Chemical-resistant protective film-forming composition containing a polymer having a hydroxyaryl group terminal
A protective film-forming composition with a diepoxy compound and proton-generating compound addresses masking and etching rate challenges, ensuring effective wet etching resistance and planarization for semiconductor substrates.
Patent Information
- Application Number
- JP2021513697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-11
- Filing Date
- 2020-04-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-04-09
AI Technical Summary
Existing protective films for semiconductor substrates during lithography processes face challenges in providing adequate masking against wet etching solutions, high etching rates for removal, and maintaining film thickness uniformity on stepped substrates.
A protective film-forming composition comprising a reaction product of a diepoxy compound and a proton-generating compound with specific functional groups, along with an organic solvent, crosslinking agents, and optional catalysts, to create a film with balanced masking, high etching rates, and planarization properties.
The composition achieves effective masking against wet etching solutions, high dry etching rates, and excellent planarization, facilitating easy microfabrication of semiconductor substrates.
Smart Images

Figure 0007563379000001 
Figure 0007563379000002 
Figure 0007563379000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for forming a protective film having excellent resistance to a wet etching solution for semiconductors in a lithography process in semiconductor manufacturing, and also to a method for manufacturing a substrate having a resist pattern to which the protective film is applied, and a method for manufacturing a semiconductor device. [Background technology]
[0002] In semiconductor manufacturing, a lithography process is widely known in which a resist underlayer film is provided between a substrate and a resist film formed thereon to form a resist pattern of a desired shape. After forming the resist pattern, the substrate is processed, and dry etching is mainly used as the process, but wet etching may be used depending on the type of substrate. Patent Document 1 discloses a protective film-forming composition for a basic hydrogen peroxide aqueous solution containing a specific crosslinking agent. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 191767 Summary of the Invention [Problem to be solved by the invention]
[0004] When the resist underlayer film is used as an etching mask to process the underlying substrate by wet etching, the resist underlayer film is required to have good masking function against the wet etching solution during processing of the underlying substrate (i.e., the masked portion can protect the substrate). In such a case, the resist underlayer film is used as a protective film for the substrate. Furthermore, when the unnecessary protective film is to be removed by dry etching after the wet etching, the protective film is required to have a high etching speed (high etching rate) so that it can be quickly removed by dry etching without damaging the underlying substrate. Furthermore, there is a demand for a protective film-forming composition that has good coverage even on so-called uneven substrates, has a small difference in film thickness after filling, and is capable of forming a flat film. In the past, a method of adding a low molecular weight compound (e.g., gallic acid) as an additive was used to impart resistance to SC-1 (ammonia-hydrogen peroxide solution), a type of wet etching chemical, but this had limitations in solving the above problems.
[0005] An object of the present invention is to solve the above problems. [Means for solving the problem]
[0006] The present invention encompasses the following: [1] The reaction product (P) of the diepoxy compound (B) and the di- or higher functional proton generating compound (C) is represented by the following formula (1):
[0007] [ka]
[0008] (in formula (1), Ar represents an aryl group having 6 to 40 carbon atoms, n represents an integer of 2 to 10, -Y- represents -OCO-, -O- or -S-, and * represents a bond to the molecular terminal of the reaction product (P), The composition for forming a protective film against a wet etching solution for semiconductors further comprises an organic solvent (S). [2] The protective film-forming composition according to [1], wherein the bifunctional or higher functional proton-generating compound (C) has a functional group selected from a hydroxyl group, a carboxyl group, a thiol group, an amino group, and an imide group. [3] The protective film-forming composition according to [1], wherein the di- or higher functional proton-generating compound (C) is an acid dianhydride. [4] The reaction product (P) is represented by the following formula (2):
[0009] [ka]
[0010] (In formula (2), Q1 and Q2 represent a divalent organic group, and A1 to A6 represent a hydrogen atom, a methyl group, or an ethyl group.) The protective film-forming composition according to any one of [1] to [3], comprising a unit structure represented by the following formula: [5]
[0011] Q1 in the formula (2) is represented by the following formula (3): [ka]
[0012] (In formula (3), R2 represents a direct bond, an alkylene group having 1 to 10 carbon atoms which may be interrupted by -O-, -S- or -SS-, an alkenylene group having 2 to 6 carbon atoms, or a divalent organic group having at least one alicyclic hydrocarbon ring having 3 to 10 carbon atoms or an aromatic hydrocarbon ring having 6 to 14 carbon atoms, and the divalent organic group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a halogen atom, a hydroxy group, a nitro group, a cyano group, a methylidene group, an alkoxy group having 1 to 6 carbon atoms, an alkoxycarbonyl group having 2 to 6 carbon atoms, and an alkylthio group having 1 to 6 carbon atoms. Z1 and Z1 each represent -COO-, -OCO-, -O-, or -S-.) The protective film-forming composition according to claim 4, represented by the formula: [6] Q2 in the formula (2) is the following formula (4):
[0013] [ka]
[0014] In the above formula (4), R1 is a direct bond or an alkylene group having 1 to 5 carbon atoms, n1 and m are integers of 0 or 1, and Z2 is represented by the following formula (5), formula (6) or formula (7):
[0015] [ka]
[0016] (In the above formula (6), X is represented by the following formula (8), formula (9), or formula (10):
[0017] [ka]
[0018] (In formula (8), formula (9) and formula (10), R 11 , R 12 , R 13 , R 14 and R 15 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, the phenyl group being optionally substituted with at least one selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, a nitro group, a cyano group, an alkoxy group having 1 to 6 carbon atoms, and an alkylthio group having 1 to 6 carbon atoms; R 13 and R 14 may be bonded to each other to form a ring having 3 to 6 carbon atoms. [7] The protective film-forming composition according to any one of [1] to [6], wherein the Ar includes a benzene, naphthalene, or anthracene structure. [8] The protective film-forming composition according to any one of [1] to [7], wherein n is an integer of 2 to 4. [9] The protective film-forming composition according to any one of [1] to [8], further comprising a crosslinking agent (K).
[10] The crosslinking agent (K) is represented by the following formula (11) or formula (12):
[0019] [ka]
[0020] (In formula (11) and formula (12), Q 2 R represents a single bond or a divalent organic group. 8 , R 9 , R 11 and R 12 each represents a hydrogen atom or a methyl group, and R 7 and R 10 respectively represent an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. n9 indicates an integer satisfying 1≦n9≦3, n10 indicates an integer satisfying 2≦n10≦5, n11 indicates an integer satisfying 0≦n11≦3, n12 indicates an integer satisfying 0≦n12≦3, and 3≦(n9+n10+n11+n12)≦6. n13 is an integer of 1≦n13≦3, n14 is an integer of 1≦n14≦4, n15 is an integer of 0≦n15≦3, n16 is an integer of 0≦n16≦3, and 2≦(n13+n14+n15+n16)≦5. m2 is an integer of 2 to 10. The protective film-forming composition according to [9], wherein the compound is selected from the group consisting of a compound represented by the formula (I) and a melamine compound, a guanamine compound, a glycoluril compound, and a urea compound.
