Method for manufacturing light-emitting device and method for removing hydrogen from light-emitting device
A method using voltage application, ultraviolet light, and heat treatment in a specific atmosphere effectively extracts hydrogen from the p-type layer of nitride semiconductor light emitting devices, addressing output reduction issues in high-Al composition devices.
Patent Information
- Application Number
- JP2021006743
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-19
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2041-01-19
AI Technical Summary
Light emitting devices made of nitride semiconductors face significant output reduction when hydrogen expelled from the p-type nitride semiconductor layer reaches the light emitting layer, particularly in devices using high-Al composition nitride semiconductors, as it is difficult to extract hydrogen without affecting device performance.
A method involving the application of a reverse or forward voltage lower than the rising voltage, combined with ultraviolet light irradiation and heat treatment in a specific atmosphere, is used to extract hydrogen from the p-type layer of nitride semiconductors, especially those with high Al composition, without passing through the light emitting layer.
This method effectively extracts hydrogen from the p-type layer, preventing a decrease in the output of the light emitting device and ensuring efficient operation even when using high-Al composition nitride semiconductors.
Smart Images

Figure 00000012_0000 
Figure 00000013_0000 
Figure 00000014_0000
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a light-emitting element and a method for extracting hydrogen from a light-emitting element. [Background technology]
[0002] Conventionally, there is known a technique for expelling hydrogen from a nitride semiconductor doped with a p-type impurity (see, for example, Patent Document 1). The technique described in Patent Document 1 includes a step of irradiating a nitride semiconductor doped with a p-type impurity with electromagnetic waves having an energy equal to or greater than the band gap energy of the nitride semiconductor, and a step of heat-treating the nitride semiconductor in an atmosphere that does not substantially contain active hydrogen.
[0003] According to Patent Document 1, hydrogen, which binds with p-type impurities and prevents them from acting as normal acceptors, is expelled from the nitride semiconductor layer, thereby lowering the resistance of the nitride semiconductor. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-238692 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in a light emitting device made of a nitride semiconductor, when hydrogen expelled from a p-type nitride semiconductor layer reaches the light emitting layer, the output of the light emitting device drops significantly (for example, by 20% or more).
[0006] In particular, in light-emitting devices that emit short-wavelength light, a p-type layer made of a nitride semiconductor with a large Al composition is used to suppress absorption of light emitted from the light-emitting layer itself, but since the high-energy light emitted from the light-emitting layer reaches the entire p-type layer made of this nitride semiconductor with a high Al composition, much hydrogen is separated from the p-type impurities and becomes capable of moving to the light-emitting layer. Also, because AlN has a stronger ability to bind hydrogen than GaN, or because it has high heat resistance, it is difficult to extract hydrogen from the p-type layer made of a nitride semiconductor with a high Al composition.
[0007] An object of the present invention is to provide a method for manufacturing a light-emitting element and a method for extracting hydrogen from a light-emitting element, which are capable of extracting hydrogen from a p-type layer made of a nitride semiconductor without reducing the output of the light-emitting element, and which are capable of effectively extracting hydrogen even when the p-type layer is made of a nitride semiconductor with a high Al composition. [Means for solving the problem]
[0008] In order to achieve the above object, one aspect of the present invention provides the following methods for producing a light-emitting device [1] to [4] and methods for removing hydrogen from a light-emitting device [5] to [8].
