Metal plate coating paint
A coating material with specific resin and wax properties enhances press formability and rust prevention, addressing the limitations of existing lubricating films by providing stable adhesion and film removability for metal plates.
Patent Information
- Application Number
- JP2022045023
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-14
- Filing Date
- 2022-03-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-03-22
AI Technical Summary
Existing lubricating films for metal plates during press forming, such as those described in Patent Documents 1 to 4, do not provide sufficient press formability for complex molding, and there is a need for improved lubricity, rust prevention, film removability, and adhesion during painting processes.
A coating material containing an acrylic resin with a glass transition point of 100°C or higher and a specific acid value to glass transition point ratio, combined with polyolefin wax of 100°C to 145°C melting point and 3.0 μm or less average particle size, along with additives for rust prevention and stability, is applied to metal plates.
The coating material achieves low sliding resistance, excellent press formability, good rust prevention, and film removability during alkaline degreasing, ensuring stable adhesion and paintability.
Smart Images

Figure 0007567841000003 
Figure 0007567841000004 
Figure 0007567841000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating material for application to metal sheets, and in particular to a coating material for application to metal sheets for obtaining a lubricating film having excellent sliding properties during press forming even during severe drawing. [Background technology]
[0002] Metal sheets such as cold-rolled steel sheets, hot-rolled steel sheets, stainless steel sheets, and aluminum sheets are widely used in a wide range of fields, mainly for automobile body applications, and in such applications, they are generally press-formed before use. In recent years, there has been a demand for the integration of parts to reduce processes and for improved design, and it is necessary to enable more complex forming.
[0003] If more complex press forming were to be performed, the metal plate could break due to being unable to withstand the forming, or die galling could occur during continuous press forming, which could have a serious adverse effect on automotive productivity.
[0004] One method for improving the press formability of metal sheets is surface treatment of the die. Although this method is widely used, the die cannot be adjusted after the surface treatment. Another problem is that the cost is high. Therefore, there is a strong demand for improving the press formability of the steel sheet itself.
[0005] One method to improve press formability without surface treatment of the die is to use a high viscosity lubricant, but this method can lead to poor degreasing after press forming, which can lead to poor paintability.
[0006] Therefore, various lubricating surface treatments have been investigated as a technique that enables press molding without using surface treatment of the mold or high-viscosity lubricating oil.
[0007] Patent Document 1 describes a technique for forming a lubricating film, which is an acrylic resin film containing synthetic resin powder, on a zinc-plated steel sheet.
[0008] Patent Document 2 describes a metal sheet coated with a lubricating film in which a solid lubricant protrudes from the surface of a resin film by 0.01 to 1.5 μm.
[0009] Patent Document 3 describes a lubricating surface-treated metal product having excellent press formability, which is coated with a 0.5 to 5 μm thick film made of polyurethane resin containing a lubricant.
[0010] Patent Document 4 describes a technique for forming an alkali-soluble organic film, which is an epoxy resin containing a lubricant added thereto, on a steel sheet. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 9-170059 [Patent Document 2] Japanese Patent Application Publication No. 10-52881 [Patent Document 3] JP 2000-309747 A [Patent Document 4] JP 2000-167981 A Summary of the Invention [Problem to be solved by the invention]
[0012] However, in Patent Documents 1 to 4, although lubricity is achieved by the lubricating effect of the lubricant contained therein, press formability is not necessarily sufficient in complex forming.
[0013] The present invention has been made in consideration of the above circumstances, and has an object to provide a paint for application to metal plates, which forms a coating film that has low sliding resistance in areas at risk of cracking during press forming, and has excellent press formability in areas where the surface pressure is high and mold galling is expected to occur, in metal plates that are subjected to complex forming that makes press forming difficult.
