Method for repairing concrete structures
By applying calcium and silicate solutions as primers and using a layered laminate structure, the method addresses adhesion issues in concrete repairs, achieving stronger bonding and durability of repair materials.
Patent Information
- Application Number
- JP2020192700
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-19
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-11-19
AI Technical Summary
Conventional methods for repairing concrete structures face challenges in achieving strong adhesion of repair materials to the concrete surface, particularly due to issues like corrosion and cracking, which can lead to weakened bonding and peeling of the repair materials.
A method involving the application of a calcium-containing solution followed by an aqueous silicate solution as primers, combined with a laminate structure composed of multiple layers of sheet-like members, including a multiaxial mesh and nonwoven fabrics, to enhance adhesion and durability of the repair material.
The method improves the adhesion of the repair material to the concrete surface, ensuring stronger bonding and resistance to peeling, while maintaining moisture permeability and fire resistance, thus enhancing the structural integrity of the repaired concrete.
Smart Images

Figure 0007563950000002 
Figure 0007563950000003 
Figure 0007563950000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for repairing a concrete structure. [Background technology]
[0002] Concrete structures have the advantages of being strong, easy to work with, and inexpensive, so many concrete structures were built in Japan, especially during the period of rapid economic growth.Concrete structures have excellent durability, but after many years of use, carbon dioxide from the atmosphere can penetrate into them along with moisture, causing neutralization, and chloride ions contained in sea breezes and droplets of antifreeze can penetrate into them, causing corrosion and expansion, resulting in cracks.
[0003] Methods for repairing such concrete structures are disclosed in, for example, Patent Documents 1-3.
[0004] Fig. 4 is a perspective view showing the concrete structure repair methods disclosed in Patent Documents 1 to 3. Fig. 4 shows a state in which a repair material 1010, in which a laminate of two or more layers of sheet-like members is impregnated with a hardenable liquid component, is adhered to a concrete structure 100. Patent Document 3 also discloses a repair method in which a repair material, in which a laminate is impregnated with a hardenable liquid component, is adhered to a concrete structure and an aqueous modifier solution is applied to the concrete structure. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6641106 [Patent Document 2] JP 2017-186825 A [Patent Document 3] JP 2019-206896 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the conventional concrete structure repair methods as described above, there is room for improvement in the adhesion of the sheet to the concrete structure.
[0007] The present disclosure has been made to solve such problems, and aims to provide a method for repairing a concrete structure that can improve the adhesion of a repair material to the surface of the concrete structure. [Means for solving the problem]
[0008] In order to achieve the above object, the first disclosed method for repairing a concrete structure includes a first application step, a first drying step, a second application step, a second drying step, an attachment step, and a hardening step. In the first application step, a solution containing calcium is applied to the surface of the concrete to be repaired. In the first drying step, the applied solution containing calcium is dried. In the second application step, after the first drying step, a composition containing an aqueous silicate solution is applied to the surface of the concrete. In the second drying step, the applied composition is dried. In the attachment step, a repair material in which a laminate is applied or impregnated with a composition containing an aqueous silicate solution and a pozzolan active substance is attached to the surface of the concrete after the second drying step. In the hardening step, the repair material is hardened after the attachment step.
[0009] Since calcium is often dissolved in deteriorated concrete, simply attaching a repair material to the surface of the concrete may reduce the hardening of the repair material composition on the concrete surface, resulting in weak adhesion.
[0010] In the method for repairing a concrete structure disclosed herein, before applying a repair material to the surface of the concrete, a solution containing calcium is applied as a first primer and allowed to dry, and a composition containing an aqueous silicate solution is applied as a second primer to the surface of the concrete and allowed to dry.
[0011] As a result, the composition that attracts the silicate aqueous solution reacts with the calcium-containing solution and gradually hardens, improving the adhesion of the applied correction material and making the repair material less likely to peel off even on deteriorated concrete structures.
[0012] In addition, the primer (a composition containing a calcium-containing solution and a silicate aqueous solution) that forms the base on which the repair material is applied is inorganic, and therefore non-flammable, and does not impede the non-flammable performance of the repair material. Furthermore, since the composition containing a calcium-containing solution and a silicate aqueous solution is inorganic, it does not form a film or the like and does not impede the moisture permeability of the repair material.
[0013] The concrete structure repair method of the second disclosure is the concrete structure repair method of the first disclosure, wherein the silicate aqueous solution in the second application step and the silicate aqueous solution in the attachment step are sodium silicate aqueous solutions.
[0014] This allows the so-called water glass to be used as a primer and hardener.
[0015] A method for repairing a concrete structure according to a third disclosure is the method for repairing a concrete structure according to the first or second disclosure, in which the calcium-containing solution is an aqueous calcium nitrate solution.
[0016] Because calcium nitrate has high solubility, it is possible to increase the calcium concentration of the solution, which promotes hardening through reaction with a composition containing an aqueous silicate solution and improves the adhesion of the repair material.
[0017] The method for repairing a concrete structure of the fourth disclosure is the method for repairing a concrete structure of any one of the first to third disclosures, in which the laminate has a first layer and a second layer. The first layer is in the form of a sheet in which multifilaments are combined in a multiaxial mesh shape. The second layer is in the form of a sheet formed from a polypropylene spunbond nonwoven fabric. The first layer and the second layer are arranged in this order from the surface side of the concrete.
