Laminate and manufacturing method thereof

A laminate structure with sealed pinholes using nickel and gold plating layers, combined with a nickel fluoride coating, addresses the inadequacies of existing corrosion-resistant methods, providing superior protection against corrosive gases in semiconductor manufacturing equipment.

JP7567797B2Active Publication Date: 2024-10-16RESONAC CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021545174
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-13
Filing Date
2020-08-11
Publication Date
2024-10-16
Estimated Expiration
2040-08-11

AI Technical Summary

Technical Problem

Existing methods for improving corrosion resistance in semiconductor manufacturing equipment components, such as nickel-phosphorus alloy plating and gold plating, are insufficient in preventing corrosion due to pinholes and do not provide adequate protection against corrosive gases like hydrogen chloride and hydrogen fluoride.

Method used

A laminate structure comprising a metal base material with a first nickel-containing plating layer, a gold plating layer, a second nickel-containing plating layer, and a nickel fluoride coating layer, where pinholes are sealed with nickel and gold, and the laminate is treated under specific conditions to enhance corrosion resistance.

Benefits of technology

The laminate exhibits excellent corrosion resistance, particularly against acids, effectively preventing corrosion in semiconductor manufacturing environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567797000002
    Figure 0007567797000002
  • Figure 0007567797000001
    Figure 0007567797000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a metal material that is applicable to a constituent member of a semiconductor production device and has excellent corrosion resistance, and in particular, corrosion resistance with respect to acids. The layered body according to the present invention comprises a metal base material, a first nickel-containing plating coat layer formed over the metal base material, a gold plating coat layer formed over the first nickel-containing plating coat layer, a second nickel-containing plating coat layer formed over the gold plating coat layer, and a nickel fluoride coat layer formed over the second nickel-containing plating coat layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and a manufacturing method thereof, and more particularly to a laminate suitable as a component of a semiconductor manufacturing device or the like and a manufacturing method thereof. [Background technology]

[0002] Conventionally, in the semiconductor manufacturing process, highly reactive and corrosive special gases (hereinafter also referred to as "corrosive gases") containing halogens such as fluorine, hydrogen chloride, boron trichloride, nitrogen trifluoride, chlorine trifluoride, and hydrogen bromide have been used in the dry etching process and cleaning of manufacturing equipment.

[0003] However, when the corrosive gas reacts with moisture in the atmosphere and undergoes hydrolysis, products such as hydrogen fluoride, oxalic acid, and hydrogen chloride are generated, which are problematic because they easily corrode the metal surfaces of components such as valves, joints, piping, and reaction chambers when the corrosive gas is used.

[0004] In the past, in order to improve corrosion resistance, a method has been used in which a metal substrate is plated with a nickel-phosphorus alloy to form a nickel fluoride passivation film (see, for example, Patent Documents 1 to 3), but these methods were sometimes insufficient.

[0005] Furthermore, pinholes on the plating surface can also be a cause of accelerating corrosion. There are several possible causes for pinholes, such as hydrogen gas generated by the plating reaction forming bubbles during the formation of the plating film and inhibiting film formation, or impurities (oxide film, dirt, oil, etc.) remaining on the substrate are not removed in the pretreatment process and inhibit film formation. In response to this, Patent Document 4 discloses a method in which a hard alloy plating layer is formed on the gold plating, improving wear resistance and preventing discoloration and corrosion due to oxidation, sulfurization, etc. caused by gas and moisture. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 2954716 [Patent Document 2] Patent No. 3094000 [Patent Document 3] JP 2004-360066 A [Patent Document 4] Patent No. 2581021 Summary of the Invention [Problem to be solved by the invention]

[0007] According to the study by the present inventors, it was found that in the method of forming a nickel fluoride passivation film on the surface of nickel-phosphorus alloy plating as in Patent Documents 1 to 3, corrosion originating from pinholes in the nickel-phosphorus alloy plating occurs, and hydrochloric acid corrosion resistance may be insufficient. In addition, the method of Patent Document 4 has a problem that a significant improvement in corrosion resistance cannot be expected because the outermost surface layer is an alloy plating.

