Modified polyglycolic acid and its manufacturing method and manufacturing device

By bonding vanadium to glycolic acid oligomers using microwaves, modified polyglycolic acid is produced, addressing the lack of industrial applications for polyglycolic acid and enabling stable secondary batteries with high energy storage capacity.

JP7565570B2Active Publication Date: 2024-10-11JAST LAB CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020071637
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-13
Publication Date
2024-10-11
Estimated Expiration
2040-02-12

AI Technical Summary

Technical Problem

Existing technologies do not utilize polyglycolic acid as an active material for secondary batteries, lacking consideration for its potential as an industrial material with electrical characteristics.

Method used

A method involving the addition of vanadium compounds to glycolic acid oligomers and irradiation with microwaves to bond vanadium, producing modified polyglycolic acid with specific valence states, suitable for use as both positive and negative electrode active materials in secondary batteries.

Benefits of technology

The modified polyglycolic acid exhibits excellent electrical characteristics, enabling the production of stable secondary batteries with high energy storage capacity and durability, eliminating the need for separate active materials and electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565570000008
    Figure 0007565570000008
  • Figure 0007565570000009
    Figure 0007565570000009
  • Figure 0007565570000010
    Figure 0007565570000010
Patent Text Reader

Abstract

To provide a method for producing a material to be an active material for a secondary battery, based on polyglycolic acid, and a device for producing the same.SOLUTION: A method for producing a modified polyglycolic acid includes adding a vanadium compound to a glycolic acid oligomer and irradiating them with a microwave, to bind vanadium to the glycolic acid oligomer. The glycolic acid oligomer has a molecular weight of 5,000 or more and 10,000 or less, preferably 6,000 or more and 8,000 or less. An amount of addition of the vanadium compound is 1 wt.% or more and 10 wt.% or less, preferably 4 wt.% or more and 6 wt.% or less. The vanadium compound is amine vanadate obtained by electrolyzing an aqueous solution of ammonium vanadate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a modified polyglycolic acid and a method and apparatus for producing the same. [Background technology]

[0002] Polyglycolic acid (PGA) is an environmentally friendly, biodegradable plastic made from glycolic acid. Due to its excellent biocompatibility, it is used in surgical sutures and medical materials, but is rarely used as an industrial material.

[0003] For example, Patent Document 1 discloses a technique for using polyglycolic acid as a surgical fiber, and Patent Document 2 discloses a technique for using polyglycolic acid to produce a composite molded product by reducing the melt viscosity of the polyglycolic acid. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-516100 A [Patent Document 2] JP 2010-215782 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, even in the technique described in the above document, no consideration is given at all to producing a material that can serve as an active material for a secondary battery based on polyglycolic acid.

[0006] An object of the present invention is to provide a technique for solving the above-mentioned problems. [Means for solving the problem]

[0007] In order to achieve the above object, the method for producing a modified polyglycolic acid according to the present invention comprises the steps of: A vanadium compound was added to glycolic acid oligomer and irradiated with microwaves. A method for producing modified polyglycolic acid by bonding vanadium to glycolic acid oligomer. Yes So, The vanadium compound is an amine vanadate.

[0008] In order to achieve the above object, the apparatus for producing modified polyglycolic acid according to the present invention comprises: A modified polyglycolic acid production apparatus for producing modified polyglycolic acid by the modified polyglycolic acid production method, a pressure vessel into which glycolic acid is introduced as a raw material and from which the produced modified polyglycolic acid is taken out; A stirring device for stirring the contents of the pressure-resistant vessel; A pressure reducing device for creating a negative pressure inside the pressure vessel; A microwave irradiation device that irradiates microwaves to the contents; A temperature control device for controlling the temperature of the contents; A control device that controls the temperature of the content, the pressure in the pressure-resistant vessel, and the stirring rotation speed of the stirring device; an exhaust condenser that generates condensed water by heat exchange with exhaust gas from the pressure-resistant vessel in response to intake by the pressure reducing device; A condensed water storage device that separates and stores the condensed water; Equipped with The pressure vessel comprises: a raw material inlet for introducing the glycolic acid; Catalysts used in the production of glycolic acid oligomers Stannous octoate and vanadium compounds as additives used in the production of modified polyglycolic acid. amine vanadate a catalyst and additive inlet into which the catalyst and additive are introduced; an outlet through which the modified polyglycolic acid is taken out; a nitrogen gas aeration port through which nitrogen gas is introduced to prevent contamination inside the pressure vessel; an internal viewing window for monitoring the condition of the contents of the pressure vessel; An internal light for illuminating the inside of the pressure vessel; having Effect of the Invention

[0010] According to the present invention, it is possible to provide a material based on polyglycolic acid that can serve as an active material for secondary batteries. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a diagram showing an outline of a production procedure for a modified polyglycolic acid according to a first embodiment. [Diagram 2] FIG. 1 is a diagram showing an outline of a procedure for producing glycolic acid according to a first embodiment. [Diagram 3] FIG. 1 is a diagram showing an outline of a manufacturing procedure for amine vanadate according to a first embodiment. [Figure 4] FIG. 13 is a diagram showing the configuration of a secondary battery using modified polyglycolic acid according to a second embodiment. [Diagram 5] FIG. 11 is a diagram showing an outline of a procedure for initializing a secondary battery according to a second embodiment. [Figure 6] FIG. 11 is a diagram showing an outline of a charging and discharging procedure for a secondary battery according to a second embodiment. [Figure 7] FIG. 1 is a diagram showing the configuration of a production apparatus for modified polyglycolic acid according to a first embodiment. [Figure 8A] 1 is a flow chart showing the steps of producing a modified polyglycolic acid according to a first embodiment. [Figure 8B] 1 shows a graph of current-potential characteristics, which are test results of the oxidation number of vanadium in the modified polyglycolic acid produced in the first embodiment. [Figure 9] FIG. 1 is a diagram showing a procedure for producing a glycolic acid oligomer according to a first embodiment. [Figure 10A] FIG. 1 is a diagram showing a configuration of an apparatus for producing amine vanadate according to a first embodiment. [Figure 10B] 1 is a flowchart showing a process for producing amine vanadate according to a first embodiment. [Figure 11A]10 is a flowchart showing a process for producing a secondary battery using modified polyglycolic acid according to a second embodiment. [Figure 11B] 10 is a flowchart showing an initial charging process of a secondary battery using modified polyglycolic acid according to a second embodiment. [Figure 11C] FIG. 13 is a diagram illustrating a prototype secondary battery using modified polyglycolic acid according to a second embodiment and its test state. [Figure 12] FIG. 11 is a diagram showing initial charging characteristics during initialization of a secondary battery according to a second embodiment. [Figure 13] FIG. 11 is a diagram showing the discharge characteristics during discharging of the secondary battery according to the second embodiment. [Figure 14] FIG. 13 is a diagram showing another example using modified polyglycolic acid. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. However, the components described in the following embodiment are merely examples, and are not intended to limit the technical scope of the present invention.

