Zn-Al-Mg hot-dip plated steel components
The Zn-Al-Mg hot-dip plated steel member addresses the challenges of corrosion resistance, adhesion, and conductivity by controlling the surface texture and composition, achieving a balanced performance with reduced scratches and improved appearance.
Patent Information
- Application Number
- JP2024536372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-09
- Filing Date
- 2024-02-09
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2044-02-09
AI Technical Summary
Existing hot-dip galvanized steel sheets face challenges in achieving a balanced improvement in corrosion resistance, adhesion of chemical conversion treatment layers, conductivity with welding electrodes, and reducing the visibility of scratches, while maintaining an appealing appearance.
A Zn-Al-Mg hot-dip plated steel member with a specific composition and surface texture, achieved through controlled cooling and binarization, combines a satin-like appearance with appropriate ratios of white and glossy areas, enhancing corrosion resistance, adhesion, and conductivity.
The solution provides a Zn-Al-Mg hot-dip plated steel member with excellent corrosion resistance, improved adhesion of chemical conversion layers, enhanced conductivity with welding electrodes, and reduced visibility of scratches, resulting in a high-quality appearance.
Smart Images

Figure 0007568999000010 
Figure 0007568999000011 
Figure 0007568999000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a Zn-Al-Mg hot-dip plated steel member. This application claims priority based on Japanese Patent Application No. 2023-018261, filed on February 9, 2023, the contents of which are incorporated herein by reference. [Background technology]
[0002] Hot-dip galvanized steel members are used as steel members with good corrosion resistance. Hot-dip galvanized steel sheets, a representative example of hot-dip galvanized steel members, are widely used in various manufacturing industries such as automobiles, home appliances, and building materials.
[0003] In order to further improve the corrosion resistance of hot-dip galvanized steel members, Zn-Al-Mg-based hot-dip galvanized steel members in which Al and / or Mg are contained in the hot-dip galvanized layer have been proposed. In addition, a technique for improving the appearance of the coating surface of Zn-Al-Mg-based hot-dip galvanized steel members has also been proposed.
[0004] Patent Document 1 describes a hot-dip galvanized steel sheet that contains Mg, Al, and Zn and has antiglare properties. Patent Document 2 describes a Zn-Al-Mg hot-dip plated steel sheet having a fine texture and a smooth, pear-like finish with many shiny portions. Patent Document 3 describes a hot-dip plated steel sheet that contains Mg, Al and Zn and has excellent appearance quality. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2015-193881 [Patent Document 2] International Publication No. 2011 / 001662 [Patent Document 3] Japanese Patent Publication No. 2004-143505 Summary of the Invention [Problem to be solved by the invention]
[0006] The hot-dip galvanized steel sheets described in Patent Documents 1 to 3 are technologies related to appearance, but in recent years, in addition to improved appearance, there has been an increasing need for further improvement in corrosion resistance and improvement in adhesion of the chemical conversion coating layer to enhance corrosion resistance. In addition, in order to improve the weldability of electric resistance welding such as spot welding, it is also necessary to improve the electrical conductivity when contacting a welding electrode. Thus, hot-dip galvanized steel members are required to improve these properties in a well-balanced manner.
[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a Zn-Al-Mg hot-dip plated steel member which has excellent corrosion resistance and adhesion of a chemical conversion coating layer, excellent electrical conductivity with a welding electrode even when a chemical conversion coating layer is formed, and further has an excellent appearance in which scratches are less noticeable. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention employs the following configuration. [1] A Zn-Al-Mg-based hot-dip plated steel member according to one embodiment of the present invention comprises a steel member and a hot-dip plated layer disposed on a surface of the steel member, The average composition of the hot-dip plating layer is, in mass%, Al: 4-22%, Mg: 1.0-10%, Fe: 0.0001-2%, Si: 0-2%, Ni: 0-2%, Ti: 0-2%, Zr: 0-2%, Sr: 0-2%, Sb: 0-2%, Pb: 0-2%, Sn: 0-2%, Ca: 0-2%, Co: 0-2%, Mn: 0-2%, P: 0-2%, B: 0~2%, Bi: 0-2%, Cr: 0-2%, Sc: 0-2%, Y: 0-2%, REM: 0~2%, Hf: 0-2%, and C: 0-2% and the balance includes Zn and impurities, In the binary image data of the image data obtained by capturing an image of the surface of the hot-dip plating layer, the total area ratio of white pixels is 30% or more and 70% or less, The binary image data is obtained by binarizing the image data by Otsu's binarization method. [2] The Zn-Al-Mg-based hot-dip plated steel member described in the above item [1] may have a chemical conversion treatment layer on a surface of the hot-dip plated layer. [3] In the Zn-Al-Mg-based hot-dip plated steel member according to the above item [2], the chemical conversion coating layer may have a metallic appearance. [4] In the Zn-Al-Mg-based hot-dip plated steel member described in [1] above, a 60 degree specular gloss Gs(60°) of a surface of the hot-dip plated layer corresponding to an area where white pixels are gathered may be 150 or less, and the 60 degree specular gloss Gs(60°) of a surface of the hot-dip plated layer corresponding to an area where black pixels are gathered may be 1.5 times or more the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where white pixels are gathered. [5] In the Zn-Al-Mg-based hot-dip plated steel member described in [2] above, a 60 degree specular gloss Gs(60°) of a surface of the hot-dip plated layer corresponding to an area where white pixels are gathered may be 150 or less, and the 60 degree specular gloss Gs(60°) of a surface of the hot-dip plated layer corresponding to an area where black pixels are gathered may be 1.5 times or more the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where white pixels are gathered. [6] In the Zn-Al-Mg-based hot-dip plated steel member described in [1] above, a 60 degree specular gloss Gs(60°) of a surface of the hot-dip plated layer corresponding to an area where white pixels are gathered may be 70 or less, and the 60 degree specular gloss Gs(60°) of a surface of the hot-dip plated layer corresponding to an area where black pixels are gathered may be 1.5 times or more the 60 degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where white pixels are gathered. [7] In the Zn-Al-Mg-based hot-dip plated steel member according to any one of [1] to [6] above, the hot-dip plated layer may contain, in an average composition, one or more elements selected from the following Group A, Group B, or Group C: Group A: Si: 0.0001~2% by mass Group B: Ni, Ti, Zr, Sr, or any one or more of these, 0.0001 to 2 mass% in total Group C: Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, C, one or more of these, 0.0001 to 2 mass% in total [8] In the Zn-Al-Mg-based hot-dip plated steel member according to the above item [5], the average composition of the hot-dip plated layer may contain the Group A element. [9] In the Zn-Al-Mg-based hot-dip plated steel member according to the above item [5], the average composition of the hot-dip plated layer may contain the B group element.
