Conductive paste and conductive film
A conductive paste using tannic acid or derivatives, copper powder, and a thermosetting resin maintains high conductivity by suppressing oxidation, addressing the limitations of conventional copper pastes.
Patent Information
- Application Number
- JP2022547595
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-10
- Filing Date
- 2021-09-07
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2041-09-07
AI Technical Summary
Conventional copper pastes suffer from oxidation issues leading to increased resistivity over time, and existing additives like organic carboxylic acids are insufficient in maintaining conductivity.
A conductive paste comprising tannic acid or its derivatives, copper powder, a thermosetting resin, and a solvent, which enhances initial conductivity and suppresses oxidation through improved dispersibility and reducing properties of copper powder.
The conductive paste maintains excellent conductivity over a long period, even under moist heat conditions, with tannic acid derivatives further enhancing oxidation suppression and flexibility.
Smart Images

Figure 0007565097000001 
Figure 0007565097000002 
Figure 0007565097000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a conductive paste and a conductive film, and more particularly to a conductive paste containing at least one of tannic acid and a tannic acid derivative (A), copper powder (B), a thermosetting resin (C), and a solvent (D), and a conductive film including a cured product of the conductive paste. [Background technology]
[0002] A technology is used to form wiring by printing conductive paste on various substrates. Silver paste and copper paste are the main conductive pastes known in the past. Silver paste has good conductivity, but is expensive and prone to migration under high humidity, which can lead to problems with short circuits. For this reason, the use of copper paste instead of silver paste has been considered, but copper paste is more susceptible to oxidation than silver paste, and therefore has the problem that its resistivity increases over time and its conductivity is easily reduced.
[0003] As methods for suppressing the oxidation of such copper pastes, there have been proposed a method of treating the surface of the copper powder with an organic substance in advance, and a method of mixing an additive that suppresses the oxidation of copper into a composition containing the copper powder.
[0004] Patent Document 1 discloses a method of effectively removing an oxide film formed on the surface of easily oxidizable metal particles by treating metal fine particles in advance with an aqueous surface treatment agent containing an organic acid, and then adding an organic carboxylic acid as an additive to suppress the oxidation of copper to a composition containing the treated copper powder. Patent Document 2 discloses a method of suppressing the oxidation of copper powder by adding an organic carboxylic acid compound to a conductive copper paste containing copper powder, thereby donating protons to the oxide film on the surface of the copper powder and dissolving it.
[0005] The method of treating copper powder with an organic acid is effective in removing the copper oxide film already present on the copper powder used as a raw material, and is effective in terms of developing initial electrical conductivity, but is not sufficient to suppress oxidation over time. In addition, the method of adding an organic carboxylic acid compound is not sufficient to suppress the oxidation of copper powder. Therefore, there is a demand for a material that can develop a more effective reducing power for copper powder, and that can develop the original electrical conductivity of copper at an early stage and maintain that electrical conductivity for a long period of time to ensure the reliability of the product. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2014-011006 A [Patent Document 2] JP 2008-130301 A Summary of the Invention
[0007] An object of the present disclosure is to provide a conductive paste and a conductive film that are excellent in initial conductivity and can maintain this excellent conductivity over a long period of time.
[0008] The conductive paste according to one embodiment of the present disclosure contains (A) at least one of tannic acid and a tannic acid derivative, (B) copper powder, (C) a thermosetting resin, and (D) a solvent.
[0009] A conductive film according to one embodiment of the present disclosure includes a cured product of the conductive paste. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Conductive paste> The conductive paste of this embodiment (hereinafter also referred to as conductive paste (X)) contains at least one of tannic acid and a tannic acid derivative (A) (hereinafter also referred to as component (A)), copper powder (B), a thermosetting resin (C), and a solvent (D). The conductive paste (X) can be suitably used for forming a conductive film by thermal curing.