[11] The protective film-forming composition according to any one of [1] to
[10] , further comprising a crosslinking catalyst.
[12] The protective film-forming composition according to any one of [1] to
[11] , further comprising a surfactant.
[13] A protective film, which is a fired product of a coating film made of the protective film-forming composition according to any one of [1] to
[13] .
[14] A method for producing a substrate having a resist pattern, comprising the steps of applying the protective film composition according to any one of [1] to
[13] onto a semiconductor substrate and baking the composition to form a protective film as a resist underlayer film, forming a resist film on the protective film, and then exposing and developing the resist film to form a resist pattern, the method being used in the production of semiconductors.
[15] A method for manufacturing a semiconductor device, comprising the steps of forming a protective film on a semiconductor substrate, on whose surface an inorganic film may be formed, using the protective film-forming composition according to any one of [1] to
[13] , forming a resist pattern on the protective film, dry-etching the protective film using the resist pattern as a mask to expose a surface of the inorganic film or the semiconductor substrate, and wet-etching and cleaning the inorganic film or the semiconductor substrate using a semiconductor wet etching solution using the protective film after the dry etching as a mask. Effect of the Invention
[0021] The protective film-forming composition of the present invention is required to have, for example, the following properties in a well-balanced manner in the lithography process in semiconductor manufacturing: (1) good masking function against a wet etching solution during processing of the base substrate, (2) high dry etching rate, and (3) excellent planarization ability for uneven substrates. By having a good balance of the properties (1) to (3), fine processing of semiconductor substrates can be easily performed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] <Terminology explanation> The terms used in the present invention have the following definitions unless otherwise specified.
[0023] Examples of the "alkylene group having 1 to 10 carbon atoms" include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, a cyclopropylene group, an n-butylene group, an isobutylene group, an s-butylene group, a t-butylene group, a cyclobutylene group, a 1-methyl-cyclopropylene group, a 2-methyl-cyclopropylene group, an n-pentylene group, a 1-methyl-n-butylene group, a 2-methyl-n-butylene group, a 3-methyl-n-butylene group, a 1,1-dimethyl-n-propylene group, a 1,2-dimethyl-n-propylene group, a 2,2-dimethyl-n-propylene group, a 1-ethyl-n- Propylene, cyclopentylene, 1-methyl-cyclobutylene, 2-methyl-cyclobutylene, 3-methyl-cyclobutylene, 1,2-dimethyl-cyclopropylene, 2,3-dimethyl-cyclopropylene, 1-ethyl-cyclopropylene, 2-ethyl-cyclopropylene, n-hexylene, 1-methyl-n-pentylene, 2-methyl-n-pentylene, 3-methyl-n-pentylene, 4-methyl-n-pentylene, 1,1-dimethyl-n-butylene, 1,2-dimethyl-n-butylene, 1,3-dimethyl-n-butylene group, 2,2-dimethyl-n-butylene group, 2,3-dimethyl-n-butylene group, 3,3-dimethyl-n-butylene group, 1-ethyl-n-butylene group, 2-ethyl-n-butylene group, 1,1,2-trimethyl-n-propylene group, 1,2,2-trimethyl-n-propylene group, 1-ethyl-1-methyl-n-propylene group, 1-ethyl-2-methyl-n-propylene group, cyclohexylene group, 1-methyl-cyclopentylene group, 2-methyl-cyclopentylene group, 3-methyl-cyclopentylene group, 1-ethyl-cyclobutylene group, 2-ethyl-cyclobutylene group cyclobutylene, 3-ethyl-cyclobutylene, 1,2-dimethyl-cyclobutylene, 1,3-dimethyl-cyclobutylene, 2,2-dimethyl-cyclobutylene, 2,3-dimethyl-cyclobutylene, 2,4-dimethyl-cyclobutylene, 3,3-dimethyl-cyclobutylene, 1-n-propyl-cyclopropylene, 2-n-propyl-cyclopropylene, 1-isopropyl-cyclopropylene, 2-isopropyl-cyclopropylene, 1,2,2-trimethyl-cyclopropylene, 1,2,3-trimethyl-cyclopropylene, 2,2,Examples of the cyclopropylene group include a 3-trimethyl-cyclopropylene group, a 1-ethyl-2-methyl-cyclopropylene group, a 2-ethyl-1-methyl-cyclopropylene group, a 2-ethyl-2-methyl-cyclopropylene group, a 2-ethyl-3-methyl-cyclopropylene group, an n-heptylene group, an n-octylene group, an n-nonylene group, and an n-decanylene group.
[0024] Examples of the "alkyl group having 1 to 10 carbon atoms" include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclopropyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, cyclopentyl, 1-methylcyclobutyl, 2-methylcyclobutyl, 3-methylcyclobutyl, 1,2-dimethylcyclopropyl, 2,3-dimethylcyclopropyl, 1-ethylcyclopropyl, 2-ethylcyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2, 2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-i-propyl-cyclopropyl, 2-i-propyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,Examples of the cyclopropyl group include 3-trimethyl-cyclopropyl group, 1-ethyl-2-methyl-cyclopropyl group, 2-ethyl-1-methyl-cyclopropyl group, 2-ethyl-2-methyl-cyclopropyl group, 2-ethyl-3-methyl-cyclopropyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, pentadecyl group, hexadecyl group, heptadecyl group, octadecyl group, nonadecyl group, and icodecyl group.
[0025] Examples of the "aryl group having 6 to 40 carbon atoms" include a phenyl group, an o-methylphenyl group, a m-methylphenyl group, a p-methylphenyl group, an o-chlorophenyl group, a m-chlorophenyl group, a p-chlorophenyl group, an o-fluorophenyl group, a p-fluorophenyl group, an o-methoxyphenyl group, a p-methoxyphenyl group, a p-nitrophenyl group, a p-cyanophenyl group, an α-naphthyl group, a β-naphthyl group, an o-biphenylyl group, a m-biphenylyl group, a p-biphenylyl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, and a 9-phenanthryl group.