[0013] [First embodiment] First, as the first embodiment, modified polyglycolic acid will be described. Note that "modified polyglycolic acid" is polyglycolic acid produced from glycolic acid as a source, which is further subjected to chemical treatment. In other words, it can be positioned as a vanadium-polyglycolic acid complex having a structure in which vanadium is bonded to polyglycolic acid bonded to a polyglycolic acid base in which multiple glycolic acids are bonded.

[0014] The present inventors have been conducting research into ways to add durability and functionality to polyglycolic acid as an industrial material while retaining its biodegradability. In the course of this research, they developed a method for obtaining modified polyglycolic acid with excellent electrical characteristics, which led to the present invention. The present invention relates to a method and device for producing modified polyglycolic acid in which vanadium element is incorporated into the polyglycolic acid molecule and oxidized and reduced by an external electric field, and provides electronic materials and battery materials with unprecedented properties.

[0015] <Structure of modified polyglycolic acid> The modified polyglycolic acid according to the present embodiment contains the same amount of modified polyglycolic acid having a structure in which vanadium having a valence of 4 is bonded to polyglycolic acid, and modified polyglycolic acid having a structure in which vanadium having a valence of 3 is bonded to polyglycolic acid. The structure is shown in the following chemical formula (1). In addition, in the chemical formula (1), the modified polyglycolic acid having a structure in which vanadium having a valence of 4 is bonded is also referred to as chemical formula (8) in [Chemical formula 8], and the modified polyglycolic acid having a structure in which vanadium having a valence of 3 is bonded is also referred to as chemical formula (9) in [Chemical formula 9].

[0016] [ka] In this way, when the modified polyglycolic acid according to the present embodiment is used as an active material for a secondary battery, for example, a material containing a substance that becomes an active material for both a positive electrode and a negative electrode is produced without separately producing the active material for both electrodes. By electrically initializing this production material, it can be used as an electronic material having various characteristics, including a secondary battery. In addition, the suitable molecular weight range of the modified polyglycolic acid of the chemical formula (1) when used in a secondary battery is about 5,000 to 7,000 in number average molecular weight. This is because the modified polyglycolic acid needs to be a relatively low molecular weight in which hydrogen atoms that serve as carriers can move.

[0017] <Outline of the manufacturing method of modified polyglycolic acid> 1 is a diagram showing an outline of a method for producing a modified polyglycolic acid according to the present embodiment. Note that the term "glycolic acid oligomer" refers to a relatively low molecular weight polyglycolic acid having a molecular weight of 5,000 or more and 10,000 or less.

[0018] The present inventors have found that polyglycolic acid with a large molecular weight is not necessary to produce modified polyglycolic acid, and that polyglycolic acid with a relatively small molecular weight (so-called glycolic acid oligomer) tends to be easier to produce. As a result, the inventors have established the technology of the present embodiment for producing modified polyglycolic acid in a complete process from acetic acid, which is the first raw material.

[0019] Step S101: Glycolic acid 101, which is the raw material, is heated and dehydrated in a polymerization vessel to perform controlled dehydration polycondensation to obtain glycolic acid oligomer 102. The molecular weight of glycolic acid oligomer 102 is desirably 5,000 or more and 10,000 or less, preferably 6,000 or more and 8,000 or less. This process is shown in the following chemical formula (2).

[0020] [ka] The reason why the glycolic acid oligomer 102 is used as an intermediate material is to facilitate binding of vanadium to polyglycolic acid, as described below.

[0021] The glycolic acid oligomer 102 (S101) is produced by the following process. Glycolic acid is heated to about 175°C to 185°C under normal pressure, and the water generated is distilled off. After that, the pressure is reduced and the temperature is kept for a certain time to obtain a glycolic acid oligomer (low molecular weight PGA), but this takes a long time and the molecular weight (degree of polymerization) is not constant and varies. Therefore, in this embodiment, concentrated glycolic acid containing a part of glycolide is first produced. Then, instead of purifying it and using it, it is subjected to dehydration condensation polymerization as it is (still containing glycolide), thereby shortening the production time and producing a glycolic acid oligomer whose molecular weight (degree of polymerization) is within a certain range as much as possible. If only purified glycolide is used for ring-opening polymerization, it will become a high molecular weight polyglycolic acid (molecular weight>10,000 or 20,000), which is disadvantageous for producing the modified polyglycolic acid of this embodiment.

[0022] Step S103: An additive containing a transition metal is added to the obtained glycolic acid oligomer 102. As the additive containing a transition metal, amine vanadate (NH2VO2) is used.

[0023] Step S105: The glycolic acid oligomer 102 to which an additive containing a transition metal (1 wt% to 10 wt%, preferably 4 wt% to 6 wt% of amine vanadate, which is a vanadium compound) has been added is irradiated with microwaves to bond vanadium (i.e., substitute oxygen for the double bond of vanadium), thereby producing a modified polyglycolic acid 103. This process is shown in the following chemical formula (3).

[0024] [ka] The resulting modified polyglycolic acid 103 contains tetravalent vanadium (V +IV )-bonded modified polyglycolic acid 131 and trivalent vanadium (V +III ) and modified polyglycolic acid 132 bound to it in approximately the same amount.

[0025] 1 shows the steps for producing glycolic acid oligomer 102, the modified polyglycolic acid 103 of this embodiment can be produced by any method as long as glycolic acid oligomer 102 having the above molecular weight is provided as a raw material. In other words, the method for producing glycolic acid oligomer 102 is not limited.

[0026] Thus, in the production of modified polyglycolic acid 103, tetravalent vanadium (V +IV )-bonded modified polyglycolic acid 131 and trivalent vanadium (V +III The modified polyglycolic acid 132 having the carboxyl group 132 bonded thereto can be produced simultaneously without being produced separately.

[0027] <Outline of the manufacturing method of glycolic acid> FIG. 2 is a diagram showing an outline of a method for producing glycolic acid, which is a source of modified polyglycolic acid, in the first embodiment.

[0028] Step S201: Hypochlorous acid is aerated into acetic anhydride to produce chloroacetic acid and water. The produced water is discharged by reduced pressure distillation. This reaction is shown in the following chemical formula (4).

[0029] [ka] Step S203: Sodium hydroxide is added to chloroacetic acid to produce glycolic acid and table salt. The produced table salt is removed using an electrodialysis device. Furthermore, the produced glycolic acid is treated with an ion exchange resin to adsorb and remove residual table salt. This glycolic acid can be used to produce glycolic acid oligomers. This reaction is shown in the following chemical formula (5).

[0030] [ka] In addition, by performing membraneless electrolysis on the salt produced in step S203, hypochlorous acid to be aerated in step S201 is produced at the positive electrode, and sodium hydroxide to be added in step S203 is produced at the negative electrode, so the materials used are recycled. This process is shown in the following chemical formula (6).

[0031] [ka] The method for producing glycolic acid is not limited to the method shown in FIG. 2, and other methods may be used.

[0032] <Outline of the manufacturing method of amine vanadate> 3 is a diagram showing an outline of a method for producing amine vanadate used as an additive in the vanadium bonding step (i.e., the step of replacing the double bond of vanadium with oxygen) in producing a modified polyglycolic acid from a glycolic acid oligomer in the first embodiment. The reaction for producing amine vanadate from an aqueous solution of ammonium vanadate is shown in the following chemical formula (7).