[0011] The present inventors have found that, in a conductive paste using copper powder as the metal powder, by using tannic acid or a derivative thereof, it is possible to obtain excellent initial conductivity and maintain the excellent conductivity for a long period of time. That is, the conductive paste (X) can realize a low initial resistivity value, and as evaluated by a moist heat test or the like, can suppress oxidation over time, and as a result, can maintain the conductivity for a long period of time. Although the reason is not necessarily clear, it can be inferred that, for example, tannic acid and tannic acid derivatives can increase the dispersibility of copper powder (B) in the conductive paste (X), and can suppress the oxidation of copper powder (B) due to their reducing properties, and can reduce copper oxide generated by the oxidation of copper to the original copper to restore the conductivity. In particular, it is considered that the component (A) exerts a high reducing power when the thermosetting resin (C) is thermally cured, and the conductive paste (X) can exhibit high initial conductivity, and in addition, it is considered that this high conductivity can be maintained for a long period of time due to the reducing power of the component (A). In this way, the conductive paste (X) has excellent initial conductivity and can maintain this excellent conductivity for a long period of time.
[0012] [Component (A)] Component (A) is at least one of tannic acid and a tannic acid derivative. "Tannic acid" includes both tannic acid in the broad sense and m-galloyl gallic acid, which is tannic acid in the narrow sense. Tannic acid in the broad sense is a general term for aromatic compounds having a large number of phenolic hydroxyl groups, such as condensed tannins, which are derivatives of flavanols, and hydrolyzed tannins in which one or more gallic acids are ester-bonded to sugars (usually glucose). The number of phenolic hydroxyl groups in one molecule of tannic acid is usually 3 to 100, preferably 10 to 50, and more preferably 20 to 30. The molecular weight of tannic acid is usually 300 to 15,000, preferably 500 to 5,000, and more preferably 1,000 to 2,500.
[0013] The term "tannic acid derivative" refers to, for example, a compound in which some or all of the hydrogen atoms in the phenolic hydroxyl group of tannic acid are substituted with a substituent (hereinafter also referred to as the substituent (S)). The tannic acid derivative is a compound in which tannic acid has been hydrophobized.
[0014] The component (A) preferably contains a tannic acid derivative. By using a tannic acid derivative obtained by hydrophobizing tannic acid as the component (A), the conductive paste (X) has a greater effect of suppressing oxidation over time, and in particular, can further suppress an increase in the resistivity in a moist heat resistance test (e.g., 85°C, 85% RH, 100 hours, etc.).
[0015] The tannic acid derivative preferably includes a tannic acid derivative in which a part or all of the phenolic hydroxyl groups of the tannic acid are reacted with a compound having an isocyanate to form a urethane bond. By introducing a urethane bond into the tannic acid derivative, the flexibility of the conductive film formed from the conductive paste (X) is increased, and thus the application to flexible substrates such as film substrates is expected.
[0016] In addition, the tannic acid derivative is preferably one in which a part or all of the phenolic hydroxyl groups of tannic acid are reacted with a silane coupling agent to form -Si-O- bonds. By introducing -Si-O- bonds into the tannic acid derivative, it is expected that the dispersibility of the copper powder (B) is further improved, and the adhesion between the conductive film formed from the conductive paste (X) and the substrate is improved.
[0017] Examples of the substituent (S) include hydrocarbon groups such as alkyl groups such as methyl groups, cycloalkyl groups such as cyclohexyl groups, aryl groups such as phenyl groups, and aralkyl groups such as benzyl groups; groups in which some or all of the hydrogen atoms of these hydrocarbon groups have been substituted with other substituents; -CONHR (R is a monovalent organic group having 1 to 20 carbon atoms); -Si(OR')2R" (R' is a monovalent hydrocarbon group having 1 to 10 carbon atoms, and R" is a monovalent organic group having 1 to 20 carbon atoms). The term "organic group" refers to a group containing at least one carbon atom.
[0018] The substituent (S) preferably contains a group having a polymerizable group. In this case, the curing shrinkage of the conductive paste (X) during thermal curing can be increased, and as a result, the conductivity can be improved. Examples of the polymerizable group include a (meth)acryloyl group, a vinyl group, an epoxy group, a glycidyl group, an amino group, and a mercapto group.
[0019] The -CONHR as the substituent (S) is formed by reacting a compound having an isocyanate group with tannic acid. Examples of the organic group represented by R include monovalent hydrocarbon groups such as substituted or unsubstituted butyl groups, and groups containing polymerizable groups such as (meth)acryloyl groups, vinyl groups, and glycidyl groups. By making R a group containing a polymerizable group, the curing shrinkage of the conductive paste (X) during thermal curing can be increased, and the conductivity can be further improved.
