 of the recess 12 is set to be greater than the thickness D2 of the barrier metal 10b. Therefore, the barrier metal 10ba on the interlayer insulating film 9 and the barrier metal 10bb on the metal silicide layer 10a are formed separately, and the barrier metal 10b is not formed on the SiC surface of the separation portion, so that the protrusion 10bc can be formed in a stable eaves shape.

[0041] Thereafter, the step of forming the electrode layer 10c shown in FIG. 4 is performed. For example, AlSi or the like is sputtered. As a result, the electrode layer 10c is formed on the barrier metal 10b as shown in FIG. 5H. The electrode layer 10c is also formed below the protruding portion 10bc so as to wrap around, and a part of the electrode layer 10c is embedded in the recess 12. Then, the electrode layer 10c and the barrier metal 10b are patterned using a mask (not shown) to form the source electrode 10.

[0042] Finally, +Then, processes such as forming a drain electrode 11 on the back surface of the mold substrate 1 are performed. In this way, the SiC semiconductor device having the vertical MOSFET according to this embodiment shown in FIG.

[0043] In the SiC semiconductor device of the present embodiment described above, a step is formed between the barrier metal 10ba formed on the surface of the interlayer insulating film 9 and the barrier metal 10bb formed on the metal silicide layer 10a. That is, the surface of the base of the electrode layer 10c has an uneven shape. In addition, the barrier metal 10bb is provided with an eaves-shaped protruding portion 10bc protruding from the inner side in the width direction of the gate trench 6, so that the dimension W1 is narrower than the dimension W2, and a part of the electrode layer 10c is inserted below the protruding portion 10bc. Therefore, unlike the SiC semiconductor device described in Patent Document 1, the electrode layer 10c can exhibit an anchor effect.

[0044] Specifically, in the SiC semiconductor device of Patent Document 1, as shown in FIG. 6A, an interlayer insulating film J3 and a barrier metal J4 are embedded on a gate electrode J2 inside a gate trench J1 to flatten the surface. Then, a laminated film J5 of Ni and Ti films and an electrode layer J6 of AlSi are formed on the barrier metal J4 and the SiC surface to configure a source electrode including the barrier metal J4, the laminated film J5, and the electrode layer J6. In this structure, the surfaces of the SiC surface and the barrier metal J4 are flat with few irregularities, so there is no step on which the electrode layer J6 and the like can get caught. For this reason, as shown in FIG. 6B, for example, the electrode layer J6 peels off at the interface with the laminated film J5, causing the source electrode to peel off.

[0045] In contrast, in the SiC semiconductor device of this embodiment, the surface of the base of the electrode layer 10c is made uneven, and a part of the electrode layer 10c is in a state of being embedded under the protruding portion 10bc. This allows the electrode layer 10c to exert an anchor effect. Therefore, even if the temperature rises and falls repeatedly when the semiconductor element is operated, the electrode layer 10c is unlikely to peel off from the barrier metal 10b and the like that serves as the base, and peeling of the source electrode 10 can be suppressed. This makes it possible to suppress an increase in resistance during current flow and a rise in temperature due to heat generation, thereby suppressing element destruction.

[0046] Furthermore, the SiC semiconductor device of this embodiment can also provide the following effects.

[0047] (1) In the SiC semiconductor device of this embodiment, the depth D1 is made larger than the thickness D2 so that the electrode layer 10c is formed in a state where the recess 12 of the gate trench 6 remains, that is, where there are irregularities on the SiC surface, so that a part of the electrode layer 10c penetrates into the recess 12. As a result, a part of the electrode layer 10c penetrates deeper, and a higher anchor effect can be obtained. Therefore, it is possible to further obtain the above-mentioned effects.

[0048] (2) The barrier metal 10ba on the interlayer insulating film 9 and the barrier metal 10bb on the SiC surface are not flat, but have a step between them. This provides an escape route for the residual stress of the barrier metal 10b, thereby suppressing the effects of the residual stress and enabling a SiC semiconductor device to have a structure capable of suppressing wafer warpage.