[0008] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a metal material that can be used as a component part of a semiconductor manufacturing device and that has excellent corrosion resistance, particularly corrosion resistance to acids. [Means for solving the problem]

[0009] The present invention relates to, for example, the following [1] to

[14] . [1] A laminate having a metal substrate, a first nickel-containing plating film layer formed on the metal substrate, a gold plating film layer formed on the first nickel-containing plating film layer, a second nickel-containing plating film layer formed on the gold plating film layer, and a nickel fluoride coating layer formed on the second nickel-containing plating film layer.

[0010] [2] The laminate according to [1], wherein pinholes in the gold plating film layer are sealed with nickel metal, and pinholes in the first and second nickel-containing plating film layers are sealed with gold metal. [3] The laminate according to [1] or [2], wherein the metal substrate comprises at least one metal selected from the group consisting of stainless steel, iron, aluminum, an aluminum alloy, copper, and a copper alloy.

[0011] [4] The laminate according to any one of [1] to [3], further comprising a nickel strike layer between the metal substrate and the first nickel-containing plating film layer, and between the gold plating film layer and the second nickel-containing plating film layer. [5] The laminate according to any one of [1] to [4], wherein the first nickel-containing plating film layer comprises a nickel-phosphorus alloy plating layer having a phosphorus concentration of 8 mass% or more and less than 10 mass%, and the second nickel-containing plating film layer comprises a nickel-phosphorus alloy plating layer having a phosphorus concentration of 10 mass% or more and 12 mass% or less.

[0012] [6] The laminate according to any one of [1] to [5], wherein the gold plating film layer comprises a displacement type gold plating film layer and a reduction type gold plating film layer, in this order from the first nickel-containing plating film layer side. [7] The laminate according to any one of the above [1] to [6], wherein the nickel fluoride coating layer has a thickness of 70 nm or more.

[0013] [8] A method for producing a laminate, comprising: a step (A) of forming a first nickel-containing plating film layer on a metal substrate; a step (B) of forming a gold plating film layer on the first nickel-containing plating film layer; a step (C) of forming a second nickel-containing plating film layer on the gold plating film layer; and a step (D) of forming a nickel fluoride film layer on the second nickel-containing plating film layer.

[0014] [9] The method for producing the laminate according to [8] above, further comprising a step (X) between the steps (C) and (D), of heat-treating the laminate obtained in the step (C) at a temperature of 250°C or higher to seal pinholes in the gold plating film layer with nickel elemental metal and to seal pinholes in the first and second nickel-containing plating film layers with gold elemental metal.

[0015]

[10] The method for producing a laminate according to [8] or [9] above, wherein the step (D) is carried out in an atmosphere having a fluorine gas concentration of 8 vol % or more and a temperature of 250° C. or more.

[11] Before the step (A) and before the step (C), a current density of 3 to 20 A / dm is applied to the metal substrate. 2 The method for producing a laminate according to any one of the above [8] to

[10] , comprising a step of carrying out nickel strike treatment under the conditions of:

[0016]

[12] The method for producing a laminate according to any one of [8] to

[11] above, wherein the step (A) includes a step of forming a nickel-phosphorus alloy plating layer having a phosphorus concentration of 8 mass% or more and less than 10 mass%, and the step (C) includes a step of forming a nickel-phosphorus alloy plating layer having a phosphorus concentration of 10 mass% or more and 12 mass% or less.

[0017]

[13] The method for producing a laminate according to any one of the items [8] to

[12] , wherein the step (B) comprises a step (b1) of forming a displacement gold plating film layer and, following the step (b1), a step (b2) of forming a reduction gold plating film layer.

[14] A component of a semiconductor manufacturing device, comprising the laminate according to any one of [1] to [7] above. Effect of the Invention

[0018] According to the present invention, it is possible to provide a laminate having excellent corrosion resistance, particularly corrosion resistance against acids. [Brief description of the drawings]

[0019] [Figure 1]FIG. 2 is a schematic diagram showing a laminate before and after a pore-sealing treatment ((a): before pore-sealing treatment, (b): after pore-sealing treatment). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, one embodiment of the present invention will be specifically described. A laminate according to one embodiment of the present invention has a metal substrate, a first nickel-containing plating film layer formed on the metal substrate, a gold plating film layer formed on the first nickel-containing plating film layer, a second nickel-containing plating film layer formed on the gold plating film layer, and a nickel fluoride film layer formed on the second nickel-containing plating film layer.

