Method for manufacturing silicon carbide semiconductor device
By employing dry etching to selectively remove backside films in silicon carbide semiconductor devices, the method addresses wafer warping and electrode defects, improving the electrical characteristics and reliability of silicon carbide semiconductor devices.
Patent Information
- Application Number
- JP2021039771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2041-03-12
AI Technical Summary
The conventional method for manufacturing silicon carbide semiconductor devices results in wafer warping due to the oxide film and polysilicon layers on the backside, leading to electrode formation defects and electrical characteristic issues, particularly in devices with temperature or current sensing capabilities.
A method involving dry etching is used to simultaneously remove the gate insulating film, gate electrode, and other backside films on the silicon carbide semiconductor substrate, ensuring selectivity and preventing simultaneous grinding of the hard SiC substrate with softer oxide films and polysilicon layers.
This approach alleviates wafer warping and associated errors, prevents electrode defects, and enhances the electrical performance of silicon carbide semiconductor devices by ensuring precise film removal without uneven grinding.
Smart Images

Figure 0007563750000001 
Figure 0007563750000002 
Figure 0007563750000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a silicon carbide semiconductor device. [Background technology]
[0002] Silicon carbide (SiC) is expected to be a next-generation semiconductor material to replace silicon (Si). Compared to conventional semiconductor elements that use silicon carbide as a semiconductor material, semiconductor elements that use silicon carbide as a semiconductor material (hereinafter referred to as silicon carbide semiconductor devices) have various advantages, such as the ability to reduce the resistance of the element in the on-state to one-hundredth of that of conventional semiconductor elements that use silicon as a semiconductor material, and the ability to be used in higher temperature environments (200°C or higher). This is due to the characteristics of the material itself, namely, that the band gap of silicon is about three times larger than that of silicon, and that the dielectric breakdown field strength is nearly one order of magnitude larger than that of silicon.
[0003] Silicon carbide semiconductor devices that have been commercially available to date include Schottky barrier diodes (SBDs) and vertical MOSFETs (insulated gate field effect transistors) having a planar gate structure or a trench gate structure.
[0004] Conventionally, there is a silicon carbide semiconductor device having a trench gate structure as a structure with a high channel density to allow a large current to flow (see, for example, Patent Document 1). In order to further improve the reliability of silicon carbide semiconductor devices, a semiconductor device has been proposed in which a high-function region such as a current sensing section, a temperature sensing section, and an overvoltage protection section is arranged on the same semiconductor substrate as a vertical MOSFET, which is a main semiconductor element. In the case of a high-function structure, in order to stably form the high-function region, a region in which only the high-function region is arranged is provided in the active region, separated from the unit cell of the main semiconductor element and adjacent to the edge termination region. The active region is a region through which a main current flows when the main semiconductor element is turned on. The edge termination region is a region for maintaining a breakdown voltage (withstand voltage) by mitigating the electric field on the front surface side of the semiconductor substrate. The breakdown voltage is the limit voltage at which the element does not malfunction or break down.
[0005] Fig. 13 is a flow chart of a conventional method for manufacturing a silicon carbide semiconductor device. Fig. 13 shows the steps after trench formation. First, a trench is formed (step S301), and isotropic etching and sacrificial oxidation are performed to remove damage to the trench, followed by activation processing to activate the ions implanted in the semiconductor layer (step S302). Next, a gate insulating film is formed in the trench (step S303), and annealing is performed to reduce the interface state between the gate insulating film and the silicon carbide substrate (step S304).
[0006] Next, a gate electrode is formed in the gate insulating film (step S305), and after forming a gate electrode pattern (step S306), an insulating film is formed on the surface of the gate electrode (step S307). Next, an interlayer insulating film is formed on the insulating film (step S308).
[0007] Next, to form a temperature sensing section, a polycrystalline polysilicon for the sensor is formed (step S309), a polycrystalline polysilicon pattern for the sensor is formed (step S310), and an insulating film is formed on the surface of the polycrystalline polysilicon for the sensor (step S311). Next, after protecting the surface with a resist (step S312), a sensor section is formed on the surface of the polycrystalline polysilicon for the sensor (step S313).
[0008] Next, the interlayer insulating film is etched to form a contact hole and a contact portion (step S314), and an electrode is buried in the contact hole to form a source electrode pad (step S315).
[0009] Next, a polyimide film is formed as a protective film around the electrodes of the semiconductor element, and then surface plating is formed (step S316). Next, the back surface is ground to reduce resistance (step S317). Next, a drain electrode is formed on the back surface (step S318), completing the silicon carbide semiconductor device.
[0010] In such a method for manufacturing a silicon carbide semiconductor device, when forming a gate insulating film and a gate electrode inside the trench gate, the gate insulating film and the gate electrode are formed by thermal oxidation or a furnace-type CVD (Chemical Vapor Deposition) device, so that a film is also formed on the back side of the surface on which the film is originally to be formed. These laminated films are ground together when the wafer is thinned in step S317.
[0011] In the manufacturing process of Si (silicon)-IGBT (Insulated Gate Bipolar Transistor), etc., oxide films and polysilicon films are formed by CVD on the reverse side of the surface on which they are originally intended to be formed during thermal oxidation. These laminated films are also ground away together when the wafer is thinned.
[0012] Also, a technique is known in which a temporary polycrystalline silicon oxide film and a temporary polycrystalline silicon film stacked on the back side are completely removed by dry etching using etchants such as CF4 (carbon tetrafluoride) and O2 (oxygen) or a combination of wet etching using a buffered hydrofluoric acid solution and dry etching in sequence (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2019-46909 A [Patent Document 2] JP 2003-243654 A Summary of the Invention [Problem to be solved by the invention]
[0014] Here, when the Si device process is applied to a device using a SiC substrate such as a SiC-MOSFET, if the deposition layer that has spread to the back surface remains, the SiC wafer warp will cause problems with ESC (Electrostatic Chuck) adhesion and transportation. In particular, in the case of devices equipped with a temperature sensor or current sensor, the oxide film and polysilicon layer are overlapped in multiple layers, so the problem becomes more pronounced. In this case, the process will not be performed normally, and poor electrical characteristics will occur in the semiconductor device.