[0049] (3) In the SiC semiconductor device of Patent Document 1, the barrier metal made of Ti or TiN, the Ni film for forming the metal silicide, and the Ti film are formed in this order by sputtering, so the number of sputtering operations is large. In contrast, in the SiC semiconductor device of this embodiment, it is only necessary to form the metal film 20 for forming the metal silicide layer 10a and the barrier metal 10b by sputtering. Since sputtering is usually performed on a single wafer basis, the number of sputtering operations leads to an increase in the manufacturing cost of the SiC semiconductor device. Therefore, if the number of sputtering operations can be reduced as in the SiC semiconductor device of this embodiment, the manufacturing process of the SiC semiconductor device can be simplified, which in turn makes it possible to reduce the manufacturing cost.

[0050] (Modification of the first embodiment) In the first embodiment, the barrier metal 10ba and the barrier metal 10bb are separated from each other, but they may be connected as shown in Fig. 7. In this case, since the barrier metal 10b is more easily formed on the metal silicide layer 10a than on the SiC surface, a protruding portion 10bc is formed at the end of the metal silicide layer 10a.

[0051] In addition, in the first embodiment, even after the barrier metal 10ba is formed, a recess remains in the recess 12, but the surface of the barrier metal 10ba may be flush with the SiC surface, or the surface of the barrier metal 10ba may protrude from the SiC surface.

[0052] In other words, it is sufficient that there is a step between the barrier metal 10ba and the barrier metal 10bb, a protruding portion 10bc is formed on the barrier metal 10bb, and the dimension W2 of the portion into which the electrode layer 10c fits is narrower than the dimension W1 between the tips of the protruding portion 10bc. Even with such a structure, the effects shown in the first embodiment can be obtained.

[0053] Second embodiment A second embodiment will be described. This embodiment shows a process for forming a gate wiring portion in comparison with the first embodiment, and other aspects are the same as those of the first embodiment, so only the differences from the first embodiment will be described.

[0054] In this embodiment, a process for forming a gate wiring portion connected to a gate electrode 8 at a location different from the vertical MOSFET, for example, at the longitudinal end of a trench gate structure, will be described with reference to Fig. 8 and Figs. 9A to 9G. Figs. 9A to 9G are cross-sectional views showing the state of each process, with the left diagram showing a cross-sectional view of a vertical MOSFET and the right diagram showing a cross-sectional view of a gate wiring portion formed at a location different from the vertical MOSFET, for example, in a connection region located between a cell region and a peripheral breakdown withstand structure. In the following description, the process with the same name as in the first embodiment is performed by the same method as in the first embodiment.

[0055] First, the process of forming the gate trench 6, the process of forming the gate insulating film 7, and the process of forming the polysilicon film shown in FIG. 8 are performed in the same manner as in the first embodiment. At this time, the gate insulating film 7 is formed on the SiC surface even at the position where the gate wiring part is to be formed, and the polysilicon film is also formed thereon. Next, the etch-back process is performed to pattern the polysilicon film, and the gate electrode 8 is formed in the gate trench 6 as shown in FIG. 9A, and the gate wiring layer 31 constituting a part of the gate wiring part is formed at another position. Then, the process of forming the interlayer insulating film 9 is performed to form the interlayer insulating film 9 on the gate electrode 8 so as to fill the inside of the gate trench 6 and cover the gate wiring layer 31. Furthermore, the etch-back process of the interlayer insulating film 9 shown in FIG. 8 is performed. At this time, the cell region where the vertical MOSFET is to be formed is opened, and a mask (not shown) that covers the area other than the cell region is formed on the interlayer insulating film 9, and then the etch-back is performed. As a result, as shown in FIG. 9B, the gate wiring layer 31 is left covered with the interlayer insulating film 9, while the interlayer insulating film 9 remains only in the gate trench 6 in the cell region.