[0021] In addition, in the laminate of one embodiment of the present invention, it is preferable that pinholes in the gold plating film layer are sealed with a metal consisting of nickel alone, and that pinholes in the first and second nickel-containing plating film layers are sealed with a metal consisting of gold alone.

[0022] A method for producing a laminate according to one embodiment of the present invention includes the steps of: (A) forming a first nickel-containing plating film layer on a metal substrate; (B) forming a gold plating film layer on the first nickel-containing plating film layer; (C) forming a second nickel-containing plating film layer on the gold plating film layer; and (D) forming a nickel fluoride film layer on the second nickel-containing plating film layer.

[0023] In addition, the method for producing a laminate according to one embodiment of the present invention preferably includes, between steps (C) and (D), a step (X) of heat-treating the laminate obtained in step (C) at a temperature of 250° C. or more for 2 hours or more to seal pinholes in the gold plating film layer with elemental nickel metal and to seal pinholes in the first and second nickel-containing plating film layers with elemental gold metal.

[0024] [Metal base material] The metal substrate used in one embodiment of the present invention is a substrate having at least a surface made of metal. The metal substrate is not particularly limited, and examples thereof include metals commonly used in components of semiconductor manufacturing equipment, and are preferably stainless steel, iron, aluminum, aluminum alloys, copper, and copper alloys.

[0025] In order to strengthen the adhesion of the metal substrate to the nickel-containing plating layer, the metal substrate may be subjected to a treatment appropriate to the substrate, such as degreasing, acid washing, or nickel strike treatment, as a pretreatment for step (A). The nickel strike treatment is a preliminary plating treatment using a nickel-containing plating bath, and the current density in the nickel strike treatment is preferably 3 to 20 A / dm 2 , more preferably 6 to 10 A / dm 2 The time for the nickel strike treatment is preferably 1 minute or more and 5 minutes or less.

[0026] [First nickel-containing plating layer] The first nickel-containing plating layer is formed on the metal substrate by step (A). When the metal substrate is subjected to a nickel strike treatment, a nickel strike layer is formed between the metal substrate and the first nickel plating layer.

[0027] From the viewpoint of improving corrosion resistance, the nickel-containing plating coating layer preferably contains phosphorus, and preferably includes a nickel-phosphorus alloy plating layer having a phosphorus concentration of 8 mass % or more and less than 10 mass %.

[0028] The nickel content in the first nickel-containing plating film layer is preferably 80 mass% or more, more preferably 85 to 95 mass%, and particularly preferably 90 to 92 mass%, when the entire nickel-containing plating film layer is taken as 100 mass%. By having the nickel content in the above range, the ratio of phosphorus in the film layer increases, and excellent corrosion resistance can be exhibited.

[0029] <Process (A)> The first nickel-containing plating layer can be formed on the metal substrate using an electroless plating bath containing a nickel salt and a phosphorus compound as a reducing agent. Examples of the nickel salt include nickel sulfate, nickel chloride, nickel acetate, and nickel carbonate. Examples of the phosphorus compound include sodium hypophosphite and potassium hypophosphite.

[0030] The deposition rate of the first nickel-phosphorus alloy plating layer is preferably 20 to 30 μm / h (hour), more preferably 22 to 25 μm / h (hour). The thickness of the first nickel-phosphorus-containing plating film layer is preferably 5 μm or more, more preferably 7 to 25 μm, and even more preferably 9 to 20 μm from the viewpoints of film performance in which pinholes are unlikely to occur and cost.

[0031] [Gold plating layer] A gold plating layer is formed on the nickel-containing plating layer by step (B). The gold content in the gold plating film is preferably 90% by mass or more, more preferably 99% by mass or more, and particularly preferably 99.9% by mass or more, when the entire gold plating film layer is taken as 100% by mass. The gold content in the above range stabilizes the corrosion resistance of the laminate of the present invention. The gold content is determined by an impurity determination method, that is, the gold plating is dissolved in aqua regia and measured by atomic absorption spectrometry and inductively coupled plasma (ICP) atomic emission spectrometry.

[0032] The thickness of the gold plating film is preferably 0.1 μm to 2 μm, more preferably 0.2 to 1.5 μm, and particularly preferably 0.3 to 0.8 μm, from the viewpoints of film performance such that pinholes are unlikely to occur and cost. It is known from the prior art that the thicker the precious metal plating film, the fewer the pinholes will occur, and high corrosion resistance is expected, but the cost is high, so it is preferable to set the thickness at an appropriate level.

