Composite substrate and method for manufacturing the same
A composite substrate design with a thin amorphous bonding layer and controlled gas content addresses low bonding strength issues, ensuring robust adhesion and efficient manufacturing of piezoelectric and semiconductor substrates.
Patent Information
- Application Number
- JP2023218694
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-25
AI Technical Summary
Conventional methods for bonding piezoelectric and semiconductor substrates in composite substrates face issues with low bonding strength and risk of separation during processing, necessitating thicker bonding layers for adequate strength, which complicates productivity.
A composite substrate design involving functional and support substrates bonded via a thin bonding layer composed of amorphous semiconductor material with controlled rare gas content, and optionally an insulating layer, achieved through controlled high-speed atomic beam irradiation and sputtering processes.
The method ensures sufficient bonding strength even with a thin bonding layer, enhancing productivity and reducing the risk of separation, while maintaining manufacturing efficiency.
Smart Images

Figure 0007566119000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite substrate and a method for manufacturing the same. [Background technology]
[0002] Conventionally, composite substrates are known that are formed by bonding a functional substrate made of a piezoelectric material such as LN (LiNbO3: lithium niobate) or LT (LiTaO3: lithium tantalate) to a support substrate made of a semiconductor material such as Si, and are used for applications such as surface acoustic wave devices. A method for fabricating such composite substrates is known in which the bonding surfaces of the functional substrate and the support substrate are activated by irradiating them with a fast atom beam (FAB) and then directly bonded together. However, this method has a problem in that the bonding strength between the substrates is low, and there is a risk of the substrates peeling off during the processing step after bonding.
[0003] In order to solve the above problem, the technology of Patent Document 1 is known. Patent Document 1 describes a method for manufacturing a composite substrate by irradiating a support substrate with a fast atomic beam to sputter the semiconductor material of the support substrate, thereby forming a bonding layer made of an amorphous semiconductor material on the piezoelectric substrate by amorphizing the semiconductor material, and then pressure-bonding the piezoelectric substrate and support substrate via this bonding layer. This method improves the bonding strength between the piezoelectric substrate and support substrate, and prevents peeling after bonding. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 7152711 Summary of the Invention [Problem to be solved by the invention]
[0005] In a composite substrate in which a functional substrate such as a piezoelectric substrate and a support substrate are bonded, it is preferable that the sputtering time is as short as possible from the viewpoint of productivity, and shortening the sputtering time results in a thinner bonding layer. On the other hand, in order to obtain a desired bonding strength in a conventional bonding method such as that in Patent Document 1, a certain thickness is required for the bonding layer.
[0006] The present invention has been made in consideration of the above, and its main object is to provide a composite substrate and a manufacturing method thereof, in which a functional substrate and a supporting substrate are bonded via a bonding layer, which is capable of obtaining sufficient bonding strength even if the bonding layer is thin. [Means for solving the problem]
[0007] The present invention First aspect of The composite substrate according to the present invention includes a functional substrate made of a functional material, and a support substrate made of a semiconductor material and bonded to the functional substrate to support the functional substrate, and the functional substrate is A first functional layer made of a crystal of the functional material. And the above 1st functional layer a rare gas-containing The functional material Made of amorphous material 2nd functional layer The support substrate has a first support layer, a second support layer that is disposed closer to the functional substrate than the first support layer and is made of an amorphous body of the semiconductor material containing the rare gas, and a bonding layer that is in contact with the functional substrate and is made of an amorphous body of the semiconductor material. The bonding layer contains the rare gas, and the content of the rare gas in the bonding layer is lower than the content of the rare gas in the second support layer. . A composite substrate according to a second aspect of the present invention comprises a functional substrate made of a functional material, and a support substrate made of a semiconductor material and bonded to the functional substrate to support the functional substrate, the functional substrate being bonded to the support substrate via an insulating layer made of an insulating material, the support substrate comprising a first support layer, a second support layer arranged closer to the functional substrate than the first support layer and made of an amorphous body of the semiconductor material containing a rare gas, and a bonding layer in contact with the insulating layer and made of the amorphous body of the semiconductor material, the insulating layer comprising a first insulating layer made of the insulating material and a second insulating layer made of the amorphous body of the insulating material and in contact with the bonding layer, the bonding layer containing the rare gas, and a content of the rare gas in the bonding layer being lower than a content of the rare gas in the second support layer. The present invention According to the third aspect of theA method for manufacturing a composite substrate including a functional substrate made of a functional material and a support substrate made of a semiconductor material and supporting the functional substrate, the method including: an activation step of irradiating a surface of the functional substrate and a surface of a semiconductor substrate made of the semiconductor material with a fast atomic beam so that at least a portion of the irradiation times of the respective surfaces overlap; a sputtering step, which is performed following the activation step, in which, after stopping the irradiation of the fast atomic beam on the surface of the functional substrate, the irradiation of the fast atomic beam on the surface of the semiconductor substrate is continued to form a sputtered film made of an amorphous body of the sputtered semiconductor material on the surface of the functional substrate; and a bonding step of bonding the functional substrate on which the sputtered film has been formed and the semiconductor substrate to obtain a bonded body. A manufacturing method for a composite substrate according to a fourth aspect of the present invention is a manufacturing method for a composite substrate including a functional substrate made of a functional material and a support substrate made of a semiconductor material and supporting the functional substrate, the manufacturing method including: an insulating layer forming step of forming an insulating layer made of an insulating material on a surface of the functional substrate; an activation step of irradiating a surface of the insulating layer and a surface of a semiconductor substrate made of the semiconductor material with a fast atomic beam so that at least a part of the irradiation times of the respective surfaces overlap; a sputtering step that is performed subsequent to the activation step, in which after stopping the irradiation of the fast atomic beam on the surface of the insulating layer, the irradiation of the fast atomic beam on the surface of the semiconductor substrate is continued to sputter the semiconductor material on the surface of the insulating layer; and a bonding step of bonding the functional substrate and the semiconductor substrate via the insulating layer onto which the semiconductor material has been sputtered by the sputtering step to obtain a bonded body. Effect of the Invention
[0008] According to the present invention, it is possible to realize a composite substrate in which a functional substrate and a supporting substrate are bonded via a bonding layer, and a manufacturing method thereof, which is capable of obtaining sufficient bonding strength even if the bonding layer is thin. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a first embodiment of the present invention. [Diagram 2] 2A to 2C are diagrams illustrating an example of a manufacturing process for the composite substrate according to the first embodiment of the present invention. [Diagram 3] 2A to 2C are diagrams illustrating an example of a manufacturing process for the composite substrate according to the first embodiment of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a second embodiment of the present invention. [Diagram 5] 6A to 6C are diagrams illustrating an example of a manufacturing process for a composite substrate according to a second embodiment of the present invention. [Figure 6] 6A to 6C are diagrams illustrating an example of a manufacturing process for a composite substrate according to a second embodiment of the present invention. [Figure 7]FIG. 11 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a third embodiment of the present invention. [Figure 8] FIG. 11 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a fourth embodiment of the present invention. [Figure 9] FIG. 2 is a diagram showing observation photographs of Example 1 and a comparative example. [Figure 10] 1 is a table showing the EDX analysis results of Examples 1 and 3. [Figure 11] 1 is a table showing the relationship between FAB irradiation time, thickness of a bonding layer, and bonding strength in a composite substrate. [Figure 12] 1 is a table showing the relationship between the FAB irradiation time and the bonding strength of a functional substrate and a semiconductor substrate in a composite substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the width, thickness, shape, etc. of each part may be shown more diagrammatically than in the embodiment, but these are merely examples and do not limit the interpretation of the present invention.