[0018] This makes it possible to repair concrete structures by coating or impregnating the laminate with a composition containing an aqueous silicate solution and a pozzolanic active substance and attaching the laminate to the concrete structure.
[0019] A fifth disclosure relates to a method for repairing a concrete structure, and is the method for repairing a concrete structure according to the fourth disclosure, wherein the laminate further comprises a third layer. The third layer is in the form of a sheet made of a nonwoven glass fabric and is disposed on the surface side of the concrete of the first layer.
[0020] This allows the repair material to have both strength and adhesion to concrete.
[0021] A concrete structure repair method according to a sixth disclosure is the concrete structure repair method according to any one of the first to fifth disclosures, further comprising a scraping step, in which the surface of the concrete is scraped prior to the first application step.
[0022] This can further improve the adhesion of the repair material. Effect of the Invention
[0023] According to the present disclosure, it is possible to provide a method for repairing a concrete structure that can improve adhesion of a repair material to the surface of a concrete structure. [Brief description of the drawings]
[0024] [Figure 1] FIG. 2 is a diagram showing a state in which a concrete structure has been repaired using a repair material (three-layer structure) according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram showing a state in which a concrete structure has been repaired using a repair material (two-layer structure) according to an embodiment of the present disclosure. [Diagram 3] FIG. 2 is a flow diagram showing a method for repairing a concrete structure according to an embodiment of the present disclosure. [Figure 4] FIG. 1 is a diagram showing a state in which a concrete structure has been repaired using a conventional method for repairing a concrete structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The concrete structure repair method according to the present disclosure will be described below. (Repair material 10, 10´) As shown in Fig. 1, a repair material 10 of the present disclosure is used to repair a concrete structure 100. The repair material 10 includes a liquid hardenable composition and a laminate 4 in which at least two layers of sheet-like members are laminated. The laminate 4 and the hardenable composition may exist separately, but at the time of repair, the laminate 4 is impregnated with the hardenable composition as described below.
[0026] As shown in Fig. 1, an impregnating material layer 5 is formed on a surface 100s of a concrete structure 100 to which a repair material 10 is applied. The impregnating material layer 5 is formed by impregnating a primer, which will be described later, into the concrete structure 100. By providing the impregnating material layer 5, the adhesive strength of the repair material 10 can be improved.
[0027] 1, by attaching the repair material 10 to a portion of the surface 100s of the concrete structure 100 where the impregnating material layer 5 is formed, the hardenable composition of the repair material 10 is applied and impregnated into the surface of the concrete structure 100. Then, the hardenable composition hardens or bonds with the concrete structure, so that the concrete structure 100 can be repaired with the repair material 10.
[0028] (Laminate 4, 4´) The laminate 4 of the repair material 10 is formed by laminating two or more layers of sheet-like members.
[0029] For example, the laminate 4 of the repair material 10 shown in Fig. 1 includes a third layer 3 arranged on an impregnating material layer 5 formed on a concrete structure 100, a first layer 1 arranged on the third layer 3, and a second layer 2 arranged on the first layer 1. The third layer 3, the first layer 1, and the second layer 2 are laminated in this order from the concrete structure 100 side.
[0030] Furthermore, the repair material 10 is not limited to the repair material 10 shown in Fig. 1, and may have a configuration like a repair material 10' shown in Fig. 2. The laminate 4' of the repair material 10' includes a first layer 1 arranged on the impregnating material layer 5 of the concrete structure 100, and a second layer 2 arranged on the first layer 1. The first layer 1 and the second layer 2 are arranged in this order from the concrete structure 100 side.
[0031] (first layer 1) The first layer 1 is preferably a sheet-like member in which multifilaments are combined in a multiaxial mesh shape. The multifilaments are preferably made of long fibers and preferably have a tensile strength of 150 N or more. The value X represented by formula (1) of the sheet-like member in which multifilaments are combined in a multiaxial mesh shape is preferably 2.0 or more, more preferably 2.5 or more, 2.8 or more, or 3.0 or more.
[0032] X = A × B (1) Here, A represents the tensile strength kN / 50 mm in one direction of the sheet-like member, and B represents the number of axes of the sheet-like member. A can take any value by changing the number of multifilaments per 50 mm. B may be in the range of 2 to 4. Among them, A is preferably 0.75 kN or more, and B is preferably 2 to 3.
[0033] With this configuration, the first layer 1 can fulfill the function of a load-bearing layer that receives concrete pieces falling from a concrete structure.
[0034] Examples of the material of the first layer 1 include polyester, polyolefin, vinylon, aramid, carbon fiber, glass fiber, etc. Among them, it is preferable that the first layer 1 is made of a vinylon mesh sheet or a glass mesh sheet. It is preferable to use glass yarn or roving as the long glass fiber. Glass yarn is made by twisting glass fiber to form a ply yarn, and roving is made by bundling glass fibers. Examples of the weaving method of the multiaxial mesh include plain weave, twill weave, entwined weave, and braided fabric. The weaving direction of the multiaxial mesh may be orthogonal biaxial or more multiaxial weave.
[0035] The thickness of the first layer 1 is preferably 0.1 mm or more and 1.5 mm or less, and more preferably 0.3 mm or more and 1 mm or less.
[0036] The first layer is 50g / mm 2 The weight is preferably 60 g / mm or more. 2 More preferably, it is equal to or greater than 75 g / mm 2 That's all.