[0026] Examples of the "alkenyl group having 2 to 10 carbon atoms" include ethenyl group, 1-propenyl group, 2-propenyl group, 1-methyl-1-ethenyl group, 1-butenyl group, 2-butenyl group, 3-butenyl group, 2-methyl-1-propenyl group, 2-methyl-2-propenyl group, 1-ethylethenyl group, 1-methyl-1-propenyl group, 1-methyl-2-propenyl group, 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group, 1-n-propylethenyl group, 1-methyl-1-butenyl group, 1-methyl-2-butenyl group, 1-methyl-3-butenyl group, 2 -ethyl-2-propenyl group, 2-methyl-1-butenyl group, 2-methyl-2-butenyl group, 2-methyl-3-butenyl group, 3-methyl-1-butenyl group, 3-methyl-2-butenyl group, 3-methyl-3-butenyl group, 1,1-dimethyl-2-propenyl group, 1-i-propylethenyl group, 1,2-dimethyl-1-propenyl group, 1,2-dimethyl-2-propenyl group, 1-cyclopentenyl group, 2-cyclopentenyl group, 3-cyclopentenyl group, 1-hexenyl group, 2-hexenyl group, 3-hexenyl group, 4-hexenyl group, 5-hexenyl group, 1-methyl-2-propenyl group, 1-methyl-2-propenyl group, 1-methyl-2-propenyl group, 1-methyl-2-propenyl group, 1-methyl-2-propenyl group, 1-methyl-2-propenyl group, ethyl-1-pentenyl, 1-methyl-2-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-n-butylethenyl, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 2-methyl-4-pentenyl, 2-n-propyl-2-propenyl, 3-methyl-1-pentenyl, 3-methyl-2-pentenyl, 3-methyl-3-pentenyl, 3-methyl-4-pentenyl, 3-ethyl-3-butenyl, 4-methyl-1-pentenyl, 4-methyl-2-pentenyl group, 4-methyl-3-pentenyl group, 4-methyl-4-pentenyl group, 1,1-dimethyl-2-butenyl group, 1,1-dimethyl-3-butenyl group, 1,2-dimethyl-1-butenyl group, 1,2-dimethyl-2-butenyl group, 1,2-dimethyl-3-butenyl group, 1-methyl-2-ethyl-2-propenyl group, 1-s-butylethenyl group, 1,3-dimethyl-1-butenyl group, 1,3-dimethyl-2-butenyl group, 1,3-dimethyl-3-butenyl group, 1-i-butylethenyl group, 2,2-dimethyl-3-butenyl group, 2,3-dimethyl-1-butenyl group, 2,3-dimethyl-2-butenyl group, 2,3-dimethyl-3-butenyl group, 2-i-propyl-2-propenyl group, 3,3-dimethyl-1-butenyl group, 1-ethyl-1-butenyl group, 1-ethyl-2-butenyl group, 1-ethyl-3-butenyl group, 1-n-propyl-1-propenyl group, 1-n-propyl-2-propenyl group, 2-ethyl-1-butenyl group, 2-ethyl-2-butenyl group, 2-ethyl-3-butenyl group, 1,1,2-trimethyl-2-propenyl group, 1-t-butylethenyl group, 1-methyl-1-ethyl-2-propenyl group, 1-ethyl-2-methyl-1-propenyl group, 1-ethyl-2-methyl-2-propenyl group, 1-i-propyl-1-propenyl group, 1-i- Propyl-2-propenyl group, 1-methyl-2-cyclopentenyl group, 1-methyl-3-cyclopentenyl group, 2-methyl-1-cyclopentenyl group, 2-methyl-2-cyclopentenyl group, 2-methyl-3-cyclopentenyl group, 2-methyl-4-cyclopentenyl group, 2-methyl-5-cyclopentenyl group, 2-methylene-cyclopentyl group, 3-methyl-1-cyclopentenyl group, 3-methyl-2-cyclopentenyl group, 3-methyl-3-cyclopentenyl group, 3-methyl-4-cyclopentenyl group, 3-methyl-5-cyclopentenyl group, 3-methylene-cyclopentyl group, 1-cyclohexenyl group, 2-cyclohexenyl group, and 3-cyclohexenyl group.
[0027] The "alkenylene group having 2 to 6 carbon atoms" refers to an alkenyl group having 2 to 6 carbon atoms, as defined above in the "alkenyl group having 2 to 10 carbon atoms", which has been divalently formed by removing one hydrogen atom.
[0028] Examples of the "alicyclic hydrocarbon ring having 3 to 10 carbon atoms" include cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, spiro-bicyclopentane, bicyclo[2.1.0]pentane, bicyclo[3.2.1]octane, tricyclo[3.2.1.0]cyclopent ... 2,7 ]octane, spiro[3,4]octane, etc.
[0029] The "aromatic hydrocarbon ring having 6 to 14 carbon atoms" refers to those having an aromatic hydrocarbon ring having 6 to 14 carbon atoms among the above-mentioned "aryl groups having 6 to 40 carbon atoms".
[0030] The "alkynyl group having 2 to 6 carbon atoms" refers to a group in which the double bond in the alkenyl group having 2 to 6 carbon atoms in the above "alkenyl group having 2 to 10 carbon atoms" is replaced with a triple bond.
[0031] Examples of the "alkoxy group having 1 to 20 carbon atoms" include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentyloxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, an n-hexyloxy group, a 1-methyl-n-pentyloxy group, a 2-methyl-n-pentyloxy group, a 3-methyl-n-pentyloxy group, a 4-methyl-n-pentyloxy group, a 1,1-dimethyl-n-butoxy group, a 1, Examples of such aryloxy groups include a 2-dimethyl-n-butoxy group, a 1,3-dimethyl-n-butoxy group, a 2,2-dimethyl-n-butoxy group, a 2,3-dimethyl-n-butoxy group, a 3,3-dimethyl-n-butoxy group, a 1-ethyl-n-butoxy group, a 2-ethyl-n-butoxy group, a 1,1,2-trimethyl-n-propoxy group, a 1,2,2-trimethyl-n-propoxy group, a 1-ethyl-1-methyl-n-propoxy group, a 1-ethyl-2-methyl-n-propoxy group, a cyclopentyloxy group, a cyclohexyloxy group, a norbornyoxy group, an adamantyloxy group, an adamantanemethyloxy group, an adamantaneethyloxy group, a tetracyclodecanyloxy group, and a tricyclodecanyloxy group.
[0032] Examples of the "alkoxycarbonyl group having 1 to 6 carbon atoms" include a methoxycarbonyl group, an ethoxycarbonyl group, and an isopropoxycarbonyl group.