[0011] (First embodiment) 1 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a first embodiment of the present invention. The composite substrate 100 in this embodiment is used for various purposes such as an optical element constituting an optical waveguide, a piezoelectric element constituting a surface acoustic wave (SAW) filter, various semiconductor elements, etc., and has a structure in which a functional substrate 10 made of a functional material such as a piezoelectric material or a semiconductor material is bonded to a support substrate 30.
[0012] The material of the functional substrate 10 may be, for example, a piezoelectric material such as LN (LiNbO3: lithium niobate), LT (LiTaO3: lithium tantalate), quartz, AlN (aluminum nitride), or PZT (Pb(Zr,Ti)O3: lead zirconate titanate). The material of the functional substrate 10 may be selected arbitrarily depending on the application of the composite substrate 100. For example, the functional substrate 10 may be made of semiconductor materials such as SiC, InP, GaN, GaP, and diamond, materials having electro-optical effects such as lithium niobate-lithium tantalate and KTP (potassium titanate phosphate), quartz, or glass, in addition to the piezoelectric material. In addition, the functional substrate 10 made of various functional materials may be used depending on the application of the composite substrate 100.
[0013] The support substrate 30 supports the functional substrate 10. Any appropriate substrate can be used as the support substrate 30. The support substrate 30 may be composed of a single crystal body or a polycrystalline body. The functional substrate 10 and the support substrate 30 are directly bonded to each other.
[0014] The material constituting the support substrate 30 may be a semiconductor material such as Si, Ge, SiC, InP, GaN, or sapphire. Alternatively, the support substrate 30 may be made of Si(1-x)Ox (where 0.008≦x≦0.408) or SOI (Silicon on Insulator). The thickness of the support substrate 30 is, for example, 0.2 to 1 mm, but any other appropriate thickness may be adopted.
[0015] Although not shown, composite substrate 100 may further include any layer. The types, functions, number, combination, arrangement, etc. of such layers may be appropriately set depending on the purpose.
[0016] The composite substrate 100 may be manufactured in any appropriate shape. In one embodiment, the composite substrate 100 may be manufactured in the form of a so-called wafer. The size of the composite substrate 100 may be appropriately set depending on the purpose, for example, the diameter of the wafer (substrate) may be 50 mm to 150 mm.
[0017] 2 and 3 are diagrams showing an example of a manufacturing process for the composite substrate according to the first embodiment of the present invention.
[0018] 2(a) shows a preparation step in the manufacturing process of the composite substrate 100. In this step, a functional substrate 10 made of a functional material and having a predetermined thickness is prepared.
[0019] Fig. 2(b) shows an activation step in the manufacturing process of the composite substrate 100. In this step, for example, a semiconductor substrate 30A made of a semiconductor material with a predetermined thickness is prepared, and activation processing is performed by irradiating the surfaces of the functional substrate 10 prepared in the preparation step of Fig. 2(a) and the semiconductor substrate 30A with a fast atomic beam (hereinafter referred to as FAB) using a rare gas such as Ar as an atomic species for a predetermined time. The irradiation time of the FAB at this time is preferably about 15 to 30 seconds, for example.
[0020] FIG. 2(c) shows a sputtering step in the manufacturing process of the composite substrate 100. In this step, the FAB irradiation on the functional substrate 10 side is stopped, and the FAB irradiation on the semiconductor substrate 30A side is continued for a predetermined time among the FAB irradiated on the functional substrate 10 side in the activation step of FIG. 2(b), respectively. The FAB irradiation time at this time is preferably about 30 seconds to 600 seconds, for example. As a result, the semiconductor material constituting the semiconductor substrate 30A is sputtered and attached to the surface of the functional substrate 10, and a sputtered film 30B made of the same semiconductor material as the semiconductor substrate 30A is formed on the functional substrate 10 side. As described later, the thickness of the bonding layer 33 (see FIG. 3(f)) in the composite substrate 100 after manufacture is preferably 0.3 nm or more and 3 nm or less, and therefore, in the sputtering step, it is preferable to form the sputtered film 30B with a thickness of 0.3 nm or more and 3 nm or less.
[0021] Fig. 3(d) shows a bonding step in the manufacturing process of the composite substrate 100. In this step, the functional substrate 10 on which the sputtered film 30B has been formed in the sputtering step of Fig. 2(c) is bonded to the semiconductor substrate 30A. As a result, the semiconductor substrate 30A and the sputtered film 30B are integrated to form the support substrate 30, and a bonded body of the functional substrate 10 and the support substrate 30 is obtained. Note that in Fig. 3(d) and subsequent figures, the positional relationship between the functional substrate 10 and the semiconductor substrate 30A (support substrate 30) is illustrated upside down compared to Figs. 2(a) to 2(c).
[0022] Fig. 3(e) shows a bonded body obtained after the bonding step of Fig. 3(d). By the bonding step of Fig. 3(d), the semiconductor substrate 30A and the sputtered film 30B are integrated as described above, forming a support substrate 30 having a bonding interface 40 therein, and a bonded body as shown in Fig. 3(e) is obtained.
[0023] In the bonded body of FIG. 3(e), a first functional layer 11 mainly composed of a crystalline body of a functional material and a second functional layer 12 arranged on the support substrate 30 side from the first functional layer 11 are formed on the functional substrate 10. The second functional layer 12 is mainly composed of an amorphous body of a functional material and is a layer containing rare gas atoms such as Ar irradiated as FAB in the activation step of FIG. 2(b). On the other hand, a first support layer 31 not in contact with the bonding interface 40, a second support layer 32 arranged on the functional substrate 10 side from the first support layer 31 and in contact with the bonding interface 40, and a bonding layer 33 arranged on the functional substrate 10 side from the second support layer 32 and in contact with the bonding interface 40 are formed on the support substrate 30. The second support layer 32 is mainly composed of an amorphous body of a semiconductor material and is a layer containing rare gas atoms such as Ar irradiated as FAB in the activation step of FIG. 2(b) or the sputtering step of FIG. 2(c). The bonding layer 33 corresponds to the sputtered film 30B before bonding, and is a layer that forms a bonding portion with the functional substrate .
[0024] The second functional layer 12 in the functional substrate 10, and the second support layer 32 and bonding layer 33 in the support substrate 30 may contain other atomic species that are mixed into these layers during the sputtering process shown in Fig. 2(c), such as Fe atoms and Al atoms that constitute the jig or base portion used to fix the semiconductor substrate 30A. Details of these layers will be described later.
[0025] Fig. 3(f) shows a thinning process in the manufacturing process of the composite substrate 100. In this process, the functional substrate 10 is polished to a predetermined thickness to be thinned from the bonded body shown in Fig. 3(e). For example, the functional substrate 10 can be polished to be thinned by using a grinding process, a CMP (Chemical Mechanical Polish) process, a surface planarization process using a gas cluster ion beam, or the like.
[0026] Through the above steps, composite substrate 100 having the structure shown in FIG. 1 is manufactured.
[0027] In addition, an annealing step of heating the bonded body to a predetermined temperature may be performed between the bonding step of Fig. 3(d) and the thin plate processing step of Fig. 3(f). The heating temperature at this time is preferably, for example, about 75 to 250°C, and more preferably 100 to 250°C. This can improve the bonding strength of the functional substrate 10.