[0037] By setting the coating weight within this range, the tensile strength can be improved, and sufficient strength of the repair materials 10, 10' can be ensured without causing breakage when concrete pieces fall off.
[0038] The first layer 1 is preferably a biaxial fabric with an opening size of 5 mm or more and 25 mm or less. By setting the opening size within this range, the adhesive strength between the second layer 2 and the concrete structure 100, which will be described later, or between the second layer 2 and the third layer 3, can be improved, and sufficient strength of the repair materials 10, 10' can be ensured. In addition, by setting the number of long fibers per unit area of the first layer 1 to an appropriate number, the resistance of the first layer 1 when it breaks through the second layer 2 can be increased, and sufficient strength of the repair materials 10, 10' can be ensured.
[0039] The first layer 1 has an opening of 5 mm to 25 mm and is 50 g / mm 2It is more preferable that the first layer 1 is a biaxial woven fabric having a basis weight of 150 N or more. It may also be a multiaxial woven fabric having an opening ratio equivalent to that of the biaxial woven fabric. In particular, it is more preferable that the first layer 1 is a sheet-like member of a biaxial or triaxial mesh in which multifilaments having a tensile strength of 150 N or more are combined with an opening of 5 mm to 25 mm.
[0040] (Second layer 2) The second layer 2 is preferably a liquid-permeable sheet-like member. The liquid-permeable sheet-like member preferably has a tear strength of 2.0 N or more. By setting the tear strength to 2.0 N or more, the second layer 2 can fulfill the function of a reinforcing layer that enhances the resistance when the first layer 1 breaks through the second layer 2.
[0041] The shape of the second layer 2 may be woven or nonwoven. Examples of the material of the second layer 2 include polyester, polyolefin, vinylon, aramid, carbon fiber, and glass fiber. Among them, it is preferable that the second layer 2 is made of polypropylene nonwoven or glass nonwoven, and it is particularly preferable that the second layer 2 is made of long fiber nonwoven. Since the glass nonwoven has excellent compatibility with the hardenable composition, the hardenable composition can easily penetrate the glass nonwoven, and when the hardenable composition is hardened, the repair material 10, 10' can be firmly fixed to the concrete structure 100. Examples of suitable glass nonwoven include chopped strand mat, glass paper, and felt.
[0042] When a polypropylene nonwoven fabric is used, the fibers may be subjected to a hydrophilization treatment in order to enhance compatibility with the curable composition. The hydrophilization treatment may be carried out by any method known in the art.
[0043] The thickness of the second layer 2 is preferably 0.1 mm or more and 1.0 mm or less, and more preferably 0.15 mm or more and 0.5 mm or less. By setting the thickness within this range, the second layer 2 fulfills the function of a reinforcing layer that enhances the resistance when the first layer 1 breaks through the second layer 2, and the amount of the curable composition impregnated into the laminates 4, 4' can be reduced, which is also economically advantageous.
[0044] The second layer 2 is 30 g / mm 2 The weight is preferably 50 g / mm or more. 2 More preferably, it is 60 g / mm 2 By setting the coating weight within such a range, the tensile strength can be improved, and sufficient strength of the repair materials 10, 10' can be ensured without causing breakage when concrete pieces fall off.
[0045] The second layer 2 is preferably a biaxial fabric with an opening size of 3 mm or more and 30 mm or less. By setting the opening size within this range, the adhesive strength with the third layer 3 described below can be improved, and sufficient strength of the repair materials 10, 10' can be ensured. In addition, by setting the number of long fibers per unit area of the first layer 1 to an appropriate number, the resistance of the first layer 1 when it breaks through the second layer 2 can be increased, and sufficient strength of the repair materials 10, 10' can be ensured.
[0046] The second layer 2 is preferably a multifilament having a tensile strength of 10 N or more, and more preferably a biaxial or triaxial mesh sheet-like member. Also, it is preferably a sheet-like member having a tear strength of 2.0 N or more.
[0047] When the repair material 10, 10' has a two-layer structure of a first layer 1 and a second layer 2 or a laminated structure of more than two layers, it is preferable that the first layer 1 is a sheet-like member in which multifilaments are combined in a multiaxial mesh shape, and the second layer 2 is a sheet-like member having a tear strength of 2.0 N or more. Furthermore, in the repair material 10, 10', it is preferable that the first layer 1 is a sheet-like member in which multifilaments having a tensile strength of 150 N or more are combined in a multiaxial mesh shape with a mesh opening of 5 mm to 25 mm, and the second layer 2 is a sheet-like member having a tear strength of 2.0 N or more.
[0048] (Third layer 3) The third layer 3 is preferably a liquid-permeable sheet-like member having a porosity of 90% or more, which can ensure the impregnation of the hardenable composition and thus fulfill the function of an adhesive layer that improves the adhesive strength between the repair material 10 and the concrete structure 100.
[0049] The third layer 3 may be in the form of a nonwoven fabric. Materials include polyester, polyolefin, vinylon, aramid, carbon fiber, glass fiber, etc., and is preferably made of polypropylene nonwoven fabric or glass nonwoven fabric. Glass nonwoven fabric has excellent compatibility with the curable composition, so the curable composition can easily penetrate the glass nonwoven fabric, and when the curable composition is cured, the repair material 10 can be firmly fixed to the concrete structure. Suitable glass nonwoven fabrics include chopped strand mat, glass paper, felt, etc.