[0033] Examples of the "alkylthio group having 1 to 6 carbon atoms" include a methylthio group, an ethylthio group, a propylthio group, a butylthio group, a pentylthio group, and a hexylthio group. The term "halogen atom" includes a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0034] <Protective film forming composition> The protective film-forming composition of the present application contains a reaction product (P) of a diepoxy compound (B) and a difunctional or higher proton-generating compound (C), and the reaction product (P) has a group represented by the following formula (1) at its terminal:
[0035] [ka]
[0036] (in formula (1), Ar represents an aryl group having 6 to 40 carbon atoms, n represents an integer of 2 to 10, -Y- represents -OCO-, -O- or -S-, and * represents a bond to the molecular terminal of the reaction product (P), The composition for forming a protective film against a wet etching solution for semiconductors further contains an organic solvent (S). The functional group possessed by the bifunctional or higher functional proton-generating compound (C) is a functional group that generates a proton, and specifically, is preferably selected from a hydroxyl group, a carboxyl group, a thiol group, an amino group, and an imide group. The di- or higher functional proton-generating compound (C) may be an acid dianhydride. The protective film-forming composition of the present application is a reaction product (P) of a diepoxy compound (B) and a difunctional or higher proton-generating compound (C); the reaction product (P) of a diepoxy compound (B) and a difunctional, trifunctional or tetrafunctional proton-generating compound (C) is preferred, the reaction product (P) of a diepoxy compound (B) and a difunctional or trifunctional proton-generating compound (C) is preferred, and the reaction product (P) of a diepoxy compound (B) and a difunctional proton-generating compound (C) is preferred. The reaction product (P) is represented by the following formula (2):
[0037] [ka]
[0038] (In formula (4), Q1 and Q2 represent a divalent organic group, and A1 to A6 represent a hydrogen atom, a methyl group, or an ethyl group.) It is preferable that the copolymer contains a unit structure represented by the following formula: Q1 in the formula (2) is represented by the following formula (3):
[0039] [ka]
[0040] (In formula (3), R2 represents a direct bond, an alkylene group having 1 to 10 carbon atoms which may be interrupted by -O-, -S- or -SS-, an alkenylene group having 2 to 6 carbon atoms, or a divalent organic group having at least one alicyclic hydrocarbon ring having 3 to 10 carbon atoms or an aromatic hydrocarbon ring having 6 to 14 carbon atoms, and the divalent organic group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a halogen atom, a hydroxy group, a nitro group, a cyano group, a methylidene group, an alkoxy group having 1 to 6 carbon atoms, an alkoxycarbonyl group having 2 to 6 carbon atoms, and an alkylthio group having 1 to 6 carbon atoms. Z1 and Z1 each represent -COO-, -OCO-, -O-, or -S-.) It is preferable that the formula is represented by the formula: Q2 in the formula (2) is the following formula (4):
[0041] [ka]
[0042] In the above formula (4), R1 is a direct bond or an alkylene group having 1 to 5 carbon atoms, n1 and m are integers of 0 or 1, and Z2 is represented by the following formula (5), formula (6) or formula (7):
[0043] [ka]
[0044] (In the above formula (6), X is represented by the following formula (8), formula (9), or formula (10):
[0045] [ka]
[0046] (In formula (8), formula (9) and formula (10), R 11 , R 12 , R 13 , R 14 and R 15 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, the phenyl group being optionally substituted with at least one selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, a nitro group, a cyano group, an alkoxy group having 1 to 6 carbon atoms, and an alkylthio group having 1 to 6 carbon atoms; R 13 and R 14 may be bonded to each other to form a ring having 3 to 6 carbon atoms. The above "ring having 3 to 6 carbon atoms" includes cyclopropane, cyclobutane, cyclopentane, cyclopentadiene and cyclohexane. It is preferable that the Ar includes a benzene, naphthalene, or anthracene structure. The above n is preferably an integer of 2 to 4.
[0047] Specific examples of the diepoxy compound (B) of the present application include the following compounds (a-1) to (a-24).
[0048] [ka]
[0049] [ka]
[0050] Specific examples of the di- or higher functional proton-generating compound (C) of the present application include the following compounds (b-1) to (b-27).
[0051] [ka]
[0052] The protective film-forming composition of the present application comprises the diepoxy compound (B), the bifunctional or higher proton-generating compound (C), and the compounds (c-1) to (c-2) exemplified below. 17 ) may be a reaction product (P) prepared by reacting
[0053] [ka]
[0054] The protective film-forming composition of the present application may further contain a crosslinking agent (K). The crosslinking agent (K) is represented by the following formula (11) or formula (12):
[0055] [ka]
[0056] (In formula (11) and formula (12), Q 2 R represents a single bond or a divalent organic group. 8 , R 9 , R 11 and R 12 each represents a hydrogen atom or a methyl group, and R 7 and R 10 respectively represent an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. n9 indicates an integer satisfying 1≦n9≦3, n10 indicates an integer satisfying 2≦n10≦5, n11 indicates an integer satisfying 0≦n11≦3, n12 indicates an integer satisfying 0≦n12≦3, and 3≦(n9+n10+n11+n12)≦6. n13 is an integer of 1≦n13≦3, n14 is an integer of 1≦n14≦4, n15 is an integer of 0≦n15≦3, n16 is an integer of 0≦n16≦3, and 2≦(n13+n14+n15+n16)≦5. m2 is an integer of 2 to 10. The compound may be a compound selected from the compounds described in WO2014 / 208542 represented by the formula:
[0057] Specific examples of the melamine compound include, but are not limited to, hexamethylol melamine, hexamethoxymethyl melamine, a compound in which 1 to 6 methylol groups of hexamethylol melamine are methoxymethylated or a mixture thereof, hexamethoxyethyl melamine, hexaacyloxymethyl melamine, a compound in which 1 to 6 methylol groups of hexamethylol melamine are acyloxymethylated or a mixture thereof, etc. Specific examples of the epoxy compound include, for example, tris(2,3-epoxypropyl)isocyanurate, trimethylolmethane triglycidyl ether, trimethylolpropane triglycidyl ether, triethylolethane triglycidyl ether, etc.
[0058] Specific examples of the guanamine compound include, but are not limited to, tetramethylol guanamine, tetramethoxymethyl guanamine, a compound in which one to four methylol groups of tetramethylol guanamine are methoxymethylated or a mixture thereof, tetramethoxyethyl guanamine, tetraacyloxyguanamine, a compound in which one to four methylol groups of tetramethylol guanamine are acyloxymethylated or a mixture thereof, and the like. Specific examples of glycoluril compounds include tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, a compound in which one to four methylol groups of tetramethylol glycoluril are methoxymethylated or a mixture thereof, a compound in which one to four methylol groups of tetramethylol glycoluril are acyloxymethylated or a mixture thereof, etc. Specific examples of urea compounds include tetramethylol urea, tetramethoxymethyl urea, a compound in which one to four methylol groups of tetramethylol urea are methoxymethylated or a mixture thereof, tetramethoxyethyl urea, etc.
[0059] Specific examples of the compound containing an alkenyl ether group include, but are not limited to, ethylene glycol divinyl ether, triethylene glycol divinyl ether, 1,2-propanediol divinyl ether, 1,4-butanediol divinyl ether, tetramethylene glycol divinyl ether, neopentyl glycol divinyl ether, trimethylolpropane trivinyl ether, hexanediol divinyl ether, 1,4-cyclohexanediol divinyl ether, pentaerythritol trivinyl ether, pentaerythritol tetravinyl ether, sorbitol tetravinyl ether, sorbitol pentavinyl ether, and trimethylolpropane trivinyl ether.
[0060] Among these, glycoluril compounds are preferred, specifically tetramethylol glycoluril, tetramethoxy glycoluril, tetramethoxymethyl glycoluril, a compound in which one to four methylol groups of tetramethylol glycoluril are methoxymethylated or a mixture thereof, and a compound in which one to four methylol groups of tetramethylol glycoluril are acyloxymethylated or a mixture thereof, with tetramethoxymethyl glycoluril being preferred.
[0061] Further examples of the crosslinking agent (K) include compounds having a partial structure of the following formula (5-1) and polymers or oligomers having a repeating unit of the following formula (5-2).
