Composition for polishing pad, polishing pad
The use of a sulfur-containing and ester-containing curing agent mixture in polishing pads addresses the issues of scratches, surface defects, and thermal instability in semiconductor CMP processes, enhancing polishing rate and stability.
Patent Information
- Application Number
- JP2023047202
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-20
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-10-23
AI Technical Summary
Existing polishing pads in semiconductor CMP processes suffer from issues such as scratches and surface defects, reduced polishing rate, and decreased thermal stability due to the use of harmful substances like MOCA, which affects the quality of semiconductor substrates.
A composition for polishing pads using a urethane-based prepolymer and a curing agent mixture comprising a sulfur-containing first curing agent and an ester-containing second curing agent, which improves physical properties like hardness and elongation, and enhances thermal stability by minimizing the rate of decrease in storage modulus at high temperatures.
The solution provides polishing pads with improved polishing rate, reduced defects, and enhanced thermal stability, ensuring stable performance over time and temperature changes without using harmful substances like MOCA.
Smart Images

Figure 0007564272000017 
Figure 0007564272000018 
Figure 0007564272000019
Abstract
Description
[Technical field]
[0001] The embodiments relate to a polishing pad composition, a polishing pad, and a method for making the same that can be used in semiconductor chemical mechanical polishing (CMP) processes. [Background technology]
[0002] In the semiconductor manufacturing process, the Chemical Mechanical Polishing (CMP) process involves attaching a semiconductor substrate such as a wafer to a head and bringing it into contact with the surface of a polishing pad formed on a platen. With the head in this state, slurry is supplied to chemically react with the surface of the semiconductor substrate while the platen and head are moved relative to each other to mechanically flatten uneven portions of the semiconductor substrate surface.
[0003] The polishing pad is an essential material that plays an important role in such a CMP process, and generally includes a polishing layer and a support layer made of a polyurethane resin, and has grooves on the surface of the polishing layer that support the large flow of the slurry and pores that support the fine flow. The pores in the polishing layer can be formed by using a solid-phase foaming agent having a fine hollow structure, a liquid-phase foaming agent using a volatile liquid, a gas-phase foaming agent such as an inert gas, or the like, or can be formed by generating gas through a chemical reaction.
[0004] The polishing layer containing the pores directly interacts with the surface of the semiconductor substrate during the CMP process, and thus affects the processing quality of the surface of the semiconductor substrate.
[0005] In particular, the polishing rate and the rate of occurrence of defects such as scratches during the CMP process can vary significantly depending on the components, physical properties, and pore shape of the polishing layer. In addition, high hardness additives in the raw materials that make up the polishing layer can cause scratches and surface defects on the semiconductor substrate during the CMP process. In particular, during the CMP process, which is performed at high temperatures of 50° C. or more, the polishing rate can decrease due to the above-mentioned surface defects, which can degrade the quality of the semiconductor substrate. Therefore, there is a continuous need for research into minimizing scratches and surface defects that occur on the semiconductor substrate during the CMP process and improving the polishing rate.
[0006] In addition, during the CMP process, the thermal stability of the polishing pad may weaken and the polishing rate may decrease during the process at a high temperature of 50°C or more, which may result in a decrease in the quality of the semiconductor substrate. Furthermore, the polishing rate also decreases when polishing is performed for a long time at a high temperature. Therefore, various researches have been conducted to solve the above problems and improve the polishing stability. For example, various methods are known for improving the polishing rate and polishing stability by using 4,4'-methylenebis(2-chloroaniline) (MOCA) as a curing agent. However, although the use of MOCA as a curing agent can improve the physical properties and polishing characteristics to a certain extent, the CMP process used for a long time requires higher thermal stability and contains harmful substances, which is problematic because it has a negative effect on the human body and the environment. Therefore, there is a strong need for research on a composition for a polishing pad and a polishing pad that can improve the polishing stability by reducing the amount of MOCA used or using a curing agent that can replace it, and has excellent thermal stability even at a high temperature of 50°C or more and minimizes the rate of change in the polishing rate even when performed for a long time. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been devised to solve the problems of the prior art. The technical problem to be solved by the present invention is to provide a composition that can ensure excellent elongation and hardness by utilizing a mixed composition of a hardener, improve scratches and surface defects that appear on the surface of a semiconductor substrate, and further improve the polishing rate, a polishing pad using the same, and a manufacturing method thereof.
[0008] In addition, the technical problem to be solved by the present invention is to provide an environmentally friendly composition for a polishing pad, which can improve physical properties such as tensile strength, hardness, and modulus and polishing rate without using 4,4'-methylenebis(2-chloroaniline) (MOCA) by realizing a suitable mixed composition of a curing agent, and can also have excellent thermal stability and further improve polishing stability since the reduction rate of storage modulus is low even at high temperatures, and also provides a polishing pad using the same and a method for manufacturing a semiconductor device using the polishing pad. [Means for solving the problem]
[0009] To achieve the above objective, one embodiment provides a composition comprising a urethane-based prepolymer and a curing agent mixture, the curing agent mixture comprising a sulfur-containing primary curing agent and an ester-containing secondary curing agent.
[0010] Another embodiment provides a composition comprising a urethane-based prepolymer and a curing agent mixture, the curing agent mixture comprising a sulfur-containing first curing agent and an ester-containing second curing agent, the first curing agent being present in greater amounts than the second curing agent.
[0011] Another embodiment provides a composition comprising a urethane-based prepolymer and a curing agent mixture, the curing agent comprising a sulfur-containing first curing agent and an ester-containing second curing agent, the first curing agent being a liquid-phase curing agent containing sulfur, the second curing agent being a solid-phase curing agent containing an ester having two or more benzene rings, and the content of the solid-phase curing agent is equal to or greater than the content of the liquid-phase curing agent by weight.
[0012] Yet another embodiment provides a method for manufacturing a polishing pad, the method including the steps of preparing a first raw material composition containing a urethane-based prepolymer, preparing a second raw material composition containing a sulfur-containing first curing agent and an ester-containing second curing agent, preparing a third raw material composition containing a foaming agent, sequentially or simultaneously mixing the first raw material composition with the second raw material composition and the third raw material composition to prepare a raw material mixture, and injecting the raw material mixture into a mold and curing it.
[0013] Yet another embodiment provides a polishing pad that includes a polishing layer that includes a urethane-based prepolymer and a curing agent mixture, the curing agent mixture including a sulfur-containing first curing agent and an ester-containing second curing agent.
[0014] Yet another embodiment provides a method for manufacturing a semiconductor device, comprising the steps of providing a polishing pad, placing an object to be polished on the polishing pad, and rotating the object to be polished relative to the polishing pad to polish the object, wherein the polishing pad comprises a urethane-based prepolymer and a curing agent mixture, and the curing agent mixture comprises a sulfur-containing first curing agent and an ester-containing second curing agent. Effect of the Invention
[0015] The composition according to the embodiment uses a curing agent mixture containing a sulfur-containing first curing agent and an ester-containing second curing agent, and the physical properties of the polishing pad can be controlled as required. Specifically, the polishing pad manufactured by containing a first curing agent in a content greater than that of the second curing agent in the curing agent mixture can provide a high polishing rate while minimizing the occurrence of defects such as scratches on the surface of a semiconductor substrate during a CMP process. In addition, by containing the second curing agent in the curing agent mixture equal to or greater than the content of the first curing agent, the composition can satisfy physical properties such as tensile strength and modulus within an appropriate range without using 4,4'-methylenebis(2-chloroaniline) (MOCA), and can realize thermal stability by minimizing the decrease rate of storage modulus due to temperature change at high temperatures, thereby further improving polishing stability. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a scanning electron microscope (SEM) image of a cross section of the polishing pad produced in Example 1. [Diagram 2] FIG. 2 is an SEM image of a cross section of the polishing pad produced in Example 3. [Diagram 3] FIG. 3 is an SEM image of a cross section of the polishing pad produced in Example 5. [Figure 4] FIG. 4 is an SEM image of a cross section of the polishing pad produced in Comparative Example 2. [Diagram 5] FIG. 5 shows the stability of the polishing rate with respect to temperature changes for the polishing pads produced in Examples 1 to 5 and Comparative Examples 1 and 2. [Figure 6] FIG. 6 shows the number of defects appearing on the surface of a semiconductor substrate (wafer) after the semiconductor substrate (wafer) was polished using the polishing pads produced in Examples 1 to 5 and Comparative Examples 1 and 2. [Figure 7] FIG. 7 shows the storage modulus as a function of temperature for the polishing pads produced in Examples 1 to 5 and Comparative Examples 1 and 2. As shown in FIG. [Figure 8] FIG. 8 shows a schematic diagram of a semiconductor device manufacturing process according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In the following description of implementation examples, when each layer, pad, etc. is described as being formed "on" or "under" each layer, pad, etc., "on" and "under" include all layers, pads, etc. that are formed "directly" or "indirectly through other components."
[0018] In addition, the reference for the top / bottom of each component will be described based on the drawings. Note that the size of each component in the drawings may be exaggerated for the purpose of explanation and does not refer to the size actually applied.
[0019] In addition, all numerical ranges expressing physical properties, dimensions, and the like of components described in this specification should be understood to be modified in all cases by the term "about" unless otherwise specified.