[0050] When using a polypropylene nonwoven fabric, it is preferable to subject the fiber surface to a surface treatment in order to increase compatibility with the curable composition.
[0051] The thickness of the third layer 3 is preferably 0.1 mm or more and 1.5 mm or less, and more preferably 0.2 mm or more and 0.8 mm or less. When the thickness of the third layer 3 is 0.1 mm or more, the adhesive strength between the repair material 10 and the concrete structure is ensured, and when the thickness is 1.5 mm or less, the amount of the hardenable composition impregnated into the laminates 4, 4' can be reduced, which is economically advantageous.
[0052] In the laminate 4, for example, a glass nonwoven fabric may be used as the third layer 3, a triaxial vinylon mesh may be used as the first layer 1, and a polypropylene spunbond nonwoven fabric may be used as the second layer 2.
[0053] (Integrated stacking) The repair material 10, 10', which is composed of at least two laminated sheet-like members, may be integrated by impregnating them with a curable composition, but it is preferable to integrate them in advance. By integrating them, it is possible to prevent the sheet members from shifting during application and impregnation.
[0054] The integration may be achieved by mechanical fiber entanglement, chemical adhesion, or the like, for example by fulling, needle punching, chemical bonding, thermal bonding, hydroentanglement, or the like.
[0055] 1 shows a case where the repair material 10 has a three-layer structure, but the repair material may have four or more layers. Even in the case where the repair material has four or more layers, it is preferable that the second layer 2 is disposed as a layer outside the first layer 1, counting from the side in contact with the concrete structure 100. This layered structure allows the repair material 10 to have both strength and adhesion to the concrete structure. Note that there is no particular limit to the maximum number of layers in the laminate 4.
[0056] (Curable composition) The hardenable composition (one example of a composition) is applied to and / or impregnated into the laminate 4, 4'. The concrete structure 100 and the repair material 10, 10' can be bonded to each other by applying and / or impregnating the laminate 4, 4' with the hardenable composition and then hardening the hardenable composition. For example, the hardenable composition can be in a liquid form. By bonding the repair material 10, 10', it is possible to prevent concrete pieces from falling off from the deteriorated portion of the concrete structure 100.
[0057] The hardenable composition includes an aqueous silicate solution and a Hozolan active substance. The aqueous silicate solution is, for example, an aqueous solution of sodium silicate, potassium silicate, lithium silicate, or a mixture thereof. In this way, a composition including an aqueous silicate solution and a Hozolan active substance may be referred to as a "geopolymer" hereinafter. The hardenable composition is usually prepared as a liquid composition.
[0058] In this way, by using an inorganic material in the hardenable composition, the fire resistance of the concrete structure 100 can be ensured without being impaired.
[0059] In geopolymers, the difference in specific gravity between the liquid component consisting of the silicate aqueous solution and the solid component consisting of the pozzolanic active substance is smaller than the difference in specific gravity between the water and cement contained in the cement slurry, so separation of the components in the hardenable composition can be suppressed.
[0060] In addition, when sodium silicate and potassium silicate are applied to and / or impregnated into the surface 100s of the concrete structure 100, they can produce a CSH gel with the calcium hydroxide in the concrete, thereby strengthening the adhesive strength between the repair material 10, 10' and the concrete structure 100.
[0061] Such a hardenable composition preferably has a viscosity of 400 to 3000 mPa s at 25° C. By setting the viscosity in this range, it is possible to ensure the impregnation into the laminates 4, 4′. In addition, it is possible to prevent the hardenable composition from dripping when applied to the concrete structure 100.
[0062] In particular, when geopolymers are used, the pozzolanic active substance preferably has an electrical conductivity difference of 0.4 mS / cm or more, more preferably 0.5 mS / cm or more, 0.6, 0 mS / cm or more, or 7 mS / cm or more, and even more preferably 0.8 mS / cm or more, 1.0 mS / cm or more, or 1.2 mS / cm or more.
[0063] By setting the electrical conductivity difference at such a level, the reactivity with the silicate solution can be sufficiently ensured, and the adhesive strength between the repair material 10, 10' and the concrete structure 100 can be increased. The electrical conductivity difference here is an index related to the reactivity of the pozzolanic active substance induced by an alkaline substance, and means the difference in electrical conductivity of the saturated calcium hydroxide aqueous solution before and after the pozzolanic active substance is added. The electrical conductivity difference is calculated as follows. The electrical conductivity of 200 ml of Ca(OH)2 saturated aqueous solution is measured at 40±1°C according to "Cement Concrete Research, Vol.19, pp.63-68, 1989" for the pozzolanic active substance. Next, 5 g of metakaolin is added, stirred, and the electrical conductivity is measured 2 minutes later. The difference from the electrical conductivity before the addition is taken as the electrical conductivity difference.
[0064] A pozzolanic active substance is a substance that hardens by reacting with water and calcium oxide, calcium hydroxide, aluminum hydroxide, etc. Examples of pozzolanic active substances include silica dust, diatomaceous earth, talc, aerosil, white carbon, kaolin, metakaolin, activated clay, acid clay, etc. Among these, metakaolin is preferred.
[0065] It is generally preferred that the pozzolan active substance has a silica content of 40% by weight or more when the silica component is converted into SiO2, or an alumina content of 30% by weight or more when the alumina component is converted into Al2O3.