[0015] For this reason, in the method for manufacturing a silicon carbide semiconductor device, the film layer that has spread to the back surface is removed when grinding the back surface, as shown in the flowchart of Fig. 13. However, when grinding the back surface, the SiC substrate, which has high hardness, and the oxide film and polysilicon, which have low hardness, are simultaneously ground, which causes uneven grinding, etc. In this case, electrode formation defects, etc. occur.
[0016] An object of the present invention is to provide a method for manufacturing a silicon carbide semiconductor device that can reduce the effects of wafer warpage due to an oxide film and polysilicon on the back surface, suppress ESC adsorption errors, transportation errors, and the like, and can suppress poor electrical characteristics and electrode formation defects of the semiconductor device, in order to solve the problems associated with the conventional techniques described above. [Means for solving the problem]
[0017] In order to solve the above-mentioned problems and achieve the object of the present invention, a method for manufacturing a silicon carbide semiconductor device according to the present invention has the following features. First, a first step is performed in which a first semiconductor layer of a first conductivity type having a lower impurity concentration than the silicon carbide semiconductor substrate is formed on a front surface of a silicon carbide semiconductor substrate of a first conductivity type. Next, a second step is performed in which a second semiconductor layer of a second conductivity type is formed on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate. Next, a third step is performed in which a third semiconductor layer of a first conductivity type is formed on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate. Next, a fourth step is performed in which a gate electrode is formed on the front surface of the silicon carbide semiconductor substrate via a gate insulating film. Next, a fifth step is performed in which a first insulating film is formed on the front surface of the gate electrode. Next, the gate insulating film, the gate electrode and the first insulating film formed on the back surface of the silicon carbide semiconductor substrate are Bulk Next, the sixth step of removing the Third semiconductor layer A seventh step of forming a first electrode on the front surface of the silicon carbide semiconductor substrate is then performed, followed by an eighth step of forming a second electrode on the back surface of the silicon carbide semiconductor substrate.
[0018] Moreover, in the above-mentioned invention, the method for manufacturing a silicon carbide semiconductor device according to the present invention further includes a ninth step, which is performed after the fifth step and before the sixth step, of forming an interlayer insulating film on the gate electrode, a tenth step of forming polysilicon on the interlayer insulating film, and an eleventh step of forming a second insulating film on a surface of the polysilicon, BulkIt is characterized by removing
[0019] In addition, the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, is characterized in that it further includes a twelfth step of forming a sensor portion on a surface of the polysilicon after the sixth step and before the seventh step.
[0020] Moreover, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, the sixth step uses dry etching.
[0021] In addition, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, the dry etching is carried out continuously in the same chamber.
[0022] Moreover, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, the dry etching is performed under the same etching conditions.
[0023] Moreover, the method for manufacturing a silicon carbide semiconductor device according to the present invention is characterized in that, in the above-described invention, the dry etching is performed by chemical dry etching, and the etching conditions are such that a selectivity between the silicon carbide semiconductor substrate and a gate insulating film formed on a back surface of the silicon carbide semiconductor substrate is 100 or more.
[0024] Moreover, the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-described invention, further includes a thirteenth step between the third step and the fourth step of selectively forming a first semiconductor region of a first conductivity type in a surface layer of the third semiconductor layer on an opposite side to the silicon carbide semiconductor substrate.
[0025] In addition, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, the method further includes a fourteenth step of forming a trench that penetrates the second semiconductor layer and the third semiconductor layer and reaches the first semiconductor layer between the third step and the fourth step, 4 In the process, the gate insulating film and the gate electrode are formed inside the trench.
[0026] In addition, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, in the twelfth step, ions are implanted into the polysilicon to form a diode.
[0027] According to the above-mentioned invention, the rear laminated film (gate insulating film on the rear surface, gate electrode on the rear surface, first insulating film on the rear surface, interlayer insulating film on the rear surface, polycrystalline polysilicon for the rear surface, and second insulating film on the rear surface) is removed all at once by dry etching. This can mitigate the influence of wafer warpage caused by the oxide film and polysilicon on the rear surface, and suppress ESC suction errors and transportation errors. In addition, the wet etching process for removing the rear laminated film can be omitted. This prevents the SiC substrate, which has high hardness, and the oxide film and polysilicon, which have low hardness, from being ground simultaneously, so that uneven grinding does not occur and electrode formation defects can be suppressed. Effect of the Invention
[0028] According to the method for manufacturing a silicon carbide semiconductor device according to the present invention, it is possible to mitigate the influence of wafer warpage due to the oxide film and polysilicon on the back surface, thereby suppressing ESC adsorption errors, transportation errors, and the like, and to suppress poor electrical characteristics and electrode formation defects of the semiconductor device. [Brief description of the drawings]
[0029] [Figure 1] 1 is a cross-sectional view showing a structure of an active region of a silicon carbide semiconductor device in accordance with a first embodiment. [Diagram 2]1 is a cross sectional view showing a structure of a temperature sensing portion of the silicon carbide semiconductor device in accordance with the first embodiment. [Diagram 3] 2 is a flowchart of a method for manufacturing a silicon carbide semiconductor device according to the first embodiment. [Figure 4] 1 is a cross-sectional view (part 1) showing a state during manufacture of a silicon carbide semiconductor device according to a first embodiment. [Diagram 5] FIG. 2 is a cross-sectional view (part 2) showing a state during manufacture of the silicon carbide semiconductor device according to the first embodiment. [Figure 6] 5 is a cross-sectional view (part 3) showing a state during the manufacture of the silicon carbide semiconductor device according to the first embodiment. FIG. [Figure 7] FIG. 4 is a cross-sectional view showing a state during the manufacture of the silicon carbide semiconductor device according to the first embodiment (part 4). [Figure 8] FIG. 5 is a cross-sectional view showing a state during the manufacture of the silicon carbide semiconductor device according to the first embodiment (part 5). [Figure 9] FIG. 6 is a cross-sectional view showing a state during the manufacture of the silicon carbide semiconductor device according to the first embodiment (part 6). [Figure 10] 10 is a flowchart of a method for manufacturing a silicon carbide semiconductor device according to a second embodiment. [Figure 11] 11 is a cross-sectional view (part 1) showing a state during the manufacture of a silicon carbide semiconductor device according to a second embodiment. FIG. [Figure 12] 13 is a cross-sectional view (part 2) showing a state during the manufacture of a silicon carbide semiconductor device according to the second embodiment. FIG. [Figure 13] 1 is a flowchart of a conventional method for manufacturing a silicon carbide semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] A preferred embodiment of the method for manufacturing a silicon carbide semiconductor device according to the present invention will be described in detail below with reference to the accompanying drawings. In this specification and the accompanying drawings, in a layer or region prefixed with n or p, electrons or holes are the majority carriers, respectively. In addition, + and - attached to n or p respectively mean that the impurity concentration is higher and lower than that of a layer or region not prefixed with n or p. Note that in the following description of the embodiment and the accompanying drawings, the same reference numerals are attached to similar configurations, and duplicated explanations are omitted. In addition, in this specification, in the notation of Miller indices, "-" means a bar attached to the index immediately following it, and adding "-" before the index represents a negative index. In addition, the description of "same" or "equivalent" should include up to 5% in consideration of variations in manufacturing.