[0033] <Process (B)> The method for forming the gold plating film layer is not particularly limited, but electroless gold plating is preferred. In the electroless gold plating method, it is preferable to perform displacement gold plating followed by reduction gold plating. That is, the step (B) preferably includes a step (b1) of forming a displacement gold plating film layer and a step (b2) of forming a reduction gold plating film layer after the step (b1).

[0034] In substitution gold plating, nickel dissolves from the nickel coating, and the gold ions in the solution are reduced by the electrons released during the process, depositing a gold plating film.In reduction gold plating, gold ions in the solution are reduced by electrons released during the oxidation reaction of a reducing agent, depositing a gold plating film.

[0035] Examples of electroless gold plating solutions include plating baths containing potassium gold cyanide, gold chloride, gold sulfite, gold thiosulfate, etc., and examples of reducing agents include sodium hydroxide, dimethylamine borane, hexamethylenetetramine, and chain polyamines having an alkyl group with three or more carbon atoms and multiple amino groups.

[0036] A gold plating film layer can be formed by carrying out displacement gold plating preferably at 50 to 90°C for 3 to 7 minutes, more preferably at 65 to 75°C for 3 to 7 minutes, and reduction gold plating preferably at 55 to 65°C for 7 to 15 minutes, more preferably at 58 to 62°C for 7 to 15 minutes.

[0037] [Second nickel-containing plating layer] The second nickel-containing plating layer is formed on the gold plating layer by step (C). When the gold plating layer is subjected to a nickel strike treatment, a nickel strike layer is formed between the gold plating layer and the second nickel plating layer.

[0038] From the viewpoint of improving corrosion resistance, the nickel-containing plating film layer preferably contains phosphorus, and preferably includes a nickel-phosphorus alloy plating layer having a phosphorus concentration of 10 mass % or more and 12 mass % or less.

[0039] The nickel content in the second nickel-containing plating film layer is preferably 80% by mass or more, more preferably 85 to 95% by mass, and particularly preferably 90 to 92% by mass, when the entire nickel-containing plating film layer is taken as 100% by mass. By having the nickel content in the above range, the ratio of phosphorus in the film layer increases, and excellent corrosion resistance can be exhibited. In addition, when electroless nickel-phosphorus alloy plating films with different phosphorus concentrations are laminated, pinhole defects are formed at different positions during film formation, so that disturbances are less likely to reach the substrate directly, and improvement in corrosion resistance can be expected.

[0040] <Process (C)> The second nickel-containing plating layer can be formed on the metal substrate using an electroless plating bath containing a nickel salt and a phosphorus compound as a reducing agent. Examples of the nickel salt include nickel sulfate, nickel chloride, nickel acetate, and nickel carbonate. Examples of the phosphorus compound include sodium hypophosphite and potassium hypophosphite.

[0041] The deposition rate of the second nickel-phosphorus alloy plating layer is preferably 10 to 15 μm / h (hour), more preferably 11 to 13 μm / h (hour). The thickness of the second nickel-phosphorus alloy plating film layer is preferably 5 μm or more, more preferably 7 to 25 μm, and even more preferably 10 to 20 μm from the viewpoints of film performance in which pinholes are unlikely to occur and cost.

[0042] [Sealing treatment] The sealing treatment is performed by sealing pinholes in the gold plating film layer with a metal consisting of nickel alone, and sealing pinholes in the first and second nickel-containing plating film layers with a metal consisting of gold alone.

[0043] <Process (X)> In step (X), between step (C) and step (D) described below, the laminate obtained in step (C) is heat-treated, whereby metal is thermally diffused to seal pinholes in the gold plating layer with elemental nickel metal, and to seal pinholes in the first and second nickel-containing plating layers with elemental gold metal. The presence of elemental gold and nickel can be confirmed by energy dispersive X-ray analysis (EDS). The heating conditions are preferably 250° C. or higher for 2 hours or longer, and more preferably 300 to 350° C. for 2 to 6 hours.