[0028] Second embodiment Fig. 4 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a second embodiment of the present invention. A composite substrate 110 in this embodiment has a structure in which a functional substrate 10 is bonded to a support substrate 30 via an insulating layer 20, as compared with the composite substrate 100 in Fig. 1 described in the first embodiment.
[0029] The insulating layer 20 made of an insulating material is disposed between the functional substrate 10 and the support substrate 30. The insulating material constituting the insulating layer 20 may be, for example, an oxide or nitride of Si, Ta, Al, Nb, Hf, or the like, and is preferably silicon oxide.
[0030] The insulating layer 20 can be formed by any suitable method. For example, it can be formed by physical vapor deposition such as sputtering, vacuum deposition, or ion beam assisted deposition (IAD), chemical vapor deposition, or atomic layer deposition (ALD). The insulating layer 20 can be formed at room temperature (25°C) to 300°C, for example.
[0031] In this embodiment, as in the first embodiment, composite substrate 110 may further include any layer. The types, functions, numbers, combinations, arrangements, etc. of such layers may be appropriately set depending on the purpose. Furthermore, composite substrate 110 may be manufactured in any appropriate shape depending on the purpose.
[0032] 5 and 6 are diagrams showing an example of a manufacturing process for a composite substrate according to the second embodiment of the present invention.
[0033] Fig. 5(a) shows a preparation step in the manufacturing process of the composite substrate 110. In this step, a functional substrate 10 having a predetermined thickness is prepared, similar to the step of Fig. 2(a) described in the first embodiment.
[0034] Fig. 5(b) shows an insulating layer forming step in the manufacturing process of the composite substrate 110. In this step, an insulating layer 20 is formed by depositing, for example, an amorphous silicon oxide film to a predetermined thickness on the surface of the functional substrate 10 prepared in the preparation step of Fig. 5(a).
[0035] Fig. 5(c) shows an activation step in the manufacturing process of the composite substrate 110. In this step, for example, a semiconductor substrate 30A made of a semiconductor material having a predetermined thickness is prepared, and activation processing is performed by irradiating the surfaces of the insulating layer 20 formed on the functional substrate 10 in the insulating layer forming step of Fig. 5(b) and the semiconductor substrate 30A with FAB using a rare gas such as Ar as an atomic species for a predetermined time, similar to the step of Fig. 2(b) described in the first embodiment.
[0036] FIG. 5(d) shows a sputtering step in the manufacturing process of the composite substrate 110. In this step, as in the step of FIG. 2(c) described in the first embodiment, among the FABs irradiated to the functional substrate 10 and the semiconductor substrate 30A in the activation step of FIG. 5(c), the FAB irradiation on the functional substrate 10 side (insulating layer 20 side) is stopped, and the FAB irradiation on the semiconductor substrate 30A side is continued for a further predetermined time. As a result, the semiconductor material constituting the semiconductor substrate 30A is sputtered and attached to the surface of the insulating layer 20 formed on the functional substrate 10, and a sputtered film 30B made of the same semiconductor material as the semiconductor substrate 30A is formed on the functional substrate 10 side (insulating layer 20 side). As in the first embodiment, the thickness of the bonding layer 33 (see FIG. 6(g)) in the composite substrate 110 after manufacture is preferably 0.3 nm or more and 3 nm or less, and therefore, in the sputtering step, it is preferable to form the sputtered film 30B with a thickness of 0.3 nm or more and 3 nm or less.
[0037] FIG. 6(e) shows a bonding step in the manufacturing process of the composite substrate 110. In this step, similar to the step of FIG. 3(d) described in the first embodiment, the functional substrate 10 on which the sputtered film 30B has been formed on the insulating layer 20 in the sputtering step of FIG. 5(d) is bonded to the semiconductor substrate 30A. As a result, the semiconductor substrate 30A and the sputtered film 30B are bonded and integrated to form the support substrate 30, and a bonded body of the functional substrate 10, the insulating layer 20, and the support substrate 30 is obtained. Note that in FIG. 6(e) and subsequent figures, the positional relationship between the functional substrate 10 and the semiconductor substrate 30A (support substrate 30) is illustrated upside down compared to FIG. 5(a) to FIG. 5(d).
[0038] Fig. 6(f) shows a bonded body obtained after the bonding step of Fig. 6(e). By the bonding step of Fig. 6(e), the semiconductor substrate 30A and the sputtered film 30B are integrated as described above, forming a support substrate 30 having a bonding interface 40 therein, and a bonded body as shown in Fig. 6(f) is obtained.
[0039] In the bonded body of FIG. 6(f), the insulating layer 20 is formed with a first insulating layer 21 mainly made of an insulating material, and a second insulating layer 22 arranged closer to the support substrate 30 than the first insulating layer 21. The second insulating layer 22 is mainly made of an amorphous body of an insulating material, and is a layer containing rare gas atoms such as Ar irradiated as FAB in the activation step of FIG. 5(c). On the other hand, the support substrate 30 is formed with a first support layer 31 not in contact with the bonding interface 40, a second support layer 32 arranged closer to the functional substrate 10 than the first support layer 31 and in contact with the bonding interface 40, and a bonding layer 33 arranged closer to the functional substrate 10 than the second support layer 32 and in contact with the bonding interface 40, as in the first embodiment.
[0040] Fig. 6(g) shows a thin plate processing step in the manufacturing process of the composite substrate 110. In this step, similar to the step of Fig. 3(f) described in the first embodiment, the functional substrate 10 is polished to a predetermined thickness for the bonded body shown in Fig. 6(f) to thin it.
[0041] Through the above steps, composite substrate 110 having the structure shown in FIG. 4 is manufactured.
[0042] In this embodiment, similarly to the first embodiment, an annealing step of heating the bonded body to a predetermined temperature may be performed between the bonding step of FIG. 6(e) and the thin plate processing step of FIG. 6(g).
[0043] (Third embodiment) 7 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a third embodiment of the present invention. A composite substrate 120 according to this embodiment has a structure in which a functional substrate 10 is directly bonded to a support substrate 30, similar to the composite substrate 100 shown in FIG. 1 described in the first embodiment.
[0044] In the composite substrate 120 of this embodiment, a ridge portion 50 is provided on the functional substrate 10 in order to use a part of the functional substrate 10 as an optical waveguide. The ridge portion 50 is a portion of the functional substrate 10 formed to have a greater thickness than other portions by providing a step in a part of the functional substrate 10. The ridge portion 50 is provided by performing a process (ridge processing) for forming a step in a part of the functional substrate 10 after the thin plate processing process of FIG. 3(f) described in the first embodiment, for example. For example, the ridge processing of the functional substrate 10 can be realized by processing using a laser beam or dry etching such as RIE (Reactive Ion Etching). Other processes may be performed thereafter. As a result, the bonding interface 40 is included inside the support substrate 30 in this embodiment as well.
[0045] (Fourth embodiment) Fig. 8 is a schematic cross-sectional view showing a schematic configuration of a composite substrate according to a fourth embodiment of the present invention. A composite substrate 130 in this embodiment has a structure in which a functional substrate 10 is bonded to a support substrate 30 via an insulating layer 20, similar to the composite substrate 110 in Fig. 4 described in the second embodiment.
[0046] The material and shape of the functional substrate 10 are the same as those described in the third embodiment. That is, in the composite substrate 130 of this embodiment, a ridge portion 50 is provided in the functional substrate 10 in order to use a part of the functional substrate 10 as an optical waveguide. The ridge portion 50 is provided by performing a process (ridge processing) for forming a step in a part of the functional substrate 10 after the thin plate processing step of FIG. 6(g) described in the second embodiment, for example. As a result, the bonding interface 40 is included inside the support substrate 30 in this embodiment as well. EXAMPLES
[0047] Examples for verifying the structure of the composite substrate according to the present invention will be specifically described below. Note that, unless otherwise specified, the following procedures were carried out at room temperature.