[0020] The -Si(OR')2R" as the substituent (S) is formed by reacting tannic acid with a silane coupling agent. Examples of the hydrocarbon group represented by R' include alkyl groups such as methyl and ethyl groups. Examples of the organic group represented by R" include substituted or unsubstituted monovalent hydrocarbon groups, and groups containing a polymerizable group such as glycidyl, epoxy, (meth)acryloyl, vinyl, amino, and mercapto groups. By using a group containing a polymerizable group as R", the curing shrinkage of the conductive paste (X) during thermal curing can be increased, and the conductivity can be further improved.
[0021] The substitution rate in the tannic acid derivative (the ratio of the number of substituents (S) in one molecule of the tannic acid derivative to the number of phenolic hydroxyl groups in one molecule of tannic acid before substitution) is preferably 10% or more. In this case, the moist heat resistance of the conductive paste (X) can be more effectively improved. The substitution rate is more preferably 15% or more, even more preferably 20% or more, and particularly preferably 30% or more. The substitution rate in the tannic acid derivative is preferably 65% or less. In this case, the oxidation inhibition effect in the conductive paste (X) can be further improved. The substitution rate is more preferably 60% or less, even more preferably 55% or less, and particularly preferably 50% or less.
[0022] The proportion of component (A) is preferably 0.05 parts by mass or more and 5.0 parts by mass or less relative to 100 parts by mass of copper powder (B). In this case, the conductivity and continuity of the conductive paste (X) can be further improved. The proportion of component (A) is more preferably 0.1 parts by mass or more and 3.0 parts by mass or less, even more preferably 0.4 parts by mass or more and 2.0 parts by mass or less, and particularly preferably 0.5 parts by mass or more and 1.2 parts by mass or less relative to 100 parts by mass of copper powder (B).
[0023] The proportion of component (A) in the conductive paste (X) is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.05% by mass or more and 5% by mass or less, even more preferably 0.1% by mass or more and 3% by mass or less, and particularly preferably 0.4% by mass or more and 1.5% by mass or less.
[0024] [Copper powder (B)] The copper powder (B) is a metal particle containing copper as a main component, with copper exposed on the particle surface.
[0025] The shape of the copper powder (B) may be, for example, spherical, flat (scale), dendritic, or amorphous. The copper powder (B) may be a combination of two or more of these shapes. The excellent electrical conductivity and oxidation resistance of the conductive paste (X) are due to the excellent reducing power of the component (A) against copper, and the shape and particle size of the copper powder (B) are not particularly limited.
[0026] From the viewpoint of printability, the average particle size of the copper powder (B) is preferably 0.1 μm or more and 30 μm or less, more preferably 0.5 μm or more and 20 μm or less, and even more preferably 1 μm or more and 10 μm or less. The average particle size is the median size, which is determined by measuring the particle size distribution (volume basis) of the copper powder (B) and indicates the particle size at 50 volume % of the cumulative distribution.
[0027] The proportion of copper powder (B) in the conductive paste (X) is preferably 50% by mass or more and 99% by mass or less, more preferably 60% by mass or more and 98% by mass or less, even more preferably 70% by mass or more and 95% by mass or less, and particularly preferably 80% by mass or more and 90% by mass or less.
[0028] [Thermosetting resin (C)] The conductive paste (X) contains a thermosetting resin (C), which allows the conductive paste (X) to be cured by heating to form a conductive film.
[0029] Examples of the thermosetting resin (C) include amino resins, urethane resins, unsaturated polyester resins, epoxy resins, cyanate resins, acrylic resins, phenolic resins such as novolac-type phenolic resins and resol-type phenolic resins, etc. The thermosetting resin (C) does not include tannic acid and tannic acid derivatives.
[0030] The thermosetting resin (C) preferably contains one having a phenolic hydroxyl group. In this case, the thermosetting resin (C) can be cured with a larger amount of shrinkage due to thermal curing, and as a result, the electrical conductivity of the conductive paste (X) can be improved. Examples of the thermosetting resin (C) having a phenolic hydroxyl group include phenolic resins.
[0031] The proportion of the thermosetting resin (C) in the conductive paste (X) is preferably 1% by mass or more and 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, and even more preferably 5% by mass or more and 15% by mass or less.
[0032] Furthermore, the conductive paste (X) may contain, for example, a curing agent, a curing accelerator, etc., in order to accelerate the curing of the thermosetting resin (C).