[0020] As used herein, the term "heteroalkyl," by itself or in combination with other terms, unless otherwise stated, refers to a stable straight or branched chain hydrocarbon radical of the specified number of carbon atoms and from one to three heteroatoms selected from the group consisting of O, N, Si and S, where the nitrogen and sulfur atoms may be optionally oxidized and the nitrogen heteroatom may be optionally quaternized. The heteroatoms O, N and S may be located at any interior position of the heteroalkyl group.
[0021] The term "heterocycloalkyl" refers to a saturated or partially unsaturated ring system radical having a total number of ring atoms from 3 to 10 and containing 1 to 5 heteroatoms selected from N, O and S, where the nitrogen and sulfur atoms as ring atoms are optionally oxidized and the nitrogen atom as a ring atom is optionally quaternized. Unless otherwise specified, a "heterocycloalkyl" can be a monocyclic, bicyclic, spirocyclic or polycyclic ring system. A "heterocycloalkyl" can be attached to the remainder of the molecule by one or more carbon rings or heteroatoms.
[0022] The term "alkylene" by itself or as part of another substituent refers to a divalent radical derived from an alkane, as exemplified by -CH2CH2CH2CH2-.
[0023] The term "heteroalkylene" by itself or as part of another substituent refers to a saturated or unsaturated, or multiply unsaturated divalent radical derived from a heteroalkyl, as exemplified by -CH-CH-S-CH-CH- and -CH-S-CH-CH-NH-CH-, -O-CH-CH=CH-, -CH-CH=C(H)CH-O-CH-, and -S-CH-C≡C-. Heteroatoms can also occupy either or both of the chain termini for a heteroalkylene group (e.g., alkyleneoxy, alkylenedioxy, alkyleneamino, alkylenediamino, and the like). The term "heteroalkylene" can also include mono- and polyhalogenated variants.
[0024] The term "aryl" typically refers to a polyunsaturated aromatic hydrocarbon ring, which may be a single ring or multiple rings (three or fewer rings) fused together, unless otherwise specified. The term "heteroaryl" refers to an aryl ring containing 1 to 5 heteroatoms selected from N, O, and S, where the nitrogen and sulfur atoms are optionally oxidized and the nitrogen atom is optionally quaternized. The heteroaryl group may be attached to the remainder of the molecule through a heteroatom. Non-limiting examples of aryl groups include phenyl, naphthyl, and biphenyl groups, and non-limiting examples of heteroaryl groups include pyridyl, pyridazinyl, pyrazinyl, pyrimidinyl, triazinyl, quinolinyl, quinoxalinyl, quinazolinyl, cinnolinyl, phthalazinyl, benzotriazinyl, purinyl, benzimidazolyl, benzopyrazolyl, benzotriazolyl, benzoisoxazolyl, isobenzofuryl, isoindolyl, indolizyl, and the like. These include an nyl group, a benzotriazinyl group, a thienopyridinyl group, a thienopyrimidinyl group, a pyrazolopyrimidinyl group, an imidazopyridine group, a benzothiazolyl group, a benzofuranyl group, a benzothienyl group, an indolyl group, a quinolyl group, an isoquinolyl group, an isothiazolyl group, a pyrazolyl group, an indazolyl group, a pteridinyl group, an imidazolyl group, a triazolyl group, a tetrazolyl group, an oxazolyl group, an isoxazolyl group, a thiadiazolyl group, a pyrrolyl group, a thiazolyl group, a furyl group, and a thienyl group.
[0025] [Composition] One implementation of the present invention provides a composition that includes a urethane-based prepolymer and a curing agent mixture, the curing agent mixture including a sulfur-containing primary curing agent and an ester-containing secondary curing agent.
[0026] [When the first hardener is contained in a larger amount than the second hardener] Specifically, one embodiment provides a composition comprising a urethane-based prepolymer and a curing agent mixture, the curing agent mixture comprising a sulfur-containing first curing agent and an ester-containing second curing agent, the first curing agent being present in an amount greater than the second curing agent.
[0027] According to one embodiment, the use of a curing agent mixture including the sulfur-containing first curing agent and the ester-containing second curing agent can improve the polishing rate and physical properties. In particular, the content of the first curing agent in the curing agent mixture is greater than the content of the second curing agent, which can minimize the occurrence of defects such as scratches that may occur on the surface of a semiconductor substrate during a CMP process and can further improve the polishing rate.
[0028] The first curing agent may include one or more selected from the group consisting of 3,5-dimethylthio-2,6-diaminotoluene, 2,6-bis(methylthio)-4-methyl-1,3-benzenediamine, molybdenum sulfide, niobium sulfide, talc (hydrated magnesium silicate), tantalum sulfide, and tungsten disulfide.
[0029] According to one embodiment of the present invention, by including a sulfur-containing compound in the polishing pad, the physical properties such as the elongation and hardness of the polishing pad are changed, and in particular, the thermal properties can be improved, as well as scratches and surface defects that appear on the surface of the semiconductor substrate can be improved.
[0030] The content of the first curing agent may be 11 to 18 parts by weight, 11 to 17 parts by weight, 12 to 16 parts by weight, 11 to 14 parts by weight, or 14 to 18 parts by weight based on 100 parts by weight of the composition. If the content of the first curing agent exceeds the above range, the thermal properties at high temperatures may decrease or the hardness may be too weak, which may cause problems in the CMP processability, and if the content of the first curing agent is less than the above range, the elongation rate may decrease, which may increase the rate of scratches and surface defects appearing on the semiconductor substrate surface, and the polishing rate may decrease.
[0031] The second curing agent may include at least one selected from the group consisting of compounds of the following Formula 1, Formula 2, and Formula 3:
[0032] [C1] JPEG0007564272000001.jpg2984[2] JPEG0007564272000002.jpg3186[3] JPEG0007564272000003.jpg3649
[0033] In the above Chemical Formula 1, L1 is at least one selected from a linear or branched alkylene group having 1 to 20 carbon atoms, a linear or branched heteroalkylene group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkylene group having 5 to 30 carbon atoms, a substituted or unsubstituted heterocycloalkylene group having 5 to 30 carbon atoms, a substituted or unsubstituted arylene group having 5 to 30 carbon atoms, and a substituted or unsubstituted heteroarylene group having 5 to 30 carbon atoms.
[0034] In addition, in the above Chemical Formula 2, L2 is at least one selected from a linear or branched alkylene group having 1 to 20 carbon atoms, a linear or branched heteroalkylene group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkylene group having 5 to 30 carbon atoms, a substituted or unsubstituted heterocycloalkylene group having 5 to 30 carbon atoms, a substituted or unsubstituted arylene group having 5 to 30 carbon atoms, and a substituted or unsubstituted heteroarylene group having 5 to 30 carbon atoms.
[0035] In addition, R1 and R2 are each independently at least one selected from a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 5 to 30 carbon atoms, a substituted or unsubstituted heterocycloalkyl group having 5 to 30 carbon atoms, a substituted or unsubstituted aryl group having 5 to 30 carbon atoms, and a substituted or unsubstituted heteroaryl group having 5 to 30 carbon atoms.
[0036] In addition, in the above Chemical Formula 3, R3 is at least one selected from a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched heteroalkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 5 to 30 carbon atoms, a substituted or unsubstituted heterocycloalkyl group having 5 to 30 carbon atoms, a substituted or unsubstituted aryl group having 5 to 30 carbon atoms, and a substituted or unsubstituted heteroaryl group having 5 to 30 carbon atoms.
[0037] The second curing agent is selected from the group consisting of 1,3-propanediol bis(4-aminobenzoate) (PDPAB), [4-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate, [4-(4-aminobenzoyl)oxybutyl]4-aminobenzoate, {4-[4-(4-aminobenzoyl)oxy-3-methylbutoxy]butyl}4-aminobenzoate, methylene bis(methylanthranilate) (MBNA), and isobutyl 3,5-diamino-4-chlorobenzoate. 4-chlorobenzoate, BDACB), and specifically may include 1,3-propanediol bis(4-aminobenzoate) (PDPAB).
[0038] The secondary curing agent may contain ester groups to provide increased hardness, tensile strength, and modulus at elevated temperatures, improved thermal properties, and improved wear properties of the CMP pad.
[0039] The content of the second curing agent may be 1 to 10 parts by weight, 2 to 10 parts by weight, 3 to 8 parts by weight, 2 to 5 parts by weight, or 5 to 10 parts by weight based on 100 parts by weight of the composition. If the content of the second curing agent exceeds the above range, the elongation rate may be high, the rate of scratches and surface defects appearing on the surface of the semiconductor substrate may increase, and the polishing rate may decrease. If the content is below the above range, the thermal properties at high temperatures may decrease or the hardness may be too weak, which may cause problems in the CMP processability.
[0040] In this way, by mixing the first and second curing agents together, excellent hardness and elongation can be secured even at high temperatures, and polishing properties can be improved. In addition, when the first curing agent is contained in a larger amount than the second curing agent in the curing agent mixture, the hardness can be appropriately adjusted to improve scratches and surface defects that appear on the surface of the semiconductor substrate, and the polishing rate can be further improved.