[0009] [1] A method for manufacturing a light-emitting device including an emission layer having an emission wavelength of 306 nm or less and a p-type layer made of AlGaInN containing Mg as an acceptor, the method comprising the steps of: forming the light-emitting device including the emission layer and the p-type layer; and irradiating the light-emitting device with ultraviolet light having a wavelength of 306 nm or less from the outside with a reverse voltage or a forward voltage lower than the turn-on voltage of the light-emitting device applied, or with no voltage applied, to the light-emitting device, thereby extracting hydrogen in the p-type layer to the outside of the light-emitting device, wherein the step of extracting hydrogen in the p-type layer to the outside of the light-emitting device is performed in an N2 atmosphere at 650°C or more, or in an N2+O2 atmosphere at 500°C or more. [2] The method for producing a light-emitting element according to [1] above, wherein a reverse voltage is applied to the light-emitting element in the step of extracting hydrogen from the p-type layer to the outside of the light-emitting element. [3] The method for producing a light-emitting device according to the above [1] or [2], wherein the AlGaInN constituting the p-type layer is AlGaN having an Al composition of 80% or more. [4] The method for producing a light-emitting element according to any one of the above [1] to [3], wherein the light-emitting element has a substrate, an n-type layer on the substrate, the light-emitting layer on the n-type layer, the p-type layer on the light-emitting layer, and a p-contact layer on the p-type layer, the p-contact layer having a band gap smaller than those of the substrate and a layer located between the substrate and the light-emitting layer, and in the step of extracting hydrogen in the p-type layer to the outside of the light-emitting element, the light-emitting element is irradiated from the substrate side with ultraviolet light having an energy lower than the band gap of the substrate and the layer located between the substrate and the light-emitting layer. [5] A method for extracting hydrogen from a light-emitting element including a light-emitting layer having an emission wavelength of 306 nm or less and a p-type layer made of AlGaInN containing Mg as an acceptor, the method comprising the steps of: irradiating the light-emitting element with ultraviolet light having a wavelength of 306 nm or less from the outside with a reverse voltage or a forward voltage lower than the start-up voltage of the light-emitting element, or with no voltage applied, and performing a heat treatment to extract hydrogen in the p-type layer to the outside of the light-emitting element, the step of extracting hydrogen in the p-type layer to the outside of the light-emitting element being carried out in an N2 atmosphere at 650°C or more, or in an N2+O2 atmosphere at 500°C or more. [6] The method for extracting hydrogen from a light-emitting element according to the above [5], wherein a reverse voltage is applied to the light-emitting element in the step of extracting hydrogen in the p-type layer to the outside of the light-emitting element. [7] The method for extracting hydrogen from a light-emitting element according to the above [5] or [6], wherein the AlGaInN constituting the p-type layer is AlGaN having an Al composition of 80% or more. [8] The method for extracting hydrogen from a light-emitting element described in any one of [5] to [7], wherein the light-emitting element has a substrate, an n-type layer on the substrate, the light-emitting layer on the n-type layer, the p-type layer on the light-emitting layer, and a p-contact layer on the p-type layer, the p-contact layer having a band gap smaller than that of the substrate and a layer located between the substrate and the light-emitting layer, and in the step of extracting hydrogen in the p-type layer to the outside of the light-emitting element, the light-emitting element is irradiated from the substrate side with ultraviolet light having an energy lower than the band gap of the substrate and a layer located between the substrate and the light-emitting layer. Effect of the Invention
[0010] According to the present invention, it is possible to provide a method for manufacturing a light-emitting element and a method for extracting hydrogen from a light-emitting element that can extract hydrogen from a p-type layer made of a nitride semiconductor without reducing the output of the light-emitting element, and that can effectively extract hydrogen even when the p-type layer is made of a nitride semiconductor with a high Al composition. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a vertical cross-sectional view of a light-emitting device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing the emission spectra of a light-emitting element having an emission wavelength of 280 nm and a light-emitting element having an emission wavelength of 340 nm before and after aging. [Diagram 3] 3(a) and (b) are graphs showing the SIMS profiles of Al, Mg, Si, and H before and after aging of the light-emitting element. [Figure 4] FIG. 4 is a bar graph showing the H concentration read from the SIMS profile of FIG. 3(b) in each of the hole supply layer, the electron blocking layer, and the light emitting layer to the n-type contact layer of the light emitting device. [Diagram 5]FIG. 5 is a graph showing SIMS profiles of Al, Mg, Si, and H of the light-emitting element immediately after manufacture, after heat treatment, and after heat treatment and ultraviolet light irradiation. [Figure 6] FIG. 6 is a bar graph showing the H concentration read from the SIMS profile of FIG. 5 in each of the hole supply layer, the electron blocking layer, and the light emitting layer to the n-type contact layer of the light emitting element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Configuration of light-emitting element) 1 is a vertical cross-sectional view of a light-emitting element 1 according to an embodiment of the present invention. The light-emitting element 1 is a flip-chip mounted light-emitting diode (LED).
[0013] The light-emitting element 1 comprises a substrate 10, a buffer layer 11 on the substrate 10, an n-type contact layer 12 on the buffer layer 11, a light-emitting layer 13 on the n-type contact layer 12, an electron blocking layer 14 on the light-emitting layer 13, a hole supply layer 15 on the electron blocking layer 14, a p-type contact layer 16 on the hole supply layer 15, a p-electrode 17 connected to the p-type contact layer 16, and an n-electrode 18 connected to the n-type contact layer 12.
[0014] In addition, the term "upper" in the configuration of the light-emitting element 1 refers to the "upper" when the light-emitting element 1 is placed in the orientation shown in FIG.
[0015] The substrate 10 is a growth substrate made of sapphire. The thickness of the substrate 10 is, for example, 400 to 1000 μm. As the material of the substrate 10, other than sapphire, AlN, Si, SiC, ZnO, etc. can be used.