[0066] The pozzolanic active substance is usually in the form of a lump or powder, and the lump or powdered pozzolanic active substance may be used as is, or may be activated by changing the state of the substance using a method such as thermal spraying, pulverization / classification, or application of mechanical energy.
[0067] The thermal spraying method is a thermal spraying technique that is used for ceramic coating. Examples of the thermal spraying technique include plasma thermal spraying, high-energy gas thermal spraying, and arc thermal spraying. Preferably, the material powder is melted at a temperature of 2000 to 16000°C, sprayed at a speed of 30 to 800 m / s, and sprayed to a powder having a specific surface area of 0.1 to 100 m. 2 It is preferable to use a powder having a particle size of 1 / g.
[0068] Any known method can be used for the pulverization and classification. For pulverization, a jet mill, a roll mill, a ball mill, etc. can be used. For classification, a sieve, specific gravity, wind force, wet sedimentation, etc. can be used. These means can be used in combination.
[0069] Examples of the method of applying mechanical energy include a method using a ball media mill, a media stirring type mill, a roller mill, etc. The applied mechanical energy is preferably 0.5 kWh / kg to 30 kWh / kg in order to minimize the load while providing adequate activation.
[0070] The total content of sodium, potassium, lithium or mixtures thereof derived from the silicate aqueous solution in the hardenable composition, for example, geopolymer, calculated as M2O (M is sodium, potassium and lithium) is preferably 5 to 30% by weight, more preferably 10 to 30% by weight, based on the dry solid content of the hardened material obtained from the hardenable composition. The content of aluminum derived from the pozzolanic active substance is preferably 20 to 40% by weight, more preferably 25 to 35% by weight, based on the dry solid content of the hardened material, calculated as Al2O3.
[0071] Furthermore, in the curable composition, the numerical value n represented by the following formula of an aqueous solution of sodium silicate, potassium silicate, lithium silicate, or a mixture thereof is preferably 0.4 to 1.1, more preferably 0.5 to 1.1, and even more preferably 0.5 to 1.0.
[0072] n=S / M (S: moles of silicon contained in the aqueous solution, M: moles of alkali metal contained in the aqueous solution)
[0073] (Other components of the curable composition) The curable composition may contain additives known in the art in addition to the above components. For example, fillers, modifiers, dispersants, curing time regulators, pigments, antioxidants, polymer emulsions, etc. are included. These are not particularly limited, and known ones can be used. The filler may be any of those generally used as a filling agent.
[0074] Examples of the modifier include carbon, cellulose, mineral fine powder, and synthesized inorganic crystal powder. Examples of the modifier include various metal salts capable of reacting with an aqueous silicate solution, such as light-burned magnesium oxide and zinc oxide. Examples of the polymer emulsion include acrylic rubber, styrene-butadiene rubber, and mixtures thereof.
[0075] These additives can be used in any content within a range that does not impair the intended action of the curable composition. In particular, the polymer emulsion is preferably blended so that the solid weight of the polymer is 3 to 10% by weight based on the total weight of the dry solid content of the curable composition. This improves the fluidity of the curable composition, improves the adhesive strength of the cured product, and suppresses drying shrinkage of the cured product.
[0076] The amount of the curable composition impregnated into the laminates 4, 4' is not particularly limited, and is preferably adjusted so that the curable composition is uniformly held throughout the laminates 4, 4' and the laminates 4, 4' are firmly integrated as a whole by the curing of the curable composition. For example, the mass ratio of the laminate to the curable composition is preferably about 1:4 to 1:12, and more preferably 1:4 to 1:10.
[0077] Also, for example, a geopolymer containing water glass, latex, methacrylonitrile, and blast furnace slag can be used as the hardening composition. In this case, when the laminate 4 uses a glass nonwoven fabric as the third layer 3, a triaxial vinylon mesh as the first layer 1, and a polypropylene spunbond nonwoven fabric as the second layer 2, the curing time can be set to, for example, 7 days or more at 23 degrees and 50% RH.
[0078] (Impregnating material layer 5) The impregnating material layer 5 is formed by applying the following two types of primers to the concrete structure 100, impregnating the concrete structure 100, and then drying the applied primers.
[0079] The impregnating material layer 5 is formed by applying a calcium-containing solution to the surface 100s of the concrete structure 100 as a first primer, and impregnating the concrete structure 100 with the solution. The calcium-containing solution is then dried. Then, as a second primer, a composition containing an aqueous silicate solution is applied onto the dried solution to impregnate the surface, and then dried. The calcium-containing solution and the composition containing an aqueous silicate solution may be dried to a state where they are dry to the touch, for example. Dry to the touch refers to a dry state where the solution or composition does not stick to the finger even when lightly touched with the finger.
[0080] Examples of solutions containing calcium include calcium nitrate aqueous solution, calcium hydroxide aqueous solution, calcium nitrite aqueous solution, calcium chloride aqueous solution, calcium formate aqueous solution, calcium acetate aqueous solution, and calcium sulfate aqueous solution. From the viewpoint of solubility, it is preferable to use calcium nitrate aqueous solution, calcium nitrite aqueous solution, and calcium chloride aqueous solution. From the viewpoint of less influence on reinforced concrete, it is more preferable to use calcium nitrate aqueous solution and calcium nitrite aqueous solution. From the viewpoint of impregnating as much calcium as possible, calcium nitrate hydrate is preferably 50% or more, and more preferably 60 to 70%. It is preferable to use calcium nitrate tetrahydrate because it has high solubility and can prepare a solution with a high calcium concentration. For example, 100 to 300 g / m of 65% calcium nitrate tetrahydrate is used. 2 In this case, it will be dry to the touch in about 90 minutes, depending on the outside temperature and humidity.