[0014] In addition, the metal sheet is required to have rust prevention properties when stored as a coil. Furthermore, when the metal sheet is used as an automobile body, it is required to have sufficient film removal properties in the alkaline degreasing step of the painting process, and further, it is required to have excellent adhesion properties in the assembly process. Furthermore, the paint is required to have stability to maintain the contained components in a uniformly dispersed state. [Means for solving the problem]
[0015] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by applying to a metal plate a coating material containing an acrylic resin having a glass transition point (Tg) of 100° C. or higher and a ratio R of the acid value to the glass transition point (R=acid value (mg-KOH / g) / Tg(° C.)) of 1.50 or higher, and a polyolefin wax having a melting point of 100° C. or higher and 145° C. or lower and an average particle size of 3.0 μm or less.
[0016] The present invention has been completed based on the above findings, and the gist of the present invention is as follows. [1] A paint for applying to metal sheets that contains an acrylic resin with a glass transition point (Tg) of 100°C or higher and a ratio of acid value to glass transition point (R = acid value (mg-KOH / g) / Tg (°C)) of 1.50 or higher, and a polyolefin wax with a melting point of 100°C or higher and 145°C or lower and an average particle size of 3.0 μm or less. [2] The coating material for applying to metal sheets according to [1], wherein the acid value of the acrylic resin is 180 mg-KOH / g or more and 350 mg-KOH / g or less. [3] The coating material for applying to metal sheets according to [1] or [2], wherein the ratio R of the acid value to the glass transition point of the acrylic resin is 2.05 or less. [4] A paint for application to metal sheets according to any one of [1] to [3], wherein, when the paint is dried, the proportion of the acrylic resin in the total solid content is 30% or more, and the proportion of the wax in the total solid content is 5% or more and 50% or less. [5] The coating material for applying to metal sheets according to any one of [1] to [4], wherein the acrylic resin has a mass average molecular weight of 5,000 or more and 30,000 or less. [6] The coating material for applying to metal sheets according to any one of [1] to [5], wherein the acrylic resin is a styrene-acrylic resin. [7] A coating material for applying to metal sheets according to any one of [1] to [6], which contains an anti-rust agent in an amount of 5% to 30% by mass of the total solid content of the coating material when the coating material is dried. [8] The coating material for applying to metal sheets according to any one of [1] to [7], wherein the rust inhibitor is at least one selected from the group consisting of aluminum salts of phosphoric acids, zinc salts, and zinc oxide. [9] The coating material for applying to metal sheets according to any one of [1] to [8], wherein the wax has an average particle size of 0.01 μm or more and 0.5 μm or less.
[10] The coating material for coating metal sheets according to any one of [1] to [9], which contains silica in an amount of 1% or more and 10% or less based on the total solid content when the coating material is dried. Effect of the Invention
[0017] According to the present invention, a metal plate having excellent press formability can be obtained by significantly reducing the coefficient of friction with a die or the like. Therefore, the metal plate has stable and excellent press formability for a metal plate subjected to complex forming. In addition, the stability of the paint is ensured, and the metal plate having the coating has good rust prevention properties. Furthermore, since the adhesive property is good, it is possible to use an adhesive in the same manner as a conventional metal plate, and since the coating can be easily removed by alkaline degreasing, the coating process is not hindered. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a schematic front view showing a friction coefficient measuring device. [Diagram 2] FIG. 2 is a schematic perspective view showing the shape and dimensions of the bead in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the present invention will be described.
[0020] The coating material for application to metal sheets of the present invention contains an acrylic resin having a glass transition point (Tg) of 100°C or higher and a ratio of acid value to glass transition point, R = acid value (mg-KOH / g) / Tg (°C), of 1.50 or higher, and a polyolefin wax having a melting point of 100°C or higher and 145°C or lower and an average particle size of 3.0 μm or less.
[0021] Hereinafter, the ratio of the acid value to the glass transition point, R=acid value (mg-KOH / g) / Tg (°C), will be expressed as R=acid value / Tg.