[0016] The buffer layer 11 has a structure in which, for example, three layers, a nucleus layer, a low-temperature buffer layer, and a high-temperature buffer layer, are laminated in this order. The nucleus layer is made of non-doped AlN grown at a low temperature, and is a layer that serves as a nucleus for crystal growth. The nucleus layer has a thickness of, for example, 10 nm. The low-temperature buffer layer is a layer made of non-doped AlN grown at a higher temperature than the nucleus layer. The low-temperature buffer layer has a thickness of, for example, 0.3 μm. The high-temperature buffer layer is a layer made of non-doped AlN grown at a higher temperature than the low-temperature buffer layer. The high-temperature buffer layer has a thickness of, for example, 2.7 μm. By providing such a buffer layer 11, it is possible to reduce the density of threading dislocations in AlN and prevent cracks.
[0017] The n-type contact layer 12 is made of n-type AlGaInN containing a donor such as Si, typically AlGaN. In order to suppress absorption by the n-type contact layer 12 of light emitted from the light emitting layer 13, it is preferable that the band gap of the n-type contact layer 12 is higher than the band gap of the light emitting layer 13 (the band gap of the well layer in the case of an MQW structure). For example, when the n-type contact layer 12 and the light emitting layer 13 are made of AlGaN, it is preferable that the Al composition of the n-type contact layer 12 is higher than the Al composition of the light emitting layer 13 (the Al composition of the well layer in the case of an MQW structure), and is preferably within a range of, for example, 50% or more and 75% or less. In this case, ideally, the n-type contact layer 12 is made of Al x Ga 1-x N (0.5≦x≦0.75). The percentage of the Al composition is the ratio of the Al content to the total value of the Ga content and the Al content.
[0018] Here, AlGaInN is a nitride semiconductor that is a compound of N and Al, Ga, or In, which are group III elements. In AlGaInN, the higher the Al composition, the larger the band gap tends to be, and the higher the In composition, the smaller the band gap tends to be.
[0019] The light emitting layer 13 is made of AlGaInN and preferably has a multiple quantum well (MQW) structure. The light emitting layer 13 has an emission wavelength of 306 nm or less, and the composition of the light emitting layer 13 (the composition of the well layer in the case of an MQW structure) is set according to the desired emission wavelength of 306 nm or less. For example, when the light emitting layer 13 is made of AlGaN and has an emission wavelength of 270 to 290 nm, the Al composition is set to about 35 to 50%.
[0020] For example, the light emitting layer 13 has an MQW structure with two well layers, i.e., a structure in which a first barrier layer, a first well layer, a second barrier layer, a second well layer, and a third barrier layer are stacked in this order. The first well layer and the second well layer are made of n-type AlGaN. The first barrier layer, the second barrier layer, and the third barrier layer are made of n-type AlGaN (with an Al composition of 100%, i.e., including AlN) having a higher Al composition than the first well layer and the second well layer.
[0021] As an example, the Al composition, thickness, and Si concentration as a dopant of the first and second well layers are 40%, 2.4 nm, and 9×10 18 cm -3 The Al composition, thickness, and Si concentration as a dopant of the first and second barrier layers are 55%, 19 nm, and 9×10 18 cm -3 The Al composition, thickness, and Si concentration as a dopant of the third barrier layer are 55%, 4 nm, and 5×10 18 cm -3 It is.
[0022] The electron blocking layer 14 is a layer for suppressing the diffusion of electrons toward the p-type contact layer 16, and is made of p-type AlGaInN containing Mg as an acceptor. The Mg concentration of the electron blocking layer 14 is, for example, 1×10 18 ~5×10 20 cm -3 It is.
[0023] In order to suppress absorption by the electron blocking layer 14 of light emitted from the light emitting layer 13, it is preferable that the band gap of the electron blocking layer 14 is higher than the band gap of the light emitting layer 13 (the band gap of the well layer in the case of an MQW structure). For example, when the electron blocking layer 14 and the light emitting layer 13 are made of AlGaN, The Al composition of the electron blocking layer 14 is preferably higher than the Al composition of the light emitting layer 13 (the Al composition of the well layer in the case of an MQW structure), and typically has an Al composition of 80% or more (including 100%). The thickness of the electron blocking layer 14 is, for example, 1 to 50 nm.
[0024] The hole supply layer 15 is made of p-type AlGaInN containing Mg as an acceptor. The Mg concentration of the hole supply layer 15 is, for example, 1×10 18 ~1×10 21 cm -3 The hole supply layer 15 is typically made of AlGaN having an Al composition higher than that of the light emitting layer 13 and lower than that of the electron blocking layer 14. The thickness of the hole supply layer 15 is, for example, 10 to 100 nm.