[0081] Examples of the silicate solution include an aqueous solution of sodium silicate, potassium silicate, lithium silicate, or a mixture thereof. Sodium silicate and potassium silicate can form a CSH gel with calcium in the solution applied to the surface of the concrete structure 100, and therefore the adhesive strength between the repair material 10, 10' and the concrete structure 100 can be made stronger.
[0082] A composition containing an aqueous sodium silicate solution is a composition containing SiO2 and Na2O, and is water glass.
[0083] For example, water glass (SiO2 / Na2O: molar ratio 1.6, solid content 26.8%) is used at 100 to 200 g / m 2 In this case, it will be dry to the touch in about 180 minutes, depending on the outside temperature and humidity.
[0084] It is preferable to scrape the surface 100s of the concrete structure 100 before applying the calcium-containing solution to the surface 100s.
[0085] <Method of repairing concrete structures> The method for repairing a concrete structure according to the present disclosure can be carried out using the above-mentioned concrete structure repair materials 10, 10'.
[0086] FIG. 3 is a flow diagram showing the concrete structure repair method of the present disclosure.
[0087] As shown in FIG. 3, the concrete structure repair method of the present disclosure includes step S10 (scraping step), step S20 (first application step), step S30 (first drying step), step S40 (second application step), step S50 (second drying step), step S60 (pasting step), and step S70 (hardening step).
[0088] (Step S10 (cleaning process)) In step S10, the surface 100s of the concrete structure 100 to be repaired is scraped with a grinder equipped with a concrete grinding blade.
[0089] (Step S20 (first application step)) In step S20, a solution containing calcium is applied to the surface 100s of the concrete structure 100 that has been subjected to the scraping treatment, and is allowed to permeate the surface 100s of the concrete structure 100.
[0090] Methods for applying and impregnating the calcium-containing solution to the concrete structure 100 include, for example, a hand lay-up method in which application and impregnation are performed manually using a roller, or a method in which application and impregnation are performed by spraying.
[0091] (Step S30 (first drying step)) In step S30, the surface 100s of the concrete structure 100 to which the calcium-containing solution has been applied is dried. When drying, the surface 100s may be left at room temperature, or may be dried with a dryer (for example, a hairdryer).
[0092] (Step S40 (second application step)) In step S40, a composition containing an aqueous silicate solution is applied to and impregnated onto the surface 100s of the concrete structure 100 on which the calcium-containing solution has been dried.
[0093] Methods for applying and impregnating the composition containing the aqueous silicate solution to the concrete structure 100 include, for example, a hand lay-up method in which application and impregnation are performed manually using a roller, or a method in which application and impregnation are performed by spraying.
[0094] (Step S50 (second drying process)) In step S50, the surface 100s of the concrete structure 100 to which the composition containing the silicate aqueous solution has been applied is dried. When drying, the surface 100s may be left at room temperature or may be dried with a dryer (e.g., a hairdryer).
[0095] (Step S60 (Attachment process)) In step S60, the repair material 10, 10' is applied to the surface 100s of the concrete structure 100 that has been coated with a composition containing an aqueous silicate solution and dried.
[0096] In the pasting step, the hardenable composition is applied to the laminates 4, 4', and the laminates 4, 4' are impregnated with the hardenable composition. For example, after applying the hardenable composition to the surface 100s of the concrete structure 100 that has been applied with a composition containing an aqueous silicate solution and dried, the laminates 4, 4' are pasted, and the pasted laminates 4, 4' are applied with the hardenable composition to paste the repair materials 10, 10'.
[0097] The laminates 4, 4' may be formed and then impregnated with the curable composition, or the laminates 4, 4' may be impregnated with the curable composition and then formed, or the laminates 4, 4' may be impregnated with the curable composition while being formed. Also, the laminates 4, 4' may be impregnated with the curable composition either before or after being attached to the target concrete structure.
[0098] Examples of methods for impregnating the laminates 4, 4' with the curable composition include (1) a hand lay-up method in which coating and impregnation are performed manually using a roller, (2) a method of coating and impregnation by spraying, (3) a method of defining the thickness of the laminates 4, 4' using a mold and then coating and impregnating the laminates 4, 4' with the curable composition by pressing, (4) a method of defining the thickness of the laminates 4, 4' using reduced pressure and then impregnating the laminates 4, 4' with the curable composition by reduced pressure injection, (5) a method of immersing the laminates 4, 4' in the curable composition, continuously impregnating the laminates 4, 4' with the curable composition, and then defining the thickness of the laminates 4, 4' using a roll, and (6) a method of continuously coating and impregnating by roll transfer, etc. These may be used in combination.
[0099] In order to improve workability during impregnation and to prevent the impregnated sheets from adhering to each other and to prevent dust from adhering to the impregnated sheets, the front and back surfaces of the laminates 4, 4' may be covered with a resin protective film. This protective film is removed when the laminates are attached to the concrete structure.