[0048] Example 1 A bonded body was produced according to the manufacturing process described with reference to Figures 2 and 3. Specifically, a LT substrate and a silicon substrate each having a diameter of 4 inches and a thickness of 500 μm were prepared, and the LT substrate was used as the functional substrate 10, and the silicon substrate was used as the semiconductor substrate 30A.
[0049] Then, after cleaning the surfaces of the functional substrate 10 and the semiconductor substrate 30A, the functional substrate 10 and the semiconductor substrate 30A were placed in a vacuum chamber in which the fabrication guns were installed facing upward and downward, so that the substrates were located within the irradiation ranges of the fabrication guns and the surfaces of the substrates faced each other. -6 The chamber was evacuated to a vacuum of the Pa range, and the surfaces of the functional substrate 10 and the semiconductor substrate 30A were simultaneously irradiated with FAB using Ar gas (accelerating voltage 1 kV, Ar flow rate 27 sccm) from each FAB gun for 15 seconds.
[0050] Thereafter, the FAB irradiation on the functional substrate 10 side was stopped, while the FAB irradiation on the semiconductor substrate 30A side was continued for another 90 seconds (total of 105 seconds). In order to prevent the internal pressure of the vacuum chamber from changing before and after the FAB irradiation on the functional substrate 10 side was stopped, the FAB irradiation from the FAB gun on the functional substrate 10 side to the surface of the functional substrate 10 was stopped while the supply of Ar gas to the FAB gun on the functional substrate 10 side was continued. As a result, a sputtered film 30B was formed on the surface of the functional substrate 10.
[0051] Next, the functional substrate 10 on which the sputtered film 30B was formed was directly bonded to the semiconductor substrate 30A. Specifically, the beam-irradiated surfaces of both substrates were overlapped, and the two substrates were bonded together by applying a pressure of 10,000 N for 2 minutes at room temperature to obtain a bonded body. As a result, a composite substrate 100 having the structure shown in FIG. 1 was obtained.
[0052] The bonding strength of the composite substrate 100 thus obtained was evaluated by a crack opening method, and was found to be 1.45 J / m 2 and had a sufficient bonding strength.
[0053] Example 2 The functional substrate 10 and the semiconductor substrate 30A similar to those in Example 1 were placed in a vacuum chamber, and the inside of the vacuum chamber was heated to 10 -6 In a state where the vacuum was drawn to the Pa range, the surfaces of the functional substrate 10 and the semiconductor substrate 30A were simultaneously irradiated with FAB using Ar gas under the same conditions as in Example 1 for 30 seconds from each FAB gun.
[0054] Thereafter, the FAB irradiation on the functional substrate 10 side was stopped, while the FAB irradiation on the semiconductor substrate 30A side was continued for another 90 seconds (total of 120 seconds). At this time, as in Example 1, in order to prevent the internal pressure of the vacuum chamber from changing before and after the FAB irradiation on the functional substrate 10 side was stopped from the FAB gun on the functional substrate 10 side while continuing to supply Ar gas to the FAB gun on the functional substrate 10 side. As a result, a sputtered film 30B was formed on the surface of the functional substrate 10.
[0055] Next, similarly to Example 1, the functional substrate 10 on which the sputtered film 30B was formed and the semiconductor substrate 30A were directly bonded to obtain the composite substrate 100 having the structure shown in FIG.
[0056] The bonding strength of the composite substrate 100 thus obtained was evaluated by a crack opening method, and was found to be 1.63 J / m 2 The bonding strength was improved compared to Example 1.
[0057] Example 3 A bonded body was produced according to the manufacturing process described with reference to Figures 5 and 6. Specifically, a LT substrate and a silicon substrate, each having a diameter of 4 inches and a thickness of 500 µm, were prepared, and the LT substrate was used as the functional substrate 10, and the silicon substrate was used as the semiconductor substrate 30A. Silicon oxide was then sputtered onto the surface of the functional substrate 10 to form an insulating layer 20 made of a silicon oxide film.
[0058] Thereafter, similarly to Example 1, the surfaces of the functional substrate 10 and the semiconductor substrate 30A on which the insulating layer 20 was formed were cleaned, and then, in a vacuum chamber in which FAB guns were installed facing upward and downward, the functional substrate 10 and the semiconductor substrate 30A were arranged so that the substrates were located within the irradiation ranges of the FAB guns and the silicon oxide surface (the surface on the insulating layer 20 side) of the functional substrate 10 and the surface of the semiconductor substrate 30A faced each other. In this state, the inside of the vacuum chamber was filled with 10 -6 The chamber was evacuated to a vacuum of the Pa range, and the surfaces of the functional substrate 10 and the semiconductor substrate 30A were simultaneously irradiated with Ar gas using FAB under the same conditions as in Example 1 for 15 seconds from each FAB gun.
[0059] Thereafter, the FAB irradiation on the functional substrate 10 side was stopped, while the FAB irradiation on the semiconductor substrate 30A side was continued for another 285 seconds (total of 300 seconds). At this time, as in Examples 1 and 2, in order to prevent the internal pressure of the vacuum chamber from changing before and after the FAB irradiation on the functional substrate 10 side was stopped from the FAB gun on the functional substrate 10 side while continuing to supply Ar gas to the FAB gun on the functional substrate 10 side. As a result, a sputtered film 30B was formed on the surface of the insulating layer 20 in the functional substrate 10.
[0060] Next, similarly to Examples 1 and 2, the functional substrate 10 having the sputtered film 30B formed on the surface of the insulating layer 20 and the semiconductor substrate 30A were directly bonded to obtain a composite substrate 110 having the structure shown in FIG.
[0061] The bonding strength of the composite substrate 110 thus obtained was evaluated by a crack opening method, and was found to be 2.01 J / m 2 The bonding strength was further improved compared to Examples 1 and 2.
[0062] In the above-mentioned Examples 1 to 3, the FAB irradiation from the FAB gun to the functional substrate 10 and the semiconductor substrate 30A is performed for a predetermined time, and then the FAB irradiation on the functional substrate 10 side is stopped first. This allows the time required for forming the sputtered film 30B to be used for cooling the functional substrate 10, so that the effect of warping on the composite substrates 100, 110 after bonding can be reduced. In particular, when the functional substrate 10 has a larger thermal expansion coefficient than the semiconductor substrate 30A, stopping the FAB irradiation on the functional substrate 10 side first can provide a higher effect in reducing warping after bonding.
[0063] (Comparative Example) In order to confirm the effect of the present invention, as a comparative example, a functional substrate 10 and a semiconductor substrate 30A similar to those in Example 1 were placed in a vacuum chamber, and the inside of the vacuum chamber was heated to 10 -6 In a state where the vacuum was drawn to the Pa range, FAB irradiation was performed only on the semiconductor substrate 30A side for 90 seconds without performing FAB irradiation on the functional substrate 10 side. The FAB irradiation conditions on the semiconductor substrate 30A side at this time were the same as those in Example 1. As a result, a sputtered film 30B was formed on the surface of the insulating layer 20 in the functional substrate 10.
[0064] Next, similarly to Examples 1 to 3, the functional substrate 10 on which the sputtered film 30B was formed and the semiconductor substrate 30A were directly bonded to obtain the composite substrate 100 having the structure shown in FIG.