[0025] The p-type contact layer 16 is made of p-type AlGaInN containing Mg as an acceptor. In order to improve the contact with the p-electrode 17, the p-type contact layer 16 may be made of AlGaInN (including GaInN and GaN) having a low Al composition. The Mg concentration of the p-type contact layer 16 is, for example, 1×10 19 ~5×10 21 cm -3 The p-type contact layer 16 has a thickness of, for example, 5 to 30 nm.
[0026] The p-electrode 17 is made of a material capable of making ohmic contact with the p-type contact layer 16, such as ITO, IZO, ZnO, Al, Rh, or Ag. The n-electrode 18 is made of a material capable of making ohmic contact with the n-type contact layer 12, such as Ti / Al or V / Al.
[0027] (Problems caused by hydrogen in the p-type layer) In the p-type layers, the electron blocking layer 14, the hole supply layer 15, and the p-type contact layer 16, immediately after deposition, Mg-NH bonds are formed by bonding between nitrogen in AlGaInN, Mg as an acceptor, and hydrogen contained in the raw material gas. Since Mg contained in the Mg-NH bonds prevents it from functioning as an acceptor, the formation of the Mg-NH bonds increases the electrical resistance of the p-type layers, decreasing the initial forward voltage (V F ) to increase
[0028] Furthermore, when the light emitting element 1 is operated immediately after the film formation, the light of 306 nm or less emitted by the light emitting layer 13 has energy of 4.1 eV or more, which is the bond energy of the NH bond, and breaks the NH bond in the Mg-NH bond, generating free hydrogen that can move to the light emitting layer 13. Then, due to a forward voltage of a magnitude equal to or greater than the turn-on voltage applied to operate the light emitting element 1, the hydrogen that has broken the bond with N is attracted to the n-electrode 18 and passes through the light emitting layer 13, causing point defects and causing a decrease in the output of the light emitting element 1. In addition, the heat generated by the p-type layer absorbing the light emitted by the light emitting layer 13 also promotes the breaking of the NH bond and the movement of the broken hydrogen.
[0029] In particular, a p-type layer made of AlGaInN with a high Al composition is prone to generate a large amount of free hydrogen that can migrate to the light emitting layer 13, and it is difficult to remove the hydrogen by heat treatment or the like, for the reasons described below.
[0030] The p-type layer made of AlGaInN with a high Al composition has a large band gap and therefore does not easily absorb the light emitted from the light-emitting layer 13. As a result, light reaches the entire p-type layer, and the NH bonds in the Mg-NH bonds in the entire p-type layer are broken, resulting in a particularly large amount of free hydrogen that can move to the light-emitting layer 13. In addition, since Al has a stronger ability to bind H than Ga, it is difficult to extract hydrogen from the p-type layer made of AlGaInN with a high Al composition. Hydrogen can be extracted more effectively by increasing the temperature of the heat treatment for extracting hydrogen, but in reality, an upper limit of the heat treatment temperature is set to suppress damage caused by heat to the light-emitting element 1, and therefore hydrogen tends to remain in AlGaInN with a high Al composition.
[0031] In the light-emitting device 1 according to the present embodiment, the electron blocking layer 14, the hole supply layer 15, and the p-type contact layer 16 correspond to the p-type layers, and among them, the Al composition of the electron blocking layer 14 is the highest. For example, when the electron blocking layer 14 is made of AlGaN with an Al composition of 80% or more, it is particularly difficult to extract hydrogen from the p-type layer, and therefore the method of extracting hydrogen of the present invention is particularly effective.
[0032] (Method of manufacturing light-emitting element) An example of a method for manufacturing the light-emitting element 1 according to the embodiment of the present invention will be described below. In forming each layer of the light-emitting element 1 by vapor phase growth, the Ga source gas, the Al source gas, and the N source gas are, for example, trimethylgallium, trimethylaluminum, and ammonia, respectively. The source gas for Si, which is an n-type dopant, and the source gas for Mg, which is a p-type dopant, are, for example, silane gas and bis(cyclopentadienyl)magnesium gas, respectively. The carrier gas is, for example, hydrogen gas or nitrogen gas.
[0033] First, a substrate 10 is prepared, and a buffer layer 11 is formed thereon. In forming the buffer layer 11, a nucleus layer made of AlN is first formed by MOVPE. The growth temperature is, for example, 880° C. The nucleus layer may be formed by sputtering. Next, a low-temperature buffer layer and a high-temperature buffer layer made of AlN are sequentially formed on the nucleus layer by MOVPE. The growth conditions for the low-temperature buffer layer are, for example, a growth temperature of 1090° C. and a growth pressure of 50 mbar. The growth conditions for the high-temperature buffer layer are, for example, a growth temperature of 1270° C. and a growth pressure of 50 mbar.
[0034] Next, an n-type contact layer 12 made of AlGaN containing Si is formed by MOVPE on the buffer layer 11. The growth conditions for the n-type contact layer 12 are, for example, a growth temperature of 980° C. and a growth pressure of 50 to 100 mbar.