[0022] The glass transition point of the acrylic resin in the coating material for application to metal sheets of the present invention is set to 100°C or higher in order to obtain good lubricity. If the glass transition point is less than 100°C, the resin softens during sliding, reducing the wax retention and the ability to prevent direct contact between the metal sheet and the die, so good sliding properties cannot be obtained. The glass transition point is preferably 110°C or higher and 150°C or lower. If the glass transition point exceeds 150°C, the resin becomes too hard and brittle during sliding, and good lubricity may not be obtained.
[0023] The glass transition point here refers to the intermediate glass transition temperature measured based on JIS K 7121 "Method of measuring glass transition temperature of plastics."
[0024] The ratio R=acid value / Tg of the acid value and glass transition point of the acrylic resin is 1.50 or more. Even if the glass transition point is 100°C or more, if the acid value is low (R<1.50), excellent lubricity cannot be obtained. Although the cause is not clear, it is considered that the carboxyl group in the acrylic resin has a high affinity with the mold, and the wax in the film is transferred to the mold during sliding. When the acrylic resin component containing wax is transferred to the mold during sliding, the mold surface is protected by the wax, and the effect of preventing direct contact with the metal plate is enhanced, improving the sliding property. Therefore, when the acid value is low (R<1.50), the sliding property is poor due to a shortage of carboxyl groups. When the glass transition point of the acrylic resin increases, the resin becomes difficult to soften due to sliding, so it becomes difficult to transfer to the mold. Therefore, in order to obtain excellent sliding property when the glass transition point increases, the acid value must also be increased. That is, the ratio R=acid value / Tg of the acid value and glass transition point must be 1.50 or more. It is preferably 1.80 or more. Although there is no particular upper limit for R, it is preferable to set it to 2.05 or less, because if R exceeds 2.05, the rust prevention properties may deteriorate.
[0025] The acid value of the acrylic resin is preferably 180 mg-KOH / g or more and 350 mg-KOH / g or less. If it is less than 180 mg-KOH / g, the film may be poorly removable by alkali, and the adhesive strength may not be sufficient. If it exceeds 350 mg-KOH / g, the rust prevention properties may be deteriorated.
[0026] Here, the acid value refers to the number of milligrams of potassium hydroxide required to neutralize the carboxyl groups contained in 1 g of resin, and is measured based on JIS K 0070 "Testing methods for acid value, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products." In this specification, the unit is shown as mg-KOH / g.
[0027] The wax used in the present invention may be any polyolefin wax having a melting point of 100° C. or higher and 145° C. or lower and an average particle size of 3.0 μm or less.
[0028] The reason why polyolefin wax is used as the wax is that it has low surface energy and self-lubricating properties, which provides good lubrication. In addition, it is relatively easy to adjust the melting point of polyolefin to 100°C or higher and 145°C or lower by controlling the density and molecular weight.
[0029] When the melting point is 100°C or more and 145°C or less, in addition to the self-lubricating property of the polyolefin wax itself, the wax becomes semi-molten due to sliding during press molding, and the lubricating film component mixed with the organic resin can cover the mold surface, and excellent lubrication effect can be obtained by suppressing direct contact between the mold and the steel plate. When the melting point is less than 100°C, the wax completely melts due to frictional heat caused by sliding during press molding, and the wax itself does not provide sufficient lubrication effect, and the above-mentioned mold covering effect cannot be obtained. In addition, when the melting point exceeds 145°C, it does not melt during sliding, and sufficient lubrication effect cannot be obtained, and the mold covering effect cannot be obtained. Furthermore, it is preferable that the melting point is 120°C or more and 140°C or less.
[0030] The melting point of the wax herein refers to the melting temperature measured based on JIS K 7121 "Method of measuring transition temperature of plastics."
[0031] If the average particle size of the wax exceeds 3.0 μm, it becomes difficult to mix with the organic resin during sliding, and the above-mentioned coating effect of the mold cannot be obtained, and sufficient lubrication cannot be obtained. The average particle size of the wax is preferably 0.5 μm or less, and even more preferably 0.3 μm or less.