[0033] As the curing agent, any agent capable of curing the thermosetting resin (C) can be used, and examples thereof include novolac resins; latent amine-based curing agents such as dicyandiamide, imidazole, BF3-amine complexes, and guanidine derivatives; aromatic amines such as metaphenylenediamine, diaminodiphenylmethane, and diaminodiphenylsulfone; curing agents containing nitrogen atoms such as cyclophosphazene oligomers; and acid anhydride-based curing agents such as polyamide resins, maleic anhydride, phthalic anhydride, hexahydrophthalic anhydride, and pyromellitic anhydride. The proportion of the curing agent is usually 0.1% by mass or more and 10% by mass or less, and preferably 0.5% by mass or more and 5% by mass or less, relative to the thermosetting resin (C).
[0034] Examples of the curing accelerator include tertiary amines such as benzyldimethylamine, imidazole, organic acid metal salts, Lewis acids, amine complex salts, etc. The ratio of the curing accelerator to the thermosetting resin (C) is usually 0.01% by mass or more and 10% by mass or less, and preferably 0.1% by mass or more and 5% by mass or less.
[0035] Solvent The conductive paste (X) contains a solvent (D), which allows the viscosity of the conductive paste (X) to be adjusted more appropriately, making it suitable for use in screen printing and the like.
[0036] Examples of the solvent (D) include polyhydric alcohols such as diols such as ethylene glycol, propylene glycol, and dipropylene glycol, and triols such as glycerin; sugar alcohols; lower alcohols such as ethanol, methanol, butanol, propanol, and isopropanol; 1-methyl-1-methoxybutanol; cellosolves such as ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), ethylene glycol mono-iso-propyl ether (iso-propyl cellosolve), ethylene glycol mono-n-butyl ether (n-butyl cellosolve), and ethylene glycol mono-t-butyl ether (t-butyl cellosolve); diethylene glycol monomethyl ether (methyl carbitol), diethylene glycol monoethyl ether (ethyl carbitol), diethylene glycol mono-n-propyl ether (n-propyl carbitol), diethylene glycol mono-iso-propyl ether (iso-propyl carbitol), ethylene glycol mono-n-butyl ether (n-butyl carbitol), diethylene glycol mono carbitols such as ethylene glycol mono-t-butyl ether (t-butyl carbitol); triglycols such as triethylene glycol monoethyl ether (ethyl triglycol); propylene glycol monoethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-t-butyl ether, propylene glycol mono-n-propyl ether, and propylene glycol mono-iso-propyl ether; dipropylene glycol monoethers such as dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, and dipropylene glycol mono-iso-propyl ether; glycol ethers such as tripropylene glycol monoethers such as tripropylene glycol monomethyl ether; glycol ether carboxylates such as cellosolve carboxylates such as ethylene glycol monomethyl ether acetate; and alkanolamines such as ethanolamine, diethanolamine, and triethanolamine.
[0037] The solvent (D) preferably contains one having an alcoholic hydroxyl group. In this case, the solvent (D) can dissolve the component (A) well, and as a result, the oxidation inhibition effect of the component (A) can be further improved. In addition, the solvent (D) having an alcoholic hydroxyl group exhibits reducing properties during heat curing, and therefore the oxidation inhibition effect of the component (A) can be further improved.
[0038] From the viewpoints of solubility of tannic acid, printability, and the like, the solvent (D) preferably contains at least one selected from the group consisting of lower alcohols and glycol ethers, and more preferably contains at least one selected from the group consisting of methanol, ethanol, and ethyl carbitol.
[0039] From the viewpoint of adjusting the viscosity of the conductive paste (X) more appropriately, the proportion of the solvent (D) is preferably 0.1% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 8% by mass or less, and even more preferably 3% by mass or more and 7% by mass or less, relative to the conductive paste (X).
[0040] [Boric acid] Boric acid includes not only orthoboric acid (H3BO3) but also metaboric acid, tetraboric acid, and the like, which are condensates of orthoboric acid. The conductive paste (X) preferably contains boric acid. This allows the conductive paste (X) to have a further low resistivity. In addition, when the thermosetting resin (C) has a hydroxyl group, the hydroxyl group and boric acid form a hydrogen bond, thereby allowing the conductive paste (X) to have a further low resistivity. In addition, boric acid also forms a hydrogen bond with the phenolic hydroxyl group of the component (A), and thus a network of the thermosetting resin (C)-boric acid-tannic acid is formed, allowing the conductive paste (X) to have a further good conductivity.