[0100] The obtained repair material 10, 10' is applied to the surface 100s of a concrete structure 100 that has been coated with a composition containing an aqueous silicate solution and dried. At this time, it is important to remove air bubbles that have entered between the repair material 10, 10' and the surface of the concrete structure 100, particularly in order to improve adhesion between the repair material 10, 10' and the surface 100s of the concrete structure 100. A suitable method for removing air bubbles is to expel the air bubbles to the outside of the repair material 10, 10' using a roll, a metal spatula, or the like.
[0101] (Step S70 (hardening process)) The hardenable composition impregnated in the laminates 4, 4' is hardened by placing the repair materials 10, 10' in close contact with the concrete structure 100. From the viewpoint of ensuring time for impregnating the surface 100s of the concrete structure 100 with the hardenable composition, the hardening time of the hardenable composition is preferably 30 to 300 minutes, and more preferably 45 to 240 minutes.
[0102] The curing time can be adjusted by the amount of water contained in the curable composition of the present disclosure, since it is an inorganic material. When the curable composition is a geopolymer, the curing time can be adjusted by the content of sodium, potassium, lithium or a mixture thereof derived from the silicate aqueous solution, the ratio (SiO2 / M2O) of SiO2 and M2O (M is sodium, potassium, or lithium) derived from the silicate aqueous solution, the electrical conductivity difference of the pozzolana active substance, the aluminum content, etc.
[0103] When the hardening of the hardenable composition is completed, the repair materials 10, 10' are fixed to the concrete structure 100, and the repair of the concrete structure 100 can be completed. EXAMPLES
[0104] The concrete structure repair method of the present disclosure will be described below using examples.
[0105] Example 1 A concrete wall exposed outdoors for more than 20 years was used as the deteriorated concrete substrate.
[0106] In step S10, the surface of the deteriorated concrete was scraped with a grinder equipped with a concrete grinding blade.
[0107] Next, in step S20, 65% calcium nitrate tetrahydrate is applied to the substrate in an amount of 200 g / m using a roller. 2 and allowed to soak into the deteriorated concrete.
[0108] Next, in step S30, the deteriorated concrete surface was allowed to dry by leaving it at room temperature for 90 minutes.
[0109] Next, 100 g of an aqueous solution of sodium silicate No. 3 as specified in IS K 1408, 25 g of an aqueous solution of 48% by weight of sodium hydroxide, and 53 g of water were added to prepare an aqueous solution of silicate, which was stirred for 24 hours to obtain an aqueous solution of silicate.
[0110] Next, in step S40, the silicate solution is applied to the deteriorated concrete surface that has been treated as described above (applied with 65% calcium nitrate tetrahydrate and dried) in an amount of 150 g / m using a roller. 2 The mixture was applied and impregnated with the solution.
[0111] Next, in step S50, the deteriorated concrete surface was left to stand at room temperature for 180 minutes to dry and perform a base treatment. The base treatment portion corresponds to the impregnating material layer 5.
[0112] Next, 56 g of sodium silicate No. 3 aqueous solution specified by JIS K 1408, 14 g of 48 wt % sodium hydroxide aqueous solution, 30 g of water, and 10 g of latex (manufactured by Nippon A&L Co., Ltd., product name: SR-151) were stirred for 24 hours to obtain an aqueous silicate solution. 77 g of metakaolin (manufactured by BASF, product name: SP-33, electrical conductivity difference 0.8 mS / cm) as a pozzolan active substance and 44 g of ground granulated blast furnace slag specified by JIS A 6206 (manufactured by Nippon Steel & Sumikin Cement Co., Ltd., product name: Esment) were mixed with the above aqueous solution to prepare a hardenable composition.
[0113] Next, we used glass nonwoven fabric (weight 25g / m 2 A triaxial mesh sheet (weight 90 g / m2) made of vinylon multifilament with a thickness of 0.2 mm and a porosity of 95%) 2 , mesh size 8 mm, thickness 0.35 mm, X=3.0) and hydrophilic polypropylene spunbond nonwoven fabric (weight 30 g / m 2 A laminate was prepared by laminating two sheets of the same material (0.2 mm thick, tear strength 16 N).
[0114] The glass nonwoven fabric corresponds to the "third layer," the triaxial mesh sheet corresponds to the "first layer," and the basis weight is 30 g / m 2 The spunbond nonwoven fabric corresponds to the "first layer."
[0115] Next, in step S60, the sheet-like laminate produced above, measuring 300 mm×300 mm, was impregnated with 100 g of a curable composition, and a repair material was applied to the surface of the impregnating material layer 5, which was the base treatment portion.
[0116] Next, in step S70, the hardenable composition impregnated in the laminate attached to the surface 100s of the concrete structure 100 was hardened to prepare a repair material for the deteriorated concrete structure.
[0117] Comparative Example 1 A repair material was prepared in the same manner as in Example 1, except that the steps of applying and drying 65% calcium nitrate tetrahydrate and applying and drying an aqueous silicate solution were omitted.
[0118] Comparative Example 2 Instead of the step of applying and drying 65% calcium nitrate tetrahydrate and the step of applying and drying an aqueous silicate solution in Example 1, CS-21 Neo (a silicate-based surface impregnating material, Aston Co., Ltd.) was applied at 200 g / m 2 The repair material was prepared in the same manner as in Example 1 except for this step.
[0119] Comparative Example 3 Instead of the step of applying and drying 65% calcium nitrate tetrahydrate and the step of applying and drying an aqueous silicate solution in Example 1, CS-21 Builder (a two-liquid mixed silicate-based surface impregnation material, main agent:auxiliary agent=5:1, Aston Co., Ltd.) was applied at 200 g / m 2 The repair material was prepared in the same manner as in Example 1 except for this step.