[10] In the Zn-Al-Mg-based hot-dip plated steel member according to the above item [5], the average composition of the hot-dip plated layer may contain the C group element. Effect of the Invention
[0009] Effects of the Invention The present invention can provide a Zn-Al-Mg hot-dip plated steel member which has excellent corrosion resistance and adhesion of a chemical conversion coating layer, and which has excellent electrical conductivity with a welding electrode even when a chemical conversion coating layer is formed, and further has an excellent appearance in which scratches are less noticeable. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram illustrating a method for producing a Zn-Al-Mg based hot-dip coated steel member. [Diagram 2] FIG. 2 shows image data illustrating each group region of white pixels and black pixels, and is binary image data obtained by subjecting image data of an image of the surface of a hot-dip plated layer to a binarization process using Otsu's binarization method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The hot-dip plating layer of Zn-Al-Mg-based hot-dip plated steel members has a matte appearance. The matte appearance is caused by the mixture of fine white areas and glossy areas on the surface of the hot-dip plating layer. The white areas have a relatively large surface roughness, which causes the incident light to be diffusely reflected, making them appear white or close to white. On the other hand, the glossy areas have a relatively small surface roughness, which makes it difficult for the incident light to be diffusely reflected, resulting in a metallic luster or a form close to metallic luster. The greater the number of white areas, the less noticeable the defects become.
[0012] Here, when a chemical conversion layer is formed on a hot-dip plated layer, it is generally formed so that the surface height of the chemical conversion layer is approximately uniform over the entire hot-dip plated layer. In this case, when the hot-dip plating layer has a large number of white areas, the surface roughness of the hot-dip plating layer increases overall, and the adhesion of the chemical conversion coating layer increases due to the anchor effect. In addition, since the surface roughness of the hot-dip plating layer is large, the chemical conversion coating layer tends to be formed relatively thick, and therefore the corrosion resistance of the hot-dip plating layer also tends to improve. On the other hand, when the number of shiny parts in the hot-dip coating layer is increased, the surface roughness of the hot-dip coating layer as a whole is reduced, and the chemical conversion coating layer can be made relatively thin. As a result, when a welding electrode is pressed against the hot-dip coating steel sheet, the electrical conductivity between the welding electrode and the hot-dip coating layer is improved. Therefore, a hot-dip coating layer with many shiny parts has improved weldability in electric resistance welding such as spot welding.
[0013] From the above, if it were possible to adjust the ratio of the white and glossy parts of the hot-dip galvanized layer to an appropriate range, it would be possible to provide an excellent appearance with less noticeable scratches, corrosion resistance of the hot-dip galvanized layer, adhesion between the hot-dip galvanized layer and the chemical conversion coating layer, and conductivity between the hot-dip galvanized layer and the welding electrode. However, it has been difficult to obtain a hot-dip galvanized layer that satisfies all of these requirements.
[0014] Therefore, the inventors further studied and confirmed the phenomenon that, when forming a hot-dip plating layer on the surface of a steel member such as a steel plate, spraying an air refrigerant containing oxygen from a cooling device equipped with multiple injection nozzles promotes the oxidation of the surface of the hot-dip plating layer, making it easier to form white areas on the surface of the hot-dip plating layer. Here, it was found that, when injecting the refrigerant, instead of injecting it from all the injection nozzles at the same time, the refrigerant is injected from some of the injection nozzles while the injection nozzles from which the refrigerant is injected are randomly switched, thereby simultaneously satisfying excellent appearance with less noticeable scratches, corrosion resistance, adhesion to the chemical conversion coating layer, and conductivity between the welding electrode. Furthermore, it was also found that, for a hot-dip plating layer having this characteristic, when a binary image containing white pixels and black pixels is obtained by binarizing a digital image of the hot-dip plating layer using a binarization method called "Otsu's binary method" used for binarization of images, the total area ratio of white pixels falls within a predetermined range. In other words, a plated steel sheet in which the total area ratio of white pixels in the above-mentioned binarized image is within a predetermined range can simultaneously satisfy an excellent appearance in which scratches are less noticeable, corrosion resistance, adhesion to the chemical conversion coating layer, and conductivity with the welding electrode.
[0015] Hereinafter, the Zn-Al-Mg hot-dip plated steel member of this embodiment will be described. The Zn-Al-Mg based hot-dip plated steel member (hereinafter referred to as hot-dip plated steel member) of this embodiment comprises a steel member and a hot-dip plated layer disposed on the surface of the steel member, the hot-dip plated layer having an average composition, in mass%, of 4-22% Al, 1.0-10% Mg, 0.0001-2% Fe, with the balance containing Zn and impurities, and in binary image data of image data obtained by capturing an image of the surface of the hot-dip plated layer, the total area ratio of white pixels is 30% or more and 70% or less. The hot-dip plated steel member of the present embodiment may further include a chemical conversion layer on the surface of the above-mentioned hot-dip plated layer. In addition, in binarized image data of image data obtained by photographing the surface of the hot-dip plated layer from above the chemical conversion treatment layer, the total area ratio of white pixels may be 30% or more and 70% or less, and the surface may have a metallic appearance.
[0016] The steel member that is the base of the hot-dip layer is, for example, a steel plate, a steel material, or a member obtained by processing these, but there is no particular restriction on the material. As will be described in detail later, general steel and the like can be used as the material of the steel member without any particular restriction, and Al-killed steel and some high alloy steels can also be applied. There is no particular restriction on the shape of the steel member. The hot-dip layer according to this embodiment is formed by applying the hot-dip method described later to the steel member. The hot-dip layer is formed on the surface of the steel member. That is, when the steel member is a steel plate, the hot-dip layer is formed on both sides of the steel plate. Note that the steel member includes not only steel plates and steel materials, but also members obtained by processing these. The steel member may be, for example, a steel product used in the fields of automobiles, home appliances, building materials, etc.
[0017] Next, the chemical components of the hot-dip plating layer will be described. The hot-dip coating layer may have an average composition of 4-22% Al, 1.0-10% Mg, 0.0001-2% Fe, and the remainder of Zn and impurities. The hot-dip coating layer may have an average composition of 4-22% Al, 1.0-10% Mg, 0.0001-2% Fe, and the remainder of Zn and impurities.
[0018] The hot-dip plated layer may contain, in an average composition, one or more elements selected from the following Group A, Group B, or Group C. In the chemical composition of the hot-dip plated layer, the lower limit of each element in the following Group A, Group B, or Group C may be 0% or more than 0%. The hot-dip plated layer may contain, in an average composition, 4-22% Al, 1.0-10% Mg, and 0.0001-2% Fe, and may further contain one or more elements selected from the following Group A, Group B, or Group C, with the balance being Zn and impurities.