[0041] The proportion of boric acid is preferably from 1.0 mass% to 40 mass%, and more preferably from 2 mass% to 20 mass%, based on the total of component (A) and thermosetting resin (C) (including the curing agent and curing accelerator).
[0042] The proportion of boric acid is preferably 0.1% by mass or more and 4% by mass or less, and more preferably 0.2% by mass or more and 2% by mass or less, relative to the conductive paste (X).
[0043] [Other ingredients] The conductive paste (X) may contain other components such as rust inhibitors, antioxidants, adhesion promoters, dispersants, chelating agents, leveling agents, thixotropic agents, and defoamers, etc. The proportion of other components is, for example, 2 mass% or less with respect to the conductive paste (X).
[0044] (viscosity) The viscosity of the conductive paste (X) at 25°C is preferably 5.0 Pa·s or more and 200 Pa·s or less. In this case, the conductive paste (X) is easy to print, does not impair the workability of screen printing, and also facilitates the formation of wiring having a good pattern. The thixotropic ratio (Ti value) of the conductive paste (X) is preferably 1.0 or more and 3.0 or less. In this case, the conductive paste (X) does not impair the workability of screen printing, and also facilitates the formation of wiring having a good pattern. The thixotropic ratio is expressed as the ratio of the viscosity at 25°C and 0.5 rpm to the viscosity at 25°C and 5 rpm (thixotropic ratio=(viscosity at 25°C and 0.5 rpm) / (viscosity at 25°C and 5 rpm)).
[0045] <Conductive film> The conductive film of this embodiment includes a cured product of the conductive paste (X). Since the conductive film of this embodiment is formed from the conductive paste (X), it has excellent initial conductivity and can maintain excellent conductivity for a long period of time. In addition, when the conductive paste (X) contains boric acid and the tannic acid derivative has a urethane bond, the conductive film also has excellent bending resistance.
[0046] The conductive film of this embodiment is formed by applying the conductive film to a substrate such as a glass plate or a PET film by, for example, a screen printing method, and then heating and curing the conductive film. The heating temperature and heating time are appropriately selected depending on the type of thermosetting resin (C), etc., but the heating temperature is usually 100°C to 250°C, and preferably 130°C to 200°C. The heating time is usually 1 minute to 5 hours, and preferably 10 minutes to 1 hour. The shape of the conductive film is not particularly limited, and includes a planar line shape or band shape such as a circuit pattern, as well as a planar line shape such as a circle or a rectangle. The thickness of the conductive film is, for example, 1 μm to 1 mm, preferably 5 μm to 100 μm, and more preferably 10 μm to 50 μm. EXAMPLES
[0047] The present disclosure will now be described in detail with reference to examples.
[0048] <Synthesis of tannic acid derivatives> In a four-neck flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer, 100 g of tannic acid (manufactured by Fuji Chemical Industry Co., Ltd., product name: "Tannic Acid", the total number of hydroxyl groups in one molecule of tannic acid is 25) and 100 g of methyl ethyl ketone were added and mixed to dissolve. 82 g of ethyl acrylate isocyanate (manufactured by Showa Denko KK, product name "Kalends AOI") as an isocyanate compound was mixed into the resulting solution and reacted at 60°C for 5 hours. Methyl ethyl ketone was evaporated from the resulting solution and dried to obtain a tannic acid derivative (1).
[0049] Similarly, tannic acid derivative (2) was obtained by reacting with 141 g of an isocyanate compound, tannic acid derivative (3) was obtained by reacting with 24 g of an isocyanate compound, tannic acid derivative (4) was obtained by reacting with 160 g of an isocyanate compound, tannic acid derivative (5) was obtained by reacting with 65 g of butyl isocyanate as an isocyanate compound, and tannic acid derivative (6) was obtained by reacting with 36 g of a silane coupling agent (Toray Dow Co., Ltd., trade name "Xiameter OFS-6040 Silane", glycidoxypropyltrimethoxysilane). The weight average molecular weight of the obtained tannic acid derivative was measured by the GPC measurement method shown below.