[0062] [ka]
[0063] Above R 11 , R 12 , R 13 , and R 14 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and the alkyl groups mentioned above can be used.
[0064] m1 is 1≦m1≦6-m2, m2 is 1≦m2≦5, m3 is 1≦m3≦4-m2, and m4 is 1≦m4≦3.
[0065] Examples of the compounds, polymers and oligomers of the formula (5-1) and the formula (5-2) are shown below.
[0066] [ka]
[0067] [ka]
[0068] The above compounds are available as products of Asahi Yukizai Kogyo Co., Ltd. and Honshu Chemical Industry Co., Ltd. For example, among the above crosslinking agents, the compound of formula (6-22) is available from Asahi Yukizai Kogyo Co., Ltd. under the trade name TMOM-BP.
[0069] The amount of the crosslinking agent added varies depending on the coating solvent used, the base substrate used, the required solution viscosity, the required film shape, etc., but is 0.001 to 80 mass %, preferably 0.01 to 50 mass %, and more preferably 0.1 to 40 mass %, based on the total solid content of the protective film-forming composition. These crosslinking agents may cause a crosslinking reaction by self-condensation, but when crosslinkable substituents are present in the above-mentioned polymer of the present invention, they can cause a crosslinking reaction with the crosslinkable substituents.
[0070] [Crosslinking catalyst] The protective film-forming composition of the present invention may contain a crosslinking catalyst as an optional component in order to promote the crosslinking reaction. As the crosslinking catalyst, in addition to an acidic compound or a basic compound, a compound that generates an acid or a base by heat may be used, but a crosslinking acid catalyst is preferable. As the acidic compound, a sulfonic acid compound or a carboxylic acid compound may be used, and as a compound that generates an acid by heat, a thermal acid generator may be used.
[0071] Examples of sulfonic acid compounds or carboxylic acid compounds include p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium trifluoromethanesulfonate (pyridinium trifluoromethanesulfonic acid), pyridinium-p-toluenesulfonate, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-phenolsulfonic acid, pyridinium-4-phenolsulfonate, benzenedisulfonic acid, 1-naphthalenesulfonic acid, 4-nitrobenzenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid.
[0072] Examples of thermal acid generators include K-PURE (registered trademark) CXC-1612, CXC-1614, TAG-2172, TAG-2179, TAG-2678, and TAG2689 (all manufactured by King Industries), and SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (all manufactured by Sanshin Chemical Industry Co., Ltd.).
[0073] These crosslinking catalysts can be used alone or in combination of two or more. As the basic compound, an amine compound or an ammonium hydroxide compound can be used, and as the compound that generates a base by heat, urea can be used.
[0074] Examples of the amine compound include tertiary amines such as triethanolamine, tributanolamine, trimethylamine, triethylamine, tri-normal propylamine, triisopropylamine, tri-normal butylamine, tri-tert-butylamine, tri-normal octylamine, triisopropanolamine, phenyldiethanolamine, stearyldiethanolamine, and diazabicyclooctane, and aromatic amines such as pyridine and 4-dimethylaminopyridine.Other examples of the amine compound include primary amines such as benzylamine and normal butylamine, and secondary amines such as diethylamine and di-normal butylamine.These amine compounds can be used alone or in combination of two or more.
[0075] Examples of ammonium hydroxide compounds include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, benzyltriethylammonium hydroxide, cetyltrimethylammonium hydroxide, phenyltrimethylammonium hydroxide, and phenyltriethylammonium hydroxide.
[0076] As a compound that generates a base by heat, for example, a compound that has a thermolabile group such as an amide group, a urethane group, or an aziridine group and generates an amine by heating can be used. Other examples of the compound that generates a base by heat include urea, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyldimethylphenylammonium chloride, benzyldodecyldimethylammonium chloride, benzyltributylammonium chloride, and choline chloride.
[0077] When the protective film-forming composition contains a crosslinking catalyst, the content thereof is 0.0001 to 20 mass %, preferably 0.01 to 15 mass %, and more preferably 0.1 to 10 mass %, based on the total solid content of the protective film-forming composition.
[0078] [Surfactants] The protective film-forming composition of the present invention may contain a surfactant as an optional component to improve the coating property on the semiconductor substrate. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether, polyoxyethylene-polyoxypropylene block copolymers, sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate ... Examples of suitable surfactants include nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan stearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorosurfactants such as F-TOP (registered trademark) EF301, EF303, and EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Megafac (registered trademark) F171, F173, R-30, R-40, and R-40-LM (manufactured by DIC Corporation), Fluorad FC430 and FC431 (manufactured by Sumitomo 3M Limited), Asahiguard (registered trademark) AG710, Surflon (registered trademark) S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by Asahi Glass Co., Ltd.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). These surfactants can be used alone or in combination of two or more. When the protective film-forming composition contains a surfactant, the content of the surfactant is 0.0001 to 10 mass %, preferably 0.01 to 5 mass %, based on the total solid content of the protective film-forming composition.
[0079] [Organic solvent (S)] The protective film-forming composition of the present invention can be prepared by dissolving the above-mentioned components in an organic solvent (S), and is used in the state of a homogeneous solution.
[0080] The organic solvent (S) of the protective film-forming composition according to the present invention can be any solvent that can dissolve the compound containing at least one pair of two hydroxyl groups adjacent to each other in the molecule, or a polymer thereof. In particular, since the protective film-forming composition according to the present invention is used in a homogeneous solution state, it is recommended to use an organic solvent that is generally used in lithography processes in combination, taking into account its coating performance.
[0081] Examples of the organic solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone. Examples of the solvent include cyclopentane, cycloheptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents can be used alone or in combination of two or more.
[0082] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, cyclohexanone, etc. are preferred, with propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate being particularly preferred.
[0083] [Other ingredients] The protective film-forming composition of the present invention may contain a light absorbing agent, a rheology control agent, an adhesive auxiliary, etc. The rheology control agent is effective in improving the fluidity of the protective film-forming composition. The adhesive auxiliary is effective in improving the adhesion between the semiconductor substrate or resist and the underlayer film.
[0084] Examples of the light absorbing agent include commercially available light absorbing agents described in "Technology and Market of Industrial Dyes" (CMC Publishing) and "Dye Handbook" (edited by the Society of Organic Synthesis Chemistry), such as CI Disperse Yellow 1, 3, 4, 5, 7, 8, 13, 23, 31, 49, 50, 51, 54, 60, 64, 66, 68, 79, 82, 88, 90, 93, 102, 114, and 124; CID isperse Orange 1, 5, 13, 25, 29, 30, 31, 44, 57, 72, and 73; CI Disperse Red 1, 5, 7, 13, 17, 19, 43, 50, 54, 58, 65, 72, 73, 88, 117, 137, 143, 199, and 210; CI Disperse Violet 43; CI Disperse Blue 96; CI Fluorescent Brightening Agent Suitable examples of the light absorbing agent that can be used include CI Solvent Orange 2 and 45, CI Solvent Red 1, 3, 8, 23, 24, 25, 27 and 49, CI Pigment Green 10, and CI Pigment Brown 2. The light absorbing agent is usually blended in an amount of 10% by mass or less, and preferably 5% by mass or less, based on the total solid content of the protective film-forming composition.