[0035] Next, the light emitting layer 13 is formed by MOVPE on the n-type contact layer 12. The light emitting layer 13 is formed by stacking the first barrier layer, the first well layer, the second barrier layer, the second well layer, and the third barrier layer in this order. The growth conditions for the light emitting layer 13 are, for example, a growth temperature of 975° C. and a growth pressure of 400 mbar.
[0036] Next, the electron blocking layer 14 is formed by MOVPE on the light emitting layer 13. The growth conditions for the electron blocking layer 14 are, for example, a growth temperature of 975° C. and a growth pressure of 400 mbar.
[0037] Next, the hole supply layer 15 is formed by MOVPE on the electron blocking layer 14. The growth conditions for the hole supply layer 15 are, for example, a growth temperature of 1000 to 1100° C. and a growth pressure of 50 mbar.
[0038] Next, the p-type contact layer 16 is formed by MOVPE on the hole supply layer 15. The growth conditions for the p-type contact layer 16 are, for example, a growth temperature of 980° C. and a growth pressure of 50 mbar.
[0039] Next, a predetermined region on the surface of the p-type contact layer 16 is dry etched to form a groove deep enough to reach the n-type contact layer 12 .
[0040] Next, a p-electrode 17 is formed on the p-type contact layer 16, and an n-electrode 18 is formed on the n-type contact layer 12 exposed on the bottom surface of the groove. The p-electrode 17 and the n-electrode 18 are formed by sputtering, vapor deposition, or the like.
[0041] Next, hydrogen contained in the p-type layers, that is, the electron blocking layer 14, the hole supply layer 15, and the p-type contact layer 16, is extracted to the outside of the light emitting element 1 by the method described below.
[0042] A reverse voltage or a forward voltage lower than the turn-on voltage of the light-emitting element 1 (e.g., 2 V) is applied between p-electrode 17 and n-electrode 18 of the light-emitting element 1, or with no voltage applied, ultraviolet light having a wavelength of 306 nm or less is irradiated from the outside and a heat treatment is performed, thereby extracting hydrogen from the p-type layers, that is, the electron blocking layer 14, the hole supply layer 15, and the p-type contact layer 16, to the outside of the light-emitting element 1.
[0043] The reason why hydrogen is extracted when a reverse voltage or a forward voltage lower than the turn-on voltage of the light-emitting element 1 is applied, or when no voltage is applied, is that when a voltage equal to or higher than the turn-on voltage of the light-emitting element 1 is applied, hydrogen whose bond with N in the Mg-NH bond has been broken is attracted to the n-electrode 18 side and moves toward the light-emitting layer 13. Here, by applying a reverse voltage, hydrogen whose bond with N has been broken is attracted to the p-electrode 17 side, and can be extracted more reliably without passing through the light-emitting layer 13.
[0044] The reason for irradiating ultraviolet light with a wavelength of 306 nm or less is to cut the NH bond in the Mg-NH bond by irradiating light with energy of 4.1 eV or more, which is the bond energy of the NH bond. If the ultraviolet light is absorbed by other layers before it reaches the p-type layer, hydrogen cannot be extracted effectively, so it is preferable that the ultraviolet light has a wavelength in a band that is not absorbed by the layers it passes through before reaching the p-type layer.
[0045] For example, as described above, the p-type contact layer 16 may be made of AlGaN (including GaN) having a low Al composition in order to improve contact with the p-electrode 17. In this case, the p-type contact layer 16 usually has a smaller band gap than the substrate 10 and the layers (buffer layer 11 and n-type contact layer 12) located between the substrate 10 and the light emitting layer 13, so it is preferable to irradiate the p-type contact layer 16 with ultraviolet light from the substrate 10 side in order to avoid absorption of ultraviolet light by the p-type contact layer 16. In this case, ultraviolet light with energy lower than the band gap of the substrate 10 and the layers located between the substrate 10 and the light emitting layer 13 is irradiated in order to suppress absorption by the substrate 10 and the layers located between the substrate 10 and the light emitting layer 13.
[0046] The heat treatment is performed to promote the breaking of the NH bond in the Mg-NH bond and the movement of hydrogen whose bond with N has been broken from the p-type layer. The hydrogen extraction step is performed in an N2 atmosphere at 650°C or higher, or in an N2+O2 atmosphere at 500°C or higher, in order to effectively extract hydrogen even when the p-type layer contains a layer made of AlGaN with an Al composition of 80% or more, such as the electron block layer 14. By performing the hydrogen extraction step in an N2 atmosphere that does not contain hydrogen, hydrogen can be extracted effectively, and in particular, by performing the hydrogen extraction step in an N2 atmosphere at 650°C or higher, hydrogen can be extracted more effectively. Furthermore, if oxygen is contained in the atmosphere, the interface energy of the crystal surface (the surface of the p-type contact layer 16) decreases, making it easier to extract hydrogen. Therefore, when the hydrogen extraction step is performed in an N2+O2 atmosphere, hydrogen can be extracted more effectively under a temperature condition of 500°C or higher.
