Polishing Pad

The polishing pad with optimized groove pitches and land area ratios addresses rigidity issues, enhancing slurry retention and discharge balance for improved polishing efficiency.

JP7564418B2Active Publication Date: 2024-10-09FUJIBO HLDG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020051075
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-23
Publication Date
2024-10-09
Estimated Expiration
2040-03-23

AI Technical Summary

Technical Problem

Conventional polishing pads with narrow groove pitches between circular grooves compromise rigidity, affecting polishing performance by imbalance in slurry retention and discharge functions.

Method used

A polishing pad with groove pitches between adjacent circular grooves set between 5 mm and 10 mm, and land area ratios of 0.70 to 0.92, ensuring balanced slurry holding and discharge functions through specific land width configurations.

Benefits of technology

Maintains rigidity while achieving well-balanced slurry holding and discharge, resulting in improved polishing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564418000002
    Figure 0007564418000002
  • Figure 0007564418000003
    Figure 0007564418000003
  • Figure 0007564418000001
    Figure 0007564418000001
Patent Text Reader

Abstract

SOLUTION: A polishing pad 1 comprises: a plurality of concentric circular grooves 2; and a plurality of liner grooves 3 crossing in a lattice state, on a polished surface of a polishing layer consisting of a rigid urethane, in which a groove pitch between the adjacent circular groove 2 and the circular groove 2 is greater than 5 mm, and equal to or less than 10 mm, an area ratio of a circular land part 4 determined from a land width of the circular land part 4 formed between the circular grooves 2, 2, and the groove width of the circular groove 2 and an area ratio of a linear land part 5 determined from a land width of a linear land part 5 formed between the linear grooves 3, 3 and the groove width of the linear groove 3 are multiplied for obtaining a land area ratio of 0.70 to 0.92.EFFECT: As an effect, deformation of a land part can be suppressed for acquiring a polishing pad 1 with preferable polishing performance.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing pad, and more particularly to a polishing pad having a polishing surface of a polishing layer made of hard urethane, on which a plurality of circular grooves arranged concentrically and a plurality of linear grooves intersecting in a lattice pattern are formed. [Background technology]

[0002] Conventionally, polishing pads have been used to polish objects such as optical materials, semiconductor substrates, and glass substrates for hard disks. Known examples of such polishing pads include a polishing layer made of hard urethane such as polyurethane, and a polishing pad in which a plurality of circular grooves arranged concentrically and a plurality of linear grooves intersecting in a lattice pattern are formed on the polishing surface of the polishing layer (Patent Documents 1 and 2). When the polishing pad is used to polish an object to be polished, liquid slurry is supplied between the object to be polished and the polishing pad, and the circular groove functions as a holding groove for holding the slurry, and the linear groove functions as a discharge groove for discharging polishing waste and used slurry. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2006-156876 A [Patent Document 2] JP 2013-35108 A Summary of the Invention [Problem to be solved by the invention]

[0004] It is desirable that the circular grooves and the straight grooves are formed so as to balance the slurry retention and discharge functions, but if the groove pitch between the circular grooves is narrow, the land portion formed between the circular grooves becomes narrow and cannot maintain rigidity, which may affect the polishing performance. In view of these problems, the present invention provides a polishing pad having improved polishing performance. [Means for solving the problem]

[0005] That is, the polishing pad in the invention of claim 1 is a polishing pad in which a plurality of circular grooves arranged concentrically and a plurality of linear grooves intersecting in a lattice pattern are formed on the polishing surface of the polishing layer made of hard urethane, The groove pitch between adjacent circular grooves is more than 5 mm and 10 mm or less, Furthermore, the land area ratio obtained by multiplying the area ratio of the circular land portion calculated by the following (Formula 1) based on the land width of the circular land portion formed between the circular grooves and the groove pitch of the circular grooves by the area ratio of the straight land portion calculated by the following (Formula 2) based on the land width of the straight land portion formed between the straight grooves and the groove pitch of the straight grooves is 0.70 to 0.92, and further, the land width of the straight land portion is set to 33 to 58 mm. Area ratio of circular land part = circular Land Department land width / circular groove pitch (Equation 1) Straight land area ratio = Straight line Land Department Land width / Straight groove pitch (Equation 2) Effect of the Invention