[0019] Group A: Si: 0.0001~2% by mass Group B: Ni, Ti, Zr, Sr, or any one or more of these, 0.0001 to 2 mass% in total Group C: Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, C, one or more of these, 0.0001 to 2 mass% in total
[0020] The composition of the hot-dip plating layer can be measured by the following method. First, a rectangular area of 50 mm x 50 mm is cut from the hot-dip plating steel sheet, 50 mm away from the end, and no obvious defects such as corrosion are present. Then, the surface coating layer and the chemical conversion coating layer are removed from the sample using a coating remover (e.g., Neo River SP-751 manufactured by Sansai Kako Co., Ltd.) that does not corrode the coating layer. If the surface coating layer and the chemical conversion coating layer cannot be sufficiently removed, they are removed by polishing with an abrasive that is less hard than the coating layer. Then, the sample is immersed in 5% hydrochloric acid containing an inhibitor (e.g., Hibilon manufactured by Sugimura Chemical Industry Co., Ltd.) to dissolve the hot-dip plating layer. The composition of the hot-dip plating layer can be determined by subjecting the obtained solution to inductively coupled plasma (ICP) emission spectrometry. However, for Si, which cannot be accurately analyzed by the above method, the Si content can be determined by further treating the obtained solution with the acid decomposition and sodium carbonate fusion method based on JIS G1258-3 and then analyzing it.
[0021] The Al content is 4 to 22 mass% in average composition. Al is an element necessary for ensuring corrosion resistance. If the Al content in the hot-dip plating layer is less than 4 mass%, the effect of improving corrosion resistance becomes insufficient, and if it exceeds 22 mass%, the effect of improving corrosion resistance becomes saturated. From the viewpoint of corrosion resistance, the Al content is preferably 5 to 20 mass%, and more preferably 6 to 20 mass%.
[0022] The Mg content is 1.0 to 10 mass% in average composition. Mg is an element necessary for improving corrosion resistance. If the Mg content in the hot-dip plated layer is less than 1.0 mass%, the effect of improving corrosion resistance is insufficient. If the Mg content in the hot-dip plated layer exceeds 10 mass%, significant dross is generated in the plating bath, making it difficult to stably manufacture hot-dip plated steel members. From the viewpoint of the balance between corrosion resistance and dross generation, the Mg content is preferably 1.5 to 8 mass%. The Mg content is more preferably 2.0 to 7.0 mass%.
[0023] The hot-dip plated layer may contain Si in the range of 0.0001 to 2 mass% as an element of group A. Si is an element effective for improving the adhesion of the hot-dip plated layer. By containing Si at 0.0001 mass% or more, the effect of improving the adhesion of the hot-dip plated layer is manifested, so that the Si content is preferably 0.0001 mass% or more. On the other hand, even if the Si content exceeds 2 mass%, the effect of improving the plating adhesion is saturated, so that the Si content is 2 mass% or less. From the viewpoint of plating adhesion, the Si content is more preferably 0.0010 to 1 mass%, and further preferably 0.0100 to 0.8 mass%. The Si content may be 0% or more than 0%.
[0024] The hot-dip plating layer may contain, as an element of group B, one or more of Ni, Ti, Zr, and Sr in an average composition in total of 0.0001 to 2 mass%, more preferably 0.001 to 1 mass%, and even more preferably 0.002 to 0.10 mass%. By containing these elements of group B, the corrosion resistance can be further improved. The contents of Ni, Ti, Zr, and Sr may be 0% or more than 0%.
[0025] The hot-dip plating layer may contain, as an element of group C, one or more of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in an average composition of 0.0001 to 2 mass% in total. More preferably, it is 0.001 to 1 mass%, and further preferably, it is 0.002 to 0.10 mass%. By containing these elements of group C, the corrosion resistance can be further improved. REM is one or more of rare earth elements having atomic numbers 57 to 71 in the periodic table. The contents of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C may be 0% or more than 0%.
[0026] The balance of the chemical components of the hot-dip plated layer is zinc and impurities. In addition, when the hot-dip plated layer is formed, Fe (iron), which is a main component of the steel member, is mixed into the hot-dip plated layer. In the hot-dip plated layer of the present embodiment, the content of Fe is in the range of 0.0001 to 2 mass% in the average composition.
[0027] Next, the appearance of the hot-dip plated layer will be described. In the hot-dip plated layer according to this embodiment, when image data of the surface of the hot-dip plated layer is binarized by Otsu's binarization method to obtain binary image data, the total area ratio of white pixels contained in the binary image data is 30% to 70%. In addition, when the steel member is a plate having an upper surface and a lower surface like a steel plate, the binary image data may be obtained by binarizing image data of one surface side or both surfaces side of the steel member (steel plate) by Otsu's binarization method.
[0028] Here, a supplementary explanation will be given regarding "image data of the surface of the hot-dip galvanized layer, the image data being captured from one side or both sides of the steel member (steel plate)". When the steel member is a steel plate, the hot-dip galvanized layer according to this embodiment is formed on the surface of the steel plate, i.e., on one side and the other side in the plate thickness direction of the steel plate. In such a case, the image data used for the binarization process may be data of an image of the surface of either one side of the hot-dip galvanized layer arranged on the one side or the other side, or may be data of an image of both surfaces of the hot-dip galvanized layer arranged on the one side and the other side.
[0029] In other words, the hot-dip galvanized steel component of this embodiment only needs to satisfy a total area ratio of white pixels contained in binary image data obtained from image data captured from one side of the steel component among image data captured of the surface of the hot-dip galvanized layer of 30% or more and 70% or less. In addition, the total area ratio of white pixels contained in the binary image data obtained from image data captured from both sides of the steel member among the image data captured of the surface of the hot-dip plated layer may satisfy 30% or more and 70% or less. When the shape of the hot-dip plated steel member according to this embodiment is not plate-like (for example, when it is a processed member), the image data is captured by capturing an image of a flat portion of the steel member.
[0030] The photographed area for obtaining image data of the surface of the hot-dip galvanized layer is selected by cutting a rectangular area of 100 mm x 100 mm that is free of obvious defects such as corrosion and is located 50 mm away from the end. If the hot-dip galvanized steel component is a processed product, a rectangular flat area of 100 mm x 100 mm that is located 50 mm away from the end or processed part is selected by cutting. If the photographed area is narrower than this, it becomes difficult to properly evaluate the appearance of the hot-dip galvanized layer. Also, if the photographed area is larger than this, the amount of data increases and the processing time increases, which is not preferable.
[0031] A sample including the selected photographed area and its surroundings is cut out from the hot-dip galvanized steel part, and image data of the photographed area is obtained using this sample.
[0032] The image data is acquired by scanning the surface of the hot-dip plating layer of the sample with a scanner connected to a computer. The image data is extracted as 256 grayscale image data with a resolution of 300 dpi (dots per inch), for example. The scanner used is preferably a flatbed scanner. When localized unevenness in brightness occurs in the image data due to the influence of distortion of the steel member, etc., it is preferable to eliminate the localized unevenness in brightness by image correction.