[0032] The average particle size of the wax is preferably 0.01 μm or more. If it is less than 0.01 μm, it will be easily dissolved in the lubricating oil during sliding, and may not exhibit sufficient lubrication improvement effect, and it will be easily aggregated in the paint for forming the film, so the paint stability is low. More preferably, it is 0.03 μm or more. Taking into consideration the mixability with the above acrylic resin, the average particle size is preferably 0.01 μm or more and 0.5 μm or less.
[0033] The average particle size is the median diameter of the volume average diameter, and can be determined by a laser diffraction / scattering method. For example, it can be determined by measuring a sample diluted with pure water using a laser diffraction / scattering type particle size distribution measuring device Partica LA-960V2 (manufactured by Horiba, Ltd.).
[0034] Among polyolefin waxes, polyethylene wax is preferred because it provides the greatest lubricating effect.
[0035] It is preferable that when the coating material for application to metal sheets of the present invention is dried, the proportion of the acrylic resin in the total solid content is 30% or more, and the proportion of the wax in the total solid content is 5% or more and 50% or less, in terms of mass proportion.
[0036] When the ratio of acrylic resin to the total solid content is 30% or more, the properties influenced by the physical properties of the acrylic resin component, such as the effect of improving lubrication due to transfer to the die during sliding, film removal, adhesion, etc., are fully obtained. When it is less than 30%, the influence of other components becomes large, and the target performance may not be obtained.
[0037] If the mass ratio of wax in the total solid content is less than 5%, sufficient lubrication effect may not be obtained. If it is 10% or more, a particularly good lubrication effect may be obtained. In addition, the mass ratio of wax in the total solid content is preferably 50% or less. If it exceeds 50%, the wax may easily fall off due to a shortage of base resin components, and the adhesion to the metal plate may be poor, and the wax may not exist stably as a film, resulting in poor adhesion. In addition, when used as an automobile body, sufficient degreasing may not be obtained in the alkaline degreasing step of the painting process, and the film may not be sufficiently removed in the alkaline degreasing step, resulting in deterioration of paintability. More preferably, it is 30% or less.
[0038] Here, the mass ratio of wax to the total solid content refers to the mass ratio of wax solid content to the mass of all solid content in the paint.
[0039] The mass average molecular weight of the acrylic resin is preferably from 5000 to 30000. If it is less than 5000, the rust prevention properties may be poor, and if it exceeds 30000, the adhesiveness may be deteriorated.
[0040] Here, the mass average molecular weight is the mass average molecular weight measured based on JIS K 7252 "Plastics - Determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography".
[0041] Furthermore, the acrylic resin is preferably a styrene-acrylic resin. By including styrene in the monomer of the resin, water resistance is improved, and rust prevention is improved. Furthermore, the effect of obtaining better sliding properties compared to a case where styrene is not included is also manifested.
[0042] The coating material for applying to metal sheets of the present invention preferably contains a rust inhibitor in a mass ratio of 5% to 30% of the total solid content. Even if the coating material does not contain a rust inhibitor, rust will not occur under normal storage conditions. However, if the content of the rust inhibitor is less than 5%, rust prevention is insufficient under unfavorable storage conditions, and rust may occur when a film is formed on the metal sheet. In particular, when the metal strip is stored in a coiled state under unfavorable storage conditions, it may absorb moisture and cause rust.
[0043] If the ratio of the rust inhibitor exceeds 30%, the adhesiveness may deteriorate, and the rust inhibitor may precipitate in the paint, causing deterioration of the paint stability. As the rust inhibitor, it is preferable to use at least one selected from the group consisting of aluminum salts of phosphoric acids, zinc salts, and zinc oxide. Here, phosphoric acids include orthophosphoric acid as well as condensed phosphoric acids such as pyrophosphoric acid, tripolyphosphoric acid, tetrapolyphosphoric acid, and metaphosphoric acid. By using these rust inhibitors, sufficient rust prevention effect can be achieved, and deterioration of paint stability is also small.