[0006] According to the above invention, the rigidity of the circular land portion formed between the circular grooves can be maintained while the slurry retention function of the circular grooves and the discharge function of the straight grooves can be balanced, thereby obtaining good polishing performance. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a plan view of a polishing pad according to the present embodiment. [Diagram 2] FIG. 4 is a cross-sectional view illustrating a relationship between grooves. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will now be described with reference to the illustrated embodiments. FIG. 1 shows a polishing pad 1 according to the present invention, which is used for polishing objects such as optical materials, semiconductor substrates, and glass substrates for hard disks. The polishing pad 1 has a polishing layer made of hard urethane having an approximately disk shape, and the polishing surface for polishing the workpiece is formed with a plurality of concentric circular grooves 2 and a plurality of linear grooves 3 intersecting in a lattice pattern. The hard urethane that constitutes the polishing layer is produced by a prepolymer method in which a urethane prepolymer, which is a reaction intermediate between a polyol component and an isocyanate component, is used to harden the polyurethane polyurea resin obtained by adding and mixing a curing agent (chain extender) such as a diamine or diol, a foaming agent, a catalyst, etc. Although not shown, the polishing pad 1 is fixed to a polishing table of a polishing device with double-sided tape or the like, and the workpiece is vacuum-adsorbed to the support table. The polishing table and the support table are rotated relative to each other by a driving means, and the support table is reciprocated in a radial direction from the center position of the polishing table, whereby the polishing pad 1 and the workpiece slide against each other while rotating relative to each other, thereby polishing the workpiece. At that time, a liquid slurry in which abrasive grains are mixed with a required chemical is supplied between the polishing pad 1 and the workpiece to be polished, and mechanical polishing by the polishing pad 1 and chemical polishing by the slurry are performed. The polishing apparatus having such a configuration is well known in the art, and will not be described in detail further. In addition to the polishing apparatus having the above configuration, polishing apparatuses having other configurations, such as a polishing apparatus in which the support platen is not driven but is rotated by the rotation of the polishing platen, can also be used.

[0009] Next, a manufacturing method for the polishing layer of the polishing pad 1 of this embodiment may include, for example, a preparation step of preparing at least a urethane bond-containing isocyanate compound as a prepolymer, a curing agent, and a hollow body; a mixing step of mixing at least the urethane bond-containing isocyanate compound and the curing agent to obtain a mixed liquid for molding a molded body; a molded body molding step of molding a polyurethane polyurea resin molded body from the mixed liquid for molding a molded body; and a polishing layer formation step of forming a polishing layer having the above polishing surface from the polyurethane polyurea resin molded body.

[0010] In the preparation step, for example, a urethane bond-containing isocyanate compound, a curing agent, and a hollow body are used as raw materials for the polyurethane polyurea resin molded body in the manufacture of the polishing pad 1. Furthermore, a polyol compound may be used together with the above components, and components other than the above may be used together within a range that does not impair the effects of the present invention.

[0011] The urethane bond-containing isocyanate compound prepared in the preparation step is a compound obtained by reacting the following polyisocyanate compound with a polyol compound under commonly used conditions, and contains a urethane bond and an isocyanate group in the molecule. In addition, other components may be contained in the urethane bond-containing isocyanate compound within the range that does not impair the effects of the present invention. The urethane bond-containing isocyanate compound may be a commercially available product, or may be a product synthesized by reacting a polyisocyanate compound with a polyol compound. The reaction is not particularly limited, and addition polymerization may be performed using a method and conditions known in the art for producing polyurethane resins. For example, the polyisocyanate compound heated to 50°C is added to a polyol compound heated to 40°C while stirring in a nitrogen atmosphere, and the mixture is heated to 80°C after 30 minutes and then reacted at 80°C for 60 minutes.