[0031] (Embodiment 1) The semiconductor device according to the present invention is configured using a wide band gap semiconductor. In the first embodiment, a trench-type MOSFET 70 will be taken as an example of a silicon carbide semiconductor device fabricated (manufactured) using silicon carbide (SiC) as a wide band gap semiconductor. Fig. 1 is a cross-sectional view showing a structure of an active region of the silicon carbide semiconductor device according to the first embodiment.
[0032] 1, the trench MOSFET 70 has a MOS gate structure with a trench gate structure on the front surface (the surface on the side of a p-type base layer 6 described later) of a semiconductor substrate. + A first n-type silicon carbide substrate (a silicon carbide semiconductor substrate of a first conductivity type) 1 is provided on the - The n-type silicon carbide epitaxial layer (first semiconductor layer of a first conductivity type) 2 and the p-type base layer (second semiconductor layer of a second conductivity type) 6 are epitaxially grown in this order. - The silicon carbide epitaxial layer 4 is - Alternatively, the n-type silicon carbide epitaxial layer 2 may be epitaxially grown on the n-type silicon carbide epitaxial layer 2. + A silicon carbide substrate 1, a p-type base layer 6, and a first n - A silicon carbide epitaxial layer 2 and a 2n- The silicon carbide epitaxial layer 4 and the silicon carbide epitaxial layer 5 form a silicon carbide semiconductor base (a semiconductor substrate made of silicon carbide).
[0033] The MOS gate structure of the trench gate structure includes a p-type base layer 6, an n-type source region (a third semiconductor layer of a first conductivity type) 7, and a + A first conductive type source region (a first semiconductor region of a first conductive type) 8, p ++ It is composed of a mold contact region 9 , a trench 10 , a gate insulating film 11 and a gate electrode 12 .
[0034] Specifically, the trench 10 penetrates the p-type base layer 6 in the depth direction y from the front surface of the silicon carbide semiconductor substrate, and has a length of 2n - The silicon carbide epitaxial layer 4 (the second n - When the silicon carbide epitaxial layer 4 is not provided, the first n - The trenches 10 reach the silicon carbide epitaxial layer 2 (hereinafter referred to as (2)). The depth direction y is the direction from the front surface to the back surface of the semiconductor substrate. The trenches 10 are arranged, for example, in a stripe shape.
[0035] Inside the trench 10, a gate insulating film 11 is provided along the inner wall of the trench 10, and a gate electrode 12 is provided on the gate insulating film 11 so as to be embedded inside the trench 10. One unit cell of the main semiconductor element is composed of the gate electrode 12 in one trench 10 and adjacent mesa regions (regions between adjacent trenches 10) sandwiching the gate electrode 12. Although only one trench MOS structure is shown in FIG. 1, more trench-structured MOS gate (insulated gate made of metal-oxide film-semiconductor) structures may be arranged in parallel.
[0036] 1st n - An n-type region (hereinafter, referred to as a second n-type region) is formed in the surface layer of the source side (the source electrode 16 side described later) of the silicon carbide epitaxial layer 2 so as to contact the p-type base layer 6. - A second silicon carbide epitaxial layer (hereinafter referred to as a 2n-type silicon carbide epitaxial layer) 4 may be provided. -The 2n-type silicon carbide epitaxial layer 4 is a so-called current spreading layer (CSL) that reduces the spreading resistance of carriers. - The silicon carbide epitaxial layer 4 is formed uniformly in a direction parallel to the front surface of the substrate (front surface of the semiconductor substrate) so as to cover the inner wall of the trench 10, for example. - The silicon carbide epitaxial layer 4 is provided from the interface with the p-type base layer 6 to a position on the drain side (the side of a drain electrode 15 described later) from the bottom surface of the trench 10.
[0037] 1st n - The surface layer of the silicon carbide epitaxial layer 2 is formed of a first p + The mold region 3 may be selectively provided. + The mold region 3 is disposed between adjacent trenches 10. - The second p type silicon carbide epitaxial layer 4 includes + The mold region 5 may be selectively provided. + The mold region 5 is a first p + At a position facing the mold region 3 in the depth direction, a 2n - The bottom surface of the first p-type silicon carbide epitaxial layer 4 is + The second p-type region 3 is in contact with the p-type base layer 6 at its top surface. + Through the p-type region 5, the p-type base layer 6 and the first p + The mold region 3 is electrically connected to the mold region 3 .
[0038] 2nd n - The silicon carbide epitaxial layer 4 and the second p + A p-type base layer 6 is provided on the surface of the n-type region 5. An n-type source region 7 is provided on the surface of the p-type base layer 6. An n-type source region 7 is provided inside the n-type + Type source region 8 and p ++ A contact region 9 is optionally provided. + The n-type source region 8 is an n-type source region 7 + The n-type source region 7 and the n-type silicon carbide substrate 1 are disposed on the surface layer opposite to the n-type source region 7. +The n-type source region 8 is in contact with the gate insulating film 11 on the side wall of the trench 10, and faces the gate electrode 10 via the gate insulating film 11 on the side wall of the trench 10. ++ A contact region 9 may be provided. ++ The n-type contact region 9 is connected to the n-type source region 7 and + The source region 8 is in contact with the p ++ The impurity concentration of the p-type contact region 9 is higher than the impurity concentration of the p-type base layer 6. The n-type source region 7 + The n-type source region 7 and the n-type + The n-type source regions 7 and 8 are in contact with each other. + The width of the n-type source region 8 is approximately the same. + The mold source region 8 is not essential.