[0041] The content ratio of the first curing agent and the second curing agent may be 1:0.1-0.9 by weight, 1:0.1-0.5 by weight, 1:0.1-0.4 by weight, or 1:0.5-0.9 by weight. If the content of the first curing agent is too high and out of the range, the thermal properties at high temperatures may be reduced or the hardness may be too weak, which may cause problems in the CMP processability, and if the content of the first curing agent is too low and out of the range, the elongation rate may be too high, which may significantly increase the rate of scratches and surface defects appearing on the surface of the semiconductor substrate, and the polishing rate may be reduced.
[0042] [When the second hardener is the same or greater than the first hardener] Another embodiment provides a composition comprising a urethane-based prepolymer and a curing agent mixture, the curing agent comprising a sulfur-containing first curing agent and an ester-containing second curing agent, the first curing agent being a liquid-phase curing agent containing sulfur, the second curing agent being a solid-phase curing agent containing an ester having two or more benzene rings, and the content of the solid-phase curing agent is equal to or greater than the content of the liquid-phase curing agent by weight.
[0043] According to one embodiment of the present invention, the thermal properties at high temperatures (50° C. to 100° C.) can be improved by using a curing agent mixture containing the sulfur-containing liquid-phase curing agent and the ester-containing solid-phase curing agent having two or more benzene rings. In particular, the content of the solid-phase curing agent (second curing agent) in the curing agent mixture is equal to or greater than the content of the liquid-phase curing agent (first curing agent), thereby minimizing the decrease rate of the storage modulus due to temperature change, and further improving the thermal stability and the stability of the polishing rate.
[0044] The liquid curing agent is a compound containing sulfur and may contain two or more sulfur elements in a molecule, specifically, may contain two sulfur elements in a molecule.
[0045] The liquid curing agent may contain an active hydrogen group, which may include at least one selected from the group consisting of an amine group (-NH2), a hydroxyl group (-OH), a carboxylic acid group (-COOH), an epoxy group, and combinations thereof, and may specifically include an amine group (-NH2).
[0046] The liquid phase curing agent may have a weight average molecular weight of 50 g / mol to 300 g / mol, for example, 100 g / mol to 250 g / mol, for example, 150 g / mol to 250 g / mol, for example, 200 g / mol to 250 g / mol.
[0047] The liquid-phase hardener may be in a liquid phase at room temperature, or may have a boiling point (bp) of 160°C to 240°C, specifically 170°C to 240°C, more specifically 170°C to 220°C.
[0048] Examples of the liquid phase curing agent may include one or more selected from the group consisting of 3,5-dimethylthio-2,6-diaminotoluene and 2,6-bis(methylthio)-4-methyl-1,3-benzenediamine.
[0049] According to one embodiment, by including a sulfur-containing compound in the polishing pad, the physical properties such as elongation rate and hardness of the polishing pad can be changed, thereby improving the polishing rate and cutting rate, and in particular, not only can the thermal properties be improved, but also scratches and surface defects that appear on the surface of the semiconductor substrate can be improved.Furthermore, since excellent physical properties can be achieved without using MOCA containing harmful substances, an excellent polishing pad that is environmentally friendly can be realized.
[0050] The content of the liquid phase hardener may be 5 parts by weight to 30 parts by weight, for example, 10 parts by weight to 30 parts by weight, for example, 15 parts by weight to 25 parts by weight, for example, 18 parts by weight to 23 parts by weight, based on 100 parts by weight of the composition. When the content of the liquid phase hardener satisfies the above range, appropriate tensile strength and modulus can be achieved, and the decrease rate of storage modulus due to temperature change at high temperatures can be minimized, thereby improving polishing stability.
[0051] The solid-phase hardener may be an ester-containing solid-phase hardener having two or more benzene rings. Specifically, the solid-phase hardener may contain two or more ester groups having a benzene ring in the molecule, and more specifically, may contain two ester groups having a benzene ring in the molecule. When the solid-phase hardener has two or more benzene rings, the molecular structure is harder than when the solid-phase hardener has one benzene ring, and the hardness of the cured product as a whole may be improved, thereby improving heat resistance and hardness.
[0052] The solid-phase hardener may also contain an active hydrogen group. The solid-phase hardener may include an amine group (-NH2) as the active hydrogen group.
[0053] The weight average molecular weight of the solid-phase curing agent may be 150 g / mol to 400 g / mol, for example, 150 g / mol to 350 g / mol, for example, 200 g / mol to 350 g / mol, for example, 250 g / mol to 350 g / mol, for example, 300 g / mol to 350 g / mol. The melting point (mp) of the solid-phase curing agent may be 100°C to 150°C, for example, 100°C to 140°C, for example, 110°C to 130°C.
[0054] The solid-phase hardener may include at least one selected from the group consisting of the compounds of Chemical Formula 1 and Chemical Formula 2.
[0055] [C1] JPEG0007564272000004.jpg2984[2] JPEG0007564272000005.jpg3186
[0056] L1, L2, R1, and R2 are as in the previous operation. Specifically, the solid-phase curing agent is 1,3-propanediol bis(4-aminobenzoate) (PDPAB), [4-(4-aminobenzoyl)oxyphenyl]4-aminobenzoate, [4-(4-aminobenzoyl)oxybutyl]4-aminobenzoate, {4-[4-(4-aminobenzoyl)oxy-3-methylbutoxy]butyl}4-aminobenzoate, and methylene bis(methyl anthranilate). The compound may include one or more selected from the group consisting of 1,3-propanediol bis(4-aminobenzoate) (PDPAB), specifically 1,3-propanediol bis(4-aminobenzoate) (MBNA).
[0057] The solid-phase hardener contains an ester group and two or more benzene rings, and thus has excellent tensile strength, modulus, and hardness at high temperatures, and has a low rate of change in polishing speed and a low rate of decrease in storage modulus as the temperature rises to a high temperature of 50°C to 100°C, particularly 50°C to 70°C, or as time passes, and therefore can further improve polishing stability. In addition, the solid-phase hardener does not contain a halogen group, unlike 4,4'-methylenebis(2-chloroaniline) (MOCA) which contains a halogen group, such as chlorine (Cl), in one benzene ring, and is therefore preferable from the viewpoint of being relatively environmentally friendly.
[0058] The content of the solid-phase hardener may be 8.5 parts by weight to 35 parts by weight, for example, 10 parts by weight to 30 parts by weight, for example, 15 parts by weight to 30 parts by weight, for example, 18 parts by weight to 28 parts by weight, for example, 18 parts by weight to 25 parts by weight, based on 100 parts by weight of the composition. When the content of the solid-phase hardener satisfies the above range, appropriate tensile strength and modulus can be achieved, and the decrease rate of the storage modulus due to temperature change at high temperatures can be minimized, and thermal stability and polishing stability can be improved.
[0059] In this way, by mixing the liquid-phase hardener and the solid-phase hardener together, it is possible to improve the physical properties and polishing characteristics that are environmentally friendly and excellent even at high temperatures without using 4,4'-methylenebis(2-chloroaniline) (MOCA). In addition, if the content of the solid-phase hardener in the hardener mixture is equal to or greater than the content of the liquid-phase hardener, it is possible to reduce the rate of change in the polishing rate due to high temperature and long-term polishing, thereby improving thermal stability. For this purpose, the content ratio of the solid-phase hardener and the liquid-phase hardener may be important.
[0060] The content ratio of the solid-phase hardener and the liquid-phase hardener may be 1:0.1-1 by weight, 1:0.2-1 by weight, 1:0.2-0.8 by weight, 1:0.2-0.7 by weight, 1:0.1-0.5 by weight, 1:0.1-0.4 by weight, or 1:0.1-0.25 by weight. If the content of the liquid-phase hardener is too high or the content of the solid-phase hardener is too low and falls outside the above range, the storage modulus may be excessively reduced as the temperature increases, and the thermal properties may be reduced, adversely affecting the polishing stability. If the content of the liquid-phase hardener is too low or the content of the solid-phase hardener is too high and falls outside the above range, the modulus may be excessively increased and the elongation may be excessively reduced.
[0061] Meanwhile, a composition according to one embodiment includes a urethane-based prepolymer. A prepolymer generally refers to a polymer having a relatively low molecular weight whose polymerization degree is stopped at an intermediate stage in order to facilitate molding in the manufacture of a final molded product. The prepolymer can be molded by itself or after reacting with other polymerizable compounds. Specifically, the urethane-based prepolymer includes a prepolymerization reaction product of one or more diisocyanate monomers and one or more polyols.
[0062] The one or more diisocyanate monomers may be one or more aromatic diisocyanate monomers and / or one or more aliphatic or cycloaliphatic diisocyanate monomers. For example, the isocyanate may be one or more isocyanates selected from the group consisting of toluene diisocyanate (TDI), 1,5-naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), tolidine diisocyanate (TODI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), dicyclohexylmethane diisocyanate (H12MDI), isophorone diisocyanate (IPDI), and the like.
[0063] The polyol refers to a compound having two or more hydroxyl groups, and may include monomolecular polyols and polymeric polyols.
[0064] Examples of the monomolecular polyol include at least one selected from the group consisting of ethylene glycol (EG), diethylene glycol (DEG), propylene glycol (PG), propanediol (PDO), and methylpropanediol (MP-diol), and examples of the polymer polyol include at least one selected from the group consisting of polytetramethylene ether glycol (PTMEG), polyether polyol, polyester polyol, polycarbonate polyol, and polycaprolactone polyol. The polymer polyol may have a weight average molecular weight of 300 g / mol to 3000 g / mol.