[0044] [Nickel fluoride coating layer] A nickel fluoride coating layer is formed on the second nickel-containing plating layer. The nickel fluoride coating layer is a passive coating. By subjecting the surface of the second nickel-containing plating layer to a fluorination treatment in step (D), a nickel fluoride coating layer is formed as a passive coating on the nickel-containing plating layer.

[0045] The thickness of the nickel fluoride coating layer is preferably 70 nm or more, more preferably 80 to 200 nm, and even more preferably 100 to 150 nm. When the nickel fluoride coating layer has a thickness within the above range, the adhesion between the gold plating layer and the second nickel-containing plating layer is improved.

[0046] <Process (D)> In step (D), after steps (A) to (C) and, if necessary, step (X), the surface of the nickel-containing plating film layer is fluorinated with fluorine gas to form a nickel fluoride film layer.

[0047] Step (D) is carried out in an atmosphere with a fluorine gas concentration of preferably 8% by volume or more, more preferably 10% by volume or more. The film formation temperature is preferably 250°C or more, more preferably 300°C or more. The fluorination treatment time is preferably 2 hours or more. Examples of the gas that is accompanied by the fluorine gas include inert gases such as nitrogen gas. In one embodiment of the present invention, a thick fluoride passivation film made of nickel fluoride is obtained under the above reaction conditions, but the thickness of the nickel fluoride coating can be adjusted arbitrarily by adjusting the thickness of the nickel alloy plating film, the reaction temperature, and the reaction time depending on the intended use of the member. The above reaction temperature means the temperature measured by a thermocouple in the gas atmosphere in the reaction furnace. EXAMPLES

[0048] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. The thickness of each layer of the laminate (except for the nickel fluoride coating layer) was calculated from the weight increase, layer area, and known density. The thickness of the nickel fluoride coating layer was calculated by X-ray photoelectron spectroscopy (XPS) using the method described below.

[0049] [Example 1] <Process (A)> The surface of stainless steel (SUS316L) was subjected to degreasing, acid washing, and nickel strike treatment as pretreatment. An electroless nickel-phosphorus plating agent "Nimden (trademark) NSX" (manufactured by Uemura Kogyo Co., Ltd.) was used on the surface of the stainless steel that had been subjected to the nickel strike treatment to form a first nickel-containing plating film layer (film thickness: 10 μm) having a phosphorus content of 8 mass% or more and less than 10 mass% at the time of film formation, at a plating temperature of 90°C, pH 4.5 to 4.8, and for a plating time of 25 minutes.

[0050] <Process (B)> Two types of electroless gold plating solutions, "Flash Gold NC (substitution type)" and "Self Gold OTK-IT (reduction type)" (both manufactured by Okuno Chemical Industries Co., Ltd.), were used in that order to treat the first nickel-containing plating film layer formed in process (A) at a substitution plating temperature of 70°C for 5 minutes and then at a reduction plating temperature of 60°C for 10 minutes, in that order, to form a gold plating film layer with a total thickness of 0.6 μm.

[0051] <Process (C)> The surface of the gold plating film layer formed in step (B) was subjected to a nickel strike treatment in the same manner as in step (A). An electroless nickel-phosphorus plating agent "Nimden (trademark) HDX" (manufactured by Uemura Kogyo Co., Ltd.) was used to form a second nickel-containing plating film layer (film thickness: 10 μm) having a phosphorus content of 10% by mass or more and 12% by mass or less at the time of film formation for a plating time of 50 minutes.

[0052] <Process (X)> The stainless steel having the first nickel-containing plating film layer, the gold plating film layer and the second nickel-containing plating film layer formed in steps (A), (B) and (C) was placed inside an atmospheric pressure gas-phase flow-type reactor, the temperature inside the reactor was raised to 300°C and maintained at that state for 2 hours.

[0053] After heating, the stainless steel was analyzed using energy dispersive X-ray analysis (EDS), which confirmed that the pinholes in the first and second nickel-containing plating layers had been sealed with elemental gold metal, and that the pinholes in the gold plating layer had been sealed with elemental nickel metal.