[0033] In general, image data can be extracted by taking a photograph using a camera. However, when taking a photograph using a camera, it is difficult to irradiate the entire hot-dip plating layer, which is the subject, with illumination light at the time of shooting completely and evenly, which may result in an inaccurate evaluation of the appearance pattern. Therefore, extraction of image data using a scanner is preferable.
[0034] The image data is grayscale 256-level gradation image data. Image data includes color image data in addition to grayscale, but color image data contains excessive information because pixels have color information. Since the surface appearance of the hot-dip plating layer in this embodiment has low saturation, grayscale gradation image data is sufficient in terms of the amount of information. Therefore, in this embodiment, grayscale 256-level gradation image data with gradations of 0 to 255 steps, which has an appropriate amount of information and is easy to handle on a computer, is preferred.
[0035] The image data is preferably image data when visible light is used as a light source, and is preferably not a secondary electron image or a backscattered electron image obtained by an electron microscope. Secondary electron images and backscattered electron images obtained by an electron microscope are convenient for observing minute surface shapes and differences in elemental composition, but do not provide any color information for objects. In contrast, the image data according to this embodiment can capture color information of the plating layer surface, even though it is grayscaled, and can reflect the impression of the plating layer observed by the naked eye under visible light.
[0036] Next, the obtained image data is subjected to binarization processing by Otsu's binarization method to obtain binarized image data. The binarization processing by Otsu's binarization method may be performed by a computer having a pre-programmed program.
[0037] Otsu's binarization method is generally known as a method for selecting a threshold level that binarizes a grayscale image and separates the target region from the background. Details are described in the following literature. The contents are briefly described below.
[0038] Nobuyuki Otsu, "Automatic Threshold Selection Method Based on Discrimination and Least Squares Criteria", IEICE Transactions on Electronics and Communication Engineers, Vol. 63, No. 4, pp. 349-356, 1980.
[0039] Consider a grayscale image with 256 levels (0 to 255). Let U be the set of all pixels in the entire image. Let k, which is in the range of 0 to 255, be used as a threshold, and let A be the set of pixels with pixel values of 0 to k, and B be the set of pixels with pixel values of k+1 to 255. Let the total numbers of U, A, and B be N and N A , N B Let the average pixel values of U, A, and B be x and x A , x B Next, Y is defined as the following equation. In this case, the method of binarizing a grayscale image using k that maximizes Y is equivalent to Otsu's binarization method. The following Y corresponds to equation (16) in the above document.
[0040] Y=(N A / N)(x A -x) 2 +(N B / N)(x B -x) 2
[0041] In this embodiment, in the binarized image data after the binarization process, pixels included in set A of pixels having pixel values of 0 to k become black pixels, and pixels included in set B of pixels having pixel values of k+1 to 255 become white pixels. In the matte appearance, the black pixels correspond to the glossy parts, and the white pixels correspond to the white parts.
[0042] In this embodiment, the total area ratio of white pixels in the binary image data of the hot-dip plating layer must be in the range of 30% to 70%. If the total area ratio of white pixels is less than 30%, the area of black pixels becomes excessively large, that is, the area of glossy parts becomes wide, and defects on the surface of the hot-dip plating layer become more noticeable. In addition, although the weldability of electric resistance welding such as spot welding is improved, the adhesion of the chemical conversion coating layer and the corrosion resistance of the hot-dip plating layer are reduced.
[0043] On the other hand, if the total area ratio of white pixels exceeds 70%, the area of white pixels becomes excessively large, i.e., the area of white parts becomes wider, and scratches become less noticeable. The adhesion of the chemical conversion coating layer and the corrosion resistance of the hot-dip plating layer are improved, but the weldability of electric resistance welding such as spot welding is reduced. Therefore, the total area ratio of white pixels is preferably in the range of 30% to 70%. Such a hot-dip plating layer will have a matte appearance with a mixture of glossy parts and white parts. In addition, the hot-dip plating layer will have a metallic appearance with a metallic texture.
[0044] In the hot-dip plated layer according to the present embodiment, the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered is 150 or less, preferably 70 or less. In addition, the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where black pixels are gathered is preferably 1.5 times or more, more preferably 2.1 times or more, of the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the region where white pixels are gathered. When a chemical conversion coating layer having visible light transparency is formed on the hot-dip plated layer and it is difficult to remove the chemical conversion coating layer, the gloss may be measured from above the chemical conversion coating.
[0045] The white pixel aggregation region is a pixel region where white pixels are aggregated in a region large enough to measure the 60-degree specular gloss Gs (60°) by a gloss meter. Specifically, as shown in FIG. 2, the white pixel aggregation region refers to a 3 mm square rectangular region where the area ratio of white pixels is 60% or more. In other words, if the area ratio of white pixels is 60% or more in this 3 mm square rectangular region, this region is considered to be a white pixel aggregation region. Similarly, the black pixel aggregation region is a pixel region where black pixels are aggregated, and refers to a 3 mm square rectangular region where the area ratio of black pixels is 60% or more as shown in FIG. 2. In other words, if the area ratio of black pixels is 60% or more in this 3 mm square rectangular region, this region is considered to be a black pixel aggregation region.
[0046] The 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where white pixels are gathered is preferably 150 or less, more preferably 70 or less. This makes it possible to obtain an appearance with a calm atmosphere and a good impression without excessively asserting the metallic luster. The lower limit of the 60-degree specular gloss Gs(60°) measured for the area where white pixels are gathered is not particularly limited, but may be 10 or more. Note that the "60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where white pixels are gathered" here refers to the average value of the 60-degree specular gloss Gs(60°) in each of the areas where 10 white pixels are gathered. The same applies to the 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer corresponding to the area where black pixels are gathered.
[0047] In addition, in the hot-dip plated layer, the 60-degree specular gloss Gs (60°) of the surface of the hot-dip plated layer corresponding to the area of a collection of black pixels is preferably 1.5 times or more the 60-degree specular gloss Gs (60°) of the surface of the hot-dip plated layer corresponding to the area of a collection of white pixels. This makes it possible to clearly show the contrast in appearance between the white part corresponding to the area of a collection of white pixels and the gloss part corresponding to the area of a collection of black pixels when the area of a collection of white pixels is adjacent to the area of a collection of black pixels, resulting in a favorable impression of the surface pattern.
[0048] The 60-degree specular gloss Gs(60°) of the surface of the hot-dip plated layer is measured using a glossmeter based on the method specified in JIS Z 8741. Specifically, the 60-degree gloss (%) is measured using the method specified in JIS Z 8741, and Gs(60°) is calculated based on the obtained gloss (%). When measuring the 60-degree specular gloss Gs(60°), that is, when identifying the area where white pixels or black pixels are gathered, each of the 3 mm square rectangular areas to be measured is set so that they do not overlap with each other.