[0065] The urethane-based prepolymer may have an isocyanate end group content (NCO%) of 6% to 12% by weight, 6% to 11% by weight, 6% to 10% by weight, 8% to 10% by weight, or 8% to 9% by weight.
[0066] In addition, the urethane-based prepolymer and the curing agent mixture may have an equivalent ratio of reactive groups in their respective molecules, for example, an equivalent ratio of the isocyanate terminal group of the urethane-based prepolymer and the NH2 group of the first curing agent and the second curing agent in the curing agent mixture of 1:0.7 to 1, specifically, an equivalent ratio of 1:0.75 to 1. If the equivalent ratio of the isocyanate terminal group of the urethane-based prepolymer and the NH2 group in the curing agent mixture is outside the above range, it may cause a problem in controlling the hardness intended in the present invention, and thus the physical properties including the polishing rate of the polishing pad may be reduced.
[0067] In addition, the curing agent mixture may further include other commonly used curing agents in addition to the first curing agent and the second curing agent. The other curing agents may be, for example, one or more of amine compounds and alcohol compounds. Specifically, the other curing agents may include one or more compounds selected from the group consisting of aromatic amines, aliphatic amines, aromatic alcohols, and aliphatic alcohols.
[0068] For example, the other curing agent may be one or more selected from the group consisting of diethyltoluenediamine (DETDA), diaminodiphenylmethane, diaminodiphenylsulfone, m-xylylenediamine, isophoronediamine, ethylenediamine, diethylenetriamine, triethylenetetramine, polypropylenediamine, polypropylenetriamine, ethylene glycol, diethylene glycol, dipropylene glycol, butanediol, hexanediol, glycerine, trimethylolpropane, and bis(4-amino-3-chlorophenyl)methane.
[0069] The composition may further comprise one or more additives selected from the group consisting of foaming agents and surfactants.
[0070] There are no particular limitations on the foaming agent, so long as it is one that is commonly used to form pores in a polishing pad.
[0071] For example, the foaming agent may be one or more selected from a solid-phase foaming agent having a hollow structure, a liquid-phase foaming agent using a volatile liquid, and an inert gas.
[0072] The solid-phase foaming agent may be a microcapsule whose size has been adjusted by thermal expansion (hereinafter referred to as "thermally expanded microcapsule"). The thermally expanded microcapsule may be obtained by heating and expanding a thermally expandable microcapsule. The thermally expanded microcapsule has an advantage that the particle size of the pores can be uniformly adjusted by having a uniform particle size as a pre-expanded microballoon structure. Specifically, the solid-phase foaming agent may be a microballoon structure having an average particle size of 5 μm to 200 μm.
[0073] The thermally expandable microcapsule may include an outer shell containing a thermoplastic resin and a foaming agent enclosed inside the outer shell. The thermoplastic resin may be one or more selected from the group consisting of vinylidene chloride copolymers, acrylonitrile copolymers, methacrylonitrile copolymers, and acrylic copolymers. Furthermore, the foaming agent may be one or more selected from the group consisting of hydrocarbons having 1 to 7 carbon atoms.
[0074] The solid-phase blowing agent may be used in an amount of 0.1 to 2.0 parts by weight based on 100 parts by weight of the composition. Specifically, the solid-phase blowing agent may be used in an amount of 0.5 to 1.5 parts by weight, or 0.8 to 1.4 parts by weight based on 100 parts by weight of the composition.
[0075] Meanwhile, the liquid foaming agent is added during the process of mixing and reacting the prepolymer and the curing agent to form pores, but is not involved in the reaction between the prepolymer and the curing agent.The liquid foaming agent is physically vaporized by heat generated during the process of mixing and reacting the prepolymer and the curing agent to form pores.
[0076] The liquid phase blowing agent may include two or more volatile liquid phase blowing agents having different boiling points. Specifically, the volatile liquid phase blowing agent may include one or more low boiling point liquid phase blowing agents and one or more high boiling point liquid phase blowing agents.
[0077] The volatile liquid phase blowing agent does not react with isocyanate, amide, and alcohol groups and may be in the liquid phase at 25°C. Specifically, the volatile liquid phase blowing agent may be selected from the group consisting of trichlorofluoromethane, 2,2-dichloro-1,1,1-trifluoroethane, 1,1-dichloro-1-fluoroethane, cyclopentane, n-pentane, cyclohexane, n-butyl acetate, bis(nonafluorobutyl)(trifluoromethyl)amine; and perfluoro compounds such as perfluorotributylamine, perfluoro-N-methylmorpholine, fluorotripentylamine, and perfluorohexane.
[0078] Commercially available examples of the perfluoro compound include FC-40 (3M), FC-43 (3M), FC-70 (3M), FC-72 (3M), FC-770 (3M), FC-3283 (3M), and FC-3284 (3M).
[0079] The low-boiling liquid phase blowing agent is vaporized in the early stage of the reaction to form mesopores having an average particle size of 45 μm to 90 μm. Specifically, the low-boiling liquid phase blowing agent may have a boiling point of 30° C. to 100° C. at 1 atmospheric pressure. More specifically, the low-boiling liquid phase blowing agent may have a boiling point of 40° C. to 70° C. at 1 atmospheric pressure. More specifically, the low-boiling liquid phase blowing agent may be one or more selected from the group consisting of trichlorofluoromethane, 2,2-dichloro-1,1,1-trifluoroethane, 1,1-dichloro-1-fluoroethane, cyclopentane, cyclohexane, n-pentane, perfluoro-N-methylmorpholine, and perfluorohexane. Commercially available low-boiling liquid phase blowing agents include FC-72 (3M), FC-770 (3M), and FC-3284 (3M).
[0080] The high-boiling liquid phase blowing agent can form micropores having an average particle size of 20 μm to 50 μm by delayed vaporization. Specifically, the high-boiling liquid phase blowing agent can have a boiling point of 100° C. to 250° C. at 1 atmospheric pressure. More specifically, the high-boiling liquid phase blowing agent can have a boiling point of 100° C. to 200° C. at 1 atmospheric pressure. More specifically, the high-boiling liquid phase blowing agent can be one or more selected from the group consisting of n-butyl acetate, bis(nonafluorobutyl)(trifluoromethyl)amine, perfluorotributylamine, and perfluorotripentylamine. Commercially available high-boiling liquid phase blowing agents include FC-40 (3M), FC-43 (3M), FC-70 (3M), and FC-3283 (3M).
[0081] The low-boiling point liquid phase blowing agent and the high-boiling point liquid phase blowing agent may have a boiling point difference of 20° C. to 80° C., specifically, 50° C. to 80° C. Specific examples of combinations of a low-boiling point liquid phase blowing agent and a high-boiling point liquid phase blowing agent include combinations of cyclopentane and n-butyl acetate, and trichlorofluoromethane and bis(nonafluorobutyl)(trifluoromethyl)amine.
[0082] The volatile liquid phase blowing agent may contain a low boiling point liquid phase blowing agent and a high boiling point liquid phase blowing agent in a molar ratio of 1:0.5 to 2. Specifically, the volatile liquid phase blowing agent may contain a low boiling point liquid phase blowing agent and a high boiling point liquid phase blowing agent in a molar ratio of 1:0.8 to 1.2. The liquid phase blowing agent may be added in an amount of 1 to 10 parts by weight per 100 parts by weight of the urethane-based prepolymer. Also, the liquid phase blowing agent may be added in an amount of 2 to 8 parts by weight per 100 parts by weight of the urethane-based prepolymer.
[0083] The gas-phase blowing agent may include an inert gas, and the type of the inert gas is not particularly limited as long as it is a gas that is not involved in the reaction between the urethane-based prepolymer and the curing agent. For example, the inert gas may be one or more selected from the group consisting of nitrogen gas (N2), carbon dioxide gas (CO2), argon gas (Ar), and helium (He). Specifically, the inert gas may be nitrogen gas (N2) or carbon dioxide gas (CO2).
[0084] The inert gas may be introduced in a volume equivalent to 10% to 30% of the total volume of the composition. Specifically, the inert gas may be introduced in a volume equivalent to 15% to 30% of the total volume of the composition.
[0085] The surfactant may prevent the pores from overlapping and clumping together. Specifically, the surfactant may be a silicone-based nonionic surfactant, but may be selected from a variety of other surfactants depending on the properties required for the polishing pad.
[0086] As the silicone-based nonionic surfactant, a silicone-based nonionic surfactant having a hydroxyl group may be used alone, or may be used together with a silicone-based nonionic surfactant not having a hydroxyl group.
[0087] The silicone nonionic surfactant having a hydroxyl group is not particularly limited as long as it has excellent compatibility with isocyanate-containing compounds and active hydrogen compounds and is widely used in the polyurethane technical field. Commercially available silicone nonionic surfactants having a hydroxyl group include, for example, DOW CORNING-193 (silicone glycol copolymer, liquid phase; specific gravity at 25° C.: 1.07; viscosity at 20° C.: 465 mm 2 / s; flash point: 92°C) (hereinafter referred to as DC-193).