[0033] [ka]

[0034] Amine vanadate (NH2VO2) is produced by electrolyzing an ammonium vanadate (NH4VO3) solution without a diaphragm (formula 301 in FIG. 3). However, as shown in FIG. 3, if the electrolysis current becomes too large in the electrolysis without a diaphragm, vanadium nitrite (V(NO2)4) is produced (formula 302 in FIG. 3) or vanadium nitrate (V(NO3)2) is produced (formula 303 in FIG. 3), and therefore cannot be used as the additive of this embodiment. Therefore, it is necessary to control the electrolysis current so that amine vanadate is produced.

[0035] The inventors conducted experiments by changing various electrolysis currents and found that the electrolysis current is preferably 3 to 5 times the limiting current of the membrane-less electrolysis device, and that if it is more than this, vanadium nitrite or vanadium nitrate is produced instead of amine vanadate. For example, when the limiting current of the membrane-less electrolysis device is 5 mA / cm 2 In the case of , the electrolysis current is 20mA / cm 2 is desirable, and the electrolysis current is 30mA / cm 2 Above this value, vanadium amine could not be produced sufficiently. Note that vanadium nitrite and vanadium nitrate produced in formulas 302 and 303 in Figure 3 are both nitric acid compounds and cannot be used as additives for producing modified polyglycolic acid from glycolic acid oligomer.

[0036] According to this embodiment, a material that serves as an active material for a secondary battery based on polyglycolic acid can be provided. Also, a manufacturing method for obtaining a modified polyglycolic acid that has durability and functionality as an industrial material and excellent electrical characteristics can be provided. That is, by using the manufacturing method for modified polyglycolic acid in which a transition metal element is incorporated into the molecule of polyglycolic acid and oxidized and reduced by an external electric field, electronic materials and battery materials with unprecedented properties can be provided. Furthermore, a manufacturing apparatus for manufacturing modified polyglycolic acid by the manufacturing method for modified polyglycolic acid of this embodiment is also provided.

[0037] [Second embodiment] Next, as the second embodiment, a secondary battery using the modified polyglycolic acid produced in the first embodiment will be described. The modified polyglycolic acid produced in the first embodiment contains the same amount of modified polyglycolic acid having a structure in which vanadium having a valence of 4 is bonded to polyglycolic acid, and modified polyglycolic acid having a structure in which vanadium having a valence of 3 is bonded to polyglycolic acid. Therefore, even if the produced modified polyglycolic acid is used as an active material, it will not function as a secondary battery as it is. That is, it is necessary to separate a positive electrode in which modified polyglycolic acid having a structure in which vanadium having a valence of 4 is bonded to polyglycolic acid serves as an active material from a negative electrode in which modified polyglycolic acid having a structure in which vanadium having a valence of 3 is bonded to polyglycolic acid serves as an active material. This process is hereinafter referred to as initialization.

[0038] Furthermore, by charging after initialization, the positive electrode active material, tetravalent (V +IV Modified polyglycolic acid with vanadium of 5 (V +V ) vanadium is bonded to the modified polyglycolic acid. +III The modified polyglycolic acid with 2-valent (V +II ) vanadium is bonded to the modified polyglycolic acid. After that, the positive electrode active material, pentavalent (V +V The modified polyglycolic acid with 4(V +IV On the other hand, the negative electrode active material, divalent (V +II Modified polyglycolic acid with vanadium of 3 (V +III The vanadium-containing polyglycolic acid is then converted back into a modified polyglycolic acid. After this, the battery is able to repeat this charge and discharge cycle stably.

[0039] <Construction of secondary battery using modified polyglycolic acid> Fig. 4 is a diagram showing the configuration of a secondary battery using modified polyglycolic acid according to this embodiment. In Fig. 4, the left diagram shows a secondary battery 401 when assembled (original type), the center diagram shows a secondary battery 402 after initializing charging, and the right diagram shows a secondary battery 403 during discharging.

[0040] Secondary battery 401 contains modified polyglycolic acid 103 as an active material, which contains equal amounts of modified polyglycolic acid having a structure in which vanadium having a valence of 4 is bonded to polyglycolic acid, and modified polyglycolic acid having a structure in which vanadium having a valence of 3 is bonded to polyglycolic acid. Modified polyglycolic acid 103 is applied to both positive electrode current collector 411 and negative electrode current collector 412, and they are pressed together with separator 413 sandwiched between them. It should be noted that the battery can be used as a secondary battery without separator 413.

[0041] In this embodiment, the material of the positive electrode current collector 411 is preferably copper or carbon, and the material of the negative electrode current collector 412 is preferably aluminum or zinc, but is not limited thereto as long as it is a conductive material. The positive and negative electrodes may be made of the same conductive material. Cellulose acetate is used as the separator 413. Preferably, it has an acetylation ratio between cellulose diacetate and cellulose triacetate. However, the separator 413 is not limited to cellulose acetate, and may be any material that can prevent compatibility between the positive electrode active material and the negative electrode active material and has many molecular meshes.

[0042] The secondary battery 402 is in a state after initialization charging, with the positive electrode collector 411 side being modified polyglycolic acid 421 bonded with pentavalent vanadium, and the negative electrode collector 412 side being modified polyglycolic acid 422 bonded with divalent vanadium.

[0043] The secondary battery 403 is in a discharging state, with the positive electrode current collector 411 side being modified polyglycolic acid 431 with tetravalent vanadium bonded thereto, and the negative electrode current collector 412 side being modified polyglycolic acid 432 with trivalent vanadium bonded thereto.

[0044] After this, charging and discharging are repeated between the charged state of secondary battery 402 and the discharged state of secondary battery 403.

[0045] (Overview of the initialization procedure) Fig. 5 is a diagram showing an outline of the initialization procedure of the secondary battery according to the second embodiment. Note that Fig. 5 shows the change in one molecule of the modified polyglycolic acid, but in the secondary battery, this process is carried out on the entire molecule.

[0046] The modified polyglycolic acid 103, which contains approximately equal amounts of modified polyglycolic acid 131 bonded with tetravalent vanadium and modified polyglycolic acid 132 bonded with trivalent vanadium, is initialized by applying a DC power supply of, for example, 2 V between both electrodes. In the modified polyglycolic acid 103 of the positive electrode, the trivalent modified polyglycolic acid 132 is converted to the tetravalent modified polyglycolic acid 131, and after the initialization is completed, most of the modified polyglycolic acid 501 of the positive electrode becomes the tetravalent modified polyglycolic acid 131. On the other hand, in the modified polyglycolic acid 103 of the negative electrode, the tetravalent modified polyglycolic acid 131 is converted to the trivalent modified polyglycolic acid 132, and after the initialization is completed, most of the modified polyglycolic acid 501 of the negative electrode becomes the trivalent modified polyglycolic acid 132.

[0047] In this way, the positive and negative electrodes of the secondary battery, which were not electrically determined at the time of manufacture, are electrically determined. This state is the same as the state of the denatured polyglycolic acid of the positive and negative electrodes that have been discharged. However, in the embodiment, the initialization is performed as a series of initial charges, so that the charging state of FIG. 6 is transitioned through these states.