[0049] In addition, the hot-dip plated steel member of this embodiment may be provided with a chemical conversion treatment layer on the surface of the hot-dip plated layer. The chemical conversion treatment layer does not have to be provided on the entire steel member, and for example, in the case of a steel plate, the chemical conversion treatment layer may be provided on both the hot-dip plated layers arranged on one side and the other side of the steel plate. The type of chemical conversion treatment is not particularly limited, and any known chemical conversion treatment can be used, but in this case, it is preferable that the chemical conversion treatment layer is a chemical conversion treatment layer that is transparent to visible light.
[0050] The hot-dip plating layer of the hot-dip plating steel member having the chemical conversion layer is obtained by binarizing the image data of the surface of the hot-dip plating layer from above the chemical conversion layer by the Otsu binarization method, and the total area ratio of white pixels contained in the binarized image data is 30% or more and 70% or less. That is, it is preferable that the chemical conversion layer provided on the hot-dip plating steel member of the present embodiment does not affect the appearance of the surface of the hot-dip plating layer. The hot-dip plating steel member having such a chemical conversion layer disposed thereon has a metallic appearance. In addition, when a coating layer is formed on the surface of the hot-dip plating layer or the surface of the chemical conversion layer, a painting process is performed on the hot-dip plating layer or the hot-dip plating steel member after the chemical conversion layer is formed. The type of the painting process is not particularly limited, and a known painting process can be used. In this case, the painting process is preferably a painting process having visible light transparency.
[0051] An example of the chemical conversion coating layer according to the present embodiment is one containing 20% by mass or more of resin and 1 to 20% by mass of silica particles having a particle size of 5 to 200 nm. This chemical conversion coating layer is obtained by applying an aqueous composition containing the resin and the silica particles to the hot-dip plating layer and drying it.
[0052] The resin contained in the chemical conversion coating layer may be a general resin, such as polyolefin resin, fluororesin, acrylic resin, urethane resin, polyester resin, epoxy resin, and phenol resin. These resins may be water-soluble resins, or may be resins (water-dispersible resins) that are originally water-insoluble but can be finely dispersed in water, such as emulsions and suspensions. In addition to water-soluble resins, resins (water-dispersible resins) that are originally water-insoluble but can be finely dispersed in water, such as emulsions and suspensions, are also included. In particular, it is preferable to contain one or more resins selected from polyolefin resins, fluororesins, acrylic resins, and phenol resins, since they have excellent weather resistance.
[0053] The resin is preferably contained in the chemical conversion layer at a ratio of 20% by mass or more. By making the resin content 20% by mass or more, the chemical conversion layer itself does not become brittle, and the hot-dip plating layer can be stably coated. Note that the chemical conversion layer may contain components other than the resin, such as Nb compounds and phosphate compounds, in addition to the resin, silica particles, and pigment, and the resin content may be the remainder of these components.
[0054] Silica particles are blended to improve the corrosion resistance of the chemical conversion layer. The silica particles preferably have an average particle size in the range of 5 to 200 nm. The silica particles are contained in the chemical conversion layer at a ratio of 1 to 20 mass %. By making the content of silica particles 1 mass % or more, the effect of improving the corrosion resistance can be obtained. In addition, by making the content of silica particles 20 mass % or less, the chemical conversion layer itself does not become brittle, and the Zn-based plating layer can be stably coated. Since it is difficult to obtain silica particles with an average particle size of less than 5 nm, and it is practically difficult to prepare or manufacture a chemical conversion layer containing silica particles with an average particle size of less than 5 nm, the lower limit of the average particle size of the silica particles is set to 5 nm or more. In addition, if the average particle size of the silica particles exceeds 200 nm, the chemical conversion layer may become cloudy and the metallic appearance of the hot-dip plating layer may be impaired.
[0055] In general, inorganic pigments such as silica particles have a small particle size, and therefore may exist in the chemical conversion coating layer in the form of secondary particles having a particle size larger than the primary particle size. The particle size of these secondary particles (particles formed by agglomeration of inorganic pigments) is hereinafter referred to as "secondary particle size." The silica particles in this embodiment may be a mixture of primary particles and secondary particles, and even if primary particles and secondary particles are mixed, the average particle size may be in the range of 5 to 200 nm.
[0056] In order to improve the corrosion resistance of the chemical conversion coating layer, titania particles, alumina particles, zirconia particles, etc. may be contained in addition to silica particles.
[0057] The chemical conversion coating layer may further contain either or both of an Nb compound and a phosphate compound. When an Nb compound or a phosphate compound is contained, the corrosion resistance of the Zn-based plating layer is improved.
[0058] As the Nb compound, a conventionally known niobium-containing compound can be used, for example, niobium oxide, niobic acid and its salts, fluoroniobate, fluorooxoniobate, etc. Among them, niobium oxide is preferable from the viewpoint of improving corrosion resistance.
[0059] Examples of the phosphoric acid compound include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, and their salts; phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), and their salts; and organic phosphoric acids such as phytic acid and their salts. The cationic species of the salts are not particularly limited, and examples thereof include Cu, Co, Fe, Mn, Sn, V, Mg, Ba, Al, Ca, Sr, Nb, Y, Ni, and Zn. These may be used alone or in combination of two or more.
[0060] The Nb compound and the phosphate compound may be contained in the chemical conversion coating layer in a total amount of 0.5 to 30 mass %. If the content is 0.5 mass % or more, the corrosion resistance is improved, and if the content is 30 mass % or less, the chemical conversion coating layer does not become brittle and can stably cover the Zn-based plating layer.
[0061] The coating weight of the chemical conversion coating layer on each side of the hot-dip coating layer is 0.1 to 15 g / m 2 It is preferable that the coating amount is 0.1 g / m 2 If the coating weight is 15 g / m or more, the coating weight of the chemical conversion coating layer is sufficient, the blackened portion on the surface of the hot-dip plating layer can be made less noticeable, and the corrosion resistance of the hot-dip plating layer can be improved. 2 If the coating amount is less than this, the reflection of light on the surface of the chemical conversion coating layer is reduced, and the metallic appearance of the surface of the hot-dip plating layer can be visually confirmed. 2 It is.
[0062] The chemical conversion coating layer may further contain at least one crosslinking agent selected from the group consisting of a silane coupling agent, a crosslinkable zirconium compound, and a crosslinkable titanium compound. These may be used alone or in combination of two or more.
[0063] The chemical conversion coating layer of the hot-dip plated steel member of this embodiment is not limited to the one described above, and it goes without saying that any known chemical conversion coating layer may be used, for example.