[0088] The commercially available silicone-based nonionic surfactant not having a hydroxyl group is, for example, DOW CORNING-190 (a silicone glycol copolymer, Gardner color number: 2; specific gravity at 25° C.: 1.037; viscosity at 25° C.: 2000 mm 2 / s; Flash point: 63°C or higher; Inverse solubility Point (1.0% aqueous solution): 36°C) (hereinafter referred to as DC-190).
[0089] The surfactant may be included in an amount of 0.1 to 2 parts by weight based on 100 parts by weight of the composition. Specifically, the surfactant may be included in an amount of 0.2 to 0.8 parts by weight, 0.2 to 0.7 parts by weight, 0.2 to 0.6 parts by weight, or 0.2 to 1.5 parts by weight based on 100 parts by weight of the composition. When the surfactant is included in an amount within the above range, pores derived from the gas phase blowing agent may be stably formed and maintained in the mold.
[0090] [Gelation time] The composition containing the curing agent mixture requires a certain period of time to gel through curing, which is called the gel time.
[0091] According to one embodiment, when the first curing agent is contained in a larger amount than the second curing agent, the gel time of the composition may be 50 seconds or more, 70 seconds or more, 80 seconds or more, or 100 seconds or more. For example, the gel time of the composition may be 50 seconds to 200 seconds, 50 seconds to 150 seconds, 50 seconds to 100 seconds, 100 seconds to 200 seconds, or 150 seconds to 200 seconds. As a specific example, the composition may have a gel time of 80 seconds to 120 seconds. The gel time may be, for example, a value measured at 70°C.
[0092] According to one implementation, when the second curing agent is present in an amount equal to or greater than the first curing agent, the gel time of the composition is as described above.
[0093] [Properties after curing] After curing, the composition may have the following physical properties adjusted to specific ranges.
[0094] According to one embodiment, when the first curing agent is contained in a larger amount than the second curing agent, the mechanical properties such as tensile strength, elongation, hardness, etc. after the composition is cured can be adjusted to a specific range.
[0095] Specifically, the tensile strength of the composition after curing is 5N / mm 2 ~30N / mm 2 , 10N / mm 2 ~25N / mm 2 , 10N / mm 2 ~20N / mm 2 , 15N / mm 2 ~30N / mm 2 or 17N / mm 2 ~23N / mm 2 It could be.
[0096] The elongation of the composition after curing may be 50% to 300%, 80% to 300%, 90% to 200%, or 100% to 150%.
[0097] The hardness of the composition after curing may be 30 Shore D to 80 Shore D, 40 Shore D to 70 Shore D, 50 Shore D to 70 Shore D, 40 Shore D to 60 Shore D, or 50 Shore D to 60 Shore D.
[0098] The modulus of the composition after curing may be from 40 MPa to 150 MPa, from 50 MPa to 120 MPa, from 50 MPa to 110 MPa, or from 50 MPa to 100 MPa.
[0099] As a specific example, the composition may have a modulus of 50 MPa to 120 MPa and an elongation of 90% to 200% after curing. 2 ~23N / mm 2 The material may have a tensile strength of 90% to 200%, an elongation of 90% to 200%, a hardness of 50 Shore D to 60 Shore D, and a modulus of 50 MPa to 120 MPa.
[0100] The composition may have a large number of micropores after curing. The average size of the micropores may be 10 μm to 50 μm, 20 μm to 50 μm, 20 μm to 40 μm, 20 μm to 30 μm, or 30 μm to 50 μm.
[0101] In addition, the composition may have a removal rate after curing of 3000 Å / min to 5000 Å / min, 3000 Å / min to 4000 Å / min, 3500 Å / min to 4000 Å / min, 3500 Å / min to 3800 Å / min, 3500 Å / min to 3770 Å / min, or 3600 Å / min to 3760 Å / min when polished for 1 hour at about 50° C. to 60° C. In particular, the composition may exhibit stable thermal properties even at high temperatures after curing.
[0102] Furthermore, after curing, the composition may have a hardness of 50 Shore D to 60 Shore D, 50 Shore D to 58 Shore D, and 40 Shore D to 55 Shore D at temperatures of 30° C., 50° C., and 70° C., respectively. Specifically, the hardness of the composition may be 55 Shore D to 60 Shore D, 52 Shore D to 55 Shore D, and 43 Shore D to 49 Shore D at temperatures of 30° C., 50° C., and 70° C., respectively.
[0103] After curing, the composition may have a hardness difference at a temperature of 30°C to 70°C of 5 Shore D to 15 Shore D, specifically 6 Shore D to 12 Shore D, and more specifically 7 Shore D to 12 Shore D.
[0104] After the composition is cured, the number of surface defects on the semiconductor substrate at a temperature of 50° C. to 60° C. may be 10 or less, 5 or less, or 4 or less. The number of defects may be based on the total area of the semiconductor substrate, specifically the wafer to be polished. For example, the size of the wafer may be 300 mm in diameter (excluding 3 mm edges), but the size may be variously changed depending on the desired purpose.
[0105] The composition according to one embodiment has excellent physical properties, particularly elongation, and can be useful in manufacturing polishing pads because it provides a high polishing rate while minimizing the occurrence of defects such as scratches on the surface of a semiconductor substrate.
[0106] According to one embodiment, when the second curing agent is contained in the same amount or more than the first curing agent, the mechanical properties such as storage modulus, tensile strength, elongation, hardness, etc. of the composition after curing can be adjusted to a specific range.
[0107] According to one embodiment, the composition has a storage modulus of 2.3×10 at a temperature of 60° C. to 80° C., specifically at a temperature of 70° C., after curing. 8 Pa or more, specifically 2.4×10 8 Pa~3.25×10 8 Pa, more specifically 2.5 × 10 8 Pa~3.2×10 8The storage modulus of the composition may be in the range of 0.1 to 1.0 Pa. The polishing pad using the composition having the storage modulus in the above range is useful for planarization of semiconductor substrate polishing, and is also useful for glass polishing, which requires a polishing pad with a high elastic modulus. In addition, such a polishing pad can perform a stable and highly efficient polishing operation.
[0108] The storage modulus refers to the energy stored without loss due to elasticity, and can be measured, for example, by using a dynamic mechanical analysis (DMS6100) device (Seiko Instruments). Specifically, it refers to the storage modulus of a composition at 50°C to 100°C when a sine wave vibration is applied and measured at a frequency of 1Hz using a tensile test jig with a dynamic viscoelasticity measuring device. The measurement conditions for the storage modulus are, for example, that during polishing, the polishing pad is pressed against the workpiece and both are rotating, and this movement corresponds to approximately 1Hz, and the polishing pad reaches approximately 40°C due to frictional heat at that time, so that it can be measured at a temperature of 50°C to 100°C, specifically 60°C to 80°C, more specifically 70°C, etc.
[0109] In addition, the higher the temperature, the lower the stored energy of the storage modulus tends to be, and the lower the rate of decrease is, the better from the viewpoint of heat resistance. For example, the greater the rate of decrease in the storage modulus due to a temperature change of 50°C to 100°C, the lower the heat resistance.
[0110] According to one embodiment, the reduction rate of the storage modulus due to a temperature change from 50°C to 100°C may be 77% or less, specifically 75% or less, more specifically 50% to 75%. If the reduction rate of the storage modulus of the polishing pad exceeds 77%, it can be considered that the heat resistance is reduced due to the temperature change. Therefore, the polishing pad according to one embodiment of the present invention is excellent in heat resistance not only at the polishing temperature, i.e., at a polishing rate at 40°C, but also at high temperatures of 50°C to 100°C.
[0111] The composition has a tensile strength of 5N / mm after curing. 2 ~23N / mm2 , 10N / mm 2 ~23N / mm 2 , 15N / mm 2 ~23N / mm 2 , 21N / mm 2 ~23N / mm 2 , or 21.8 N / mm 2 ~22.5N / mm 2 It could be.
[0112] The elongation of the composition after curing may be 50% to 300%, 70% to 200%, 80% to 250%, or 80% to 150%.
[0113] The hardness of the composition after curing may be 30 Shore D to 80 Shore D, 40 Shore D to 70 Shore D, 50 Shore D to 70 Shore D, 40 Shore D to 60 Shore D, or 50 Shore D to 60 Shore D.
[0114] The modulus of the composition after curing may be from 40 MPa to 150 MPa, from 50 MPa to 120 MPa, from 50 MPa to 110 MPa, or from 63 MPa to 100 MPa.
[0115] As a specific example, the composition has a modulus of 63 MPa to 100 MPa and a compressibility of 21 N / mm after curing. 2 ~23N / mm 2 The tensile strength may be
[0116] The composition may have a large number of micropores after curing. The average size of the micropores may be 10 μm to 50 μm, 20 μm to 50 μm, 20 μm to 40 μm, 20 μm to 30 μm, or 30 μm to 50 μm.
[0117] The composition may have a polishing rate after curing at about 50° C. to 60° C. of 3000 Å / min to 5000 Å / min, 3000 Å / min to 4000 Å / min, 3500 Å / min to 4000 Å / min, 3500 Å / min to 3820 Å / min, 3620 Å / min to 3820 Å / min, or 3720 Å / min to 3820 Å / min.