[0048] (Overview of charging and discharging procedures) Fig. 6 is a diagram showing an outline of the charge / discharge procedure of the secondary battery according to the second embodiment. Note that Fig. 5 shows the change in one molecule of the modified polyglycolic acid, but in the secondary battery, this process is carried out on the entire molecule.

[0049] The modified polyglycolic acid 421 of the charged positive electrode and the modified polyglycolic acid 422 of the charged negative electrode are structural formulas of modified polyglycolic acid when they reach a charged state during initial charging through the changes shown in Fig. 5. That is, the modified polyglycolic acid 421 of the positive electrode is a modified polyglycolic acid bonded with pentavalent vanadium, and the modified polyglycolic acid 422 of the negative electrode is a modified polyglycolic acid bonded with divalent vanadium.

[0050] On the other hand, the structural formulas of the denatured polyglycolic acid 431 of the discharged positive electrode and the denatured polyglycolic acid 432 of the discharged negative electrode correspond to the initialized state in Fig. 5. That is, the denatured polyglycolic acid 431 of the positive electrode is a denatured polyglycolic acid bonded with tetravalent vanadium, and the denatured polyglycolic acid 432 of the negative electrode is a denatured polyglycolic acid bonded with trivalent vanadium.

[0051] As shown in FIG. 6, such a change in the valence of vanadium is realized by hydrogen atoms bonded to vanadium acting as carriers and hopping to vanadium in the nearby modified polyglycolic acid at the counter electrode. The structure of the modified polyglycolic acid of this embodiment is such that vanadium can easily capture and release hydrogen atoms. As described above, since this is hydrogen atom hopping, the amount of current is small, but since the modified polyglycolic acid contains vanadium corresponding to the polymerization number (10 moles or more / 1 liter), it is possible to store a large amount of electricity. Furthermore, since vanadium is double-bonded to carbon, there is no change in the basic skeleton, and it is stable as an active material.

[0052] In addition, the carrier of the secondary battery is hydrogen atoms or hydrogen ions, and it was found that the distance between the positive and negative electrodes must be such that hydrogen molecules can move with charging and discharging. It was also found that the molecular weight of the modified polyglycolic acid must be low enough that hydrogen atoms can move. According to experiments, it was found that the distance between the electrodes is preferably 30 to 10 μm, and that the molecular weight of the modified polyglycolic acid is 5,000 to 10,000 to function well.

[0053] According to this embodiment, a secondary battery that can be used semi-permanently and can be easily carried can be provided. In other words, since no electrolyte is used, tanks for storing active materials and electrolytes, and pumps for circulating them are not required. In addition, even if the battery is small, it is possible to store a large amount of electricity because the modified polyglycolic acid contains vanadium corresponding to the polymerization number. Furthermore, since vanadium is double-bonded to carbon, there is no change in the basic structure, and the battery is stable as an active material.

[0054] Although the present invention has been described above with reference to the embodiments, the present invention is not limited to the above embodiments. Various modifications that can be understood by those skilled in the art can be made to the configuration and details of the present invention within the technical scope of the present invention. Furthermore, any combination of separate features included in each embodiment is also included in the technical scope of the present invention. EXAMPLES

[0055] [First Example] As a first example, an example of production of a modified polyglycolic acid according to an embodiment will be described.

[0056] <Production equipment for modified polyglycolic acid> FIG. 7 is a diagram showing the configuration of a production apparatus 700 for modified polyglycolic acid according to this embodiment.

[0057] The production apparatus 700 for modified polyglycolic acid includes a pressure-resistant vessel consisting of a reaction vessel 701 and a lid 702, an agitator 704, a pressure reducing device (vacuum pump) 713, and a microwave irradiator (microwave generator) 705. The production apparatus 700 for modified polyglycolic acid further includes a temperature adjusting device (heat transfer oil supplying section) 714, a control device 720, an exhaust condenser (heat exchanger) 707, and a condensed water storage device 708.

[0058] Glycolic acid is put into the pressure vessel as a raw material, and the modified polyglycolic acid produced is taken out. The agitator 704 agitates the contents of the pressure vessel. The pressure reducing device (vacuum pump) 713 creates a negative pressure inside the pressure vessel. The microwave irradiator (microwave generator) 705 irradiates the contents with microwaves. The waveguide from the microwave irradiator 705 is provided with a glass plate 706 that maintains the pressure inside the pressure vessel. The temperature regulator (heat medium oil supply unit) 714 adjusts the temperature of the contents by a medium heat heating method using the heat medium oil 703. The controller 720 monitors and controls the temperature of the contents, the pressure inside the pressure vessel, and controls the agitation rotation speed by the agitator 704. The exhaust condenser (heat exchanger) 707 exchanges heat with the exhaust from the pressure vessel following the intake by the pressure reducing device 713 to produce condensed water. The condensed water storage device 708 separates and stores the condensed water, and discharges it to the outside.

[0059] The pressure vessel has a raw material inlet 710 into which glycolic acid (GA) is introduced, and a catalyst and additive inlet 712 into which a catalyst used in the production of glycolic acid oligomers and a vanadium compound are introduced as additives used in the production of modified polyglycolic acid. The pressure vessel further has an outlet 711 from which modified polyglycolic acid (GPA) is taken out, and a nitrogen gas aeration port 709 into which nitrogen gas is introduced to prevent contamination inside the pressure vessel. The pressure vessel also has an internal viewing window for monitoring the state of the contents of the pressure vessel, not shown, and an internal light for illuminating the inside of the pressure vessel.

[0060] The control device 720 has a content temperature control unit 721 that monitors the temperature of the contents and controls the contents to an appropriate temperature corresponding to the manufacturing process by adjusting the heat transfer oil 703 by the heat transfer oil supply unit 714. The control device 720 also has an in-vessel pressure control unit 722 that monitors the pressure inside the pressure-resistant container and controls the pressure inside the pressure-resistant container by the pressure reducing device 713. The control device 720 also has a content agitation control unit 723 that appropriately agitates the contents by the agitation device 704 in accordance with the manufacturing process. The control device 720 also has a processing time control unit 724 that controls each processing time in accordance with the manufacturing process of the modified polyglycolic acid. Although four control units 721 to 724 are illustrated in FIG. 7, other control units may be added. Meanwhile, any of the control units 721 to 724 of the control device 720 may be manually operated by an operator. The control device 720 may further display a state or input an operation by an external computer 730. The control device 720 and the external computer 730 may be integrated.

[0061] (Production of Modified Polyglycolic Acid) Fig. 8A is a flow chart showing the steps of producing modified polyglycolic acid according to this embodiment using the above-mentioned modified polyglycolic acid production apparatus 700. Fig. 8A also shows a temperature profile 800 of the contents according to the steps of producing modified polyglycolic acid. The step numbers in the temperature profile 800 correspond to the step numbers in the flow chart.

[0062] Step S801 (Charging Glycolic Acid): Glycolic acid is charged from the raw material charging port 710 in the pressure-resistant vessel of the production apparatus 700 for modified polyglycolic acid.