[0085] The rheology control agent is mainly added to improve the fluidity of the protective film forming composition, and to improve the uniformity of the thickness of the protective film and the filling ability of the protective film forming composition into the hole, especially in the baking process.Specific examples include phthalic acid derivatives such as dimethyl phthalate, diethyl phthalate, diisobutyl phthalate, dihexyl phthalate, and butyl isodecyl phthalate, adipic acid derivatives such as di-n-butyl adipate, diisobutyl adipate, diisooctyl adipate, and octyl decyl adipate, maleic acid derivatives such as di-n-butyl maleate, diethyl maleate, and dinonyl maleate, oleic acid derivatives such as methyl oleate, butyl oleate, and tetrahydrofurfuryl oleate, and stearic acid derivatives such as normal butyl stearate and glyceryl stearate.These rheology control agents are usually blended at a ratio of less than 30% by mass based on the total solid content of the protective film forming composition.
[0086] The adhesion promoter is added mainly for the purpose of improving the adhesion between the substrate or resist and the protective film-forming composition, and in particular to prevent the resist from peeling off during development. Specific examples include chlorosilanes such as trimethylchlorosilane, dimethylmethylolchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane; alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylmethylolethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole; methyloltrimethylsilane; and methyloltrimethylsilane. Examples of the adhesive auxiliary include silanes such as chlorosilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and γ-glycidoxypropyltrimethoxysilane, heterocyclic compounds such as benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, urazole, thiouracil, mercaptoimidazole, and mercaptopyrimidine, and ureas such as 1,1-dimethylurea and 1,3-dimethylurea, or thiourea compounds. These adhesive auxiliary agents are usually blended in an amount of less than 5% by mass, preferably less than 2% by mass, based on the total solid content of the protective film-forming composition.
[0087] [Protective film forming composition] The solid content of the protective film-forming composition according to the present invention is usually 0.1 to 70% by mass, preferably 0.1 to 60% by mass. The solid content is the content of all components excluding the solvent from the protective film-forming composition. The proportion of the polymer in the solid content is preferably 1 to 100% by mass, 1 to 99.9% by mass, 50 to 99.9% by mass, 50 to 95% by mass, and 50 to 90% by mass, in that order.
[0088] [Method of manufacturing a substrate having a resist pattern and a semiconductor device] Hereinafter, a method for producing a substrate having a resist pattern and a method for producing a semiconductor device using the protective film-forming composition according to the present invention will be described.
[0089] The substrate having a resist pattern according to the present invention can be produced by applying the above-mentioned protective film-forming composition onto a semiconductor substrate and baking it.
[0090] Examples of semiconductor substrates to which the protective film-forming composition of the present invention can be applied include silicon wafers, germanium wafers, and compound semiconductor wafers such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.
[0091] When using a semiconductor substrate with an inorganic film formed on its surface, the inorganic film is formed by, for example, ALD (atomic layer deposition), CVD (chemical vapor deposition), reactive sputtering, ion plating, vacuum deposition, or spin-coating (spin-on glass: SOG). Examples of the inorganic film include polysilicon film, silicon oxide film, silicon nitride film, silicon oxynitride film, BPSG (Boro-Phospho Silicate Glass) film, titanium nitride film, titanium oxynitride film, tungsten nitride film, gallium nitride film, and gallium arsenide film.
[0092] The protective film-forming composition of the present invention is applied onto such a semiconductor substrate by a suitable application method such as a spinner or coater. Then, the protective film is formed by baking using a heating means such as a hot plate. The baking conditions are appropriately selected from a baking temperature of 100° C. to 400° C. and a baking time of 0.3 minutes to 60 minutes. Preferably, the baking temperature is 120° C. to 350° C., the baking time is 0.5 minutes to 30 minutes, and more preferably, the baking temperature is 150° C. to 300° C., and the baking time is 0.8 minutes to 10 minutes. The thickness of the protective film formed is, for example, 0.001 μm to 10 μm, preferably 0.002 μm to 1 μm, and more preferably 0.005 μm to 0.5 μm. If the baking temperature is lower than the above range, crosslinking becomes insufficient, and the formed protective film may not be resistant to a resist solvent or a basic hydrogen peroxide aqueous solution. On the other hand, if the baking temperature is higher than the above range, the protective film may be decomposed by heat.
[0093] Exposure is performed through a mask (reticle) for forming a predetermined pattern, and for example, i-rays, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet) or EB (electron beam) is used. An alkaline developer is used for development, and the development temperature is appropriately selected from 5°C to 50°C and the development time is appropriately selected from 10 seconds to 300 seconds. As the alkaline developer, for example, aqueous solutions of alkalines such as inorganic alkalines such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and ammonia water, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-butylamine, tertiary amines such as triethylamine and methyldiethylamine, alcohol amines such as dimethylethanolamine and triethanolamine, quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline, cyclic amines such as pyrrole and piperidine, etc. can be used. Furthermore, an appropriate amount of alcohols such as isopropyl alcohol and surfactants such as nonionic surfactants can be added to the aqueous solutions of the alkalines. Among these, the preferred developer is a quaternary ammonium salt, more preferably tetramethylammonium hydroxide and choline. Furthermore, a surfactant or the like can be added to these developers. Instead of the alkaline developer, a method can be used in which development is performed with an organic solvent such as butyl acetate to develop the part of the photoresist where the alkaline dissolution rate is not improved.
[0094] Next, the protective film is dry-etched using the formed resist pattern as a mask, whereby if the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed, and if the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed.
[0095] Furthermore, the protective film after dry etching (and the resist pattern if any remains on the protective film) is used as a mask to perform wet etching using a wet etching solution for semiconductors, thereby forming a desired pattern.
[0096] As the semiconductor wet etching solution, a general chemical solution for etching semiconductor wafers can be used, and for example, either an acidic substance or a basic substance can be used.
[0097] Examples of substances that exhibit acidity include hydrogen peroxide, hydrofluoric acid, ammonium fluoride, acidic ammonium fluoride, ammonium hydrogen fluoride, buffered hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, and mixtures of these.
[0098] Examples of substances that exhibit basicity include basic hydrogen peroxide solution, which is obtained by mixing an organic amine such as ammonia, sodium hydroxide, potassium hydroxide, sodium cyanide, potassium cyanide, or triethanolamine with hydrogen peroxide solution to make the pH basic. A specific example is SC-1 (ammonia-hydrogen peroxide solution). Other substances that can make the pH basic, such as mixing urea with hydrogen peroxide solution and heating to cause thermal decomposition of the urea to generate ammonia, and finally making the pH basic, can also be used as a wet etching chemical.
[0099] Among these, acidic hydrogen peroxide solution or basic hydrogen peroxide solution is preferable.
[0100] These chemical solutions may contain additives such as a surfactant.