[0050] (Measurement of weight average molecular weight) The weight average molecular weight was determined by GPC using standard polystyrene as the standard. The measurement conditions are as follows: - Equipment: Shimadzu Corporation, "Prominence LC-20AD" Columns: Showa Denko Co., Ltd., "GPC KF-801, GPC KF-803, GPC KF-805" (total of 3) Guard column: Showa Denko Co., Ltd., "GPC-KF-G 4A" Sample concentration: Tannic acid or a tannic acid derivative was diluted with tetrahydrofuran to a concentration of 0.5% by mass. Mobile phase solvent: Tetrahydrofuran ·Flow rate: 1.0mL / min Column temperature: 40℃
[0051] Table 1 below shows the weight average molecular weights of the synthesized tannic acid derivatives and tannic acid, as well as the substitution rates of hydrogen atoms of phenolic hydroxyl groups in the tannic acid derivatives.
[0052] [Table 1]
[0053] <Preparation of conductive paste> Example 1 0.40 g of tannic acid derivative (1), 4.6 g of epoxy resin (EPICLON EXA4816, manufactured by DIC Corporation), 0.02 g of hardening accelerator (Curesol 2PHZ-PW, manufactured by Shikoku Kasei Corporation), and 0.5 g of boric acid were mixed and dissolved in 3.0 g of ethyl carbitol solvent. 48.0 g of copper particles (manufactured by Fukuda Metal Foil and Powder Co., Ltd., product name "Cu-HWF-4") were mixed with the obtained resin solution and mixed with a hybrid mixer, and then kneaded with a roll mill to obtain conductive paste 1 (DP-1).
[0054] Example 2 A conductive paste 2 (DP-2) was obtained in the same manner as in Example 1, except that boric acid was not added.
[0055] Example 3 A conductive paste 3 (DP-3) was obtained in the same manner as in Example 1, except that tannic acid was used instead of the tannic acid derivative (1).
[0056] Example 4 A conductive paste 4 (DP-4) was obtained in the same manner as in Example 1, except that the tannic acid derivative (6) was used.
[0057] Example 5 Conductive paste 5 (DP-5) was obtained in the same manner as in Example 2, except that a resol-type phenolic resin (manufactured by Meiwa Kasei Co., Ltd., product name: "MWF-2620", solid content 70 mass%) was used as the thermosetting resin instead of the epoxy resin and curing accelerator.
[0058] Example 6 A conductive paste 6 (DP-6) was obtained in the same manner as in Example 1, except that the tannic acid derivative (2) was used.
[0059] Example 7 Conductive paste 7 (DP-7) was obtained in the same manner as in Example 1, except that the solvent was changed to ethyl carbitol acetate.
[0060] Example 8 A conductive paste 8 (DP-8) was obtained in the same manner as in Example 1, except that the tannic acid derivative (3) was used.
[0061] Example 9 A conductive paste 9 (DP-9) was obtained in the same manner as in Example 1, except that the tannic acid derivative (4) was used.
[0062] Example 10 A conductive paste 10 (DP-10) was obtained in the same manner as in Example 1, except that the tannic acid derivative (5) was used.
[0063] Comparative Example 1 Conductive paste 11 (DP-11) was obtained in the same manner as in Example 1, except that tannic acid and tannic acid derivatives were not added.
[0064] [Evaluation of conductive paste] (Viscosity, Ti value measurement) The viscosity (5 rpm and 0.5 rpm) at 25° C. of each of the conductive pastes obtained in Examples 1 to 9 and Comparative Example 1 was measured using a cone-plate viscometer (manufactured by Toki Sangyo Co., Ltd.) In addition, the Ti value (=viscosity at 0.5 rpm / viscosity at 5 rpm) was calculated from these measured values.
[0065] (Evaluation of copper powder dispersibility) In order to evaluate the dispersibility of the copper powder in the obtained conductive paste, a grind gauge (manufactured by Taiyu Kizai Co., Ltd., "GM-7470", 0 to 25 μm) was used to check the coarse particles with reference to JIS K5600-2-5 (degree of dispersion).
[0066] Based on the results of confirming the coarse particles, the dispersibility of the copper powder was evaluated according to the following criteria. A: The grind gauge result was 7.5 μm or less. B: The grind gauge result was 10.0 μm. C: The grind gauge judgment result was 12.5 μm or more.