[0056] Thereafter, a process of forming a metal film 20, a process of forming a silicide by heat treatment, and a process of removing the metal film 20 are performed as shown in Fig. 8. As a result, the metal film 20 is formed on the SiC surface and the interlayer insulating film 9 as shown in Fig. 9C, and after silicidation, the metal film 20 on the interlayer insulating film 9 is removed as shown in Fig. 9D, resulting in a state in which a metal silicide layer 10a is formed on the SiC surface. In addition, since the gate wiring layer 31 is covered with the interlayer insulating film 9, it remains covered with the interlayer insulating film 9 even after the metal film 20 thereon is removed.

[0057] Then, a photolithography process for the gate wiring portion shown in FIG. 8 is performed. Specifically, in the photolithography process, a mask (not shown) having an opening at a position corresponding to the gate wiring layer 31 is formed, and then etching is performed to open a gate contact hole 9a connected to the gate wiring layer 31 in the interlayer insulating film 9 as shown in FIG. 9E. Next, a process for forming a barrier metal 10b shown in FIG. 8 is performed. For example, the barrier metal 10b is formed by sputtering Ti and TiN in order. At this time, as shown in FIG. 9F, since the gate contact hole 9a is formed, the barrier metal 10b is formed so as to contact the gate wiring layer 31 as well.

[0058] 8, a metal silicide is also formed at the contact portion between the gate wiring layer 31 and the barrier metal 10b to form an ohmic contact layer. For example, the heat treatment is performed at 600 to 800°C, for example, 700°C. This allows the metal constituting the barrier metal 10b and the polysilicon constituting the gate wiring layer 31 to undergo a silicidation reaction to form a metal silicide layer. This allows, for example, Ti to be used both for forming the barrier metal 10b and for forming the ohmic contact layer with the gate wiring layer 31.

[0059] Moreover, the barrier properties of TiN can be improved by oxidizing or annealing it. Therefore, when TiN is used as the barrier metal 10b, it is preferable to expose the sample to the atmosphere after forming the TiN film to oxidize the TiN. If the sample is exposed to the atmosphere during oxidation, oxidation can be achieved without increasing the process cost. Furthermore, the above-mentioned heat treatment serves as an annealing treatment of TiN. These methods also make it possible to improve the barrier properties of TiN.

[0060] Thereafter, the step of forming the electrode layer 10c shown in Fig. 8 is performed by sputtering, for example, AlSi. As a result, the electrode layer 10c is formed on the barrier metal 10b, as shown in Fig. 9G. Then, the electrode layer 10c and the barrier metal 10b are patterned using a mask not shown, thereby forming the source electrode 10 and a gate wiring portion including the gate wiring layer 31 and the barrier metal 10b and electrode layer 10c in contact therewith.

[0061] Finally, + Then, processes such as forming a drain electrode 11 are performed on the back surface of the mold substrate 1. In this way, the SiC semiconductor device according to this embodiment having the vertical MOSFET and the gate wiring portion is completed.

[0062] As described above, the gate wiring portion can be configured using the barrier metal 10b and electrode layer 10c used in forming the source electrode 10 in the vertical MOSFET. If the barrier metal 10b is made of a metal that undergoes a silicidation reaction, an ohmic contact layer can be obtained by performing a heat treatment. If the barrier metal 10b is made of TiN, the barrier properties can be improved by exposure to air or heat treatment.

[0063] (Other embodiments) Although the present disclosure has been described based on the above-described embodiment, it is not limited to the embodiment, and includes various modifications and modifications within the equivalent range. In addition, various combinations and forms, and other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure.

[0064] (1) For example, in the above embodiment, an example of a vertical MOSFET having a trench gate structure has been described, but of course, other configurations may be provided based on the above vertical MOSFET as a basic structure. For example, various structures may be provided, such as a structure in which a p-type deep layer is provided below the trench gate structure to suppress the equipotential line from rising up to the trench gate structure and improve the breakdown voltage.

[0065] (2) In addition, in each of the above embodiments, a metal silicide layer 10a is formed as a metal layer on the SiC surface, and a barrier metal 10bb and an electrode layer 10c are sequentially disposed on the metal silicide layer 10a. However, a metal other than the metal silicide layer 10a may be disposed as the metal layer.