[0064] Next, a method for manufacturing the hot-dip plated steel member of this embodiment will be described. FIG. 1 shows a hot-dip plating facility suitable for manufacturing the hot-dip plated steel member of this embodiment. The hot-dip plating facility shown in FIG. 1 includes a hot-dip plating bath 2, a sink roll 3 arranged in the hot-dip plating bath 2, a pair of wiping nozzles 4 arranged above the hot-dip plating bath 2, a cooling device 5 arranged above at least one of the pair of wiping nozzles 4, and a top roll 7 arranged above the cooling device 5. The cooling device 5 may be arranged above both of the pair of wiping nozzles 4.
[0065] The hot-dip galvanizing bath 2 contains, in mass%, Al: 4-22%, Mg: 1.0-10%, and the remainder contains Zn and impurities. The hot-dip galvanizing bath may further contain Si: 0.0001-2 mass%. The hot-dip galvanizing bath may further contain one or more of Ni, Ti, Zr, and Sr in a total amount of 0.0001-2 mass%. The hot-dip galvanizing bath may further contain one or more of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in a total amount of 0.0001-2 mass%. The temperature of the hot-dip galvanizing bath 2 varies depending on the composition, but is preferably in the range of, for example, 400-500°C. This is because the desired hot-dip galvanizing layer can be formed if the temperature of the hot-dip galvanizing bath 2 is in this range.
[0066] The cooling device 5 cools the hot-dip plating layer and has a plurality of cooling nozzles that spray a coolant toward the steel member. An example of the coolant is air with added oxygen, such as 26% oxygen-74% nitrogen.
[0067] Hereinafter, a method for manufacturing a hot-dip plated steel member using the manufacturing facility of Fig. 1 will be described. The hot-dip plated steel member according to this embodiment only needs to have a hot-dip plated layer on the surface of the steel member, and for example, the timing of processing the steel sheet does not matter. That is, the hot-dip plated steel member according to this embodiment may be obtained by forming a hot-dip plated layer on the surface of a steel sheet / steel material to obtain a plated steel sheet / steel material, and then processing these, or the hot-dip plated steel member according to this embodiment may be obtained by forming a hot-dip plated layer on the surface of a steel member that has been processed in advance. In the following description of the manufacturing method, the steel member is a plate-shaped steel plate. First, a hot-rolled steel sheet is manufactured, and if necessary, hot-rolled sheet annealing is performed. After pickling, cold rolling is performed to obtain a cold-rolled sheet. The cold-rolled sheet is degreased, washed with water, and then annealed (cold-rolled sheet annealing).
[0068] Next, as shown in Fig. 1, the annealed steel sheet 1 is immersed in a hot-dip galvanizing bath 2, and then the direction of travel is changed by a sink roll 3 and the steel sheet is pulled up vertically. High-pressure gas such as air or nitrogen is sprayed onto the surface of the pulled-up steel sheet 1 from a wiping nozzle 4 arranged above the hot-dip galvanizing bath 2 to remove the excess amount of hot-dip coating adhering to the surface of the steel sheet 1.
[0069] The total coating weight of the hot-dip coating layer on both sides of the steel sheet is 30 to 600 g / m 2 It is preferable to adjust the amount of adhesion so that it is in the range of 30 g / m 2 If the coating weight is less than 600g / m, the corrosion resistance of the hot-dip galvanized steel sheet decreases, which is not preferable. 2 If the thickness exceeds 100 mm, the molten metal adhering to the steel sheet will drip, making it impossible to smooth the surface of the hot-dip coating layer, which is not preferable. If the steel member is not in the form of a plate, the thickness of the hot-dip coating layer should be 30 to 600 g / m2 in total for the entire steel member. 2 It is preferable to adjust it so that
[0070] Next, as shown in Fig. 1, the hot-dip plating layer attached to the surface of the steel sheet 1 is cooled by a cooling device 5 equipped with multiple injection nozzles. At this time, the coolant is not injected from all the injection nozzles at the same time, but rather, the injection nozzles from which the coolant is injected are randomly switched while the coolant is injected from some of the injection nozzles. Air coolant containing oxygen, such as 26% oxygen-74% nitrogen, is injected from the injection nozzles.
[0071] In the area where the coolant is sprayed, the surface oxidation of the hot-dip plated layer is promoted, and white parts are likely to be formed. On the other hand, in the area where the coolant is not sprayed, the cooling rate of the hot-dip plated layer is slowed, and glossy parts are likely to be formed. In this way, the desired hot-dip plated steel member can be obtained by randomly switching the spray nozzles that spray the coolant. It is preferable that a plurality of spray nozzles are arranged at intervals of 25 mm. The spray nozzles are switched ON and OFF at 0.1 second intervals, and are adjusted to be randomly switched using random numbers so that the coolant is sprayed from 30 to 60% of the spray nozzles out of all the spray nozzles. The coolant flow rate is adjusted to be 5 to 20°C / s as the average cooling rate of the entire steel sheet.
[0072] The above-mentioned cooling control for the hot-dip plated layer may be performed, for example, only on the hot-dip plated layer arranged on one side of the steel sheet, or may be performed on the hot-dip plated layers arranged on both one side and the other side of the steel sheet.
[0073] When cooling a steel sheet after hot-dip galvanization, cooling is usually performed under the same conditions on one side and the other side of the steel sheet, so that the total area ratio of white pixels contained in the binarized image data obtained from image data captured from both sides of the steel sheet satisfies 30% to 70%. On the other hand, when cooling is performed on one side of the steel sheet under the above-mentioned preferable conditions and cooling is performed on the other side under conditions that deviate from the preferable conditions, the total area ratio of white pixels contained in the binarized image data obtained from image data captured from both one sides of the steel sheet may satisfy 30% to 70%.
[0074] A chemical conversion layer may be further formed on the hot-dip plated layer after cooling. The coating method of the aqueous composition used to form the chemical conversion layer is to apply the aqueous composition to the surface of the hot-dip plated layer to form a film. The coating method is not particularly limited, and generally used methods such as roll coating, air spraying, airless spraying, and immersion can be appropriately adopted. As a drying method after applying the aqueous composition, any method such as hot air, induction heating, near infrared, and far infrared may be used, or these may be used in combination. The heating temperature of the coated object is 50 to 250°C, preferably 70 to 220°C.
[0075] According to the hot-dip galvanized steel member of this embodiment, in the binary image data obtained by binarizing image data of the surface of the hot-dip galvanized layer using Otsu's binarization method, the total area ratio of white pixels contained in the binary image data is 30% or more and 70% or less, so that the corrosion resistance of the hot-dip galvanized steel member and the adhesion of the chemical conversion coating layer are improved, the electrical conductivity with the welding electrode is increased, and furthermore, an excellent appearance can be obtained. EXAMPLES
[0076] Next, an embodiment of the present invention will be described. Note that in the following embodiment, the steel member is a plate-shaped steel plate. The cold-rolled steel sheet was degreased and washed with water. Then, the steel sheet was subjected to cold-rolled sheet annealing. The cold-rolled sheet annealed steel sheet was immersed in a hot-dip galvanizing bath and then pulled out. Then, the coating weight was adjusted by gas wiping, and further cooling was performed to form a hot-dip galvanized layer on the steel sheet. In this manner, samples No. 1 to 110 (hot-dip galvanized steel members) shown in Tables 1A to 3C were produced.