[0044] Furthermore, the coating material for coating metal sheets of the present invention preferably contains silica in a mass ratio of 1% to 10% of the total solid content. By containing silica, it is possible to suppress the precipitation of the rust inhibitor, improving the stability of the coating material. In addition, the water repellency of the coating film is increased, resulting in sufficient rust prevention. If the silica content is less than 1%, it is difficult to obtain the above-mentioned effect, and if it exceeds 10%, adhesion may deteriorate. It is preferable to use colloidal silica with a particle size of 5 nm to 200 nm.
[0045] In the present invention, the coating composition may contain, as components other than the acrylic resin, wax, rust inhibitor, and silica, surface conditioners, antifoaming agents, dispersants, and the like that are generally added to coating materials.
[0046] Next, the metal plate of the present invention will be described in detail. In the present invention, a lubricated metal plate is provided in which any of the above-mentioned coating materials is applied to at least one side of the metal plate and dried to form a lubricating film. As the solvent for the coating material, water or an organic solvent can be used, but water is preferably used. The concentration of the total solid content in the coating material is preferably 1 to 30% by mass.
[0047] If it is less than 1% or more than 30%, uneven coating may occur. There are no particular limitations on the coating method, but examples include the use of a roll coater or bar coater, or coating by spraying, dipping, or brushing. The steel sheet after coating can be dried by a general method. Examples include drying with hot air, drying with an IH heater, and infrared heating. In addition, the amount of coating on one side of the metal sheet must be 0.3 to 2.5 g / m2 in terms of dry mass. 2 It is preferable to apply the coating so that the coating density is 0.3g / m 2 If it is less than 2.5g / m, sufficient sliding properties may not be obtained. 2If the temperature exceeds this range, the ease of removal of the coating by alkali and adhesion may deteriorate. The maximum temperature that the steel sheet reaches during drying is preferably 60°C or higher and lower than the melting point of the wax used. If the temperature is lower than 60°C, drying takes a long time and rust prevention may be poor. If the temperature exceeds the melting point of the wax used, the wax may melt and combine, causing the particle size to become coarse, resulting in a deterioration of lubricity.
[0048] The metal plate is not particularly limited, and any metal plate can be used, such as a hot-rolled steel plate, a cold-rolled steel plate, a stainless steel plate, a galvanized steel plate, an aluminum plate, or a titanium plate. EXAMPLES
[0049] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.
[0050] A cold-rolled steel sheet SPCD (JIS G 3141) with a thickness of 0.7 mm and a tensile strength of 270 MPa was used. The paint with the composition shown in Table 1 was adjusted with pure water to a solids concentration of 15 mass%, applied with a bar coater, and dried with an IH heater so that the maximum temperature of the steel sheet reached was 80°C, to produce a lubricated steel sheet. The coating weight per side was 1.0 g / m 2 The coating amount was adjusted so that the following was obtained: Colloidal silica with a volume average particle size of 9 nm was used as the silica.
[0051] The coating weight was determined by removing the coating from the steel sheet after coating application, and dividing the difference in mass of the steel sheet before and after coating removal by the area.
[0052] (1) Method for evaluating press formability (sliding characteristics) In order to evaluate the press formability, the friction coefficient of each test material was measured as follows.
[0053] FIG. 1 is a schematic front view showing a friction coefficient measuring device. As shown in the figure, a friction coefficient measuring sample 1 taken from a test material is fixed to a sample stage 2, and the sample stage 2 is fixed to the upper surface of a horizontally movable slide table 3. A slide table support base 5 that can move up and down and has a roller 4 in contact with the slide table 3 is provided on the lower surface of the slide table 3, and a first load cell 7 is attached to the slide table support base 5 to measure the pressing load N applied by a bead 6 to the friction coefficient measuring sample 1 by pushing up the slide table 3. A second load cell 8 is attached to one end of the slide table 3 to measure the sliding resistance force F for moving the slide table 3 in the horizontal direction while the pressing force is applied. The test was performed by applying press cleaning oil Pleton R352L manufactured by Sugimura Chemical Industry Co., Ltd. as a lubricant to the surface of the sample 1.