[0039] The interlayer insulating film 13 is provided on the entire front surface of the silicon carbide semiconductor substrate so as to cover the gate electrode 12. A contact hole is opened in the interlayer insulating film 13, penetrating the interlayer insulating film 13 in the depth direction y to reach the front surface of the substrate. On the drain side of the interlayer insulating film 13, a gate insulating film 11 and an insulating film 22 on the surface of the gate electrode are provided.
[0040] The source electrode 16 is formed by bonding a silicon carbide semiconductor substrate (n + The p-type source region 8 is in ohmic contact with the p-type source region 8 and is electrically insulated from the gate electrode 12 by an interlayer insulating film 13. ++ When the n-type contact region 9 is provided, the source electrode 16 is + Type source region 8 and p ++ The source electrode 16 is in ohmic contact with the contact region 9. A barrier metal (not shown) for preventing diffusion of metal atoms from the source electrode 16 to the gate electrode 12 side may be provided between the source electrode 16 and the interlayer insulating film 13. A source electrode pad 14 is provided on the source electrode 16. +A drain electrode 15 serving as a back surface electrode is provided on the back surface of the type silicon carbide substrate 1. A barrier metal (not shown) may also be provided between the source electrode 16 and the interlayer insulating film 13 and the source electrode pad .
[0041] (Method of Manufacturing Silicon Carbide Semiconductor Device According to First Embodiment) Next, a method for manufacturing the silicon carbide semiconductor device according to the first embodiment will be described. Fig. 3 is a flowchart of the method for manufacturing the silicon carbide semiconductor device according to the first embodiment. Fig. 3 illustrates steps after trench formation. Figs. 4 to 9 are cross-sectional views showing states during the manufacturing process of the silicon carbide semiconductor device according to the embodiment.
[0042] First, n-type silicon carbide + A type silicon carbide substrate 1 is prepared. + A first n-type silicon carbide layer is formed on a first main surface (front surface) of the silicon carbide substrate 1 while doping it with n-type impurities, for example, nitrogen (N) atoms. - A silicon carbide epitaxial layer 2 is epitaxially grown.
[0043] Next, the 1nth - On the surface of the silicon carbide epitaxial layer 2, a mask for ion implantation (not shown) having a predetermined opening is formed by photolithography, for example, of an oxide film. Then, using this oxide film as a mask, p-type impurities, for example, aluminum (Al) atoms are ion-implanted by an ion implantation method to form a first n-type silicon carbide epitaxial layer. - A first p-type epitaxial layer having a depth of 0.3 μm to 1.0 μm is formed on the surface of the silicon carbide epitaxial layer 2. + For example, mold region 3 is 2.0×10 17 / cm 3 Above 2.0×10 18 / cm 3 The impurity concentrations are as follows: The state up to this point is shown in Figure 4.
[0044] Next, the 1nth -A second n-type silicon carbide epitaxial layer having a thickness of 0.3 μm to 1.0 μm and doped with n-type impurities such as nitrogen is formed on the surface of the n-type silicon carbide epitaxial layer 2. - The silicon carbide epitaxial layer 4 is formed at a thickness of, for example, 1.0×10 16 / cm 3 Above 5.0×10 17 / cm 3 The impurity concentration is as follows:
[0045] Next, the 2nd - On the surface of the silicon carbide epitaxial layer 4, a mask for ion implantation (not shown) having a predetermined opening is formed by photolithography, for example, of an oxide film. Then, using this oxide film as a mask, p-type impurities, for example, aluminum atoms, are ion-implanted by an ion implantation method to form a 2n-type silicon carbide epitaxial layer. - The surface layer of the silicon carbide epitaxial layer 4 is provided with a 2n-type - The second p-type silicon carbide epitaxial layer 4 is + The mold area 5 is, for example, 2.0 × 10 17 / cm 3 Above 2.0×10 18 / cm 3 The impurity concentrations are as follows: The state up to this point is shown in FIG.
[0046] Next, the 2nd - On the surface of the silicon carbide epitaxial layer 4, a p-type base layer 6 is formed, for example, at a thickness of 5.0×10 16 / cm 3 Above 2.0×10 18 / cm 3 The p-type base layer 6 is formed by epitaxial growth at the following impurity concentration. After the p-type base layer 6 is formed by epitaxial growth, p-type impurities such as aluminum may be further ion-implanted into the channel region of the p-type base layer 6. The p-type base layer 6 is also formed by epitaxial growth at the following impurity concentration. - Alternatively, the n-type silicon carbide epitaxial layer 4 may be epitaxially grown, and then p-type impurities such as aluminum are ion-implanted to form the n-type n-type impurity layer 4 .
[0047] Next, an n-type source region 7 having a thickness of about 0.5 μm is formed on the surface of the p-type base layer 6 by, for example, 1.0×10 16 / cm 3 Above 1.0×10 18 / cm 3 After the n-type source region 7 is formed by epitaxial growth, n-type impurities such as phosphorus (P) or nitrogen are further ion-implanted into the surface of the n-type source region 7 to form n-type impurities in the surface layer of the n-type source region 7. + The source region 8 is, for example, 1.0×10 18 / cm 3 Above 5.0×10 19 / cm 3 The impurity concentration is as follows: + The n-type source region 8 can also be selectively formed by forming an ion implantation mask having a predetermined opening on the n-type source region 7 out of, for example, an oxide film as a mask and then performing an ion implantation method using this oxide film as a mask.