[0101] The temperature at which the semiconductor wet etching solution is used is preferably 25° C. to 90° C., and more preferably 40° C. to 80° C. The wet etching time is preferably 0.5 to 30 minutes, and more preferably 1 to 20 minutes. EXAMPLES
[0102] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these. The weight average molecular weights of the polymers shown in Synthesis Examples 1 to 4 below in this specification are the results of measurement by gel permeation chromatography (hereinafter abbreviated as GPC). For the measurement, a GPC device manufactured by Tosoh Corporation was used, and the measurement conditions etc. are as follows. GPC column: Shodex KF803L, Shodex KF802, Shodex KF801 (registered trademark) (Showa Denko K.K.) Column temperature: 40℃ Solvent: Tetrahydrofuran (THF) Flow rate: 1.0ml / min Standard sample: Polystyrene (manufactured by Tosoh Corporation)
[0103] <Synthesis Example 1> 20.00 g of monoallyl diglycidyl isocyanurate (manufactured by Shikoku Chemical Industry Co., Ltd., product name MA-DGIC), 12.69 g of 3,3'-dithiodipropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., product name: DTDPA), 4.22 g of gallic acid hydrate, and 1.81 g of tetrabutylphosphonium bromide as a catalyst were dissolved in 58.09 g of propylene glycol monomethyl ether, and then reacted at 105°C for 24 hours to obtain a solution containing a reaction product (solid content 40% by mass). The repeating unit and terminal structure of the obtained reaction product are represented by formula (D-1). When the obtained reaction product was subjected to GPC analysis, it was found to have a weight average molecular weight of 3100 in terms of standard polystyrene.
[0104] [ka]
[0105] <Synthesis Example 2> 20.00 g of diglycidyl terephthalate (product name EX-711, Nagase ChemteX Corporation), 12.33 g of 3,3'-dithiodipropionic acid (product name: DTDPA, Sakai Chemical Industry Co., Ltd.), 4.11 g of gallic acid hydrate, and 1.76 g of tetrabutylphosphonium bromide as a catalyst were dissolved in 57.29 g of propylene glycol monomethyl ether, and then reacted at 105°C for 24 hours to obtain a solution containing a reaction product (solid content 40% by mass). The repeating unit and terminal structure of the obtained reaction product are represented by formula (D-2). When the obtained reaction product was subjected to GPC analysis, it was found to have a weight average molecular weight of 3900 in terms of standard polystyrene.
[0106] [ka]
[0107] <Synthesis Example 3> 20.00 g of 1,3'-diglycidylhydantoin (manufactured by Shikoku Chemical Industry Co., Ltd.), 12.69 g of 3,3'-dithiodipropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., trade name: DTDPA), 4.23 g of gallic acid hydrate, and 1.81 g of tetrabutylphosphonium bromide as a catalyst were dissolved in 58.09 g of propylene glycol monomethyl ether, and then reacted at 105°C for 24 hours to obtain a solution containing a reaction product (solid content 40% by mass). The repeating unit and terminal structure of the obtained reaction product are represented by formula (D-3). When the obtained reaction product was subjected to GPC analysis, it was found to have a weight average molecular weight of 3900 in terms of standard polystyrene.
[0108] [ka]
[0109] <Synthesis Example 4> 20.00 g of monoallyl diglycidyl isocyanurate (manufactured by Shikoku Chemical Industry Co., Ltd., product name MA-DGIC), 16.42 g of 3,3'-dithiodipropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., product name: DTDPA), and 0.659 g of ethyltriphenylphosphonium bromide as a catalyst were dissolved in 92.71 g of propylene glycol monomethyl ether, and then reacted at 105°C for 24 hours to obtain a solution containing a reaction product (solid content 20% by mass). The obtained reaction product has a repeating unit of formula (D-4). When the obtained reaction product was subjected to GPC analysis, it was found to have a weight average molecular weight of 4600 in terms of standard polystyrene.
[0110] [ka]
[0111] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the description of the following examples. In addition, as the basic hydrogen peroxide aqueous solution, a chemical solution having the composition shown in Table 1 below was used, but the basic hydrogen peroxide aqueous solution applied to the present invention is not limited to this composition.
[0112] <Example 1> 0.552 g of pyridinium trifluoromethanesulfonate, 18.84 g of propylene glycol monomethyl ether acetate, and 152.99 g of propylene glycol monomethyl ether were added to 27.62 g of the solution containing the polymer obtained in Synthesis Example 1 to prepare a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a protective film-forming composition.
[0113] <Example 2> 0.552 g of pyridinium trifluoromethanesulfonate, 18.84 g of propylene glycol monomethyl ether acetate, and 152.99 g of propylene glycol monomethyl ether were added to 27.62 g of the solution containing the polymer obtained in Synthesis Example 2 to prepare a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a protective film-forming composition.
[0114] <Example 3> 0.552 g of pyridinium trifluoromethanesulfonate, 18.84 g of propylene glycol monomethyl ether acetate, and 152.99 g of propylene glycol monomethyl ether were added to 27.62 g of the solution containing the polymer obtained in Synthesis Example 3 to prepare a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a protective film-forming composition.
[0115] <Example 4> 0.552 g of pyridinium trifluoromethanesulfonate, 1.105 g of TMOM-BP (manufactured by Honshu Chemical Industry Co., Ltd.), 18.84 g of propylene glycol monomethyl ether acetate, and 152.99 g of propylene glycol monomethyl ether were added to 27.62 g of the solution containing the polymer obtained in Synthesis Example 1 to prepare a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a protective film-forming composition.
[0116] <Comparative Example 1> 0.552 g of pyridinium trifluoromethanesulfonate, 18.84 g of propylene glycol monomethyl ether acetate, and 125.37 g of propylene glycol monomethyl ether were added to 55.24 g of the solution containing the polymer obtained in Synthesis Example 4 to prepare a solution. The solution was filtered using a polyethylene microfilter having a pore size of 0.02 μm to prepare a protective film-forming composition.
[0117] (Formation of coating film) The protective film-forming compositions prepared in Examples 1 to 3 and the film-forming composition prepared in Comparative Example 1 were applied by spin coating onto a silicon substrate having a titanium nitride film formed on its surface, and baked at 220°C for 60 seconds to produce a coating film with a thickness of 100 nm.
[0118] (Resistance test to basic hydrogen peroxide solution) The coating films formed on silicon substrates having titanium nitride films formed thereon using the protective film-forming compositions prepared in Examples 1 to 3 and the film-forming composition prepared in Comparative Example 1 were immersed in a basic hydrogen peroxide aqueous solution having the composition shown in Table 1 below for 1 minute at the temperature shown in the same table, and then washed with water and dried, after which the state of the coating film was visually observed. The results are shown in Table 2 below. In Table 2, "◯" indicates a state in which no peeling was observed in the coating film even after 1 minute of treatment, and "×" indicates a state in which peeling was observed in part or all of the coating film after 1 minute of treatment.