[0066] (3) In addition, in the above embodiments, an n-channel type vertical MOSFET in which the first conductivity type is n-type and the second conductivity type is p-type has been described as an example, but a p-channel type vertical MOSFET in which the conductivity types of each component are inverted may also be used. In the above description, a vertical MOSFET has been described as an example of a semiconductor element having a trench gate structure, but the present invention can also be applied to an IGBT having a similar trench gate structure. In the case of an n-channel type IGBT, the following can be applied to the above embodiments: + The only difference is that the conductivity type of the substrate 1 is changed from n-type to p-type, and the other structures and manufacturing methods are the same as those of the above-mentioned embodiments. [Explanation of symbols]

[0067] 1...n + Type board, 2...n - 3…p-type drift layer, 4…p-type base region 3a...p-type contact region, 4...n+ 6...gate trench 7...gate insulating film, 8...gate electrode, 9...interlayer insulating film, 10...source electrode 10a...metal silicide layer, 10b, 10ba, 10bb...barrier metal 10bc...protrusion, 10c...electrode layer, 11...drain electrode, 12...recess, 20...polysilicon film, 31...gate wiring layer

Claims

1. A silicon carbide semiconductor device having a semiconductor element with a trench gate structure, A substrate (1) of a first or second conductivity type made of silicon carbide; A drift layer (2) of a first conductivity type formed on the substrate and having a lower impurity concentration than the substrate; A second conductivity type channel layer (3) formed on the drift layer and having a contact region (3 a) formed on a surface layer portion thereof; a first conductivity type region (4) formed at a position different from the contact region on the channel layer and having a first conductivity type impurity concentration higher than that of the drift layer; the trench gate structure including a gate insulating film (7) formed on an inner wall surface of a gate trench (6) penetrating the first conductive type region and the channel layer, and a gate electrode (8) formed on the gate insulating film; an interlayer insulating film (9) covering the gate electrode in the gate trench; a first electrode (10) electrically connected to the contact region and the first conductivity type region; A second electrode (11) formed on the back side of the substrate, A recess (12) is formed by forming a step between an upper surface of the interlayer insulating film and an upper surface of the first conductivity type region, the first electrode has a metal layer (10a) formed on a surface of the contact region and the first conductivity type region, a barrier metal (10b) formed on the metal layer and in the recess, and an electrode layer (10c) formed on the barrier metal, a step is formed between a first barrier metal (10ba) formed in the recess and a second barrier metal (10bb) formed on the metal layer, the second barrier metal has a protrusion (10bc) protruding toward an inner side in a width direction of the gate trench, and a part of the electrode layer extends below the protrusion, and a dimension (W1) between tips of the protrusions on both sides in the width direction of the gate trench is narrower than a dimension (W2) of a portion into which the electrode layer extends below the protrusion.

2. The silicon carbide semiconductor device according to claim 1 , wherein said metal layer is a metal silicide layer (10a).

3. The first barrier metal and the second barrier metal are separated from each other, 3 . The silicon carbide semiconductor device according to claim 1 , wherein a depth (D1) of said recess is larger than a thickness (D2) of said first barrier metal. 4 .

4. The first barrier metal and the second barrier metal are connected to each other, 3. The silicon carbide semiconductor device according to claim 1, wherein the metal layer is formed on an end of the protrusion such that a dimension between tips of the protrusions on both sides in a width direction of the gate trench is narrower than a dimension of a portion into which the electrode layer enters below the protrusion.

5. 5. The silicon carbide semiconductor device according to claim 1, wherein said barrier metal is composed of either Ti or TiN, or has a laminated structure of both.

Citation Information

Patent Citations

  • Vertical gate semiconductor device and its manufacturing method

    JP2005116649A

  • Semiconductor device

    JP2006229181A

  • Semiconductor device and method of manufacturing the same

    JP2019003967A

  • Switching element and manufacturing method therefor

    JP2019186458A

  • Semiconductor device including air-gap

    US20180083099A1