[0048] Next, an ion implantation mask (not shown) having a predetermined opening is formed of, for example, an oxide film. Then, using this oxide film as a mask, p-type impurities, for example, aluminum atoms, are ion-implanted by an ion implantation method to form the n-type source region 7 and the n + A part of the source region 8 is p ++ The contact area 9 is, for example, 1.0×10 20 / cm 3 The impurity concentration may be set to p ++ The impurity concentration of the p-type contact region 9 is higher than that of the p-type base layer 6, and is 1.0×10 19 / cm 3 Above 5.0×10 20 / cm 3 It is preferable to form it so that: ++ The contact region 9 is formed so that its bottom surface reaches the p-type base layer 6. The state up to this point is shown in FIG.
[0049] Next, n +A trench forming mask having a predetermined opening is formed on the surface of the source region 8 by photolithography, for example, an oxide film. Next, an n + A second n-type source region 8, an n-type source region 7, and a p-type base layer 6 are formed. - A trench 10 is formed so as to reach the silicon carbide epitaxial layer 4 (step S101). Next, the trench forming mask is removed.
[0050] Next, after removing damage to the trench by isotropic etching, the surface of the silicon carbide substrate is protected with carbon. Next, a heat treatment (annealing) is performed in an inert gas atmosphere at about 1750° C. to form the first p + Type area 3, 2nd p + type area 5, n + Type source region 8 and p ++ An activation process is performed on the mold contact region 9 (step S102). As described above, the ion implantation regions may be activated all at once by a single heat treatment, or the heat treatment may be performed each time an ion implantation is performed. The state up to this point is shown in FIG.
[0051] Next, n + Type source region 8 and p ++ A gate insulating film 11 is formed along the surface of the contact region 9 and the bottom and sidewalls of the trench 10 (step S103). This gate insulating film 11 may be formed by thermal oxidation at a temperature of about 1300° C. in an oxygen atmosphere. Alternatively, this gate insulating film 11 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).
[0052] Next, the p-type base layer 6 and the second n - In order to reduce the interface state existing between the silicon carbide substrate such as the silicon carbide epitaxial layer 4 and the gate insulating film 11, a heat treatment (annealing) is performed in an atmosphere containing oxygen nitride (Step S104).
[0053] Next, a polycrystalline silicon layer doped with, for example, phosphorus atoms is provided on the gate insulating film 11. This polycrystalline silicon layer may be formed so as to fill the trench 10. This polycrystalline silicon layer is patterned by photolithography and left inside the trench 10 to form the gate electrode 12 (step S105). A p-type polycrystalline silicon film may be used for the gate electrode 12. Next, a gate electrode pattern is formed to connect the gate electrode 12 to a gate electrode pad (not shown) provided on the surface of the semiconductor chip (step S106).
[0054] Next, an insulating film 22 is formed on the surface of the gate electrode 12 (step S107). This insulating film 22 is formed of a thermal oxide film by annealing in an oxygen atmosphere at 1000° C., for example. By forming the gate insulating film 11, gate electrode 12, and insulating film 22 as described above, a rear gate insulating film 23, a rear gate electrode 24, and a rear first insulating film 25 are formed on the rear surface side. The state up to this point is shown in FIG.
[0055] Next, the front surface is protected with a protective film (step S108). For example, the protective film is formed using a resist for photolithography. Next, the rear surface laminated film is removed all at once by dry etching (step S109). Here, the rear surface laminated film is the rear surface gate insulating film 23, the rear surface gate electrode 24, and the rear surface first insulating film 25. This dry etching is preferably performed in the same chamber to continuously remove the rear surface laminated film all at once. In addition, it is preferable that the dry etching conditions are the same for removing the rear surface gate insulating film 23, the rear surface gate electrode 24, and the rear surface first insulating film 25. For example, chemical dry etching is performed, and the etching conditions are: + The selection ratio between the n-type silicon carbide substrate 1 and the gate insulating film 23 on the back surface is set to 100 or more, and when the gate insulating film 23 on the back surface is removed by etching, + It is preferable to prevent the silicon carbide substrate 1 from being removed by etching. Specifically, it is preferable to perform chemical dry etching using CF4 and O2 as etchants.
[0056] Next, the protective film formed on the surface is removed, for example, by ashing in oxygen plasma and stripping with SPM (sulfuric acid-hydrogen peroxide mixture).
[0057] Next, for example, phosphorus glass is deposited to a thickness of about 1 μm so as to cover the gate insulating film 11 and the gate electrode 12, forming the interlayer insulating film 13 (step S110). The interlayer insulating film 13 and the gate insulating film 11 are patterned by photolithography. + Type source region 8 and p ++ A contact hole exposing the mold contact region 9 and a contact part are formed (step S111). The state up to this point is shown in FIG.
[0058] Next, a conductive film that will become the source electrode 16 is formed in the contact hole provided in the interlayer insulating film 13 and on the interlayer insulating film 13. The conductive film is, for example, a nickel (Ni) film. After that, a heat treatment is performed at a temperature of, for example, about 700° C. to selectively react the conductive film with silicon carbide, and then the unreacted conductive film is selectively removed to leave the source electrode 16 only in the contact hole, and n + Type source region 8 and p ++ The contact region 9 is brought into contact with a source electrode 16 .
[0059] Next, a metal layer to become the source electrode pad 14 is formed on the source electrode 16 on the front surface of the silicon carbide semiconductor substrate and on the interlayer insulating film 13 by, for example, sputtering. At this time, a barrier metal (not shown) made of titanium or titanium nitride may be formed first. The thickness of the metal layer on the interlayer insulating film 13 may be, for example, 5.5 μm. The metal layer may be made of, for example, aluminum containing silicon at a rate of 1% (Al-Si). Next, the metal film is selectively removed to form the source electrode pad 14 (step S112).
[0060] Next, a polyimide film (not shown) is selectively formed on the source electrode pad 14, and using the polyimide film as a mask, a surface electrode film is selectively formed by NiP (nickel phosphorus) electroless plating on the portion of the source electrode pad 14 where the polyimide film is not provided (step S113).
[0061] Next, n + The front surface of the silicon carbide substrate 1 is covered with a protective film (not shown) for protection, and then, in order to reduce resistance, + The second main surface (rear surface) of the silicon carbide substrate 1 is mechanically ground with a grinder or the like (step S114). + The silicon carbide substrate 1 is thinned.