[0065] The bonding strength of the composite substrate 100 thus obtained was evaluated by a crack opening method, and was found to be 0.74 J / m 2 Thus, sufficient bonding strength was not obtained.
[0066] (Checking the laminated structure) Cross sections including bonding interface 40 of composite substrates 100 produced in Example 1 and Comparative Example were observed with a transmission electron microscope (TEM) to confirm the layered structure of composite substrate 100. Fig. 9(a) shows an observation photograph of Example 1, and Fig. 9(b) shows an observation photograph of the Comparative Example.
[0067] From the observation photograph of Example 1 shown in FIG. 9(a), it can be seen that two layers are formed inside the functional substrate 10. These layers are referred to as the first functional layer 11 and the second functional layer 12, in order from the side farthest from the support substrate 30. It can also be seen that three layers are formed inside the support substrate 30. These layers are referred to as the first support layer 31, the second support layer 32, and the bonding layer 33, in order from the side farthest from the functional substrate 10. The second functional layer 12 and the bonding layer 33 are in contact with each other, and a bonding interface 40 formed in the above-mentioned bonding process exists between the second support layer 32 and the bonding layer 33. That is, in the bonding process, the surface of the second functional layer 12 in the semiconductor substrate 30A before bonding and the surface of the sputtered film 30B formed on the functional substrate 10 before bonding are bonded to each other, so that the sputtered film 30B becomes the bonding layer 33, and a bonded body of the functional substrate 10 and the support substrate 30 having the bonding interface 40 inside the support substrate 30 is formed.
[0068] 9(a), it can be seen that the second functional layer 12 does not have a crystalline structure and is composed of an amorphous body of LT, whereas the first functional layer 11 is composed of a crystalline body of LT. That is, in Example 1, it can be seen that the second functional layer 12, which corresponds to a portion of the functional substrate 10 before bonding from the surface irradiated with FAB in the activation step to a predetermined depth, is formed as a layer in which LT, the material of the functional substrate 10, has been made amorphous.
[0069] 9(a), it can be seen that the second support layer 32 and the bonding layer 33 do not have a crystalline structure and are composed of amorphous Si, whereas the first support layer 31 is composed of crystalline Si. That is, in Example 1, it can be seen that the second support layer 32, which corresponds to a portion of the semiconductor substrate 30A before bonding from the surface irradiated with FAB in the activation step and the sputtering step to a predetermined depth, and the bonding layer 33, which corresponds to the sputtered film 30B formed on the surface of the functional substrate 10 in the sputtering step, are each formed as a layer in which silicon, which is the material of the support substrate 30, has been made amorphous.
[0070] 9(b), the functional substrate 10 is composed of only a first functional layer 11 having a crystalline structure, and the second functional layer 12 as in Example 1 is not formed on the functional substrate 10. That is, in the comparative example, the functional substrate 10 before bonding is not irradiated with FAB in the activation process, and therefore the second functional layer 12 made of an amorphous film of LT is not formed, and as a result, it is understood that the bonding strength is lower than that in Example 1.
[0071] As described above, in Example 3, the insulating layer 20 made of a silicon oxide film is formed on the surface of the functional substrate 10 before bonding, and the surface of the insulating layer 20 is activated, and then the sputtered film 30B is formed to bond the functional substrate 10 and the semiconductor substrate 30A. Therefore, in the composite substrate 110 of Example 3, two layers corresponding to the first functional layer 11 and the second functional layer 12 in FIG. 9(a) are formed in the insulating layer 20, not in the functional substrate 10. That is, in Example 3, the first insulating layer 21 located on the side farther from the support substrate 30 and the second insulating layer 22 corresponding to the portion from the surface irradiated with FAB in the activation step before bonding to a predetermined depth are formed in the insulating layer 20.
[0072] (Structural analysis) In a cross section including the bonding interface 40 of the composite substrate 100 produced in Example 1, EDX analysis was performed on each of the first functional layer 11, the second functional layer 12, the first support layer 31, the second support layer 32, and the bonding layer 33, thereby performing a structural analysis of the composite substrate 100. Similarly, in a cross section including the bonding interface 40 of the composite substrate 110 produced in Example 3, EDX analysis was performed on each of the first insulating layer 21, the second insulating layer 22, the first support layer 31, the second support layer 32, and the bonding layer 33, thereby performing a structural analysis of the composite substrate 110.
[0073] 10(a) shows the proportions of elemental components obtained from the EDX analysis results for each of the first functional layer 11, the second functional layer 12, the first support layer 31, the second support layer 32, and the bonding layer 33 in Example 1. In addition, for the second functional layer 12, the second support layer 32, and the bonding layer 33, the measurement results of the thickness of each layer are also shown.
[0074] From the table of FIG. 10(a), the rare gas Ar used in the FAB irradiation is contained in a larger amount in the second functional layer 12 and the second support layer 32 than in the first functional layer 11 and the first support layer 31. The content of Ar is also higher in the second support layer 32 than in the second functional layer 12. From these results, it can be seen that the second functional layer 12 and the second support layer 32 contain Ar resulting from the FAB irradiated in the activation process and the sputtering process, respectively, and that the second support layer 32 is irradiated with FAB for a longer time than the second functional layer 12, so that the second functional layer 12 contains more Ar. Note that, although the table of FIG. 10(a) shows that the first functional layer 11 and the first support layer 31 contain a small amount of Ar, there may be cases where they do not contain any Ar.
[0075] 10(a), the Ar content in the bonding layer 33 is lower than that in the second functional layer 12 and the second support layer 32. This shows that the Ar irradiated as FAB in the sputtering process is not contained much in the bonding layer 33 corresponding to the sputtered film 30B.
[0076] 10(a) shows that the bonding layer 33 contains more Al than the other layers. This is thought to be because, in the sputtering process, the FAB is irradiated not only onto the semiconductor substrate 30A but also onto the jig and base that fix the semiconductor substrate 30A, and these components are mixed into the bonding layer 33.
[0077] 10(b) shows the ratio of elemental components obtained from the EDX analysis results for each of the first insulating layer 21, the second insulating layer 22, the first supporting layer 31, the second supporting layer 32, and the bonding layer 33 in Example 3. In addition, for the second supporting layer 32 and the bonding layer 33, the measurement results of the thickness of each layer are also shown.
[0078] In the insulating layer 20 of Example 3, unlike the functional substrate 10 of Example 1, both the first insulating layer 21 and the second insulating layer 22 are made of amorphous silicon oxide, so that the boundary between the first insulating layer 21 and the second insulating layer 22 is difficult to distinguish even when looking at a TEM observation photograph. Therefore, the thickness of the second insulating layer 22 is not listed in the table of FIG. 10(b). However, in the insulating layer 20 of Example 3, similar to the functional substrate 10 of Example 1, it is considered that the second insulating layer 22 made of an amorphous body containing a large amount of Ar is present in the vicinity of the bonding layer 33 (for example, within a range of about several nm from the boundary surface with the bonding layer 33) in the same manner as the second functional layer 12. Therefore, in the table of FIG. 10(b), the EDX analysis result for the insulating layer 20 near the boundary surface with the bonding layer 33 is shown as the EDX analysis result of the second insulating layer 22.