[0067] Table 2 below shows the measured values of paste viscosity (Pa·s) (5 rpm, 0.5 rpm), Ti value, and the evaluation results of copper powder dispersibility.
[0068] [Table 2]
[0069] <Conductive film formation> The obtained conductive pastes 1 to 11 (DP-1 to DP-11) were each applied to a PET film by screen printing in the form of a strip-like wiring having a width of 1 mm, a length of 50 mm and a thickness of 20 μm, and then cured by heating at 150° C. for 30 minutes to obtain substrates 1 to 11 with conductive films 1 to 11 (DM-1 to 11).
[0070] [Evaluation of conductive films] (Measurement of the resistance value of a conductive film) The resistance values (Ω) of the obtained conductive films 1 to 11 (DM-1 to DM-11) were measured using a four-point probe resistance measuring meter (manufactured by HIOKI CORPORATION, RESISTANCE METER RM3544-01).
[0071] (Durability test) A durability test was carried out under a high temperature and high humidity environment for the substrates with conductive films 1 to 11. That is, the substrates with conductive films 1 to 11 (DM-1 to DM-11) were held in a high temperature and high humidity chamber at 85°C and 85% RH for 100 hours, and then the resistance values of the conductive films 1 to 11 (DM-1 to DM-11) were measured and the specific resistance values after the durability test were calculated.
[0072] (Bending resistance evaluation) The obtained conductive films 1 to 11 (DM-1 to DM-11) were wrapped around a 2 mmΦ iron core using a bending tester, bent, and then the resistivity was measured after unfolding. The bending resistance was evaluated according to the following criteria. S: The increase in resistivity before and after bending is 20% or less. A: The increase in resistivity before and after bending is more than 20% and 40% or less. B: The increase in resistivity before and after bending is more than 40% and 100% or less. C: The increase in resistivity before and after bending is more than 100%.
[0073] Table 3 below shows the resistance value (Ω) of the conductive film, the thickness of the conductive film (μm), the resistivity (volume resistivity) (μΩ·cm) calculated from the resistance value and thickness, the resistivity after the durability test (μΩ·cm), the rate of change after the durability test (= (resistivity after durability test / resistivity before durability test-1) × 100(%)), and the evaluation results of bending resistance.
[0074] [Table 3]
[0075] As can be seen from the results of Tables 2 and 3, the conductive pastes of the Examples have excellent initial conductivity and can maintain excellent conductivity for a long period of time. In particular, the conductive pastes of Examples 1 to 5 have excellent copper powder dispersibility, and Examples 1, 3, 4, and 5 have low resistivity of about 100 μΩ·cm and can provide excellent conductive films. Furthermore, Examples 1, 2, 4, 5, 6, 7, 8, and 10, which use tannic acid derivatives with a substitution rate of 10 to 65%, can provide conductive films with excellent durability. The conductive paste of Comparative Example 1 has poor copper powder dispersibility, and the conductive film has a high resistivity from the beginning, which is thought to be due to oxidation during the conductive paste preparation process, and the resistivity also increases in the moisture resistance test.
[0076] Furthermore, as can be seen from the results in Table 3, the conductive films of Examples 1, 6, 7, 9 and 10 formed from the conductive paste in which a tannic acid derivative having a urethane bond was combined with boric acid had good bending resistance.
[0077] The conductive paste of Example 9, which uses a tannic acid derivative with a hydrogen atom substitution rate of the phenolic hydroxyl group exceeding a certain value, shows an increase in the initial resistivity, a decrease in the dispersibility of the copper powder, and a high rate of increase in the resistivity value after the durability test, which suggests that the effect of the tannic acid derivative is reduced.The conductive paste of Example 7 does not use a solvent having a hydroxyl group, which suggests that the rust prevention effect of the tannic acid derivative during paste preparation is reduced.
[0078] (summary) As is apparent from the above, the conductive paste of the first aspect of the present disclosure contains at least one of tannic acid and a tannic acid derivative (A), copper powder (B), a thermosetting resin (C), and a solvent (D).
[0079] According to the first aspect, the conductive paste has excellent initial conductivity and can maintain this excellent conductivity for a long period of time.
[0080] The conductive paste of the second embodiment is the conductive paste of the first embodiment, wherein the component (A) contains a tannic acid derivative, and the tannic acid derivative is a tannic acid in which hydrogen atoms in some of the phenolic hydroxyl groups of tannic acid are replaced with substituents, and the replacement rate is 10% or more and 65% or less.