[0120] Comparative Example 4 Instead of the step of applying and drying 65% calcium nitrate tetrahydrate and the step of applying and drying an aqueous silicate solution in Example 1, CS-21 Builder (a two-liquid mixed silicate-based surface impregnation material, main agent:auxiliary agent=1:1, Aston Co., Ltd.) was applied at 200 g / m 2 The repair material was prepared in the same manner as in Example 1 except for this step.
[0121] Comparative Example 5 A repair material was prepared in the same manner as in Example 1, except that the process of applying and drying 65% calcium nitrate tetrahydrate in Example 1 was omitted.
[0122] (Adhesion strength evaluation) The adhesive strength of the concrete structure repair materials of each Example and Comparative Example to concrete was evaluated using a Kenken-type simplified tensile tester (Technotester R-10000ND). Specifically, the concrete walls to which the repair materials prepared in each Example had been applied were cured outdoors for 7 days, and then the adhesive strength was measured based on the standard method of using the simplified tensile tester. The simplified tensile test was performed on three specimens for each Example and Comparative Example, and the average was taken as the adhesive strength. The results are shown in Table 1.
[0123] For example, the adhesive strength is 1N / mm 2 A value of 1N / mm is considered good. 2 If it is smaller than this, it is not acceptable.
[0124] [Table 1]
[0125] From Example 1 and Comparative Example 1, it can be seen that the adhesive strength of the repair material to the concrete is increased by applying and drying 65% calcium nitrate tetrahydrate, and then applying and drying a composition containing an aqueous silicate solution.
[0126] In Comparative Example 2, CS-21 Neo uses a silicate-based surface impregnation material, but does not use calcium. Since calcium dissolves in deteriorated concrete, it is believed that by applying a solution containing calcium as in Example 1, the adhesive strength is strengthened by the reaction with the silicate solution.
[0127] In Comparative Examples 3 and 4, a silicate-based surface impregnation material is used as the main agent, and calcium hydroxide is used as the auxiliary agent.
[0128] In Comparative Examples 3 and 4, the base agent and auxiliary agent are mixed and then applied to the concrete, but in this Example 1, 65% calcium nitrate tetrahydrate is applied and dried, and then a composition containing an aqueous silicate solution is applied and dried. Therefore, it is considered that the adhesive strength is stronger in Example 1 because the hardening proceeds more gradually than in Comparative Examples 3 and 4.
[0129] In addition, since the solubility of calcium hydroxide is considerably lower than that of calcium nitrate, the calcium concentration is insufficient in Comparative Examples 3 and 4. It is believed that by applying calcium nitrate as in Example 1, the adhesive strength is strengthened by reaction with the silicate aqueous solution.
[0130] In Comparative Example 5, no solution containing calcium was applied. Since calcium is dissolved in deteriorated concrete, it is believed that by applying a solution containing calcium as in Example 1, the adhesive strength is strengthened by the reaction with the silicate solution.
[0131] As described above, the results of the adhesive strength evaluation of the repair materials in the examples confirmed that the concrete repair material disclosed herein can significantly improve the reinforcing performance and adhesion performance of deteriorated concrete. [Explanation of symbols]
[0132] 1 First layer 2 Second layer 3 Third layer 4, 4´ Laminate 10, 10´ Repair materials 100 Concrete Structures 100s surface
Claims
1. A first application step of applying a calcium-containing solution to a surface of concrete to be repaired; a first drying step of drying the applied calcium-containing solution; A second application step of applying a composition containing an aqueous silicate solution to the surface of the concrete after the first drying step; A second drying step of drying the applied composition; a step of applying a repair material obtained by applying or impregnating a laminate with a composition containing a silicate aqueous solution and a pozzolan active substance to the surface of the concrete after the second drying step; a curing step of curing the repair material after the attaching step; A method for repairing a concrete structure comprising the steps of:
2. The silicate aqueous solution in the second application step and the silicate aqueous solution in the attachment step are sodium silicate aqueous solutions. The method for repairing a concrete structure according to claim 1.
3. The calcium-containing solution is an aqueous calcium nitrate solution.
3. The method for repairing a concrete structure according to claim 1 or 2.
4. The laminate comprises: A sheet-like first layer in which multifilaments are combined in a multiaxial mesh shape; A sheet-like second layer formed from a polypropylene spunbond nonwoven fabric, The first layer and the second layer are placed in this order from the surface side of the concrete. The method for repairing a concrete structure according to any one of claims 1 to 3.
5. The laminate further includes a sheet-like third layer formed of a glass nonwoven fabric and arranged on the surface side of the concrete of the first layer. The method for repairing a concrete structure according to claim 4.
6. The method further includes a scraping step of scraping the surface of the concrete before the first application step. The method for repairing a concrete structure according to any one of claims 1 to 5.
Citation Information
Patent Citations
Two-component permeated crystalline concrete crack waterproof repairing liquid and construction method thereof
CN109336531A
Crack repairing agent and waterproofing and repairing construction method for concrete structure, and improving method for concrete
JP1999193638A
Repairing execution method for concrete structure
JP2002235444A
Reaction promotion material used for silicate-based surface impregnation method, and concrete reinforcement method
JP2014201929A
Method for enhancing strength and extending life of existing concrete structure
JP2016188156A