[0077] For some samples, a chemical conversion layer was formed on the surface of the hot-dip plated layer after the formation of the hot-dip plated layer. The method for coating the aqueous composition used to form the chemical conversion layer was to apply the aqueous composition to the surface of the hot-dip plated layer by roll coating. Drying after application was performed by hot air drying. The heating temperature of the coated object was 50 to 250°C. The chemical conversion layer contained 20% by mass or more of resin and 1 to 20% by mass of silica particles having a particle size of 5 to 200 nm. The adhesion amount of the chemical conversion layer was 0.1 to 15 g / m 2 The formed chemical conversion coating layers, except for No. 97, were colorless and transparent when observed visually.
[0078] The composition of the hot-dip plating layer was measured by the following method. First, a rectangular area of 50 mm x 50 mm was cut from the hot-dip plating steel member, which was free of obvious defects such as corrosion and was 50 mm away from the end, to take a sample. Next, the surface coating and chemical conversion coating layer were removed from the sample using a coating remover (Neo River SP-751, manufactured by Sansai Kako Co., Ltd.) that does not corrode the coating. If the surface coating and chemical conversion coating layers could not be sufficiently removed, they were removed by polishing with an abrasive that is lower in hardness than the plating layer. The hot-dip plating layer was then dissolved by immersing the sample in 5% hydrochloric acid containing an inhibitor (Hibiron, manufactured by Sugimura Chemical Industry Co., Ltd.). The composition of the hot-dip plating layer was determined by inductively coupled plasma (ICP) emission spectrometry. However, for Si, which could not be accurately analyzed by the above method, the obtained solution was further treated by acid decomposition and sodium carbonate fusion method based on JIS G1258-3, and then analyzed. The average composition of the hot-dip plated layer was almost the same as the composition of the hot-dip plated bath, except for Fe. The Fe content of the hot-dip plated layer was 0.0001 to 2 mass % in all examples.
[0079] For cooling after gas wiping, a cooling device with multiple cooling nozzles that spray the coolant toward one side and the other side of the steel plate was used. Multiple spray nozzles were arranged at 25 mm intervals. The coolant was air with oxygen added to it, with a composition of 26% oxygen and 74% nitrogen. For cooling, the coolant was not sprayed from all the spray nozzles at the same time, but was sprayed from some of the spray nozzles while the spray nozzles spraying the coolant were randomly switched. The spray nozzles were switched on and off at 0.1 second intervals, and random numbers were used to randomly switch so that the coolant was sprayed from 30 to 60% of the total spray nozzles. The coolant flow rate was adjusted to be 5 to 20°C / s as the average cooling rate of the entire steel plate.
[0080] However, for No. 103 and No. 109, cooling after gas wiping was performed under conventional conditions. In other words, the coolant was air without adding additional oxygen. In addition, the spray nozzle was not turned on and off randomly. The coolant flow rate was adjusted so that the average cooling rate of the entire steel sheet was 5 to 20°C / s.
[0081] For Nos. 104 and 110, oxygen was added to air to cool the steel using a gas with a composition of 26% oxygen and 74% nitrogen. Cooling was not performed by simultaneously spraying the coolant from all the injection nozzles, but rather by spraying the coolant from some of the nozzles while randomly switching the nozzles spraying the coolant. The injection nozzles were switched on and off at 0.1 second intervals, and random numbers were used to randomly switch the nozzles so that 80% of the injection nozzles sprayed the coolant. The coolant flow rate was adjusted to be 5 to 20°C / s as the average cooling rate for the entire steel plate.
[0082] Furthermore, for No. 97, a white pigment was added to the above-mentioned chemical conversion coating layer to make it opaque. For No. 97, the total area ratio of white pixels and glossiness were evaluated before the formation of the chemical conversion coating layer, and the corrosion resistance, adhesion, and conductivity were evaluated after the formation of the chemical conversion coating layer, as described below, but the appearance evaluation and the conspicuousness of scratches were omitted.
[0083] A rectangular area with a side length of 100 mm was set as the photographing area for the hot-dip plating layer on one side of the obtained hot-dip plated steel member. A sample including the set photographing area and its surroundings was cut out from the hot-dip plated steel member. Then, the surface of the hot-dip plating layer of the cut-out sample was scanned with a flatbed scanner connected to a computer to obtain image data. For samples having a chemical conversion layer, scanning was performed from above the chemical conversion layer to obtain image data. The image data was extracted as image data of 256 grayscale levels with a resolution of 300 dpi. If localized unevenness in brightness occurred in the image data, the localized unevenness in brightness was eliminated by image correction.
[0084] Next, the obtained image data was subjected to binarization processing by the above-mentioned Otsu's binarization method to obtain binarized image data. The binarization processing by the Otsu's binarization method was performed by a computer with a pre-installed program. Then, the total area ratio of white pixels in the binarized image data was calculated. The results are shown in Tables 2A to 2C.
[0085] (Metal appearance) The metallic appearance was evaluated based on the appearance of the surface when the surface of the hot-dip plated layer of the hot-dip plated steel member was shown to five panelists. That is, the metallic appearance was evaluated based on whether each panelist could visually recognize the metallic appearance of the plated layer surface. The evaluation was based on the following scoring system, with a score of 3 or 2 being considered a pass. The results are shown in Tables 3A to 3C.
[0086] 3: More than 3 out of 5 people were able to see the metallic appearance of the plating. 2: Two out of five people were able to see the metallic appearance of the plating. 1: Less than 1 in 5 people could see the metallic appearance of the plating.
[0087] (60 degree mirror gloss Gs(60°)) Using a glossmeter, the 60° gloss (%) was measured for each of the areas corresponding to the aggregated areas of white pixels and the areas corresponding to the aggregated areas of black pixels of the hot-dip plated layer, based on the method specified in JIS Z 8741. The 60° specular gloss Gs(60°) was calculated from the obtained 60° gloss (%) based on the description in JIS Z 8741.
[0088] A white pixel aggregation region is a rectangular region of 3 mm square where the area ratio of white pixels is 60% or more in the binarized image data.A black pixel aggregation region is a rectangular region of 3 mm square where the area ratio of black pixels is 60% or more in the binarized image data.
[0089] (Appearance evaluation) In addition, the visual invisibility of scratches was evaluated. The plating appearance was evaluated visually. Specifically, after making a scratch on the plating layer surface, if the scratch was not visible from a distance of 2 m, the invisibility of the scratches was judged to be good and rated as F. On the other hand, if the scratch was visible even from a distance of 2 m, the invisibility of the scratches was deemed insufficient and rated as P. F was judged to be pass.