[0081] According to the second aspect, the effect of suppressing oxidation of the conductive paste over time can be further enhanced, and in particular, in a moist heat resistance test, the increase in resistivity can be further suppressed, and moist heat resistance can be more effectively improved.
[0082] The conductive paste of the third embodiment is the conductive paste of the first embodiment, in which the component (A) contains a tannic acid derivative, and the tannic acid derivative forms a urethane bond by reacting some or all of the phenolic hydroxyl groups of the tannic acid with a compound having an isocyanate group.
[0083] According to the third aspect, the effect of inhibiting oxidation over time becomes greater, and in particular, in a moist heat resistance test, the increase in resistivity can be further inhibited. Furthermore, by introducing a urethane bond into the tannic acid derivative, the flexibility of the conductive film formed from the conductive paste becomes higher, and therefore application to flexible substrates such as film substrates is expected.
[0084] The conductive paste of the fourth aspect is in any one of the first to third aspects, further containing boric acid.
[0085] According to the fourth aspect, the conductive paste can have a further reduced resistivity. When the thermosetting resin (C) has a hydroxyl group, the hydroxyl group and boric acid form hydrogen bonds to further reduce the resistivity. In addition, boric acid also forms hydrogen bonds with the phenolic hydroxyl group of the component (A), so that a network of the thermosetting resin (C)-boric acid-tannic acid is formed, thereby achieving even better conductivity.
[0086] The conductive paste of a fifth aspect is any one of the first to fourth aspects, wherein the solvent (D) has an alcoholic hydroxyl group.
[0087] According to the fifth aspect, the solvent (D) can dissolve the component (A) well, so that the oxidation suppression effect of the component (A) can be further improved. In addition, the solvent (D) having an alcoholic hydroxyl group exhibits reducing properties during heat curing, so that the oxidation suppression effect of the component (A) can be further improved.
[0088] The conductive paste of a sixth aspect is any one of the first to fifth aspects, wherein the thermosetting resin (C) has a phenolic hydroxyl group.
[0089] According to the sixth aspect, it is possible to increase the cure shrinkage due to thermal curing of the thermosetting resin (C), and as a result, it is possible to further improve the conductivity of the conductive paste.
[0090] The conductive film of the seventh aspect includes a cured product of the conductive paste of any one of the first to sixth aspects.
[0091] According to the seventh aspect, the conductive film has excellent initial conductivity and can maintain the excellent conductivity for a long period of time. [Industrial Applicability]
[0092] According to the conductive paste of the present disclosure, it is possible to form a conductive film by thermal curing, which has excellent initial conductivity, excellent moisture resistance, and is capable of maintaining this excellent conductivity for a long period of time, without the need for special equipment that requires inert gas or the like.
Claims
1. A composition comprising a tannic acid derivative (A), copper powder (B), a thermosetting resin (C), and a solvent (D), The conductive paste is characterized in that the tannic acid derivative (A) is a tannic acid in which some of the hydrogen atoms in the phenolic hydroxyl groups are substituted with substituents, and the substitution rate is 10% or more and 65% or less.
2. A composition comprising a tannic acid derivative (A), copper powder (B), a thermosetting resin (C), and a solvent (D), The conductive paste is one in which the tannic acid derivative (A) is obtained by reacting a part or all of the phenolic hydroxyl groups of tannic acid with a compound having an isocyanate group to form a urethane bond.
3. A conductive paste as described in claim 1 or 2, further containing boric acid.
4. A conductive paste described in any one of claims 1 to 3, wherein the solvent (D) has an alcoholic hydroxyl group.
5. A conductive paste described in any one of claims 1 to 4, wherein the thermosetting resin (C) has a phenolic hydroxyl group.
6. A conductive film comprising a hardened conductive paste described in any one of claims 1 to 5.
Citation Information
Patent Citations
Manufacture of conductive copper paste and conductive copper paste manufactured thereby
JP1993135619A
Fiber-like conductive substance and conductive resin composition containing it
JP1994215631A
Manufacture of electronic part and conductive paste used therefor
JP1998074661A
Conductive copper paste
JP2008130301A
Conductive ink composition and manufacturing method thereof
JP2008531810A