[0012] First, the polyisocyanate compound means a compound having two or more isocyanate groups in the molecule. The polyisocyanate compound is not particularly limited as long as it has two or more isocyanate groups in the molecule. For example, diisocyanate compounds having two isocyanate groups in the molecule include m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-tolylene diisocyanate (2,6-TDI), 2,4-tolylene diisocyanate (2,4-TDI), naphthalene-1,4-diisocyanate, diphenylmethane-4,4'-diisocyanate (MDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyl Examples of the diisocyanate include diphenylmethane-4,4'-diisocyanate, xylylene-1,4-diisocyanate, 4,4'-diphenylpropane diisocyanate, trimethylene diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, cyclohexylene-1,2-diisocyanate, cyclohexylene-1,4-diisocyanate, p-phenylene diisothiocyanate, xylylene-1,4-diisothiocyanate, and ethylidine diisothiocyanate. Furthermore, as the polyisocyanate compound, a diisocyanate compound is preferable, among which 2,4-TDI, 2,6-TDI and MDI are more preferable, and 2,4-TDI and 2,6-TDI are particularly preferable. These polyisocyanate compounds may be used alone, or a plurality of polyisocyanate compounds may be used in combination.

[0013] Next, the above-mentioned polyol compound means a compound having two or more alcoholic hydroxyl groups (OH) in the molecule. Examples of the polyol compound used in the synthesis of the urethane bond-containing isocyanate compound include diol compounds, triol compounds, and the like, such as ethylene glycol, diethylene glycol (DEG), butylene glycol, and the like; polyether polyol compounds, such as poly(oxytetramethylene) glycol (or polytetramethylene ether glycol) (PTMG), and the like; polyester polyol compounds, such as the reaction product of ethylene glycol and adipic acid, and the reaction product of butylene glycol and adipic acid, and the like; polycarbonate polyol compounds, polycaprolactone polyol compounds, and the like. Also, trifunctional propylene glycol with ethylene oxide added thereto can be used. Among these, PTMG or a combination of PTMG and DEG is preferred. The above polyol compounds may be used alone or in combination of two or more.

[0014] Here, the NCO equivalent of the prepolymer, which indicates the molecular weight of PP (prepolymer) per NCO group, is preferably 200-800, more preferably 300-700, and even more preferably 400-600. Specifically, the NCO equivalent of the prepolymer can be determined as follows. NCO equivalent of prepolymer = (parts by mass of polyisocyanate compound + part by mass of polyol compound) / [(number of functional groups per molecule of polyisocyanate compound x parts by mass of polyisocyanate compound / molecular weight of polyisocyanate compound) - (number of functional groups per molecule of polyol compound x parts by mass of polyol compound / molecular weight of polyol compound)]

[0015] As the curing agent (also called a chain extender), for example, a polyamine compound and / or a polyol compound can be used. The polyamine compound means a compound having two or more amino groups in the molecule, and an aliphatic or aromatic polyamine compound, particularly a diamine compound, can be used. Examples of such compounds include ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, 3,3'-dichloro-4,4'-diaminodiphenylmethane (methylenebis-o-chloroaniline) (hereinafter abbreviated as MOCA), and polyamine compounds having a similar structure to MOCA. Furthermore, the polyamine compound may have a hydroxyl group, and examples of such amine compounds include 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine. As the polyamine compound, a diamine compound is preferable, MOCA, diaminodiphenylmethane, and diaminodiphenylsulfone are more preferable, and MOCA is particularly preferable. The polyamine compound may be used alone or in combination of two or more polyamine compounds. In order to facilitate mixing with other components and / or to improve the uniformity of the bubble diameter in the subsequent molding process, the polyamine compound is preferably degassed under reduced pressure while being heated as necessary. As a method for degassing under reduced pressure, a method known in the art for producing polyurethanes may be used, and for example, degassing can be performed using a vacuum pump at a vacuum degree of 0.1 MPa or less. When a solid compound is used as the curing agent (chain extender), it can be melted by heating and degassed under reduced pressure.