[0062] Next, n + On the second main surface (rear surface) of the silicon carbide substrate 1, a conductive film serving as the drain electrode 15, for example, a molybdenum film and a nickel film, are successively formed by, for example, a sputtering method. Then, a heat treatment such as laser annealing is performed to form an n + The drain electrode is formed by reacting the silicon carbide substrate 1 with a conductive film to form an ohmic junction (step S115).
[0063] Next, a film of titanium, nickel and gold is formed in this order as a drain electrode pad (not shown) on the surface of the drain electrode 15. In this manner, the trench MOSFET 70 shown in FIG.
[0064] As described above, according to the first embodiment, the rear surface laminated film (the gate insulating film on the rear surface, the gate electrode on the rear surface, and the first insulating film on the rear surface) is removed all at once by dry etching. This reduces the influence of wafer warpage caused by the oxide film and polysilicon on the rear surface, and suppresses ESC suction errors and transportation errors. In addition, the wet etching process for removing the rear surface laminated film can be omitted. This prevents the SiC substrate, which has high hardness, and the oxide film and polysilicon, which have low hardness, from being ground simultaneously, so that uneven grinding does not occur, and it is possible to suppress the occurrence of electrode formation defects.
[0065] (Embodiment 2) Next, a second embodiment will be described. The structure of a silicon carbide semiconductor device manufactured by the method for manufacturing a silicon carbide semiconductor device according to the second embodiment is different from that of the silicon carbide semiconductor device according to the first embodiment in that it has a temperature sensing portion. The structure of a trench MOSFET 70 is the same as that of the first embodiment, and therefore description thereof will be omitted.
[0066] 2 is a cross-sectional view showing the structure of a temperature sensor unit of the silicon carbide semiconductor device according to the first embodiment. The temperature sensor unit has a function of detecting the temperature of the main semiconductor element by utilizing the temperature characteristics of a diode. For this reason, the temperature sensor unit is provided in an active region through which a main current flows when the main semiconductor element is on. Here, a temperature sensor unit is shown as an example of the sensor unit, but a sensor unit other than a temperature sensor unit may be used as long as it is made of polysilicon.
[0067] For example, the temperature sensing section is provided with a diode made of a p-type polysilicon layer 20 and an n-type polysilicon layer 21, which will be described later. The forward voltage Vf of this diode changes with temperature, and the higher the temperature, the lower the forward voltage Vf. For this reason, the relationship between temperature and forward voltage Vf is obtained in advance, and the temperature of the trench MOSFET 70 can be measured by measuring the forward voltage Vf of the diode while the trench MOSFET 70 is in operation.
[0068] As shown in FIG. 2, the temperature sensor section has n + A first main surface (front surface) of the silicon carbide substrate 1, for example, a (0001) surface (Si surface), is provided with a first n-type - A first n-type silicon carbide epitaxial layer 2 is deposited on the first n-type silicon carbide epitaxial layer 2. - A p-type base layer 6 is provided on the first main surface side of the silicon carbide epitaxial layer 2. - Between the silicon carbide epitaxial layers 2, a 2n - A first n-type silicon carbide epitaxial layer 4 may be provided. - The first p-type silicon carbide epitaxial layer 2 + The mold region 3 is a 1n -The second p-type silicon carbide epitaxial layer 4 + A mould area 5 may be provided.
[0069] In addition, on the p-type base layer 6, ++ A contact region 9 is provided on the entire surface, and an interlayer insulating film 13 is provided thereon. A p-type polysilicon layer 20 and an n-type polysilicon layer 21 are provided on the interlayer insulating film 13. The p-type polysilicon layer 20 and the n-type polysilicon layer 21 are a polysilicon diode formed by a pn junction.
[0070] An anode electrode 30 is provided on the p-type polysilicon layer 20, and an anode electrode pad (not shown) is electrically connected to the p-type polysilicon layer 20 via the anode electrode 30. A cathode electrode 31 is provided on the n-type polysilicon layer 21, and the cathode electrode pad (not shown) is electrically connected to the n-type polysilicon layer 21 via the cathode electrode 31. In addition, an insulating film 29 is provided to cover the p-type polysilicon layer 20 and the n-type polysilicon layer 21.
[0071] (Method of Manufacturing Silicon Carbide Semiconductor Device According to Second Embodiment) Next, a method for manufacturing a silicon carbide semiconductor device according to the second embodiment will be described. Fig. 10 is a flowchart of the method for manufacturing a silicon carbide semiconductor device according to the second embodiment. Figs. 11 and 12 are cross-sectional views showing a state during manufacturing of the silicon carbide semiconductor device according to the second embodiment. In the cross-sectional views showing the state during manufacturing, drawings that are the same as those in the first embodiment are omitted.
[0072] First, as in the first embodiment, an n-type silicon carbide + From the step of preparing a silicon carbide substrate 1, + A process is performed in which a trench forming mask having a predetermined opening is formed of, for example, an oxide film by photolithography on the surface of the source region 8. At this time, the first p + Type region 3 and 2p + Type region 5 and p ++A mold contact region 9 is formed.
[0073] Next, dry etching is performed to remove the + A second n-type source region 8, an n-type source region 7, and a p-type base layer 6 are formed. - A trench 10 is formed so as to reach the silicon carbide epitaxial layer 4 (step S201). Next, the trench forming mask is removed.
[0074] Next, after performing isotropic etching to remove damage to the trench, activation processing is performed while the surface is protected with carbon (step S202). + Type area 3, 2nd p + type area 5, n + Type source region 8 and p ++ The mold contact regions 9 are activated. The state up to this point is shown in FIG.
[0075] Next, n + Type source region 8 and p ++ A gate insulating film 11 is formed along the surface of the contact region 9 and the bottom and sidewalls of the trench 10 (step S203). This gate insulating film 11 may be formed by thermal oxidation at a temperature of about 1300° C. in an oxygen atmosphere. Alternatively, this gate insulating film 11 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).
[0076] Next, a heat treatment (annealing) is performed in an atmosphere containing oxygen nitride. - The interface state existing between the silicon carbide substrate such as the silicon carbide epitaxial layer 4 and the gate insulating film 11 is reduced (step S204).