[0119] [Table 1]
[0120] [Table 2]
[0121] The results in Table 2 above show that the coating films prepared using the protective film-forming compositions prepared in Examples 1 to 3 have sufficient resistance to a basic hydrogen peroxide aqueous solution. That is, it was found that these coating films can serve as protective films against a basic hydrogen peroxide aqueous solution. On the other hand, it was shown that the coating film prepared using the film-forming composition prepared in Comparative Example 1 does not have resistance to a basic hydrogen peroxide aqueous solution, and it was revealed that these coating films cannot serve as protective films against a basic hydrogen peroxide aqueous solution. [Industrial Applicability]
[0122] The protective film-forming composition of the present invention has excellent resistance when a wet etching solution is applied to substrate processing and a high dry etching rate, making substrate processing easy, and provides a protective film that has excellent planarization properties when applied to a substrate with a step.
Claims
1. The reaction product (P) of the diepoxy compound (B), the difunctional or higher proton generating compound (C), and at least one compound selected from the group consisting of the following (c-1) to (c-17) is represented by the following formula (1): 【Chemistry 1】 (in formula (1), Ar represents an aryl group having 6 to 40 carbon atoms, n represents an integer of 2 to 10, -Y- represents -OCO-, -O- or -S-, and * represents a bonding portion with the molecular terminal of the reaction product (P), The composition for forming a protective film against a wet etching solution for semiconductors further comprises an organic solvent (S). 【Chemistry 17】
2. 2. The protective film-forming composition according to claim 1, wherein the bifunctional or higher functional proton-generating compound (C) has a functional group selected from the group consisting of a hydroxyl group, a carboxyl group, a thiol group, an amino group, and an imide group.
3. The protective film-forming composition according to claim 1 , wherein the di- or higher functional proton-generating compound (C) is an acid dianhydride.
4. The reaction product (P) is represented by the following formula (2): 【Chemistry 2】 (In formula (2), Q 1 and Q. 2 represents a divalent organic group; A 1 or A 6 represents a hydrogen atom, a methyl group, or an ethyl group. The protective film-forming composition according to claim 1 , comprising a unit structure represented by the following formula:
5. Q in the formula (2) 1 is expressed by the following formula (3): 【Chemistry 3】 (In formula (3), R 2 represents a direct bond, an alkylene group having 1 to 10 carbon atoms which may be interrupted by -O-, -S- or -S-S-, an alkenylene group having 2 to 6 carbon atoms, or a divalent organic group having at least one alicyclic hydrocarbon ring having 3 to 10 carbon atoms or an aromatic hydrocarbon ring having 6 to 14 carbon atoms, and the divalent organic group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a halogen atom, a hydroxy group, a nitro group, a cyano group, a methylidene group, an alkoxy group having 1 to 6 carbon atoms, an alkoxycarbonyl group having 2 to 6 carbon atoms, and an alkylthio group having 1 to 6 carbon atoms. 1 and Z 1 each represents -COO-, -OCO-, -O-, or -S-.) The protective film-forming composition according to claim 4 , wherein the protective film-forming composition is represented by the formula:
6. Q in the formula (2) 2 is expressed by the following formula (4): 【Chemistry 4】 (In the above formula (4), R 1 represents a direct bond or an alkylene group having 1 to 5 carbon atoms; n1 and m each represent an integer of 0 or 1; Z 2 is expressed by the following formula (5), formula (6) or formula (7): 【Chemistry 5】 (In the above formula (6), X is the following formula (8), formula (9) or formula (10): 【Chemistry 6】 (In formula (8), formula (9) and formula (10), R 11 , R 12 , R 13 , R 14 and R 15 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group, or a phenyl group, the phenyl group being optionally substituted with at least one selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, a nitro group, a cyano group, an alkoxy group having 1 to 6 carbon atoms, and an alkylthio group having 1 to 6 carbon atoms; R 13 and R 14 may be bonded to each other to form a ring having 3 to 6 carbon atoms.
7. The protective film-forming composition according to claim 1 , wherein the Ar includes a benzene, naphthalene, or anthracene structure.
8. The protective film-forming composition according to claim 1 , wherein the n is an integer of 2 to 4.
9. The protective film-forming composition according to claim 1 , further comprising a crosslinking agent (K).
10. The crosslinking agent (K) is represented by the following formula (11) or (12): 【Chemistry 7】 (In formula (11) and formula (12), Q 2 represents a single bond or a divalent organic group. 8 , R 9 , R 11 and R 12 each represents a hydrogen atom or a methyl group, R 7 and R 10 each represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. n9 is an integer satisfying 1≦n9≦3, n10 is an integer satisfying 2≦n10≦5, n11 is an integer satisfying 0≦n11≦3, n12 is an integer satisfying 0≦n12≦3, and 3≦(n9+n10+n11+n12)≦6. n13 is an integer of 1≦n13≦3, n14 is an integer of 1≦n14≦4, n15 is an integer of 0≦n15≦3, n16 is an integer of 0≦n16≦3, and 2≦(n13+n14+n15+n16)≦5. m2 is an integer of 2 to 10.
10. The protective film-forming composition according to claim 9, wherein the compound is selected from the group consisting of a compound represented by the formula:
11. The protective film-forming composition according to claim 1 , further comprising a crosslinking catalyst.
12. The protective film-forming composition according to claim 1 , further comprising a surfactant.
13. A protective film, which is a fired product of a coating film comprising the protective film-forming composition according to any one of claims 1 to 12.
14. 14. A method for producing a substrate having a resist pattern, comprising the steps of applying the protective film composition according to claim 1 onto a semiconductor substrate and baking the composition to form a protective film as a resist underlayer film, forming a resist film on the protective film, and then exposing and developing the resist film to form a resist pattern, the method being used in the production of a semiconductor.
15. A reaction product (P) of a diepoxy compound (B) and a di- or higher functional proton generating compound (C) is formed on a semiconductor substrate, on the surface of which an inorganic film may be formed, the reaction product (P) being represented by the following formula (1): 【Chemistry 1】 (in formula (1), Ar represents an aryl group having 6 to 40 carbon atoms, n represents an integer of 2 to 10, -Y- represents -OCO-, -O- or -S-, and * represents a bonding portion with the molecular terminal of the reaction product (P), A method for manufacturing a semiconductor device, comprising the steps of forming a protective film using a protective film-forming composition for a semiconductor wet etching solution, the composition further comprising an organic solvent (S), forming a resist pattern on the protective film, dry etching the protective film using the resist pattern as a mask to expose a surface of the inorganic film or the semiconductor substrate, and wet etching and cleaning the inorganic film or the semiconductor substrate using the semiconductor wet etching solution as a mask after the dry etching.
Citation Information
Patent Citations
Epoxy resin
JP1989043521A
Liquid epoxy resin composition
JP1994128360A
Organic film material, organic film formation method, pattern formation method, and compound
JP2016216367A
Composition for forming resist underlayer film and method for forming resist pattern using the same
WO2009104685A1
Composition for forming resist underlayer film and method for forming resist pattern using same
WO2011004721A1