[0016] The polyol compound used as the curing agent is not particularly limited as long as it is a diol compound, a triol compound, etc. The polyol compound may be the same as or different from the polyol compound used to form the prepolymer. Specific examples include low molecular weight diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 3-methyl-1,5-pentanediol, and 1,6-hexanediol, and high molecular weight polyol compounds such as poly(oxytetramethylene) glycol, polyethylene glycol, and polypropylene glycol. The above polyol compounds may be used alone or in combination of two or more.

[0017] Here, the components are mixed so that the R value, which is the equivalent ratio of the active hydrogen groups (amino groups and hydroxyl groups) present in the curing agent to the isocyanate groups present at the terminals of the urethane bond-containing isocyanate compound, is 0.60 to 1.40. The R value is preferably 0.65 to 1.30, and more preferably 0.70 to 1.20.

[0018] The hollow body means a microsphere having a void. The microsphere includes those having a spherical shape, an elliptical shape, and shapes similar thereto. Examples of hollow bodies include unfoamed heat-expandable microspheres having an outer shell (polymer shell) made of a thermoplastic resin and a low-boiling point hydrocarbon contained in the outer shell, and those obtained by thermally expanding unfoamed heat-expandable microspheres. As disclosed in JP-A-57-137323, etc., the polymer shell may be made of a thermoplastic resin such as an acrylonitrile-vinylidene chloride copolymer, an acrylonitrile-methyl methacrylate copolymer, or a vinyl chloride-ethylene copolymer. Similarly, the low-boiling point hydrocarbon encapsulated in the polymer shell may be, for example, isobutane, pentane, isopentane, petroleum ether, etc. In addition to using the hollow bodies, bubbles may be formed by chemical foaming such as water foaming or foaming due to mechanical stirring, or these methods may be combined.

[0019] Next, the mixing step will be described. In the mixing step, the urethane bond-containing isocyanate compound as a prepolymer, the curing agent, and the hollow bodies prepared in the preparation step are fed into a mixer and stirred and mixed. The mixing step is performed in a state where the components are heated to a temperature at which the fluidity of each component can be ensured. Although there is no particular restriction on the order of mixing, it is preferable to prepare a mixed liquid obtained by mixing a urethane bond-containing isocyanate compound and a hollow body, and a mixed liquid obtained by mixing a curing agent and other components as necessary, and then feed both mixed liquids into a mixer and mix and stir them. In this way, a mixed liquid for molding a molded body is prepared.

[0020] Next, in the molded body forming process, the mixed liquid for molding the molded body prepared in the above mixing process is poured into a mold frame at 50 to 100°C, and the prepolymer and the curing agent react to form a polyurethane polyurea resin, whereby the mixed liquid hardens and a polyurethane polyurea resin molded body is formed.

[0021] In the abrasive layer forming step, the polyurethane polyurea resin molded body obtained in the molded body molding step is sliced ​​into sheets, and the sliced ​​resin sheets are cut into circles. One side of the disk-shaped resin sheet obtained in this manner becomes the polishing surface, and by performing cutting processing or the like on this polishing surface using a required cutter, it is possible to form the concentric circular grooves 2 or lattice-like linear grooves 3 having any desired pitch, width and depth, thereby obtaining the polishing pad 1 of this embodiment.

[0022] 2 is a cross-sectional view showing the relationship between adjacent circular grooves 2 formed in the polishing pad 1. Note that although adjacent circular grooves 2 are described here, the diagram can also be used to explain the relationship between linear grooves 3. In this embodiment, the groove pitch between adjacent circular grooves 2 is measured based on the end face of the polishing pad 1 on the center side of the groove, and the groove pitch of the circular grooves 2 in this embodiment is set to a dimension of more than 5 mm and 10 mm or less. Each circular groove 2 is formed to have a groove width of 0.4 to 0.8 mm and a depth of 0.6 mm. By specifying the groove pitch of the circular grooves 2, the dimensions of the circular land portion 4 formed between the circular grooves 2, i.e., the portion that comes into contact with the workpiece during polishing, are set in the range of 4.2 to 9.6 mm. Specifically, when the groove pitch is 5.6 mm and the groove width of the circular groove 2 is 0.4 mm, the land width of the circular land portion 4 is 5.2 mm.