[0077] Next, a polycrystalline silicon layer doped with, for example, phosphorus atoms is provided on the gate insulating film 11. This polycrystalline silicon layer may be formed so as to fill the trench 10. This polycrystalline silicon layer is patterned by photolithography and left inside the trench 10 to form the gate electrode 12 (step S205). A p-type polycrystalline silicon film may be used for the gate electrode 12. Next, a gate electrode pattern is formed to connect the gate electrode 12 to a gate electrode pad (not shown) provided on the surface of the semiconductor chip (step S206).
[0078] Next, an insulating film 22 is formed on the surface of the gate electrode 12 (step S207). This insulating film 22 is formed of a thermal oxide film by annealing in an oxygen atmosphere at 1000° C., for example. By forming the gate insulating film 11, gate electrode 12, and insulating film 22 as described above, a rear gate insulating film 23, a rear gate electrode 24, and a rear first insulating film 25 are formed on the rear surface side. The state up to this point is shown in FIG.
[0079] Next, for example, phosphorus glass is deposited to a thickness of about 1 μm so as to cover the gate insulating film 11 and the gate electrode 12, forming the interlayer insulating film 13 (step S208). By forming the interlayer insulating film 13, a rear interlayer insulating film 26 is formed on the rear surface side. Next, a sensor portion is formed on the surface of the interlayer insulating film 13. For example, undoped polycrystalline polysilicon 32 is formed on the surface of the interlayer insulating film 13 (step S209), and this polycrystalline polysilicon 32 is patterned by photolithography to form a polycrystalline polysilicon pattern for the sensor (step S210).
[0080] Next, an insulating film 29 is formed on the surface of the polycrystalline polysilicon for the sensor (step S211). This insulating film 29 is formed of a thermal oxide film by annealing in an oxygen atmosphere at 1000°C, for example. By forming the polycrystalline polysilicon for the sensor 32 and the insulating film 29 of the polycrystalline polysilicon for the sensor, the polycrystalline polysilicon for the sensor 27 on the back surface and the insulating film 28 of the polycrystalline polysilicon for the sensor on the back surface (hereinafter referred to as the second insulating film) are formed on the back surface side. The state up to this point is shown in Figures 11 and 12.
[0081] Next, the front surface is protected with a protective film (step S212). For example, the protective film is formed using a resist for photolithography. Next, the rear surface laminated film is removed all at once by dry etching (step S213). Here, the rear surface laminated film is the rear surface gate insulating film 23, the rear surface gate electrode 24, the rear surface first insulating film 25, the rear surface interlayer insulating film 26, the rear surface sensor polycrystalline polysilicon 27, and the rear surface second insulating film 28.
[0082] This dry etching is preferably performed by continuously removing the rear laminated films all at once in the same chamber. For example, the semiconductor substrate is placed in the chamber, and the rear second insulating film 28, rear sensor polycrystalline polysilicon 27, rear interlayer insulating film 26, rear first insulating film 25, rear gate electrode 24, and rear gate insulating film 23 are successively removed in this order. It is also preferable that the dry etching is performed under the same etching conditions for removing the rear gate insulating film 23, rear gate electrode 24, rear first insulating film 25, rear sensor polycrystalline polysilicon 27, and rear second insulating film 28. For example, chemical dry etching is performed under the following etching conditions: + The selectivity between the n-type silicon carbide substrate 1 and the gate insulating film 23 on the rear surface is 100 or more, and when the gate insulating film 23 on the rear surface is removed by etching, + The etching is performed so as not to remove the silicon carbide substrate 1. Specifically, it is preferable to perform chemical dry etching using a mixture of CF4 and O2.
[0083] Next, the protective film formed on the surface is removed. For example, the protective film is removed by ashing in oxygen plasma and peeling with SPM. Next, a sensor portion is formed on the surface of the sensor polycrystalline polysilicon (step S214). For example, p-type impurities and n-type impurities that will become the anode and cathode portions are ion-implanted into parts of the sensor polycrystalline polysilicon 32 to form the p-type polysilicon layer 20 and the n-type polysilicon layer 21.
[0084] Next, the interlayer insulating film 13 and the gate insulating film 11 are patterned by photolithography. + Type source region 8 and p ++ A contact hole exposing the mold contact region 9 and a contact part are formed (step S215). The state up to this point is shown in FIG.
[0085] Next, a conductive film that will become the source electrode 16 is formed in the contact hole provided in the interlayer insulating film 13 and on the interlayer insulating film 13. The conductive film is, for example, a nickel (Ni) film. After that, a heat treatment is performed at a temperature of, for example, about 700° C. to selectively react the conductive film with silicon carbide, and then the unreacted conductive film is selectively removed to leave the source electrode 16 only in the contact hole, and n + Type source region 8 and p ++ The contact region 9 is brought into contact with a source electrode 16 .
[0086] Next, a metal layer to become the source electrode pad 14 is formed on the source electrode 16 on the front surface of the silicon carbide semiconductor substrate and on the interlayer insulating film 13 by, for example, sputtering. At this time, a barrier metal (not shown) made of titanium or titanium nitride may be formed first. The thickness of the metal layer on the interlayer insulating film 13 may be, for example, 5.5 μm. The metal layer may be made of, for example, aluminum containing silicon at a rate of 1% (Al-Si). Next, the metal film is selectively removed to form the source electrode pad 14 (step S216).
[0087] Next, a polyimide film (not shown) is selectively formed on the source electrode pad 14, and using the polyimide film as a mask, a surface electrode film is selectively formed by NiP (nickel phosphorus) electroless plating on the portion of the source electrode pad 14 where the polyimide film is not provided (step S217).
[0088] Next, n + The front surface of the silicon carbide substrate 1 is covered with a protective film (not shown) for protection, and then, in order to reduce resistance, + The second main surface (rear surface) of the silicon carbide substrate 1 is mechanically ground with a grinder or the like (step S218). + The silicon carbide substrate 1 is thinned.
[0089] Next, n + On the second main surface (rear surface) of the silicon carbide substrate 1, a conductive film serving as the drain electrode 15, for example, a molybdenum film and a nickel film, are successively formed by, for example, a sputtering method. Then, a heat treatment such as laser annealing is performed to form an n + The drain electrode is formed by reacting the silicon carbide substrate 1 with a conductive film to form an ohmic junction (step S219).