[0063] Step S803 (heat dehydration): The raw glycolic acid that was added contains about 10% water (concentration is 90%), so it is dehydrated and concentrated in a reduced pressure environment. Nitrogen gas is passed through the pressure vessel, and the temperature is adjusted to 180°C for dehydration for 1 to 2 hours. The dehydration status is estimated from the amount of condensed water discharged from the heat exchanger.

[0064] Step S805 (cooling): The temperature of the contents is lowered to 60° C. If the catalyst is added at a high temperature, it will react rapidly and partial oxidation will proceed, which is undesirable.

[0065] Step S807 (Catalyst Addition): The catalyst is added. The catalyst used is a mixture of equal amounts of tin octoate and dodecyl alcohol (polymerization initiator). The amount added is preferably 0.2 wt% of the content. It is not preferable to add the entire amount of catalyst at once, so it is added little by little in several batches. After the entire amount has been added, the contents are stirred for 1 to 2 hours.

[0066] Step S809 (dehydration condensation polymerization): Set the temperature to 170°C, and once the contents have reached the set temperature, carry out polymerization for 6 to 8 hours. During this time, maintain the nitrogen flow rate at 10 liters per minute and the pressure inside the vessel at 0.1 Atm. The progress of polymerization is determined by measuring the number average molecular weight of the contents. When the number average molecular weight reaches between 5,000 and 10,000, polymerization is terminated. After that, it is advisable to set the temperature to 220°C and continue for 1 to 2 hours, allowing unreacted materials to evaporate and be removed from the system.

[0067] The above steps S803 to S809 correspond to step 101 (dehydration condensation polymerization) in Fig. 1. That is, in this example, the aim was to produce a glycolic acid oligomer having a uniform molecular weight in as short a time as possible.

[0068] Step S811 (cooling): The temperature of the contents is reduced to 90°C.

[0069] Step S813 (additive addition): Additive (amine vanadate: 1 to 10% of the content) is added from the catalyst and additives inlet 712. The additive is not added all at once, but is added little by little in several portions.

[0070] The above steps S811 and S813 correspond to step 103 (addition of amine vanadate) in FIG.

[0071] Step S815 (bonding of vanadium by microwaves): After the entire amount of additive (amine vanadate) has been added, the temperature of the contents is raised to 170°C, and the microwave irradiation device (microwave generator) 705 is operated. The irradiation time is 2 to 4 hours. The purpose of this bonding of vanadium by microwaves is to bond amine vanadate to a predetermined position (oxygen double bond) of the glycolic acid oligomer molecule. In other words, vanadium is replaced with oxygen of the double bond. This reaction can also be achieved by irradiation with radiation such as gamma rays, but this is not common, and it is difficult to achieve by any method other than bonding (i.e., replacement) by microwave irradiation. The microwave output is 0.1 to 1 kW per 10 kg of contents. The microwave is introduced into the container through a waveguide fitted with a glass plate 706 as shown in FIG. 7. The glass plate 706 is used to maintain the pressure inside the pressure-resistant container. Nitrogen gas is also passed through the waveguide to prevent the inside of the tube from becoming dirty.

[0072] Step S105 (termination operation, removal of modified PGA): Since the production of modified polyglycolic acid is completed, the temperature of the contents is lowered to 120° C. or less, and the contents are then removed from the removal port 711. Removing the contents at a high temperature is not preferable, as it may increase the risk of burns or cause the modified polyglycolic acid to oxidize.

[0073] The above-mentioned conditions such as temperature adjustment in the manufacturing process for manufacturing modified polyglycolic acid using glycolic acid as a raw material are only examples, and manufacturing is possible if the treatment is performed within the following range. For example, in the dehydration process, the mixture is heated to 105-110°C at atmospheric pressure to evaporate water. After that, the mixture is dehydrated for about 2 hours at 170-180°C in a reduced pressure environment (approximately 1 / 10 atmospheric pressure). If the temperature is too high, the contents will evaporate and the yield will decrease. If the temperature is below 160°C, the dehydration time will be longer. If the temperature is high when mixing the catalyst (vanadium vanadate), partial reaction will occur and undesirable results will occur, so the mixture is mixed at about 40-70°C. In the embodiment, the mixture is stirred at 60°C for about 2 hours. The temperature of the dehydration condensation polymerization is also determined by the degree of vacuum, but it is performed at 160-170°C to avoid unnecessary evaporation of the contents. The inside of the container is stirred for 15-20 hours while introducing nitrogen gas into the container in a reduced pressure environment of about 1 / 10 atmospheric pressure. Then, when the number average molecular weight of the contents reaches 3000 or more, the temperature of the contents is raised to 170-190°C, and at the same time the pressure inside the container is lowered to about 1 / 15 atmosphere. If the temperature is not raised here, it will not become a high molecular weight product and will remain in the oligomer form. To make a polymer product to be used as a biodegradable plastic (resin), the temperature is raised to around 200°C and polymerization continues, but if it is to be used as a battery material, it will not be polymerized and will end in an oligomer state. In the heating process for evaporating unreacted materials, the temperature is temporarily raised to 220-250°C, but there is no problem if this process is omitted.

[0074] In addition, when the additive (amine vanadate) is added, the temperature of the contents is lowered to 120°C or less to prevent a sudden reaction. In the embodiment, the temperature is set to 90°C. In addition, in the bonding process by microwave irradiation, the temperature of the irradiated part is slightly higher than that of other parts. This is because the additive absorbs electromagnetic waves and becomes hot, which creates a temperature difference with the molecules of the resin skeleton of the glycolic acid oligomer, and vanadium bonds to the hydrogen bond site. When the temperature difference is measured with an optical fiber thermometer, it is about 50 to 100°C. In other words, the vanadium atoms of the additive molecules are activated and replace the hydrogen in the polyglycolic acid molecules. If the microwave output is too large or too small, this reaction does not occur. For this reason, the temperature of the contents is adjusted to between 160 and 180°C, and the microwave output is about 10Kg / Kw.

[0075] A modified polyglycolic acid was produced by the modified polyglycolic acid production process according to this embodiment using a modified polyglycolic acid production apparatus 700. The produced modified polyglycolic acid contains the same amount of modified polyglycolic acid having a structure in which vanadium having a valence of 4 is bonded to polyglycolic acid and modified polyglycolic acid having a structure in which vanadium having a valence of 3 is bonded to polyglycolic acid. In the produced modified polyglycolic acid, the oxygen atom double-bonded to the carbon chain of polyglycolic acid is replaced with a tetravalent vanadium atom or a trivalent vanadium atom.

[0076] (Verification of the valence of vanadium in modified polyglycolic acid) The oxidation number of vanadium contained in the modified polyglycolic acid was tested by the following procedure to verify the valence of vanadium in the modified polyglycolic acid produced in this example.

[0077] (1) The sample (modified PGA) is applied to a well-polished copper plate (3 mm thick) to a thickness of 20 μm. The temperature of the sample when applied is 130°C, and the copper plate is also preheated to 130°C. (2) The copper plate with the sample applied is allowed to cool naturally. (3) Graphite cut to the same size as the copper plate is placed on the applied surface and pressed against it. With the graphite still pressed against it, the sample is slowly heated to 90°C and then allowed to cool naturally. (4) A CV measurement is performed using the copper plate and graphite as electrodes.