[0054] Figure 2 is a schematic perspective view showing the shape and dimensions of the bead used. The bead 6 slides while its underside is pressed against the surface of the sample 1. The shape of the bead 6 shown in Figure 2 is 10 mm wide, 59 mm long in the sliding direction of the sample, and the lower parts of both ends in the sliding direction are curved surfaces with a curvature of 4.5 mmR, and the underside of the bead against which the sample is pressed has a flat surface with a width of 10 mm and a length of 50 mm in the sliding direction.
[0055] The friction coefficient measurement test was performed using the bead shown in Figure 2, with a pressing load N of 400 kgf and a sample pull-out speed (horizontal movement speed of the slide table 3) of 20 cm / min. The friction coefficient μ between the test material and the bead was calculated by the formula: μ = F / N. The sliding properties were evaluated as follows: a friction coefficient of 0.119 or less was rated as excellent sliding properties, ⊚; a coefficient of friction between 0.119 and 0.130 was rated as good sliding properties, and a coefficient of friction exceeding 0.130 was rated as insufficient and x.
[0056] (2) Evaluation method for film removal Assuming that the metal sheet according to the present invention is used in automobile applications, the film removal property during degreasing was evaluated. In order to determine the film removal property of the film, first, each test piece was degreased with an alkaline degreaser Fine Cleaner E6403 (manufactured by Nihon Parkerizing Co., Ltd.). The degreasing treatment was performed by immersing the test piece in a degreasing solution with a degreaser concentration of 20 g / L and a temperature of 40° C. for a predetermined time and washing with tap water. The surface carbon intensity of the test piece after the degreasing treatment was measured using a fluorescent X-ray analyzer, and the film peeling rate was calculated by the following formula using the measured value, the previously measured surface carbon intensity before degreasing, and the measured value of the surface carbon intensity of the untreated metal sheet.
[0057] Film peeling rate (%) = [(carbon strength before degreasing - carbon strength after degreasing) / (carbon strength before degreasing - carbon strength of untreated steel plate)] x 100 The removability of the coating was evaluated according to the following criteria, based on the immersion time in the alkaline degreasing solution at which the coating peeling rate was 98% or more. A time of 120 seconds or less was rated as good removability and rated as ◯, and a time of more than 120 seconds was rated as insufficient removability and △.
[0058] (3) Evaluation method for rust prevention Assuming that the metal plate according to the present invention is stored in a coiled state as a metal strip, the rust prevention properties in a stacked state were evaluated. Each test piece was processed to a size of 150 mm x 70 mm, and rust prevention oil was applied at 1.0 g / m per side. 2 The two test pieces were then overlapped and subjected to a surface pressure of 0.02 kgf / mm 2 The test was carried out in an environment with a temperature of 50°C and a humidity of 95% RH under a load so as to obtain the above value. The rust prevention properties were evaluated by checking the inside surfaces of the overlapped pieces every 7 days and judging the number of days until rust appeared. A period of 56 days or more was evaluated as particularly good rust prevention with an ⊚, a period of 21 days or more was evaluated as good rust prevention with an ◯, and a period of less than 21 days was evaluated as insufficient rust prevention with an △.
[0059] (4) Method for evaluating adhesion Each test piece was cut to a size of 100 x 25.4 mm, immersed in anti-rust oil, and then stood vertically for 24 hours to remove excess oil. Two pieces were used, and epoxy adhesive was uniformly applied to the 25.4 mm x 13 mm area to a thickness of 0.2 mm, then overlapped and clamped with clips, baked at 180°C for 20 minutes, and dried and hardened. After cooling, a shear tensile test was performed using an autograph tester to measure the shear adhesive strength. When a similar shear tensile test was performed using two metal plates (original plates) without a lubricating film, the shear adhesive strength was 29.0 MPa. Adhesion was evaluated as good adhesion with an adhesive strength of 20 MPa or more, and poor adhesion with an adhesive strength of less than 20 MPa.