[0054] <Process (D)> After step (X), the atmosphere in the atmospheric gas-phase flow reactor was replaced with nitrogen gas, and then 100% by volume of oxygen gas was introduced to completely replace the nitrogen gas with oxygen gas, and this state was maintained for 12 hours. Next, the oxygen gas was replaced with nitrogen gas, and then 10% by volume of fluorine gas (the remaining 90% by volume was nitrogen gas) was introduced, and this state was maintained for 12 hours to form a nickel fluoride coating layer. Furthermore, nitrogen gas was circulated for 12 hours to stabilize the film formation. For the stainless steel having the nickel fluoride coating as the obtained outermost surface layer, the presence of nickel fluoride was confirmed from the F and Ni amount ratio detected by X-ray photoelectron spectroscopy (XPS). The thickness of the nickel fluoride coating was calculated from the sputtering time of F and Ni and the known sputtering rate of 2.4 nm / min (SiO2 equivalent), and was found to be 103 nm.

[0055] [Example 2] After carrying out step (A) in the same manner as in Example 1, a gold plating film layer having a thickness of 1.2 μm was formed in the same manner as in Example 1, except that the gold reduction plating treatment was changed to 20 minutes in step (B) of Example 1. Thereafter, steps (C), (X) and (D) were carried out in the same manner as in Example 1. The thickness of the nickel fluoride film was measured in the same manner as in Example 1 and was found to be 103 nm.

[0056] [Example 3] In Example 1, an aluminum alloy (A5052) was used instead of the stainless steel (SUS316L), and degreasing, activation, acid cleaning, and zinc replacement were performed as pretreatment. Thereafter, steps (A), (B), (C), (X), and (D) were performed in the same manner as in Example 1. The thickness of the nickel fluoride coating was determined in the same manner as in Example 1, and was found to be 103 nm. The activation was performed for 30 seconds at room temperature using a mixed acid of acidic ammonium fluoride and nitric acid as a treatment agent. The acid cleaning was performed for 25 seconds at room temperature using nitric acid as a cleaning agent. The zinc replacement was performed for 25 seconds at room temperature using a zincate bath as a treatment agent. The acid cleaning and zinc replacement were each performed twice under the above conditions.

[0057] [Comparative Example 1] The surface of stainless steel (SUS316L) was subjected to degreasing, acid cleaning, and nickel strike treatment as pretreatment. A first nickel-containing plating film layer having a phosphorus content of 8% by mass or more and less than 10% by mass at the time of film formation was formed on the surface of the stainless steel subjected to the nickel strike treatment at a plating temperature of 90°C and a pH of 4.5 to 4.8 at a film formation rate of 10 μm / 25 minutes using an electroless nickel-phosphorus plating agent "Nimden (trademark) NSX" (manufactured by Uemura Kogyo Co., Ltd.). Next, a second nickel-containing plating film layer having a phosphorus content of 10% by mass or more and less than 12% by mass at the time of film formation was formed at a film formation rate of 10 μm / 50 minutes using an electroless nickel-phosphorus plating agent "Nimden (trademark) HDX" (manufactured by Uemura Kogyo Co., Ltd.). As a result, a nickel-containing plating film layer having a total thickness of 20 μm was formed on the stainless steel subjected to the nickel strike treatment. Thereafter, step (D) was carried out in the same manner as in Example 1 to form a nickel-containing plating film layer and a nickel fluoride film layer on the surface of the stainless steel that had been subjected to the nickel strike treatment.

[0058] [Comparative Example 2] In Comparative Example 1, the metal substrate was changed from stainless steel (SUS316L) to an aluminum alloy (A5052), and the pretreatments included degreasing, activation, acid cleaning, and zinc substitution treatment. Then, an electroless nickel-phosphorus alloy plating layer and a nickel fluoride coating layer were formed in the same manner as in Comparative Example 1.

[0059] [Comparative Example 3] In Example 1, only steps (A), (B) and (C) were performed, i.e., steps (X) and (D) were not performed, and a first nickel-containing plating film layer, a gold plating film layer and a second nickel-containing plating film layer were formed on the stainless steel.

[0060] [evaluation] A hydrochloric acid corrosion resistance test was carried out on the coatings on the surfaces of the metal substrates obtained in the above Examples 1 to 3 and Comparative Examples 1 to 3. The evaluation results are shown in Table 1.