[0078] The test conditions were as follows: Positive electrode: graphite Negative electrode: copper plate Sweep voltage: 0 to 2 V Step voltage: 10 mV Step time: 0.1 sec

[0079] FIG. 8B shows a graph 810 of current-potential characteristics, which is a test result of the oxidation number of vanadium of the modified polyglycolic acid produced according to this example.

[0080] 8B, when the modified polyglycolic acid having tetravalent vanadium bonded thereto and the modified polyglycolic acid having trivalent vanadium bonded thereto are contained in approximately equal amounts, the CV measurement produces a current-potential curve 811 as shown by the solid line. On the other hand, when the amount of the modified polyglycolic acid having trivalent vanadium bonded thereto is greater than the amount of the modified polyglycolic acid having tetravalent vanadium bonded thereto, the CV measurement produces a current-potential curve 812 as shown by the dashed line. When the amount of the modified polyglycolic acid having tetravalent vanadium bonded thereto is greater than the modified polyglycolic acid having trivalent vanadium bonded thereto, the CV measurement produces a current-potential curve 813 as shown by the dashed line.

[0081] In this example, the microwave irradiation time was controlled to adjust the current-potential curve to 811. As a result, it was possible to obtain a modified polyglycolic acid containing approximately equal amounts of modified polyglycolic acid bound to tetravalent vanadium and modified polyglycolic acid bound to trivalent vanadium.

[0082] (Procedure for producing glycolic acid oligomer) Fig. 9 is a diagram showing in detail the procedure for producing a glycolic acid oligomer according to this embodiment. Fig. 9 corresponds to step S101 (dehydration condensation polymerization) in Fig. 1. In Fig. 9, the same steps as in Fig. 8 are given the same step numbers.

[0083] Step S803 (heat dehydration): The raw material glycolic acid is heated and dehydrated in a pressure-resistant polymerization vessel to obtain concentrated glycolic acid and glycolide 911, which is a dimer of glycolic acid. Hereinafter, this product is called concentrated glycolic acid 901.

[0084] Step S809 (dehydration polycondensation): A catalyst is added to concentrated glycolic acid 901 containing glycolide 911, and dehydration polycondensation is carried out under a reduced pressure environment while monitoring the number average molecular weight to obtain glycolic acid oligomer 102. Stannous octoate is suitable as the catalyst, and dodecyl alcohol is used as the polymerization initiator.

[0085] (Amine vanadate manufacturing equipment) Fig. 10A is a diagram showing the configuration of an apparatus 1000 for producing amine vanadate according to this embodiment. The apparatus 1000 for producing amine vanadate is a membrane-less electrolysis apparatus for electrolyzing the contents, and can also be used in the process for producing hypochlorous acid and sodium hydroxide from saline by membrane-less electrolysis in the process for producing glycolic acid in Fig. 2.

[0086] The amine vanadate manufacturing apparatus 1000 includes a vessel consisting of a reaction vessel 1001 and a lid 1002, a stirrer 1003, two electrode terminals 1004 and 1005, two electrodes 1006 and 1007, and a control device 1010. Ammonium vanadate is introduced into the vessel as a raw material, and the produced amine vanadate is taken out. The two electrodes 1006 and 1007 are preferably titanium electrodes coated with platinum (Pt).

[0087] The control device 1010 has an electrolysis power supply unit 1011, an electrolysis mode setting unit 1012, an electrolysis current detection unit 1013, and an electrolysis voltage detection unit 1014. When the electrolysis mode setting unit 1012 has set the constant voltage mode, the electrolysis power supply unit 1011 adjusts the voltage between the two electrodes 1006 and 1007 to a constant voltage. On the other hand, when the electrolysis mode setting unit 1012 has set the constant current mode, the electrolysis power supply unit 1011 adjusts the current between the two electrodes 1006 and 1007 to a constant current, and determines the end of electrolysis based on a detection signal of a predetermined electrolysis voltage threshold (1.5 V) from the electrolysis voltage detection unit 1014. The electrolysis mode setting unit 1012 initially sets the constant voltage mode, and when the electrolysis current detection unit 1013 detects a predetermined electrolysis current (20 mA / cm 2 ), the constant voltage mode is switched to the constant current mode. The electrolysis current detection unit 1013 detects the electrolysis current to monitor the electrolysis current, and also detects the electrolysis current at a predetermined electrolysis current (20 mA / cm) in the constant voltage mode. 2 ) to the electrolysis mode setting unit 1012. The electrolysis voltage detection unit 1014 detects and monitors the electrolysis voltage, and notifies the electrolysis mode setting unit 1012 of the end of electrolysis when the electrolysis voltage falls to a predetermined electrolysis voltage threshold (1.5 V) in the constant current mode.

[0088] (Amine vanadate manufacturing process) FIG. 10B is a flow chart showing the steps of producing amine vanadate according to this embodiment using the above-mentioned amine vanadate production apparatus 1000.

[0089] Step S1001 (initial setting): 500 ml of water is poured into the reaction vessel 1001 of the manufacturing apparatus 1000. Then, the stirring device 1003 is operated, and a direct current of 12 V is applied between the two electrodes 1006 and 1007. The current application mode is the constant voltage mode.

[0090] Step S1003 (adding ammonium vanadate): 0.1 mol (about 11.7 g) of ammonium vanadate is measured out and added little by little so as not to accumulate at the bottom of the reaction vessel 1001. It is confirmed that the electrolysis current increases slightly and the color of the solution inside the reaction vessel 1001 changes slightly to yellow.

[0091] Step S1005 (monitoring and adjusting electrolysis current): The limiting current (5 mA / cm in this example) in the manufacturing equipment 1000 is 2 ) about 3 to 5 times (15mA / cm 2 ~25mA / cm 2 ) range. If the electrolysis current is too high (>30mA / cm 2 ), but care must be taken since nitrate and nitrite compounds are produced. Such reactions have already been described with reference to FIG.

[0092] Step S1007 (determination of electrolytic current): If the electrolytic current is 20 mA / cm 2 It is determined whether or not

[0093] Step S1009 (constant current mode): Electrolysis current is 20 mA / cm 2 When this is reached, the current supply mode is set to constant current mode.

[0094] Step S1011 (monitoring and determining electrolysis voltage): It is determined whether the electrolysis voltage has dropped to 1.5 V.

[0095] Step S1013 (End of electrolysis): When the electrolysis voltage drops to 1.5 V, the electrolysis is ended. The color of the solution inside the reaction vessel 1001 becomes transparent yellow-orange. The content, that is, the produced amine vanadate, is sealed and stored in a cool, dark place.

[0096] By this production process, amine vanadate, which is an essential additive for producing modified polyglycolic acid from glycolic acid oligomer, could be stably produced.

[0097] The modified polyglycolic acid of this example was produced by carrying out the above-mentioned production steps. The produced modified polyglycolic acid contains the same amount of modified polyglycolic acid having a structure in which vanadium having a valence of 4 is bonded to polyglycolic acid and modified polyglycolic acid having a structure in which vanadium having a valence of 3 is bonded to polyglycolic acid.