[0060] (5) Evaluation method for paint stability 25 g of each paint, which had been adjusted with pure water to a solids concentration of 15% by mass, was placed in a φ18 mm × 180 mm test tube, shaken well, and then left to stand, and the time until precipitation occurred at the bottom of the test tube was evaluated. Paint stability was evaluated as good (○) when no precipitation occurred after 24 hours, and as insufficient (△) when precipitation occurred within 24 hours.
[0061] [Table 1]
[0062] [Table 2]
[0063] According to Table 2, all of the metal sheets coated with the coating material for metal sheets of the present invention have excellent press formability. In contrast, all of the metal sheets of the comparative examples not having the technical features of the present invention have poor press formability. [Industrial Applicability]
[0064] The coating material for coating metal sheets of the present invention is excellent in sliding property during press forming, film removal by alkali, rust prevention, adhesion, and coating stability. Since the lubricated metal sheet coated with this coating material has these excellent properties, it can be used in a wide range of fields, mainly for automobile bodies. [Explanation of symbols]
[0065] 1. Sample for measuring friction coefficient 2 Sample stage 3 Slide table 4. Lola 5 Slide table support 6 Beads 7 First load cell 8 Second Load Cell 9. Rail
Claims
1. A coating material for applying to metal sheets contains an acrylic resin having a glass transition point (Tg) of 100°C or higher and a ratio of the acid value to the glass transition point, R=acid value (mg-KOH / g) / Tg(°C), of 1.80 to 2.05, and a polyolefin wax having a melting point of 100°C or higher and 145°C or lower and an average particle size of 3.0 μm or less.
2. 2. The coating material for coating metal sheets according to claim 1, wherein the acid value of the acrylic resin is from 180 mg-KOH / g to 350 mg-KOH / g.
3. 3. The paint for coating metal sheets according to claim 1 or 2, wherein the proportion of the acrylic resin in the total solid content is 30% or more, and the proportion of the wax in the total solid content is 5% or more and 50% or less, in terms of mass proportion when the paint is dried.
4. The coating material for coating metal sheets according to any one of claims 1 to 3, wherein the acrylic resin has a mass average molecular weight of 5,000 or more and 30,000 or less.
5. The paint for coating metal sheets according to any one of claims 1 to 4, wherein the acrylic resin is a styrene-acrylic resin.
6. 6. The paint for coating metal sheets according to claim 1, wherein the paint contains an anti-rust agent in an amount of 5% to 30% by mass based on the total solid content when the paint is dried.
7. 7. The paint for coating metal sheets according to claim 6, wherein the rust inhibitor is at least one selected from the group consisting of aluminum salts, zinc salts, and zinc oxide of phosphoric acids.
8. The paint for coating metal sheets according to any one of claims 1 to 7, wherein the wax has an average particle size of 0.01 µm or more and 0.5 µm or less.
9. 9. The paint for coating metal sheets according to claim 1, which contains silica in an amount of 1% to 10% by mass based on the total solid content of the paint when dried.
Citation Information
Patent Citations
Lurication treated steel panel and film forming composition used therein
JP1997099517A
Film removing type lubricated steel plate having excellent deep draw property and score resistance
JP1997156029A
Galvanized steel sheet covered with alkali-soluble resin coating film having excellent adhesiveness by adhesive
JP1997170059A
Lubricating coating composition of removable film forming type having excellent deep drawing property, mold dragging resistance and temporary corrosionproof
JP1997296132A
Resin coated metal plate with mold drag resistance and corrosion resistance and its manufacture
JP1998052881A