[0079] In the table of FIG. 10(b), as in the table of FIG. 10(a), the rare gas Ar used in the FAB irradiation is contained in a larger amount in the second insulating layer 22 and the second supporting layer 32 than in the first insulating layer 21 and the first supporting layer 31. The content of Ar is higher in the second supporting layer 32 than in the second insulating layer 22. From these results, it can be seen that in the example 3 as well as in the example 1, the second insulating layer 22 and the second supporting layer 32 contain Ar resulting from the FAB irradiated in the activation step and the sputtering step, and the second supporting layer 32 is irradiated with FAB for a longer time than the second insulating layer 22, so that the second insulating layer 22 contains more Ar. In the table of FIG. 10(b), the first insulating layer 21 and the first supporting layer 31 contain a small amount of Ar, but there may be cases where they do not contain Ar.
[0080] 10(b), the content of Ar in the bonding layer 33 is lower than that in the second insulating layer 22 and the second support layer 32. This shows that, as in Example 1, in Example 3 as well, the Ar irradiated as FAB in the sputtering process is not contained much in the bonding layer 33 corresponding to the sputtered film 30B.
[0081] Also, in the table of FIG. 10(b), as in the table of FIG. 10(a), it is found that the bonding layer 33 contains more Al than the other layers for the reasons described above.
[0082] (Relationship between bonding layer thickness and bonding strength) Among the manufacturing parameters described in Example 3, the FAB irradiation time to the semiconductor substrate 30A in the sputtering process was changed, and the other parameters were kept the same as in Example 3. Using multiple composite substrates 110 each manufactured in this manner, the relationship between the thickness and bonding strength of the bonding layer 33 in the support substrate 30 was measured.
[0083] Fig. 11 is a table showing the relationship between the FAB irradiation time, the thickness of the bonding layer 33, and the bonding strength in the composite substrate 110. The table in Fig. 11 shows the FAB irradiation time to the semiconductor substrate 30A in the activation step combined with the sputtering step, and the thickness and bonding strength of the bonding layer 33 of each composite substrate 110 produced when the FAB irradiation time to the functional substrate 10 and the semiconductor substrate 30A in the activation step is fixed at 15 seconds, and the FAB irradiation time to the semiconductor substrate 30A in the sputtering step is changed to 50 seconds, 90 seconds, 195 seconds, 285 seconds, and 585 seconds. The case where the FAB irradiation time in the sputtering step is set to 285 seconds corresponds to the above-mentioned Example 3.
[0084] From the table of FIG. 11, it can be seen that if the thickness of the bonding layer 33 is 0.3 nm or more, the bonding strength is 1 J / m 2 This shows that a sufficient bonding strength can be obtained. 2 In order to obtain such a bonding strength, a bonding layer thickness of at least about 2 nm was required, whereas in composite substrate 110 to which the present invention is applied, if bonding layer 33 has a thickness of 0.3 nm or more, it is possible to obtain a bonding strength equal to or greater than that of the composite substrate described in Patent Document 1. This is also true for the other composite substrates 100, 120, and 130.
[0085] From the viewpoints of shortening the manufacturing time in the sputtering process, miniaturizing the product, and the like, it is preferable to make the thickness of bonding layer 33 as thin as possible as long as sufficient bonding strength can be obtained in manufactured composite substrates 100 to 130. For example, if the maximum thickness of bonding layer 33 is 3 nm, the above results indicate that the thickness of bonding layer 33 in composite substrates 100 to 130 can be set to 0.3 nm or more and 3 nm or less.
[0086] (Relationship between FAB irradiation time and bonding strength in the activation process) Among the manufacturing parameters described in Examples 1 and 2, the FAB irradiation time of the functional substrate 10 in the activation process was changed, and the other parameters were kept the same as in Examples 1 and 2. Using multiple composite substrates 100 each produced with these parameters, the relationship between the thickness of the bonding layer 33 in the support substrate 30 and the bonding strength was measured.
[0087] Fig. 12 is a table showing the relationship between the FAB irradiation time to the functional substrate 10 and the semiconductor substrate 30A in the composite substrate 100 and the bonding strength. The table in Fig. 12 shows the FAB irradiation time to the semiconductor substrate 30A in the activation process combined with the sputtering process and the bonding strength of each composite substrate 100 produced when the FAB irradiation time to the functional substrate 10 and the semiconductor substrate 30A in the activation process is changed to 15 seconds, 30 seconds, 300 seconds, and 510 seconds, and the FAB irradiation time to the semiconductor substrate 30A in the sputtering process is fixed to 90 seconds. The cases where the FAB irradiation time in the sputtering process is set to 15 seconds and 30 seconds correspond to the above-mentioned Example 1 and Example 2, respectively.
[0088] From the table in FIG. 12, if the FAB irradiation time in the activation process is 300 seconds or less, the bonding strength is 1 J / m 2 On the other hand, it can be seen that the bonding strength decreases when the FAB irradiation time in the activation step exceeds 300 seconds. This is thought to be because the longer the FAB irradiation time of the functional substrate 10 in the activation step, the greater the surface roughness of the functional substrate 10 becomes, and when this surface roughness exceeds a certain level, it leads to a decrease in the bonding strength.
[0089] 11 and 12 are merely examples. These values may vary depending on the types of functional and semiconductor materials used in the functional substrate 10 and the semiconductor substrate 30A, the voltage and current of the FAB, the rare gas flow rate, etc. Therefore, instead of adjusting the FAB irradiation time, it is also possible to form the bonding layer 33 with a desired thickness by adjusting the voltage, current, rare gas flow rate, etc. of the FAB.
[0090] According to the embodiment of the present invention described above, the following advantageous effects are achieved.
[0091] (1) Composite substrates 100 to 130 each include a functional substrate 10 made of a functional material, and a support substrate 30 made of a semiconductor material and bonded to the functional substrate 10 to support the functional substrate 10. The functional substrate 10 includes a first layer (first functional layer 11 or first insulating layer 21) and a second layer (second functional layer 12 or second insulating layer 22) made of an amorphous body containing a rare gas and disposed closer to the support substrate 30 than the first layer. The support substrate 30 includes a first support layer 31, a second support layer 32 made of an amorphous body of a semiconductor material containing a rare gas and disposed closer to the functional substrate 10 than the first support layer 31, and a bonding layer 33 made of an amorphous body of a semiconductor material and disposed in contact with the functional substrate 10. By doing this, it is possible to realize composite substrates 100-130 in which a functional substrate 10 and a supporting substrate 30 are bonded via a bonding layer 33, which can provide sufficient bonding strength even if the bonding layer 33 is thin.
[0092] (2) In the composite substrates 100, 120, the functional substrate 10 has a first functional layer 11 made of a crystalline body of a functional material, and a second functional layer 12 made of an amorphous body of the functional material and in contact with the bonding layer 33. In this configuration, the first layer is the first functional layer 11, and the second layer is the second functional layer 12. As a result, even when the functional substrate 10 and the support substrate 30 are directly bonded without the insulating layer 20 therebetween, the composite substrates 100, 120 can be realized that are capable of obtaining sufficient bonding strength.
[0093] (3) In the composite substrates 110 and 130, the functional substrate 10 is bonded to the support substrate 30 via the insulating layer 20 made of an insulating material, and the insulating layer 20 has a first insulating layer 21 made of an insulating material and a second insulating layer 22 made of an amorphous body of the insulating material and in contact with the bonding layer 33. In this configuration, the first layer is the first insulating layer 21, and the second layer is the second insulating layer 22. As a result, even when the functional substrate 10 and the support substrate 30 are bonded to each other via the insulating layer 20, the composite substrates 110 and 130 can be realized that are capable of obtaining sufficient bonding strength.
[0094] (4) The thickness of bonding layer 33 in composite substrates 100 to 130 is preferably 0.3 nm or more and 3 nm or less, which makes it possible to shorten the manufacturing time and reduce the product size while maintaining sufficient bonding strength.