[0118] In particular, the difference in polishing rate of the composition after curing may be about 1 Å / min to 100 Å / min, 3 Å / min to 80 Å / min, or 4 Å / min to 60 Å / min, depending on the change in temperature and time, for example, about 50°C for 1 hour to 60°C for 8 hours. That is, the composition according to one embodiment shows little change in polishing rate even with the change in temperature and time after curing, and may exhibit stable thermal properties even at high temperatures. According to one embodiment of the present invention, the change in polishing rate due to the change in temperature from about 50°C to about 60°C may be 2% or less, specifically less than 2%, or 0.2% to 1.9%, more specifically 0.3% to 1.9%.
[0119] The composition may have a hardness of 50 Shore D to 60 Shore D, 50 Shore D to 58 Shore D, and 40 Shore D to 55 Shore D at temperatures of 30° C., 50° C., and 70° C. after curing, respectively. Specifically, the hardness of the composition may be 55 Shore D to 60 Shore D, 52 Shore D to 55 Shore D, and 43 Shore D to 49 Shore D at temperatures of 30° C., 50° C., and 70° C., respectively.
[0120] The composition may have a hardness difference at a temperature of 30°C to 70°C after curing of 5 Shore D to 15 Shore D, specifically 6 Shore D to 12 Shore D, and more specifically 7 Shore D to 12 Shore D.
[0121] The composition according to one embodiment has excellent heat resistance due to a low rate of decrease in storage modulus at high temperatures, excellent tensile strength and modulus, and can improve polishing stability at high temperatures for long periods of time, so it can be usefully used in the manufacture of polishing pads.
[0122] The specific components of the polishing layer will be described in detail below with reference to a method for producing a polishing pad according to one embodiment of the present invention.
[0123] [Polishing pad manufacturing method] A method for manufacturing a polishing pad according to one embodiment includes the steps of preparing a first raw material composition containing a urethane-based prepolymer, preparing a second raw material composition containing a sulfur-containing first curing agent and an ester-containing second curing agent, preparing a third raw material composition containing a foaming agent, sequentially or simultaneously mixing the first raw material composition with the second raw material composition and the third raw material composition to produce a raw material mixture, and injecting the raw material mixture into a mold and curing it.
[0124] The types and contents of the urethane-based prepolymer contained in the first raw material composition, the first curing agent (or liquid-phase curing agent) and the second curing agent (or solid-phase curing agent) contained in the second raw material composition, and the foaming agent contained in the third raw material composition are as described above in the composition.
[0125] The step of preparing the raw material mixture may be performed by mixing the first raw material composition with the second raw material composition and then further mixing them with the third raw material composition, or by mixing the first raw material composition with the third raw material composition and then further mixing them with the second raw material composition.
[0126] As an example, the urethane-based prepolymer, the curing agent mixture, and the blowing agent may be added to the mixing process substantially at about the same time, and when the blowing agent, the surfactant, and the inert gas are added, they may also be added to the mixing process substantially at about the same time.
[0127] As another example, the urethane prepolymer, blowing agent, and surfactant may be premixed and then the curative mixture charged, or the curative mixture and the inert gas charged together.
[0128] In the mixing, the urethane prepolymer and the curing agent mixture are mixed to start the reaction, and the foaming agent and the inert gas can be evenly dispersed in the raw material. In this case, the reaction rate regulator can adjust the reaction rate by intervening in the reaction between the urethane prepolymer and the curing agent mixture from the initial stage of the reaction. Specifically, the mixing can be performed at a speed of 1000 rpm to 10000 rpm, or 4000 rpm to 7000 rpm. When the speed is within the above range, it can be more advantageous for the inert gas and the foaming agent to be evenly dispersed in the raw material.
[0129] The step of preparing the raw material mixture may be carried out at a temperature of 50° C. to 150° C., and may be carried out under vacuum degassing conditions as necessary.
[0130] The raw material mixture is poured into the mold and then cured under the temperature condition of 60°C to 120°C and 50 kg / m 2 ~200kg / m 2 The reaction may be carried out under pressure conditions of 0.1 to 1000 MPa.
[0131] The manufacturing method may further include a step of cutting the surface of the obtained polishing pad, a step of processing grooves in the surface, a step of bonding with a lower layer, a step of inspecting, a step of packaging, etc. These steps may be performed by a conventional method for manufacturing a polishing pad.
[0132] [Polishing pad] A polishing pad according to one embodiment includes a polishing layer including a urethane-based prepolymer and a curing agent mixture, the curing agent mixture including a sulfur-containing first curing agent and an ester-containing second curing agent, the first curing agent being present in greater amounts than the second curing agent.
[0133] The thickness of the polishing pad may be 0.8 mm to 5.0 mm, 1.0 mm to 4.0 mm, 1.0 mm to 3.0 mm, 1.5 mm to 2.5 mm, 1.7 mm to 2.3 mm, or 2.0 mm to 2.1 mm. When the thickness is within the above range, the particle size deviation between the upper and lower parts of the pores is minimized, and the basic physical properties of the polishing pad can be sufficiently exhibited.
[0134] The specific gravity of the polishing pad is 0.6 g / cm 3 ~0.9g / cm 3 , or 0.7 g / cm 3 ~0.85g / cm 3 It could be.
[0135] The polishing pad may have similar physical and porosity properties as the composition according to one implementation has after curing.
[0136] The polishing rate of the polishing pad may be 3000 Å / min to 5000 Å / min, 3000 Å / min to 4000 Å / min, 3500 Å / min to 4000 Å / min, 3500 Å / min to 3800 Å / min, 3500 Å / min to 3770 Å / min, or 3600 Å / min to 3760 Å / min during polishing for 1 hour at about 50° C. to 60° C. In particular, the polishing pad may exhibit stable thermal properties even at high temperatures.
[0137] The polishing rate may be an initial polishing rate immediately after the polishing pad is cured (i.e., immediately after production). When the initial polishing rate is within the above range, it is advantageous to suppress pad glazing and maintain an excellent polishing rate at an appropriate level in subsequent repeated polishing processes.
[0138] The polishing pad may have grooves for mechanical polishing on the surface thereof. The grooves may have a depth, width, and interval appropriate for mechanical polishing, and are not particularly limited.
[0139] The polishing pad according to another embodiment may include an upper pad and a lower pad, where the upper pad may have the same composition and physical properties as the polishing pad according to the first embodiment.
[0140] The lower pad supports the upper pad and absorbs and disperses impacts applied to the upper pad. The lower pad may include nonwoven fabric or suede.
[0141] Also, an adhesive layer may be inserted between the upper and lower pads. The adhesive layer may include a hot melt adhesive. The hot melt adhesive may be one or more selected from the group consisting of polyurethane-based resins, polyester-based resins, ethylene vinyl acetate-based resins, polyamide-based resins, and polyolefin-based resins. Specifically, the hot melt adhesive may be one or more selected from the group consisting of polyurethane-based resins and polyester-based resins.
[0142] According to one embodiment, the polishing pad comprises a mixture of a urethane-based prepolymer and a curing agent, the curing agent comprising a sulfur-containing first curing agent and an ester-containing second curing agent, the first curing agent being a liquid-phase curing agent containing sulfur, and the second curing agent being a solid-phase curing agent containing an ester having two or more benzene rings, and the content of the solid-phase curing agent by weight is equal to or greater than the content of the liquid-phase curing agent.
[0143] The thickness of the polishing pad may be the same if the first curing agent is present in greater amount than the second curing agent.
[0144] The polishing pad may have similar physical and porosity properties as the composition according to one implementation has after curing.
[0145] The polishing rate of the polishing pad may be 3000 Å / min to 5000 Å / min, 3000 Å / min to 4000 Å / min, 3500 Å / min to 4000 Å / min, 3500 Å / min to 3820 Å / min, 3620 Å / min to 3820 Å / min, or 3720 Å / min to 3820 Å / min at about 50°C to 60°C.
[0146] In particular, by changing the temperature and time, for example, from about 50°C for 1 hour to about 60°C for 8 hours, the polishing rate difference of the polishing pad can be about 1 Å / min to 100 Å / min, 3 Å / min to 80 Å / min, or 4 Å / min to 60 Å / min.
[0147] That is, the polishing pad according to one embodiment shows little change in polishing rate with changes in temperature and time, and can show stable thermal properties even at high temperatures. The polishing pad according to one embodiment can have a polishing rate change rate of 2% or less, specifically less than 2%, or 0.2% to 1.9%, more specifically 0.3% to 1.9%, with a temperature change of about 50°C to about 60°C. The polishing rate can be an initial polishing rate immediately after the polishing pad is hardened (i.e., immediately after manufacture). When the initial polishing rate is within the above range, it is advantageous to suppress the pad glazing phenomenon and maintain an excellent polishing rate at an appropriate level in the subsequent repeated polishing process.
[0148] The polishing pad may have grooves for mechanical polishing on the surface thereof. The grooves may have a depth, width, and interval appropriate for mechanical polishing, and are not particularly limited.
[0149] The polishing pad according to another embodiment may include an upper pad and a lower pad, where the upper pad may have the same composition and physical properties as the polishing pad according to the first embodiment.
[0150] The lower pad supports the upper pad and absorbs and disperses impacts applied to the upper pad. The lower pad may include nonwoven fabric or suede.