[0098] The process shown in this example made it possible to stably obtain each material, product, and manufactured product in a simple manner.

[0099] [Second Example] As a second embodiment, an example of manufacturing a secondary battery using the modified polyglycolic acid manufactured in the first embodiment will be described.

[0100] <Manufacturing process of secondary battery using modified polyglycolic acid> 11A is a flow chart showing the steps of manufacturing a secondary battery using modified polyglycolic acid according to this embodiment. The steps of manufacturing a secondary battery will be described below with reference to FIG.

[0101] Step S1101 (Coating of Modified Polyglycolic Acid): Coat the modified polyglycolic acid 103 on two current collectors 411 and 412. The modified polyglycolic acid 103 produced in the first embodiment is coated to a thickness of 20 μm on the surface of a 20 μm thick copper plate for a positive electrode and a 20 μm thick aluminum plate for a negative electrode, which are the two current collectors.

[0102] Step S1103 (bonding of current collectors): The two electrodes coated with the modified polyglycolic acid 103 are bonded together with a separator 413 made of cellulose acetate having a thickness of 10 μm sandwiched therebetween.

[0103] Step S1105 (pressure welding): The two current collectors 411 and 412 are heated to 90° C. and pressed together until the distance between them becomes 10 μm or more and 30 μm or less.

[0104] This process provided an as-assembled (original) secondary battery 401. This secondary battery 401 is a battery that contains only stable unpolarized modified polyglycolic acid 103, so its performance does not deteriorate even after long-term storage. An initial charging process can be carried out when the battery is to be used.

[0105] <Initial charging process of secondary battery using modified polyglycolic acid> FIG. 11B is a flowchart showing the initial charging process of a secondary battery using modified polyglycolic acid according to this embodiment.

[0106] Step S1107 (initial charging starts): Initial charging is performed by applying a constant voltage of 2 V between the two current collectors 411 and 412. A slight current flow was observed, which increased with time.

[0107] Step S1109 (end of initial charging): The current peaked at about 5 mA and decreased, and the initial charging was ended when it reached 0.01 mA. The release voltage at this time was 1.4 V, which was confirmed to be equal to the oxidation-reduction potential of vanadium.

[0108] This process provides a secondary battery 402 after initialization charging, that is, a secondary battery 402 for which the initialization process and charging process have been completed. This secondary battery 402 is a battery that has already completed the charging process and has been charged and tested, and it is possible to provide a secondary battery 402 with few defects.

[0109] (Prototype secondary battery and its test condition) FIG. 11C is a diagram illustrating a prototype battery 1100 of a secondary battery using modified polyglycolic acid according to this embodiment and its test state.

[0110] A prototype secondary battery 1100 was manufactured as follows. First, two electrodes 1101 and 1102 measuring 40×50 mm were cut from an aluminum sheet having a thickness of 0.1 mm. One of the electrodes, 1102, was attached to an acrylic plate 1104. Then, modified polyglycolic acid 1103 was applied as an active material to each of the two electrodes 1101 and 1102, and the two were attached together with a cellulose acetate sheet (separator: not shown) sandwiched therebetween.

[0111] A direct current of 2.5 V was applied between the two electrodes of prototype battery 1100 for 5 minutes to initialize it, and then it was charged at 2 V for 10 minutes. After leaving it for 30 minutes, the no-load voltage was measured with voltmeter 1120. The no-load voltage was 1.45 V (see 1121). When it was discharged at a constant current with an electronic load of 100 mA, the electromotive force was 1.25 V, and when it was discharged until the terminal voltage reached 0.7 V, the duration was about 15 minutes. The discharge capacity of this prototype battery 1100 was calculated as follows: 0.1 (A) × 15 (min) ÷ 60 (min) = 0.025 Ah (= 25 mAh).

[0112] (Initial charging characteristics when initializing secondary batteries) Fig. 12 is a diagram showing initial charging characteristics 1200 in the initialization of the secondary battery according to this embodiment. The initial charging characteristics 1200 are characteristics when the secondary battery 401 in Fig. 4 is initially charged to the secondary battery 402 according to Fig. 11B. The current flow was observed when a 2V DC power supply was connected to the electrode pair.

[0113] At first, there was a valence change from tetravalent vanadium on the positive electrode side to trivalent vanadium, and from trivalent vanadium on the negative electrode side to tetravalent vanadium near separator 413, and almost no current flowed. Gradually, valence changes began to occur near current collectors 411 and 412, which were far from separator 413, and a state was observed in which the current started out small and then increased over time.

[0114] Then, when the initialization period ends and the charging period begins, the valence of the tetravalent vanadium on the positive electrode side changes to pentavalent vanadium, and the valence of the trivalent vanadium on the negative electrode side changes to divalent vanadium, causing the current to peak at about 5 mA and then decrease. The initial charging was terminated when the positive electrode side became pentavalent vanadium, the negative electrode side became divalent vanadium, and the current dropped to 0.01 mA. The release voltage at this time was 1.4 V, which was confirmed to be equal to the oxidation-reduction potential of vanadium.

[0115] The initialization time in the initial charge characteristic in FIG. 12 is the time required for all the vanadium on the positive electrode side to be converted to tetravalent vanadium by initialization of the tetravalent vanadium and trivalent vanadium contained in the modified polyglycolic acid. It is also the time required for all the vanadium on the negative electrode side to be converted to trivalent vanadium by initialization of the tetravalent vanadium and trivalent vanadium contained in the modified polyglycolic acid. If this reaction is not completed, the battery will not function. In addition, the secondary battery prototyped in this embodiment took about 1.5 times the initialization time to charge, but once initialized, the charging time is shorter from the next time onwards because there is no initialization time.

[0116] (Discharge characteristics of secondary batteries) 13 is a diagram showing a discharge characteristic 1300 during discharge of the secondary battery according to this embodiment. The discharge characteristic 1300 is a characteristic when discharging from the secondary battery 402 in FIG.

[0117] When an electronic load was connected to the positive and negative electrodes and the discharge was terminated at 10 mA with the final voltage set to 0.5 V, the electrode area was 1 cm 2 A discharge output of 1 mAh was obtained per battery.

[0118] The battery function was not lost and it was possible to charge it again even when the terminal voltage fell below 0.1 V as the discharge progressed. Furthermore, no significant change in characteristics was observed even after multiple charge / discharge cycles, demonstrating that the modified polyglycolic acid of this example can be used as an active material for secondary batteries.

[0119] More specifically, the discharge characteristics were as follows. The no-load electromotive force of the prototype battery immediately after the initial charge was 1.4V, and the no-load electromotive force after leaving it for 1 hour was 1.35V. The voltage was 1.3V when a 10mA electronic load was connected. A constant current discharge test was performed with the final voltage set to 0.5V, and the discharge continued for approximately 10 hours. After that, a 10Ω resistor was connected and the time it took for the voltage to drop to 0.1V was measured, which was approximately 1 hour. It also took approximately 8 hours for the terminal voltage to reach 1V, and this time is thought to be the practical life of the prototype battery. From the above results, it is considered that the 1cm discharge to 0.5V 2 The current capacity per unit is 1mAh, and the discharge current per unit is 1cm to 1V. 2 The current capacity per cell was 0.8 mAh.