[0095] 10(a) and 10(b), the bonding layer 33 contains a rare gas such as Ar, and the content of the rare gas in the bonding layer 33 is lower than the content of the rare gas in the second support layer 32. The bonding layer 33 may also contain a metal element such as Al. In this manner, the surface of the semiconductor substrate 30A is irradiated with FAB to bond the functional substrate 10 and the semiconductor substrate 30A together using the sputtered film 30B formed on the surface of the functional substrate 10 as the bonding layer 33, and the composite substrates 100 to 130 can be fabricated using the semiconductor substrate 30A as the support substrate 30.
[0096] (6) As shown in Fig. 10(a), the first functional layer 11 contains a rare gas such as Ar or does not contain a rare gas, and when the first functional layer 11 contains a rare gas, the content of the rare gas in the first functional layer 11 is less than the content of the rare gas in the second functional layer 12. Also, the content of the rare gas in the second functional layer 12 is less than the content of the rare gas in the second support layer 32. In this manner, the surface of the functional substrate 10 before bonding is activated by irradiating the surface of the functional substrate 10 with FAB, and then the functional substrate 10 and the semiconductor substrate 30A are bonded to produce the composite substrates 100, 120.
[0097] (7) As shown in Fig. 10(b), the first insulating layer 21 contains a rare gas such as Ar or does not contain a rare gas, and when the first insulating layer 21 contains a rare gas, the content of the rare gas in the first insulating layer 21 is less than the content of the rare gas in the second insulating layer 22. Also, the content of the rare gas in the second insulating layer 22 is less than the content of the rare gas in the second support layer 32. In this manner, the surface of the insulating layer 20 is activated by irradiating the surface of the functional substrate 10 before bonding on which the insulating layer 20 is formed with FAB, and then the insulating layer 20 and the semiconductor substrate 30A are bonded to produce the composite substrates 110, 130.
[0098] 10(a) and 10(b), the first support layer 31 contains a rare gas such as Ar or does not contain a rare gas, and when the first support layer 31 contains a rare gas, the content of the rare gas in the first support layer 31 is lower than the content of the rare gas in the second support layer 32. In this manner, the functional substrate 10 and the semiconductor substrate 30A are bonded after FAB irradiation is performed on the surface of the semiconductor substrate 30A, and the composite substrates 100 to 130 can be fabricated using the semiconductor substrate 30A as the support substrate 30.
[0099] (9) A method for manufacturing a composite substrate 100, 120 including a functional substrate 10 made of a functional material and a support substrate 30 made of a semiconductor material and supporting the functional substrate 10 includes an activation step (FIG. 2(b)) of irradiating the surface of the functional substrate 10 and the surface of a semiconductor substrate 30A made of a semiconductor material with FAB so that at least a part of the irradiation time of each of them overlaps, a sputtering step (FIG. 2(c)) that is performed following the activation step, in which after stopping the irradiation of the FAB on the surface of the functional substrate 10, the irradiation of the FAB on the surface of the semiconductor substrate 30A is continued to sputter the semiconductor material on the surface of the functional substrate 10, and a bonding step (FIG. 3(d)) of bonding the functional substrate 10 on which the semiconductor material has been sputtered by the sputtering step and the semiconductor substrate 30A to obtain a bonded body. In this way, the support substrate 30 is formed by integrating the semiconductor substrate 30A with the sputtered film 30B, and the composite substrate 100, 120 can be manufactured.
[0100] (10) A method for manufacturing a composite substrate 110, 130 including a functional substrate 10 made of a functional material and a support substrate 30 made of a semiconductor material and supporting the functional substrate 10 includes an insulating layer formation process (FIG. 5(b)) for forming an insulating layer 20 made of an insulating material on the surface of the functional substrate 10, an activation process (FIG. 5(c)) for irradiating the surface of the insulating layer 20 and the surface of a semiconductor substrate 30A made of a semiconductor material with FAB so that at least a part of the irradiation time of each of the insulating layer 20 and the semiconductor substrate 30A made of a semiconductor material overlap each other, a sputtering process (FIG. 5(d)) that is performed following the activation process, in which after stopping the irradiation of the FAB on the surface of the insulating layer 20, the irradiation of the FAB on the surface of the semiconductor substrate 30A is continued to sputter a semiconductor material onto the surface of the insulating layer 20, and a bonding process (FIG. 6(e)) for bonding the functional substrate 10 and the semiconductor substrate 30A via the insulating layer 20 onto which the semiconductor material has been sputtered by the sputtering process to obtain a bonded body. In this manner, the functional substrate 10 and the support substrate 30 can be bonded via the insulating layer 20 to produce the composite substrates 110, 130.
[0101] (11) In the sputtering steps of Fig. 2(c) and Fig. 5(d), it is preferable to form sputtered film 30B with a thickness of 0.3 nm or more and 3 nm or less. In this way, composite substrates 100-130 can be produced that maintain sufficient bonding strength while shortening the manufacturing time and enabling the product to be made more compact.
[0102] (12) The functional substrate 10 and the semiconductor substrate 30A may be placed in a vacuum chamber in which a first fabrication gun and a second fabrication gun are installed. In the activation step of FIG. 2(b) and FIG. 5(c), a rare gas such as Ar may be supplied to the first fabrication gun and the second fabrication gun, respectively, and the rare gas may be irradiated from the first fabrication gun to the surface of the functional substrate 10 or the insulating layer 20, and the rare gas may be irradiated from the second fabrication gun to the surface of the semiconductor substrate 30A. In addition, in the sputtering step of FIG. 2(c) and FIG. 5(d), the irradiation of the fabrication gas from the first fabrication gun to the surface of the functional substrate 10 or the insulating layer 20 may be stopped while the supply of the rare gas to the first fabrication gun is continued. In this way, the activation step may be appropriately performed on the functional substrate 10 and the semiconductor substrate 30A, and the sputtering step may be appropriately performed on the semiconductor substrate 30A, and as a result, the composite substrates 100 to 130 may be manufactured.
[0103] In each embodiment of the present invention described above, the first FAB gun irradiates the surface of the functional substrate 10 or the insulating layer 20 with FAB, and the second FAB gun irradiates the surface of the semiconductor substrate 30A with FAB simultaneously. This makes it possible to prevent impurities such as an oxide film formed on the surface of the semiconductor substrate 30A from adhering to the surface of the functional substrate 10 or the insulating layer 20. However, the present invention is not limited to this. For example, a method may be adopted in which the first FAB gun starts FAB irradiation on the functional substrate 10 side first, the second FAB gun starts FAB irradiation on the semiconductor substrate 30A side with a delay of a predetermined time, and then the FAB irradiation on the functional substrate 10 side is stopped first. In this way, the same effect as described above can be obtained.
[0104] The present invention is not limited to the above-described embodiment, and can be implemented using any components without departing from the spirit of the present invention.