[0047] The light-emitting element to which the method of extracting hydrogen from a p-type layer of the present invention can be applied is not limited to the light-emitting element 1 according to the present embodiment, and can also be applied to light-emitting elements having other configurations. That is, according to the present invention, there can be provided a method for manufacturing a light-emitting element including a light-emitting layer emitting light having a wavelength of 306 nm or less and a p-type layer made of AlGaInN containing Mg as an acceptor, the method including: forming a light-emitting element including the light-emitting layer and the p-type layer; irradiating the light-emitting element with ultraviolet light having a wavelength of 306 nm or less from the outside with a reverse voltage or a forward voltage lower than the start-up voltage of the light-emitting element applied to the light-emitting element, or with no voltage applied, and performing a heat treatment to extract hydrogen in the p-type layer to the light-emitting element; and performing the step of extracting H in the p-type layer to the light-emitting element in an N2 atmosphere at 650° C. or more or an N2+O2 atmosphere at 500° C. or more.
[0048] Furthermore, the method of extracting hydrogen from a p-type layer of the present invention can be carried out independently on a manufactured light-emitting device, not as a part of the manufacturing process. That is, according to the present invention, there can be provided a method of extracting hydrogen from a light-emitting device including a light-emitting layer having an emission wavelength of 306 nm or less and a p-type layer made of AlGaInN containing Mg as an acceptor, the method including the steps of irradiating the light-emitting device with ultraviolet light having a wavelength of 306 nm or less from the outside and performing a heat treatment to extract hydrogen from the p-type layer to the outside of the light-emitting device while applying a reverse voltage or a forward voltage lower than the start-up voltage of the light-emitting device, or while applying no voltage, and performing the step of extracting hydrogen from the p-type layer to the outside of the light-emitting device in an N2 atmosphere at 650°C or more or in an N2+O2 atmosphere at 500°C or more.
[0049] (Effects of the embodiment) According to the above-described embodiment of the present invention, hydrogen is extracted from the p-type layer made of a nitride semiconductor without passing through the light-emitting layer, thereby preventing a decrease in the output of the light-emitting device. Moreover, even if the p-type layer is made of a nitride semiconductor with a high Al composition, hydrogen can be effectively extracted. EXAMPLES
[0050] The following is a result of examining the effect of hydrogen in the p-type layer on the output of the light-emitting device 1 that emits light with a wavelength of 306 nm or less and has an energy of 4.1 eV or more, which is the bond energy of NH. Table 1 below shows the configuration of the light-emitting device 1 used in this examination.
[0051] [Table 1]
[0052] The light-emitting element 1 according to this embodiment having the configuration shown in Table 1 has an emission wavelength of 280 nm included in the UVC wavelength range. In this embodiment, a light-emitting element (referred to as light-emitting element A) having an emission wavelength of 340 nm included in the UVA wavelength range was used as a comparative example.
[0053] FIG. 2 is a graph showing the emission spectra of the light-emitting element 1 having an emission wavelength of 280 nm and the light-emitting element A having an emission wavelength of 340 nm before and after aging (application of a forward voltage of 9 V for 100 hours).
[0054] 2, "UVC" indicates the emission spectrum of the light-emitting element 1, and "UVA" indicates the emission spectrum of the light-emitting element A. Moreover, the spectra represented by the dotted lines are spectra measured before aging, and the spectra represented by the solid lines are spectra measured after aging.
[0055] 2, the intensity of the emission spectrum of the light-emitting element A hardly changes before and after aging. This is probably because the emission wavelength of the light-emitting element A is 340 nm, and its energy is lower than the NH bond energy of 4.1 eV, so the NH bond in the Mg-NH bond is not broken and almost no hydrogen migrates to the light-emitting layer.
[0056] 2, the intensity of the emission spectrum of the light-emitting element 1 decreases after aging. This is believed to be because the emission wavelength of the light-emitting element 1 is 280 nm, and the energy is higher than the NH bond energy of 4.1 eV, so that the NH bond in the Mg-NH bond is broken and the broken hydrogen migrates to the light-emitting layer 13 due to the forward voltage applied to the light-emitting element 1, etc.
[0057] Fig. 3(a) is a graph showing secondary ion mass spectrometry (SIMS) profiles of Al, Mg, Si, and H before and after aging of the light-emitting element A. Fig. 3(b) is a graph showing SIMS profiles of Al, Mg, Si, and H before and after aging of the light-emitting element 1.