[0120] According to this embodiment, the following noteworthy effects can be obtained. There is no need to worry about over-discharge. That is, charging and discharging are possible even if the terminal voltage drops to 0.1V. Constant voltage charging is sufficient. There is no particular need to limit the current as long as the voltage range (1.5 to 2V) is within which the molecular structure of the modified polyglycolic acid is not destroyed. Initialization takes some time, but after that, the battery can be charged at a faster rate than a general lithium-ion battery. Since charging and discharging are performed by oxidation and reduction of the active material, modified polyglycolic acid, the electrical performance of the battery is not dependent on the electrode material. Oxidation and OH formation do not occur in the electrodes. Therefore, a battery that can be supplied with a large current and is relatively lightweight can be provided. The raw materials are inexpensive, and the manufacturing process does not require a drying room (drying is not a requirement) or an advanced clean room, so it can be manufactured at a low cost. The manufacturing process of modified polyglycolic acid is consistent and simple, so manufacturing that takes several days with other manufacturing processes can be completed in about one day. The main raw material is biodegradable plastic that is friendly to the global environment and is harmless to living organisms. The material itself is difficult to burn, so there is no risk of toxic gas generation or explosion. No toxic chemicals are used in manufacturing.

[0121] [Other Examples] 14 is a diagram showing another embodiment using modified polyglycolic acid. FIG 14 shows an example of application as a memory 1400.

[0122] As shown in FIG. 14, the modified polyglycolic acid 1403 of this embodiment is printed in a slit shape on the positive electrode 1401 and the negative electrode 1402. Then, the matrix in which both electrodes 1401 and 1402 are attached so as to be perpendicular to each other can operate as a memory. That is, by applying a predetermined voltage to the positive electrode address 1411 and the negative electrode address 1421 to perform initialization, the contact portion is separated into tetravalent and trivalent vanadium to become a memory element, and the other portion becomes an inactive portion with the same amount of tetravalent and trivalent vanadium. After that, the matrix operates as a memory by the positive electrode address 1411 and the negative electrode address 1421. The memory of this embodiment can handle a large current and can be applied to various things.

[0123] Furthermore, the fact that the modified polyglycolic acid of this embodiment is produced as an active material having approximately equal amounts of tetravalent vanadium and trivalent vanadium makes it possible to apply the same in various fields by utilizing the initialization process, which is a significant advantage.

Claims

1. 1. A method for producing a modified polyglycolic acid, comprising adding a vanadium compound to a glycolic acid oligomer and irradiating the resulting mixture with microwaves to bond vanadium to the glycolic acid oligomer, The method for producing a modified polyglycolic acid, wherein the vanadium compound is an amine vanadate.

2. 2. The method for producing a modified polyglycolic acid according to claim 1, wherein the molecular weight of the glycolic acid oligomer is from 5,000 to 10,000.

3. 3. The method for producing a modified polyglycolic acid according to claim 2, wherein the molecular weight of the glycolic acid oligomer is 6,000 or more and 8,000 or less.

4. A method for producing a modified polyglycolic acid described in any one of claims 1 to 3, wherein the amount of the amine vanadate added is 1 wt% or more and 10 wt% or less.

5. A method for producing a modified polyglycolic acid as described in claim 4, wherein the amount of the amine vanadate added is 4 wt% or more and 6 wt% or less.

6. The method for producing a modified polyglycolic acid according to claim 1 , wherein the glycolic acid oligomer is produced by heating and dehydrating glycolic acid in a reduced pressure environment.

7. 7. The method for producing a modified polyglycolic acid according to claim 6, wherein the glycolic acid oligomer is produced by heating and dehydrating the glycolic acid in a reduced pressure environment to obtain concentrated glycolic acid containing glycolide, adding tin octylate as a catalyst to the concentrated glycolic acid, and subjecting the resulting mixture to dehydration condensation polymerization while monitoring the molecular weight.

8. A production apparatus for modified polyglycolic acid for producing modified polyglycolic acid by the production method of modified polyglycolic acid according to claim 7, a pressure vessel into which glycolic acid is introduced as a raw material and from which the produced modified polyglycolic acid is taken out; A stirring device for stirring the contents of the pressure-resistant vessel; A pressure reducing device for creating a negative pressure inside the pressure vessel; A microwave irradiation device that irradiates microwaves to the contents; A temperature control device for controlling the temperature of the contents; A control device that controls the temperature of the content, the pressure in the pressure-resistant vessel, and the stirring rotation speed of the stirring device; an exhaust condenser that generates condensed water by heat exchange with exhaust gas from the pressure-resistant vessel in response to intake by the pressure reducing device; A condensed water storage device that separates and stores the condensed water; Equipped with The pressure vessel comprises: a raw material inlet for introducing the glycolic acid; a catalyst and additive inlet into which tin octylate as a catalyst used for producing glycolic acid oligomers and amine vanadate, which is a vanadium compound, as an additive used for producing modified polyglycolic acid are introduced; an outlet through which the modified polyglycolic acid is taken out; a nitrogen gas aeration port through which nitrogen gas is introduced to prevent contamination inside the pressure vessel; an internal viewing window for monitoring the condition of the contents of the pressure vessel; An internal light for illuminating the inside of the pressure vessel; having The temperature control device is a production device for modified polyglycolic acid, and controls the temperature of the contents by a medium heat heating method using heat transfer oil.

9. The control device includes: In the step of producing concentrated glycolic acid containing glycolide by heating and dehydrating the glycolic acid in a reduced pressure environment, the temperature of the glycolic acid is set to 180° C., and a dehydration state is estimated from the amount of the condensed water, In the step of adding tin octoate as a catalyst to the concentrated glycolic acid, the temperature of the concentrated glycolic acid is set to 60° C., In the step of producing the glycolic acid oligomer by dehydration condensation polymerization of the concentrated glycolic acid to which the catalyst has been added, the temperature of the concentrated glycolic acid is kept at 170° C., the pressure in the pressure-resistant vessel is maintained at 0.1 Atm, and the dehydration condensation polymerization is terminated when the number average molecular weight is 5,000 or more and 10,000 or less, In the step of adding amine vanadate to the glycolic acid oligomer, the temperature of the content is set to 90° C., In the step of irradiating the glycolic acid oligomer to which the vanadate amine has been added with microwaves to bond vanadium to the glycolic acid oligomer to produce the modified polyglycolic acid, the temperature of the content is set to 170° C., 9. The apparatus for producing a modified polyglycolic acid according to claim 8, wherein the temperature of the content is adjusted to 120° C. when the production of the modified polyglycolic acid is completed.

Citation Information

Patent Citations

  • Method for manufacturing aliphatic polyesters

    JP1993287056A

  • High-strength bioabsorbable material containing polyglycolic acid

    JP2005516100A

  • Synthesis method and synthesis apparatus for polyhydroxycarboxylic acid

    JP2008001733A

  • Manufacturing method of polyglycolic acid having lowered melt viscosity

    JP2010215782A

  • JPP6712004B