[0151] Also, an adhesive layer may be inserted between the upper pad and the lower pad. The adhesive layer is as mentioned above.
[0152] [Method of manufacturing semiconductor devices] A method for manufacturing a semiconductor device according to an embodiment may include polishing a surface of a semiconductor substrate using a polishing pad according to an embodiment.
[0153] The method for manufacturing a semiconductor element may include a step of mounting a polishing pad including a polishing layer on a platen, and rotating the polishing surface of the polishing layer relative to a surface of a semiconductor substrate so that the polishing surface of the polishing layer and the surface of the semiconductor substrate come into contact with each other, thereby polishing the surface of the semiconductor substrate.
[0154] Specifically, a method for manufacturing a semiconductor device according to one embodiment includes the steps of providing a polishing pad, placing an object to be polished on the polishing pad, and rotating the object to be polished relative to the polishing pad to polish the object.
[0155] More specifically, after the polishing pad according to one embodiment is attached to a platen, a semiconductor substrate containing oxide or a metal such as tungsten is placed on the polishing pad. At this time, the surface of the semiconductor substrate directly contacts the polishing surface of the polishing pad. A polishing slurry may be sprayed onto the polishing pad for polishing. Then, the semiconductor substrate and the polishing pad may rotate relative to each other to polish the surface of the semiconductor substrate.
[0156] In this regard, a schematic flow chart of a semiconductor device manufacturing process according to one embodiment is shown in FIG. 8, after the polishing pad 110 according to the embodiment is mounted on a platen 120, a semiconductor substrate 130 is placed on the polishing pad 110. At this time, the surface of the semiconductor substrate 130 directly contacts the polishing surface of the polishing pad 110. For polishing, a polishing slurry 150 may be sprayed onto the polishing pad through a nozzle 140. The flow rate of the polishing slurry 150 supplied through the nozzle 140 is about 10 cm. 3 / min ~ approx. 1000cm 3 / min., for example, about 50 cm 3 / min ~ approx. 500cm 3 / min, but is not limited to this.
[0157] Thereafter, the semiconductor substrate 130 and the polishing pad 110 may rotate relative to each other to polish the surface of the semiconductor substrate 130. At this time, the rotating direction of the semiconductor substrate 130 and the rotating direction of the polishing pad 110 may be the same or opposite to each other. The rotating speed of the semiconductor substrate 130 and the polishing pad 110 may be selected according to the purpose within a range of about 10 rpm to about 500 rpm, and may be, for example, about 30 rpm to about 200 rpm, but is not limited thereto.
[0158] The semiconductor substrate 130 may be attached to the polishing head 160 and brought into contact with the polishing surface of the polishing pad 110 under a predetermined load, so that the surface of the semiconductor substrate 130 may be polished. The load applied so that the surface of the semiconductor substrate 130 comes into contact with the polishing surface of the polishing pad 110 is about 1 gf / cm. 2 ~About 1000gf / cm 2 For example, the range may be selected according to the purpose, for example, about 10 gf / cm 2 ~About 800gf / cm 2 It may be, but is not limited to this.
[0159] In one embodiment, the method for manufacturing a semiconductor device may further include processing the polishing surface of the polishing pad 110 with a conditioner 170 simultaneously with polishing the semiconductor substrate 130 to maintain the polishing surface of the polishing pad 110 in a state suitable for polishing.
[0160] A polishing pad according to one implementation can have improved polishing properties by using a curing agent mixture that includes a sulfur-containing primary curing agent and an ester-containing secondary curing agent.
[0161] The polishing pad according to one embodiment contains a larger amount of sulfur-containing first curing agent than ester-containing second curing agent, and therefore has excellent hardness even at high temperatures, and can improve scratches and surface defects that appear on the surface of a semiconductor substrate and further improve the polishing rate, making it useful for semiconductor devices.
[0162] In addition, the polishing pad according to one embodiment contains an ester-containing second curing agent having two or more benzene rings in the same amount or in a larger amount than the sulfur-containing first curing agent, and thus can achieve thermal stability by minimizing the decrease in storage modulus due to temperature change at high temperatures as well as physical properties such as tensile strength and modulus within an appropriate range, thereby further improving polishing stability.
[0163] (Example) The present invention will now be described in more detail with reference to the following examples, however, the following examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0164] Example 1 [1-1: Preparation of urethane prepolymer] Toluene diisocyanate (TDI) and dicyclohexylmethane diisocyanate (H12MDI) as isocyanate compounds, and polytetramethylene ether glycol (PTMEG) and diethylene glycol (DEG) as polyols were placed in a four-neck flask and reacted at 80°C for 3 hours to prepare a urethane prepolymer with an NCO group content of 9% by weight.
[0165] [1-2: Manufacturing of polishing pads] The prepared urethane prepolymer was filled in a casting machine equipped with tanks and input lines for supplying raw materials such as urethane prepolymer, curing agent, inert gas, and foaming agent. In addition, 3,5-dimethylthio-2,6-diaminotoluene (DMTDA) as a first curing agent and 1,3-propanediol bis(4-aminobenzoate) (PDPAB) as a second curing agent were filled in an amount of 80:20 by weight ratio, and nitrogen gas (N2) was prepared as an inert gas. In addition, based on 100 parts by weight of the composition for manufacturing polishing pads, 1.18 parts by weight of a solid-phase foaming agent (AkzoNobel) and 0.39 parts by weight of a silicone surfactant (EVONIK) were filled in each tank. The raw materials were stirred while being fed into the mixing head at a constant speed through each input line. At this time, the equivalent ratio of the NCO group of the urethane prepolymer and the NH2 group of the mixed curing agent of the first curing agent and the second curing agent was 1:1, and the total input rate was maintained at a rate of 10 kg / min. In addition, the inert gas was constantly input at 20 volume% based on the total volume of the composition for manufacturing a polishing pad. The injected raw materials were mixed at a high speed of 5000 rpm and injected into a mold (1000 mm long, 1000 mm wide, 3 mm high), solidified, and a sheet-shaped porous polyurethane polishing layer was obtained. At this time, the injection amount of nitrogen gas, which is an inert gas, was adjusted to a density of the porous polyurethane of 0.8 g / cm. 3 It was made to be like this.
[0166] The stirred raw material was discharged into a mold (1000 mm x 1000 mm x 3 mm) to terminate the reaction, and a solid cake-like molded body was obtained. After that, the upper and lower ends of the molded body were cut to a thickness of 0.5 mm each to obtain an upper pad with a thickness of 2 mm.
[0167] The upper pad was then subjected to a surface milling process and a groove forming process, and was then laminated to the lower pad with a hot melt adhesive to produce a polishing pad.
[0168] Example 2 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was PDPAB in a weight ratio of 60:40.
[0169] Example 3 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was PDPAB in a weight ratio of 50:50.
[0170] Example 4 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was PDPAB in a weight ratio of 40:60.
[0171] Example 5 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent, DMTDA, and the second curing agent, PDPAB, were mixed in a weight ratio of 20:80.
[0172] Comparative Example 1 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was PDPAB in a weight ratio of 100:0.
[0173] Comparative Example 2 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was PDPAB in a weight ratio of 0:100.
[0174] Comparative Example 3 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was MOCA in a weight ratio of 60:40.
[0175] Comparative Example 4 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was MOCA in a weight ratio of 50:50.
[0176] Comparative Example 5 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was MOCA in a weight ratio of 40:60.
[0177] Comparative Example 6 A polishing pad was prepared in the same manner as in Example 1, except that the first curing agent was DMTDA and the second curing agent was MOCA in a weight ratio of 0:100. Specific process conditions for the upper pad of the polishing pad are summarized in Tables 1 and 2 below.
[0178] [Table 1]
[0179] [Table 2]
[0180] (Test Example) The polishing pads obtained in the above Examples and Comparative Examples were tested for the following items, and the results are shown in Tables 3 and 4 and FIGS.
[0181] (1)Hardness The Shore D hardness of the polishing pads manufactured according to the examples and comparative examples was measured, and the polishing pads manufactured according to the examples and comparative examples were cut into pieces of 2 cm x 2 cm (thickness: 2 mm) and left to stand for 16 hours in environments with temperatures of 25°C, 30°C, 50°C, and 70°C and a relative humidity of 50±5%. Then, the hardness of the multi-layer polishing pad was measured using a hardness tester (D-type hardness tester).
[0182] (2) Specific gravity The polishing pads manufactured according to the examples and comparative examples were cut into 4 cm x 8.5 cm rectangles (thickness: 2 mm) and left to stand for 16 hours in an environment with a temperature of 23 ± 2°C and a humidity of 50 ± 5%. The specific gravity of the polishing pads was measured using a hydrometer.
[0183] (3) Tensile strength The polishing pads manufactured according to the above examples and comparative examples were cut into pieces of 4 cm x 1 cm (thickness: 2 mm), and the maximum strength value just before the breakage of the polishing pads was measured using a universal testing machine (UTM) at a speed of 50 mm / min.
[0184] (4) Growth rate The polishing pads prepared according to the above examples and comparative examples were cut into pieces of 4 cm x 1 cm (thickness: 2 mm), and the maximum deformation of the polishing pad just before it broke was measured using a universal testing machine (UTM) at a speed of 50 mm / min, and the ratio of the maximum deformation to the initial length was expressed as a percentage (%).