[0058] The profiles represented by the dotted lines for each element in Figures 3(a) and (b) are profiles measured before aging, and the profiles represented by the solid lines are profiles measured after aging.
[0059] The ranges indicated by "12", "13", "14", and "15" in Fig. 3(b) correspond to the n-type contact layer 12, the light emitting layer 13, the electron blocking layer 14, and the hole supply layer 15, respectively, and can be confirmed by the changes in the concentrations of Al, Si, and Mg. "12", "13", "14", and "15" in Fig. 3(a) correspond to the AlGaN layer with an Al composition of 20 to 30% corresponding to the n-type contact layer 12, the MQW structure with an AlGaN layer with an Al composition of 7.5% corresponding to the light emitting layer 13 as a well layer, the AlGaN layer with an Al composition of 50% corresponding to the electron blocking layer 14, and the AlGaN layer with an Al composition of 20 to 30% corresponding to the hole supply layer 15, respectively.
[0060] According to Fig. 3(a), there is almost no change in the H concentration before and after aging. This means that there is almost no movement of hydrogen due to the light emission of light-emitting element A. This is thought to be because the light emitted by light-emitting element A does not break the NH bonds in the Mg-NH bonds in the p-type layer, and hydrogen cannot move from the p-type layer.
[0061] 3(b), after aging, the H concentration in the electron blocking layer 14, which is a p-type layer, decreases, and the H concentration in the n-type contact layer 12 increases. This means that hydrogen in the electron blocking layer 14 moves toward the n-type contact layer 12 through the light-emitting layer 13 due to the light emission of the light-emitting element 1. This is thought to be because the light emitted by the light-emitting element 1 breaks the NH bond in the Mg-NH bond in the electron blocking layer 14, and the broken hydrogen moves toward the n-electrode 18 due to the forward voltage applied to the light-emitting element 1, etc.
[0062] FIG. 4 shows the H concentration (cm) read from the SIMS profile of FIG. 3(b) in each of the hole supply layer 15, the electron blocking layer 14, and the light emitting layer 13 to the n-type contact layer 12 of the light emitting element 1. -2 4 is a bar graph showing the concentration before aging and the concentration after aging.
[0063] Next, the results of verification of the effect of the method of extracting hydrogen from a p-type layer according to the present invention in a light-emitting device 1 that emits light with a wavelength of 306 nm or less and has an energy of 4.1 eV or more, which is the bond energy of NH, are shown. The configuration of the light-emitting device 1 used in this verification is shown in Table 2 below. In this verification, the light-emitting device 1 in a wafer state before being divided into individual pieces was used.
[0064] [Table 2]
[0065] FIG. 5 is a graph showing SIMS profiles of Al, Mg, Si, and H of the light-emitting element 1 immediately after manufacture, after heat treatment at 550° C. in an air atmosphere, and after heat treatment at 550° C. in an air atmosphere and irradiation with ultraviolet light having a peak wavelength of 280 nm.
[0066] 5, the profile of each element represented by the dashed and dotted line is the profile measured immediately after production, the profile represented by the dotted line is the profile measured after heat treatment, and the profile represented by the solid line is the profile measured after heat treatment and UV light irradiation. Note that the heat treatment and UV light irradiation were performed without applying a voltage to the light-emitting element 1.
[0067] The areas indicated by "12," "13," "14," and "15" in FIG. 5 correspond to the n-type contact layer 12, the light-emitting layer 13, the electron blocking layer 14, and the hole supply layer 15, respectively, and these can be confirmed by changes in the concentrations of Al, Si, and Mg.
[0068] 5, the H concentration in the p-type electron blocking layer 14 and hole supply layer 15 decreases after the heat treatment, and further decreases after the heat treatment and UV light irradiation. No increase in the H concentration is observed in the light-emitting layer 13 or n-type contact layer 12. This is thought to be because the heat treatment breaks the NH bonds in the Mg-NH bonds in the p-type layer, and hydrogen that has broken its bond with N migrates to the p-electrode 17 side and is extracted without passing through the light-emitting layer 13, and because the combination of the heat treatment and UV light irradiation allows hydrogen to be extracted more effectively.
[0069] The reason why the difference between the H concentration after only the heat treatment and the H concentration after the heat treatment and the UV irradiation is not large is because the UV irradiation could not be performed with a sufficient amount of light due to the device used for measuring the SIMS profile shown in Fig. 5. If the UV irradiation is performed with a sufficient amount of light, the H concentration of the p-type layer can be reduced more significantly. As described above, the hydrogen extraction process is performed in an air atmosphere, but when the process is performed in an N2 atmosphere at 650°C or higher or an N2+O2 atmosphere at 500°C or higher, the H concentration of the p-type layer can be reduced more significantly in both the case of performing only the heat treatment and the case of performing the heat treatment and the UV irradiation.