[0061] <Hydrochloric acid corrosion resistance test> A test piece measuring 15 mm in length, 15 mm in width, and 1 mm in thickness was immersed in a 35% by weight hydrochloric acid solution at 25°C for 5 hours. The mass loss [mg / dm 2 ] and the hydrochloric acid corrosion resistance was evaluated according to the following criteria. (Evaluation Criteria) A: 0.1 mg / dm 2 less than B: 0.1 mg / dm 2 More than 3.0 mg / dm 2 less than C: 3.0 mg / dm 2 More than 10.0 mg / dm 2 less than D: 10.0 mg / dm 2 End

[0062] [Table 1]

[0063] In Table 1, SUS stands for stainless steel (SUS316L) and Al stands for aluminum alloy (A5052). [Explanation of symbols]

[0064] 1...Metal base material 2. First nickel-containing plating layer 3. Gold plating layer 4. Second nickel-containing plating layer 5. Nickel fluoride coating layer 6. Pinhole 7. Area where pinholes have been sealed

Claims

1. A metal substrate; a first nickel-containing plating coating layer formed on the metal substrate; a gold plating film layer formed on the first nickel-containing plating film layer; a second nickel-containing plating layer formed on the gold plating layer; a nickel fluoride coating layer formed on the second nickel-containing plating layer, The pinholes in the gold plating layer are sealed with nickel metal, and A laminate, wherein pinholes in the first and second nickel-containing plating layers are sealed with elemental gold metal.

2. 2. The laminate of claim 1, wherein the metal substrate comprises at least one metal selected from the group consisting of stainless steel, iron, aluminum, an aluminum alloy, copper, and a copper alloy.

3. 3. The laminate according to claim 1, further comprising a nickel strike layer between the metal substrate and the first nickel-containing plating film layer and between the gold plating film layer and the second nickel-containing plating film layer.

4. The laminate according to any one of claims 1 to 3, wherein the first nickel-containing plating film layer comprises a nickel-phosphorus alloy plating layer having a phosphorus concentration of 8 mass% or more and less than 10 mass%, and the second nickel-containing plating film layer comprises a nickel-phosphorus alloy plating layer having a phosphorus concentration of 10 mass% or more and 12 mass% or less.

5. The laminate according to any one of claims 1 to 4, wherein the gold plating film layer comprises a substitution gold plating film layer and a reduction gold plating film layer in this order from the first nickel-containing plating film layer side.

6. The laminate according to any one of claims 1 to 5, wherein the nickel fluoride coating layer has a thickness of 70 nm or more.

7. A step (A) of forming a first nickel-containing plating film layer on a metal substrate; (B) forming a gold plating film layer on the first nickel-containing plating film layer; (C) forming a second nickel-containing plating layer on the gold plating layer; and A method for producing a laminate, comprising: (D) forming a nickel fluoride coating layer on the second nickel-containing plating layer, The method for producing a laminate includes a step (X) between the steps (C) and (D), in which the laminate obtained in the step (C) is heat-treated at a temperature of 250° C. or higher to seal pinholes in the gold plating film layer with nickel elemental metal and to seal pinholes in the first and second nickel-containing plating film layers with gold elemental metal.

8. The method for producing a laminate according to claim 7, wherein the step (D) is carried out in an atmosphere having a fluorine gas concentration of 8 vol % or more and a temperature of 250° C. or more.

9. Before the step (A) and before the step (C), a current density of 3 to 20 A / dm is applied to the metal substrate. 2 The method for producing a laminate according to claim 7 or 8, further comprising a step of performing nickel strike treatment under the conditions of

10. The step (A) includes a step of forming a nickel-phosphorus alloy plating layer having a phosphorus concentration of 8% by mass or more and less than 10% by mass, and The method for producing a laminate according to any one of claims 7 to 9, wherein the step (C) includes a step of forming a nickel-phosphorus alloy plating layer having a phosphorus concentration of 10 mass% or more and 12 mass% or less.

11. The method for producing a laminate according to any one of claims 7 to 10, wherein the step (B) comprises a step (b1) of forming a substitution gold plating film layer, and a step (b2) of forming a reduction gold plating film layer after the step (b1).

12. A component of a semiconductor manufacturing device, comprising the laminate according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for plating stainless steel with gold

    JP1994158384A

  • Highly corrosion resistant nickel-gold plating

    JP2001234360A

  • Corrosion resistant material, and its production method

    JP2004360066A

  • Metallic material with outermost surface layer of nickel fluoride film and method for producing the same

    JP2008056978A

  • Metalized substrate, and its manufacturing method

    JP2008311316A