[0105] The above-mentioned embodiments and modifications are merely examples, and the present invention is not limited to these contents as long as the characteristics of the invention are not impaired. In addition, although various embodiments and modifications have been described above, the present invention is not limited to these contents. Other aspects that are conceivable within the scope of the technical idea of the present invention are also included in the scope of the present invention. [Explanation of symbols]
[0106] 10: Functional substrate 11: 1st functional layer 12:Second functional layer 20: Insulating layer 21: First insulating layer 22: Second insulating layer 30: Support substrate 30A: Semiconductor substrate 30B: Sputtered film 31: 1st support layer 32:Second support layer 33: Bonding layer 40: Bonding interface 50: Ridge 100, 110, 120, 130: Composite board
Claims
1. A functional substrate made of a functional material; a support substrate made of a semiconductor material and bonded to the functional substrate to support the functional substrate; the functional substrate includes a first functional layer made of a crystal of the functional material, and a second functional layer arranged closer to the support substrate than the first functional layer and made of an amorphous body of the functional material containing a rare gas; the support substrate includes a first support layer, a second support layer disposed closer to the functional substrate than the first support layer and made of an amorphous body of the semiconductor material containing the rare gas, and a bonding layer in contact with the functional substrate and made of an amorphous body of the semiconductor material; the bonding layer contains the rare gas; A composite substrate, wherein the bonding layer has a lower content of the rare gas than the second support layer.
2. A functional substrate made of a functional material; a support substrate made of a semiconductor material and bonded to the functional substrate to support the functional substrate; the functional substrate is bonded to the support substrate via an insulating layer made of an insulating material; the support substrate includes a first support layer, a second support layer that is disposed closer to the functional substrate than the first support layer and is made of an amorphous body of the semiconductor material containing a rare gas, and a bonding layer that is in contact with the insulating layer and is made of an amorphous body of the semiconductor material; the insulating layer includes a first insulating layer made of the insulating material, and a second insulating layer made of an amorphous body of the insulating material and in contact with the bonding layer; the bonding layer contains the rare gas; A composite substrate, wherein the bonding layer has a lower content of the rare gas than the second support layer.
3. The composite substrate according to claim 1 or 2, The thickness of the bonding layer is 0.3 nm or more and 3 nm or less.
4. The composite substrate according to claim 1 or 2, The bonding layer comprises a metal element.
5. 2. The composite substrate according to claim 1 , the first functional layer contains the rare gas or does not contain the rare gas; A composite substrate, wherein when the first functional layer contains the rare gas, the content of the rare gas in the first functional layer is lower than the content of the rare gas in the second functional layer.
6. The composite substrate according to claim 5 , A composite substrate, wherein the content of the rare gas in the second functional layer is lower than the content of the rare gas in the second support layer.
7. The composite substrate according to claim 2, the first insulating layer contains the rare gas or does not contain the rare gas; A composite substrate, wherein when the first insulating layer contains the rare gas, the content of the rare gas in the first insulating layer is lower than the content of the rare gas in the second insulating layer.
8. The composite substrate according to claim 7, A composite substrate, wherein the content of the rare gas in the second insulating layer is less than the content of the rare gas in the second support layer.
9. The composite substrate according to claim 1 or 2, the first support layer contains the rare gas or does not contain the rare gas; A composite substrate, wherein when the first support layer contains the rare gas, the content of the rare gas in the first support layer is lower than the content of the rare gas in the second support layer.
10. A method for manufacturing a composite substrate including a functional substrate made of a functional material and a support substrate made of a semiconductor material and supporting the functional substrate, comprising: an activation step of irradiating a surface of the functional substrate and a surface of a semiconductor substrate made of the semiconductor material with a fast atomic beam so that the irradiation times of the fast atomic beams overlap at least partially; a sputtering step, which is carried out following the activation step, in which, after stopping the irradiation of the surface of the functional substrate with the fast atomic beam, the irradiation of the surface of the semiconductor substrate with the fast atomic beam is continued to sputter the semiconductor material onto the surface of the functional substrate; a bonding step of bonding the functional substrate on which the semiconductor material has been sputtered in the sputtering step to the semiconductor substrate to obtain a bonded body.
11. A method for manufacturing a composite substrate including a functional substrate made of a functional material and a support substrate made of a semiconductor material and supporting the functional substrate, comprising: an insulating layer forming step of forming an insulating layer made of an insulating material on a surface of the functional substrate; an activation step of irradiating a surface of the insulating layer and a surface of a semiconductor substrate made of the semiconductor material with a fast atomic beam so that the irradiation times of the fast atomic beams overlap at least partially; a sputtering step, which is carried out following the activation step, in which, after stopping the irradiation of the surface of the insulating layer with the fast atomic beam, the irradiation of the surface of the semiconductor substrate with the fast atomic beam is continued to sputter the semiconductor material onto the surface of the insulating layer; a bonding step of bonding the functional substrate and the semiconductor substrate via the insulating layer on which the semiconductor material is sputtered in the sputtering step to obtain a bonded body.
12. The method for producing a composite substrate according to claim 10, In the sputtering step, a sputtered film made of an amorphous body of the sputtered semiconductor material is formed on the surface of the functional substrate to a thickness of 0.3 nm or more and 3 nm or less.
13. The method for producing a composite substrate according to claim 11, In the sputtering step, a sputtered film made of an amorphous body of the sputtered semiconductor material is formed on the surface of the insulating layer to a thickness of 0.3 nm or more and 3 nm or less.
14. The method for producing a composite substrate according to claim 10, the functional substrate and the semiconductor substrate are placed in a vacuum chamber in which a first high-speed atom beam gun and a second high-speed atom beam gun are installed; In the activation step, a rare gas is supplied to each of the first high-speed atom beam gun and the second high-speed atom beam gun, and the high-speed atomic beam of the rare gas is irradiated from the first high-speed atom beam gun onto the surface of the functional substrate, and is irradiated from the second high-speed atom beam gun onto the surface of the semiconductor substrate; a first high-speed atomic beam gun that is adapted to supply a rare gas to the first high-speed atomic beam gun and a second high-speed atomic beam gun that is adapted to supply a rare gas to the first high-speed atomic beam gun;
15. The method for producing a composite substrate according to claim 11, the functional substrate and the semiconductor substrate are placed in a vacuum chamber in which a first high-speed atom beam gun and a second high-speed atom beam gun are installed; In the activation step, a rare gas is supplied to each of the first high-speed atom beam gun and the second high-speed atom beam gun, and the high-speed atom beam generated by the rare gas is irradiated onto the surface of the insulating layer from the first high-speed atom beam gun and onto the surface of the semiconductor substrate from the second high-speed atom beam gun; a first high-speed atom beam gun that is adapted to supply a rare gas to the first high-speed atom beam gun and a second high-speed atom beam gun that is adapted to supply a rare gas to the first high-speed atom beam gun;
16. The method for producing a composite substrate according to claim 14, a first high-speed atomic beam gun for irradiating a surface of the functional substrate with the high-speed atomic beam, and a second high-speed atomic beam gun for irradiating a surface of the semiconductor substrate with the high-speed atomic beam, the second high-speed atomic beam gun for irradiating a surface of the functional substrate with the high-speed atomic beam, the second high-speed atomic beam gun for irradiating a surface of the semiconductor substrate with the high-speed atomic beam,
17. 16. The method for producing a composite substrate according to claim 15, a first high-speed atom beam gun for irradiating a surface of the insulating layer with the high-speed atomic beam and a second high-speed atom beam gun for irradiating a surface of the semiconductor substrate with the high-speed atomic beam, the second high-speed atom beam gun being capable of irradiating the surface of the insulating layer with the high-speed atomic beam.
Citation Information
Patent Citations
Method of manufacturing surface acoustic wave element
JP2004343359A
Junction board, surface acoustic wave element, and surface acoustic wave device
JP2005252550A
Composite substrate, and method for manufacturing composite substrate
JP2017139720A
Manufacturing method of joint substrate and joint substrate
JP2019217530A
Bonded body of piezoelectric material substrate and supporting substrate
JP2020102856A