[0090] Next, a film of titanium, nickel and gold is formed in this order as a drain electrode pad (not shown) on the surface of the drain electrode 15. In this manner, the trench MOSFET 70 shown in FIG.
[0091] As described above, according to the second embodiment, the rear surface laminated film (the rear surface gate insulating film, the rear surface gate electrode, the rear surface first insulating film, the rear surface interlayer insulating film, the rear surface sensor polycrystalline polysilicon, and the rear surface second insulating film) are removed all at once by dry etching. This can mitigate the influence of wafer warpage caused by the rear surface oxide film and polysilicon, and suppress ESC adsorption errors and transportation errors. In addition, the wet etching process for removing the rear surface laminated film can be omitted. This prevents the SiC substrate, which has high hardness, and the oxide film and polysilicon, which have low hardness, from being ground simultaneously, and therefore prevents uneven grinding and suppresses electrode formation defects.
[0092] The present invention can be modified in various ways without departing from the spirit of the present invention, and in each of the above-mentioned embodiments, for example, the dimensions and impurity concentration of each part are set in various ways according to the required specifications. In addition, in each of the embodiments, the first conductivity type is n-type and the second conductivity type is p-type, but the present invention is similarly valid even if the first conductivity type is p-type and the second conductivity type is n-type. In addition, although the description has been given using a trench-type MOSFET, the present invention is similarly valid for a planar-type MOSFET. [Industrial Applicability]
[0093] INDUSTRIAL APPLICABILITY As described above, the method for manufacturing a silicon carbide semiconductor device according to the present invention is useful for power semiconductor devices used in power conversion devices such as inverters, power supply devices for various industrial machines, and igniters for automobiles. [Explanation of symbols]
[0094] 1n + Silicon carbide substrate 2 1stn - Silicon carbide epitaxial layer 3 1st p. + type area 4 2nd n - Silicon carbide epitaxial layer 5 2nd p. + type area 6 p-type base layer 7 n-type source region 8n + Type Source Area 9 p ++ Mold Contact Area 10. Trench 11 Gate insulating film 12 Gate electrode 13 Interlayer insulating film 14 Source electrode pad 15 Drain electrode 16 Source electrode 20 p-type polysilicon layer 21 n-type polysilicon layer 22 Insulating film on the surface of the gate electrode 23 Gate insulating film on the back surface 24 Gate electrode on the back side 25 First insulating film on the back surface 26 Backside interlayer insulating film 27 Polycrystalline polysilicon for the backside sensor 28 Second insulating film on the back surface 29 Insulating Film 30 Anode electrode 31 Cathode electrode 32 Polycrystalline silicon for sensors 70 Trench MOSFET
Claims
1. a first step of forming a first semiconductor layer of a first conductivity type on a front surface of a silicon carbide semiconductor substrate of a first conductivity type, the first semiconductor layer having an impurity concentration lower than that of the silicon carbide semiconductor substrate; a second step of forming a second semiconductor layer of a second conductivity type on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate; a third step of forming a third semiconductor layer of a first conductivity type on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate; a fourth step of forming a gate electrode on a front surface of the silicon carbide semiconductor substrate via a gate insulating film; a fifth step of forming a first insulating film on a surface of the gate electrode; a sixth step of collectively removing the gate insulating film, the gate electrode, and the first insulating film formed on a back surface of the silicon carbide semiconductor substrate; a seventh step of forming a first electrode on a surface of the third semiconductor layer; an eighth step of forming a second electrode on a back surface of the silicon carbide semiconductor substrate; A method for manufacturing a silicon carbide semiconductor device comprising the steps of:
2. After the fifth step and before the sixth step, a ninth step of forming an interlayer insulating film on the gate electrode; a tenth step of forming polysilicon on the interlayer insulating film; an eleventh step of forming a second insulating film on a surface of the polysilicon; and 2. The method for manufacturing a silicon carbide semiconductor device according to claim 1 , wherein in the sixth step, the gate insulating film, the gate electrode, the first insulating film, the interlayer insulating film, the polysilicon, and the second insulating film formed on a back surface of the silicon carbide semiconductor substrate are collectively removed.
3. 3. The method for manufacturing a silicon carbide semiconductor device according to claim 2, further comprising a twelfth step of forming a sensor portion on a surface of the polysilicon after the sixth step and before the seventh step.
4. 4. The method for manufacturing a silicon carbide semiconductor device according to claim 1, wherein dry etching is used in said sixth step.
5. The method for manufacturing a silicon carbide semiconductor device according to claim 4 , wherein the dry etching is carried out continuously in the same chamber.
6. 5. The method for manufacturing a silicon carbide semiconductor device according to claim 4, wherein the dry etching is performed under the same etching conditions.
7. 7. The method for manufacturing a silicon carbide semiconductor device according to claim 6, wherein the dry etching is performed by chemical dry etching, and the etching conditions are such that a selectivity between the silicon carbide semiconductor substrate and a gate insulating film formed on a back surface of the silicon carbide semiconductor substrate is 100 or more.
8. 2. The method for manufacturing a silicon carbide semiconductor device according to claim 1, further comprising, between said third step and said fourth step, a thirteenth step of selectively forming a first semiconductor region of a first conductivity type in a surface layer of said third semiconductor layer on an opposite side to said silicon carbide semiconductor substrate side.
9. A fourteenth step is further included between the third step and the fourth step, of forming a trench penetrating the second semiconductor layer and the third semiconductor layer and reaching the first semiconductor layer, 2 . The method for manufacturing a silicon carbide semiconductor device according to claim 1 , wherein in the fourth step, the gate insulating film and the gate electrode are formed inside the trench.
10. 4 . The method for manufacturing a silicon carbide semiconductor device according to claim 3 , wherein in said twelfth step, ions are implanted into said polysilicon to form a diode.
Citation Information
Patent Citations
Silicon carbide semiconductor device and method for manufacturing the same
JP2003243654A
Manufacturing method for semiconductor device and method for annealing semiconductor substrate
JP2005209707A
Silicon carbide semiconductor device and its manufacturing method
JP2007066944A
Method of forming trench of silicon carbide semiconductor substrate
JP2009289987A
Semiconductor device
JP2016181583A