[0023] On the other hand, the groove pitch between adjacent straight grooves 3 can be set to be smaller than 100 mm, within the range of 35 to 60 mm, and the straight grooves 3 are formed with a groove width of 2 mm and a depth of 0.6 mm. Even in this case, by specifying the groove pitch, the land width of the linear land portion 5 formed between the linear grooves 3 is set in the range of 33 to 58 mm. If the groove pitch of the linear grooves is 100 mm or more, it becomes difficult to discharge slurry and polishing debris, and polishing scratches tend to occur easily.

[0024] In this embodiment, the groove pitch of the circular groove 2 is set to a dimension exceeding 5 mm and not exceeding 10 mm, and the relationship between the land width of the circular land portion 4 and the land width of the straight land portion 5 is specified as follows, and it has become clear through the following experiments that good polishing results can be obtained. In the polishing pad 1 of this embodiment, if the ratio of the area where the land portion is formed to the area of ​​the entire polishing surface is taken as the land area ratio, the polishing pad 1 of this embodiment is formed so that the land area ratio is 0.70 to 0.92.

[0025] Specifically, the method for calculating the land area ratio will be explained. First, the land area ratio of the circular groove 2 (area ratio of the circular land portion 4) and the land area ratio of the straight groove 3 (area ratio of the straight land portion 5) are calculated as follows. Land area ratio of circular groove 2 = Land width of circular groove 2 / Groove pitch of circular groove 2 (Equation 1) Land area ratio of straight groove 3 = land width of straight groove 3 2 / groove pitch of straight groove 3 2 (Formula 2) Based on the formulas 1 and 2, the land area ratio in the entire polishing pad 1 is calculated as follows. Land area ratio = Land area ratio of circular groove 2 × Land area ratio of straight groove 3 (Equation 3)

[0026] [Table 1]

[0027] Table 1 above shows the results of experiments carried out under the following conditions to evaluate the polishing performance of polishing pad 1 according to Examples 1 to 4 of the present invention and Comparative Examples 1 to 4 based on the land area ratio. In the above Examples 1 to 4 and Comparative Examples 1 to 4, a polishing pad 1 having a polishing layer made of the same material was used, and circular grooves 2 and linear grooves 3 were formed on the polishing surface of the polishing pad 1 with the groove pitch and groove width shown in Table 1.

[0028] The polishing pad 1 used in the above examples and comparative examples was produced as follows. 2.8 parts of expanded hollow microparticles with a particle size of 15 to 25 μm, in which the shell portion is made of acrylonitrile-vinylidene chloride copolymer and isobutane gas is contained in the shell, were added and mixed with 100 parts of urethane prepolymer with an NCO equivalent of 460, which was made by reacting 2,4-tolylene diisocyanate (TDI), poly(oxytetramethylene) glycol (PTMG) and diethylene glycol (DEG), to obtain a urethane prepolymer mixed liquid. The obtained urethane prepolymer mixed liquid was charged into a first liquid tank and kept at 80°C. In addition to the first liquid tank, 25.5 parts of 3,3'-dichloro-4,4'-diaminodiphenylmethane (methylenebis-o-chloroaniline) (MOCA) and 8.5 parts of polypropylene glycol were charged into a second liquid tank as a curing agent, and the curing agent was melted and mixed by heating at 120°C to obtain a curing agent melt liquid.

[0029] Next, the liquids in the first liquid tank and the second liquid tank were poured into a mixer equipped with two injection ports, and mixed and stirred to obtain a mixed liquid. At this time, the mixing ratio was adjusted so that the R value, which represents the equivalent ratio of the amino group and hydroxyl group in the curing agent to the isocyanate group at the end of the urethane prepolymer, was 0.90.