[0070] FIG. 6 shows the H concentration (cm ) read from the SIMS profile of FIG. 5 in each of the hole supply layer 15, the electron blocking layer 14, and the light emitting layer 13 to the n-type contact layer 12 of the light emitting element 1. -2 ) is a bar graph showing
[0071] In Figure 6, "c" is the concentration immediately after production, "d" is the concentration after heat treatment at 550°C in an air atmosphere, and "e" is the concentration after heat treatment at 550°C in an air atmosphere and irradiation with ultraviolet light with a peak wavelength of 280 nm.
[0072] Although the embodiment and examples of the present invention have been described above, the present invention is not limited to the above embodiment and examples, and various modifications are possible without departing from the spirit of the invention. Furthermore, the components of the above embodiment and examples can be combined in any manner without departing from the spirit of the invention.
[0073] In addition, the above-described embodiments and examples do not limit the scope of the invention according to the claims. It should be noted that not all of the combinations of features described in the embodiments and examples are necessarily essential to the means for solving the problems of the invention. [Explanation of symbols]
[0074] 1 Light emitting element 10 Substrate 11 Buffer layer 12 n-type contact layer 13 Emitting layer 14 Electron Block Layer 15 Hole supply layer 16 p-type contact layer 17p electrode 18n electrode
Claims
1. A method for manufacturing a light-emitting device including a light-emitting layer having an emission wavelength of 306 nm or less and a p-type layer made of AlGaInN containing Mg as an acceptor, comprising: forming the light emitting device comprising the light emitting layer and the p-type layer; a step of irradiating the light emitting device with ultraviolet light having a wavelength of 306 nm or less from the outside while applying a reverse voltage to the light emitting device, and performing a heat treatment to extract hydrogen in the p-type layer to the outside of the light emitting device; Including, The step of extracting hydrogen from the p-type layer to the outside of the light emitting device is performed by N 2 In an atmosphere of 500°C or higher 2 +O 2 Conduct under atmospheric conditions. A method for manufacturing a light-emitting device.
2. The AlGaInN constituting the p-type layer is AlGaN having an Al composition of 80% or more. The method for producing the light-emitting device according to claim 1 .
3. the light-emitting element has a substrate, an n-type layer on the substrate, the light-emitting layer on the n-type layer, the p-type layer on the light-emitting layer, and a p-contact layer on the p-type layer; the p-contact layer has a band gap smaller than those of the substrate and a layer located between the substrate and the light-emitting layer; In the step of extracting hydrogen from the p-type layer to the outside of the light-emitting element, the light-emitting element is irradiated from the substrate side with ultraviolet light having an energy lower than a band gap of the substrate and a layer located between the substrate and the light-emitting layer. The method for producing the light-emitting device according to claim 1 .
4. A method for extracting hydrogen from a light-emitting device including a light-emitting layer having an emission wavelength of 306 nm or less and a p-type layer made of AlGaInN containing Mg as an acceptor, comprising the steps of: a step of irradiating the light emitting element with ultraviolet light having a wavelength of 306 nm or less from the outside while applying a reverse voltage to the light emitting element, and performing a heat treatment to extract hydrogen in the p-type layer to the outside of the light emitting element; The step of extracting hydrogen from the p-type layer to the outside of the light emitting device is performed by N 2 Atmosphere or N 2 +O 2 Conduct under atmospheric conditions. A method for extracting hydrogen from a light-emitting element.
5. The AlGaInN constituting the p-type layer is AlGaN having an Al composition of 80% or more. The method for extracting hydrogen from a light-emitting device according to claim 4.
6. the light-emitting element has a substrate, an n-type layer on the substrate, the light-emitting layer on the n-type layer, the p-type layer on the light-emitting layer, and a p-contact layer on the p-type layer; the p-contact layer has a band gap smaller than those of the substrate and a layer located between the substrate and the light-emitting layer; In the step of extracting hydrogen from the p-type layer to the outside of the light-emitting element, the light-emitting element is irradiated from the substrate side with ultraviolet light having an energy lower than a band gap of the substrate and a layer located between the substrate and the light-emitting layer. A method for extracting hydrogen from a light-emitting device according to claim 4 or 5.
Citation Information
Patent Citations
Method of lowering resistance of semiconductor nitride
JP1999238692A
Activation method of compound semiconductor thin film to p-type
JP2000031084A
Group iii nitride semiconductor laminate structure, and manufacturing method thereof
JP2010021439A
Hydrogen desorption method for nitride semiconductor
JP2020136305A