[0185] (5) Modulus Each of the polishing pads manufactured according to the above examples and comparative examples was tested in the same manner as in the tensile strength measurement method described below, and the slope of the stress-strain curve in the initial elastic region was calculated. The results are summarized in Tables 3 and 4 below.
[0186] [Table 3]
[0187] [Table 4]
[0188] As shown in Tables 3 and 4, it can be seen that the physical properties of the polishing pad change depending on the contents of the first curing agent and the second curing agent.
[0189] Specifically, the polishing pads of Examples 1 and 2, which had a higher content of the first curing agent compared to the content of the second curing agent, exhibited significantly superior elongation while maintaining appropriate hardness, modulus, and tensile strength.
[0190] Furthermore, the polishing pads of Examples 3 to 5, in which the content of the second curing agent was the same as or greater than that of the first curing agent, were significantly superior in terms of tensile strength, modulus, and hardness at different temperatures (30°C / 50°C / 70°C).
[0191] On the other hand, in the case of Comparative Example 2, in which only PDPAB was used as the second curing agent, the tensile strength and modulus were too high. In particular, the modulus of Comparative Example 2 was nearly twice as high as the modulus of the polishing pads of Examples 3 to 5.
[0192] Furthermore, all of the examples were able to achieve physical properties equal to or better than those of polishing pads using MOCA, even without using MOCA, which contains harmful substances.
[0193] (6) Stoma characteristics The cross sections of the polishing pads were observed with a scanning electron microscope (SEM) and are shown in Figures 1 to 4. Figures 1 to 4 are SEM images of the cross sections of the polishing pads produced in Examples 1, 3, and 5, and Comparative Example 2, respectively. As can be seen from Figures 1 to 4, the polishing pads of each Example have fine and uniform pores distributed over a wide area.
[0194] In addition, for Examples 3 and 5 and Comparative Example 2, the pore characteristics were calculated based on the SEM images and are summarized in Table 5 below. - Number average diameter: The average of the sum of the pore diameters on the SEM image divided by the number of pores - Number of pores: 0.3 cm on SEM image 3 Number of pores per unit - Pore area ratio: Percentage of the area of pores only to the total area of the SEM image
[0195] [Table 5]
[0196] As shown in Table 5, the polishing pads of Examples 3 and 5 have a number average diameter of pores of about 20 μm to 26 μm, and a pore area ratio of about 41% to 45%.
[0197] (7)Removal rate The initial removal rate immediately after the polishing pad was produced was measured as follows. Silicon oxide was deposited on a silicon wafer with a diameter of 300 mm by a chemical vapor deposition (CVD) process. A polishing pad was attached to a CMP device, and the silicon oxide layer of the silicon wafer was placed facing the polishing surface of the polishing pad. The silicon oxide film was polished for 60 seconds at a load of 4.0 psi and a speed of 150 rpm while supplying a calcined ceria slurry onto the polishing pad at a rate of 250 mL / min.
[0198] Polishing was performed at 50°C to 60°C for 1 hour, and the polished silicon wafer was removed from the carrier, placed in a spin dryer, washed with distilled water, and then dried with nitrogen for 15 seconds. The change in film thickness of the dried silicon wafer before and after polishing was measured using a spectroscopic interference wafer thickness meter (SI-F80R, Keyence Corporation). The polishing rate was then calculated using the following formula 1. The results are shown in Table 6 below. [Formula 1] Polishing rate (Å / min) = polished thickness of silicon wafer (Å) / polishing time (min)
[0199] [Table 6]
[0200] In addition, after polishing the silicon oxide film, the polishing temperature and time were further divided, and the polishing rate was calculated in the same manner as above. Specifically, the polishing was performed at 51.3°C for 1 hour, at 56.2°C for 4 hours, and at 60.3°C for 8 hours. The results are shown in Tables 7 to 9 below and in Figure 5.
[0201] [Table 7]
[0202] [Table 8]
[0203] [Table 9]
[0204] The results show that the polishing pads of the examples maintain a constant polishing rate within an appropriate range. In addition, the polishing rate change rate is maintained constant even with changes in temperature and time, whereas the polishing pad of Comparative Example 1 shows a large change, increasing by more than 13%.
[0205] (8) Number of defects After performing the CMP process using a polishing pad in the same manner as in (7) above, the number of defects appearing on the wafer surface after polishing was measured using a defect inspection device (AIT XP+, KLA-Tencor) (conditions: threshold 150, die filter threshold 280). The results are shown in Table 10 below and Figure 6.
[0206] [Table 10]
[0207] From the results, it can be seen that when a curing agent mixture containing a larger amount of the first curing agent is used (Examples 1 and 2), the polishing rate of the polishing pad is excellent and the number of defects is significantly lower than that of the comparative example.
[0208] Specifically, from the results of Tables 6 and 10, the polishing rates of Examples 1 and 2 were generally excellent at 3733 Å / min and 3740 Å / min, while the polishing rate of the polishing pad of Comparative Example 1, which did not use PDPAB, was significantly lower at 3715 Å / min, and the polishing rate of the polishing pad of Comparative Example 2, which used only PDPAB, was 3763 Å / min, indicating that the initial polishing rate was excessively high due to increased hard segment aggregation. As a result, the polishing rate of the polishing pad of Comparative Example 2 is expected to rapidly decrease due to the pad glazing phenomenon.
[0209] Therefore, it can be confirmed that in the case of the polishing pads of Examples 1 and 2, the polishing rate can be improved and the number of defects can be significantly reduced.
[0210] (9) Storage modulus The storage modulus of the polishing pads of the examples and comparative examples was measured in tension mode at a frequency of 1 Hz and a temperature rise rate of 10° C. / min using a dynamic mechanical analysis device DMS6100 (Seiko Instruments Inc.).
[0211] In this case, the storage modulus (E') was measured in the temperature range of -60°C to 140°C, and the decrease rate (ΔE') of the storage modulus in the temperature range of 50°C to 100°C was calculated. The decrease rate (ΔE') of the storage modulus can be calculated by the following formula 2.
[0212] [Formula 2] JPEG0007564272000016.jpg18147
[0213] In the above formula 2, E' 50 is the storage modulus at 50°C, and E' 100 is the storage modulus at 100°C. The results are shown in Figure 7.
[0214] As can be seen from FIG. 7, when a hardener mixture containing the second hardener in an amount equal to or greater than the amount of the first hardener is used (Examples 3 to 5), the rate of decrease in the storage modulus of the polishing pad is significantly reduced compared to Comparative Examples 1 and 2.
[0215] Specifically, it was confirmed that the reduction in storage modulus of the polishing pads of Examples 3 to 5 was 75% or less, specifically, the reduction in storage modulus of the polishing pads of Examples 1, 2, and 3 was approximately 75%, 71%, and 70%, respectively, whereas in the case of the polishing pad of Comparative Example 1, the reduction in storage modulus was 84% or more.
[0216] Therefore, in the case of the polishing pads of Examples 3 to 5, the rate of decrease in the storage elastic modulus decreased, and it is therefore understood that the heat resistance was significantly improved. [Explanation of symbols]
[0217] 110: Polishing pad 120: Platen 130: Semiconductor substrate 140: Nozzle 150: Abrasive slurry 160: Polishing head 170: Conditioner
Claims
1. A mixture of a urethane-based prepolymer and a curing agent is included. the curing agent mixture comprises a sulfur-containing primary curing agent and an ester-containing secondary curing agent; The first curing agent is contained in a larger amount than the second curing agent, the first curing agent is 3,5-dimethylthio-2,6-diaminotoluene; the second curing agent is 1,3-propanediol bis(4-aminobenzoate); The first curing agent is contained in an amount of 11 parts by weight to 18 parts by weight based on 100 parts by weight of the composition; The composition comprises the second curing agent in an amount of 1 part by weight to 10 parts by weight based on 100 parts by weight of the composition.
2. The composition according to claim 1, wherein the content ratio of the first curing agent and the second curing agent is 1:0.1-0.9 by weight.
3. after said composition has cured, a modulus of 50 MPa to 120 MPa and an elongation of 90% to 200%, 2. The composition of claim 1, wherein after the composition has cured, it has a hardness of from 50 Shore D to 60 Shore D, from 50 Shore D to 58 Shore D, and from 40 Shore D to 55 Shore D at temperatures of 30° C., 50° C., and 70° C., respectively.
4. 2. The composition of claim 1, wherein the first curing agent is a liquid phase curing agent containing sulfur, and the second curing agent is a solid phase curing agent containing an ester having two or more benzene rings.
5. 5. The composition of claim 4, wherein the solid phase hardener has a melting point (m.p.) of 100°C to 150°C.
Citation Information
Patent Citations
Composite polyurea elastomer composition
JP1993125139A
Polyurethaneurea elastomer for kinetic application
JP2000248040A
Curing agent for polyurethane coating film material, and two liquid type kit for polyurethane coating film material using the same
JP2011202017A
Curing agent for polyurethane coating material and two-liquid kit for polyurethane coating material using the same
JP2011202018A
Two-pack kit for polyurethane coating waterproof material
JP2011202019A