[0030] The resulting mixture was poured into a mold preheated to 100°C and cured primarily at 110°C for 30 minutes. The resulting block-shaped molded product was removed from the mold and cured secondary at 130°C for 2 hours in an oven to obtain a polyurethane polyurea resin molded product. The resulting polyurethane polyurea resin molded product was allowed to cool to 25°C, heated again in an oven at 120°C for 5 hours, and then sliced ​​to a thickness of 1.3 mm to obtain a polyurethane foam sheet (polishing layer). Thereafter, concentric circular grooves and lattice-patterned linear grooves were formed on the surface of the polishing layer as shown in Examples 1 to 4 or Comparative Examples 1 to 4 below, and double-sided tape was attached to the back surface not used for polishing to form a polishing pad.

[0031] In the polishing pad 1 of Example 1, circular grooves 2 were formed with a groove pitch of 5.6 mm, a groove width of 0.4 mm, a groove depth of 0.6 mm, and a land width of 5.2 mm, and linear grooves 3 were formed with a groove pitch of 35 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 33 mm. As a result, the land area ratio of Example 1 was 0.83. In the polishing pad 1 of Example 2, circular grooves 2 were formed with a groove pitch of 5.6 mm, a groove width of 0.8 mm, a groove depth of 0.6 mm, and a land width of 4.8 mm, and linear grooves 3 were formed with a groove pitch of 35 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 33 mm. As a result, the land area ratio of Example 2 was 0.76. In the polishing pad 1 of Example 3, circular grooves 2 were formed with a groove pitch of 5.6 mm, a groove width of 0.4 mm, a groove depth of 0.6 mm, and a land width of 5.2 mm, and linear grooves 3 were formed with a groove pitch of 60 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 58 mm. As a result, the land area ratio of Example 3 was 0.87. In the polishing pad 1 of Example 4, circular grooves 2 were formed with a groove pitch of 5.6 mm, a groove width of 0.8 mm, a groove depth of 0.6 mm, and a land width of 4.8 mm, and linear grooves 3 were formed with a groove pitch of 60 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 58 mm. As a result, the land area ratio of Example 4 was 0.80.

[0032] In the polishing pad 1 of Comparative Example 1, circular grooves 2 were formed with a groove pitch of 2.8 mm, a groove width of 0.4 mm, a groove depth of 0.6 mm, and a land width of 2.4 mm, and linear grooves 3 were formed with a groove pitch of 35 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 33 mm. As a result, the land area ratio of Comparative Example 1 was 0.76. In the polishing pad 1 of Comparative Example 2, circular grooves 2 were formed with a groove pitch of 2.8 mm, a groove width of 0.8 mm, a groove depth of 0.6 mm, and a land width of 2.0 mm, and linear grooves 3 were formed with a groove pitch of 35 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 33 mm. As a result, the land area ratio of Comparative Example 2 was 0.63. In the polishing pad 1 of Comparative Example 3, the circular grooves 2 were formed with a groove pitch of 11.2 mm, a groove width of 0.4 mm, a groove depth of 0.6 mm, and a land width of 10.8 mm, and the linear grooves 3 were formed with a groove pitch of 35 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 33 mm. As a result, the land area ratio of Comparative Example 3 was 0.86. In the polishing pad 1 of Comparative Example 4, circular grooves 2 were formed with a groove pitch of 11.2 mm, a groove width of 0.4 mm, a groove depth of 0.6 mm, and a land width of 10.8 mm, and linear grooves 3 were formed with a groove pitch of 120 mm, a groove width of 2 mm, a groove depth of 0.6 mm, and a land width of 118 mm. As a result, the land area ratio of Comparative Example 4 was 0.93.

[0033] In the experiment, the surface of a tantalum nitride film substrate was polished as the workpiece using an Ebara Corporation F-REX300X polishing machine. The rotation speed of the holding platen of the polishing machine was set to 70 rpm, the rotation speed of the polishing platen was set to 71 rpm, and polishing was performed while pressing the polishing pad 1 against the workpiece with a polishing pressure of 3.5 psi. A slurry, a CuBM slurry manufactured by Fujifilm, was supplied between the polishing pad 1 and the workpiece at a temperature of 20° C. and a rate of 200 ml / min. The dresser used was A188 manufactured by 3M Co., Ltd. The pad break was performed at 32N for 20 minutes, and the conditioning was performed at 35N for 4 scans ex-situ.

[0034] Then, polishing was carried out for 60 seconds using the above polishing device, and the polishing rate of the polished workpiece was measured as follows. For the tantalum nitride film on the substrate before and after the polishing test, 121 locations were randomly selected across the entire substrate, and the thicknesses of those locations before and after the polishing test were measured. Based on the measured thickness, the average thickness before the polishing test and the average thickness after the polishing test were calculated, and the average polished thickness was calculated by taking the difference between these average values. The polishing rate (Å / min) was calculated by dividing the average polished thickness by the polishing time. The thickness was measured using an optical film thickness and film quality measuring instrument (KLA Tencor, model number "ASET-F5x") in DBS mode.

[0035] As a result of the above experiment, as shown in Table 1, in Examples 1 to 4, the polishing rate exceeded 950, and good polishing results were obtained in all cases, whereas in the above Comparative Examples 1 to 4, good polishing results were not obtained. The reason for this is that, when comparing Example 2 and Comparative Example 1, although the land area ratio is the same, it is presumed that the groove pitch of the circular groove 2 in Comparative Example 1 is 5 mm or less, and therefore the rigidity of the circular land portion 4 could not be maintained during polishing. Similarly, in Comparative Example 2, the groove pitch of the circular grooves 2 was 5 mm or less and the land area ratio was less than 0.70, so it is presumed that a good polishing rate was not obtained. In addition, in Comparative Example 3, although the land area ratio was 0.83, it is presumed that because the groove pitch of the circular grooves 2 was greater than 10 mm, the slurry was not sufficiently retained and therefore a good polishing rate was not obtained. Furthermore, in Comparative Example 4, since the land area ratio was greater than 0.92, the balance between the slurry retention capacity of the circular grooves 2 and the slurry discharge capacity of the straight grooves 3 was poor, and since the groove pitch of the circular grooves 2 was greater than 10 mm, the slurry was no longer sufficiently retained, and therefore it is presumed that a good polishing rate was not obtained. [Explanation of symbols]

[0036] 1 Polishing pad 2 Circular groove 3 Straight groove 4 Circular land 5 Straight land section

Claims

1. A polishing pad having a polishing surface of a polishing layer made of hard urethane, on which a plurality of circular grooves arranged concentrically and a plurality of linear grooves intersecting in a lattice pattern are formed, The groove pitch between adjacent circular grooves is more than 5 mm and is 10 mm or less; The polishing pad further comprises a land area ratio of 0.70 to 0.92, the land area ratio being calculated by multiplying the area ratio of the circular land portion calculated by the following formula (1) based on the land width of the circular land portion formed between the circular grooves and the groove pitch of the circular grooves by the area ratio of the straight land portion calculated by the following formula (2) based on the land width of the straight land portion formed between the straight grooves and the groove pitch of the straight grooves, and the land area ratio being 0.70 to 0.92, and the land width of the straight land portion is set to 33 to 58 mm. Area ratio of circular land portion=land width of circular land portion / groove pitch of circular groove (Equation 1) Area ratio of straight land portion=land width of straight land portion / groove pitch of straight grooves (Equation 2)

2. 2. The polishing pad according to claim 1, wherein the circular groove has a groove width set to 0.4 to 0.8 mm.

Citation Information

Patent Citations

  • Polishing member, polishing method, polishing device, manufacture of semiconductor device and semiconductor device

    JP2000354952A

  • Polishing pad, polishing method, semiconductor device and manufacturing method thereof

    JP2006156876A

  • Polishing pad

    JP2013035108A

  • Metal film polishing pad and polishing method using the same

    JP2014038916A

  • Composite polishing layer chemical mechanical polishing pad