[0090] (Corrosion resistance) The corrosion resistance of hot-dip galvanized steel members was evaluated by corrosion weight loss after the CCT test. The hot-dip galvanized steel members were cut into 150 x 70 mm pieces, and the corrosion weight loss after 30 cycles of CCT was investigated using a CCT in accordance with JASO-M609. Corrosion weight loss: 30 g / m 2 F: corrosion weight loss of less than 30g / m 2 More than 50g / m 2 G: corrosion weight loss of less than 50g / m 2 The above cases were rated as P, and F and G were rated as pass. The results are shown in Tables 3A to 3C. When a chemical conversion coating layer was present, it was removed and then the corrosion resistance was evaluated.
[0091] (Adhesion) The adhesion of the chemical conversion coating layer was evaluated as follows. First, the test piece was immersed in boiling water for 30 minutes, and then a checkerboard pattern of cuts was made on the surface of the test piece at intervals of 1 mm, and the percentage of cuts where the chemical conversion coating layer remained without peeling (number of cuts remaining / number of cuts (100)) was investigated. In other words, the adhesion of the chemical conversion coating layer was evaluated based on the percentage of the 100 checkerboard cuts where peeling of the chemical conversion coating layer was not observed. Peeling of the chemical conversion coating layer was observed with a scanning electron microscope. The evaluation criteria for adhesion were as follows, with F and G being judged as passing. <Evaluation criteria> F=95% or more G = 90% or more but less than 95% P = less than 90%
[0092] (Conductive) The electrical conductivity was evaluated as follows. First, a test piece was cut out from the hot-dip galvanized steel member on which the chemical conversion coating layer was formed, and the interlaminar resistance (Ω cm) was measured using the obtained test piece in accordance with the method for measuring surface insulation resistance specified in JIS C 2550:2019. 2 The test voltage was 0.5 V, the measurement current range was 0 to 1 A, and the contact area of the 10 contact electrodes was 1 cm 2 x 10, test pressure 2N / mm 2 ±5%. Interlayer resistance is 5Ω cm 2 Less than P, Ω cm 2 More than 7Ω cm 2 Less than G, 7 Ω cm 2 The above was rated F.
[0093] As shown in Tables 1A to 3C, Nos. 1 to 48 are examples in which no chemical conversion coating layer was formed. Nos. 1 to 48 had chemical components in the hot-dip plating layer that satisfied the range of the present invention, and the manufacturing conditions were within the preferred range, so the total area ratio of white pixels was in the range of 30 to 70%, and they showed a good appearance. They also had excellent corrosion resistance.
[0094] As shown in Tables 1B to 3C, Nos. 49 to 98 were formed with a chemical conversion coating layer. Nos. 49 to 98 had the chemical components of the hot-dip plating layer within the range of the present invention, and the manufacturing conditions were within the preferred range, so the total area ratio of white pixels was in the range of 30 to 70%, and they showed a good appearance. They also had excellent corrosion resistance. Furthermore, the adhesion of the chemical conversion coating layer was excellent, and the interlayer resistance was low, so the conductivity with the welding electrode was good and the weldability was also excellent.
[0095] No. 99 to 102 were formed with a chemical conversion coating layer. No. 99 to 102 had reduced corrosion resistance because the chemical components of the hot-dip plating layer were outside the range of the present invention.
[0096] No chemical conversion coating layer was formed on No. 103. Although the chemical composition of the hot-dip plating layer of No. 103 satisfied the range of the present invention, the cooling conditions after hot-dip plating were conventional cooling conditions, so that the total area ratio of white pixels was less than 30%, and defects were easily noticeable.
[0097] No. 104 was formed with a chemical conversion coating layer. Although the chemical composition of the hot-dip plating layer of No. 104 satisfied the range of the present invention, the cooling conditions after hot-dip plating were outside the preferred cooling conditions, so that the total area ratio of white pixels exceeded 70%, and a metallic appearance was not obtained, resulting in a deterioration in appearance.
[0098] A chemical conversion coating layer was formed in Nos. 105 to 108. Nos. 105 to 108 had reduced corrosion resistance because the chemical components of the hot-dip plating layer were outside the range of the present invention.
[0099] No. 109 was formed with a chemical conversion coating layer. Although the chemical composition of the hot-dip coating layer of No. 109 satisfied the range of the present invention, the cooling conditions after hot-dip coating were conventional cooling conditions, so the total area ratio of white pixels was less than 30%, and scratches were easily noticeable. In addition, the adhesion of the chemical conversion coating layer was reduced.
[0100] No. 110 was formed with a chemical conversion coating layer. Although the chemical composition of the hot-dip plating layer of No. 110 satisfied the range of the present invention, the cooling conditions after hot-dip plating were not within the preferred cooling conditions, so the total area ratio of white pixels exceeded 70%, and a metallic appearance was not obtained, resulting in poor appearance. In addition, the electrical conductivity was reduced, and the weldability was poor.
[0101] [Table 1A]
[0102] [Table 1B]
[0103] [Table 1C]
[0104] [Table 2A]
[0105] [Table 2B]
[0106] [Table 2C]
[0107] [Table 3A]
[0108] [Table 3B]
[0109] [Table 3C] [Industrial Applicability]
[0110] The Zn-Al-Mg-based hot-dip plated steel member of the present disclosure has excellent corrosion resistance and adhesion of a chemical conversion coating layer, and even when a chemical conversion coating layer is formed, has excellent electrical conductivity with a welding electrode. Furthermore, it has an excellent appearance in which scratches are less noticeable, and therefore has high industrial applicability. [Explanation of symbols]
[0111] 1...Steel plate 2. Hot-dip galvanizing bath 3. Sync Roll 4…Wiping nozzle 5…Cooling device
Claims
1. A steel member and a hot-dip plating layer disposed on a surface of the steel member, The average composition of the hot-dip plating layer is, in mass%, Al: 4 to 22%, Mg: 1.0-10.0%, Fe: 0.0001-2%, Si: 0 to 2%, Ni: 0 to 2%, Ti: 0 to 2%, Zr: 0 to 2%, Sr: 0 to 2%, Sb: 0 to 2%, Pb: 0 to 2%, Sn: 0 to 2%, Ca: 0 to 2%, Co: 0 to 2%, Mn: 0 to 2%, P: 0 to 2%, B: 0 to 2%, Bi: 0 to 2%, Cr: 0 to 2%, Sc: 0 to 2%, Y: 0-2%, REM: 0-2%, Hf: 0 to 2%, and C: 0 to 2% with the remainder being Zn and impurities, In the binary image data of the image data obtained by capturing an image of the surface of the hot-dip plating layer, the total area ratio of white pixels is 30% or more and 70% or less, The binary image data of the Zn-Al-Mg based hot-dip plated steel member is obtained by binarizing the image data by Otsu's binarization method.
2. The Zn-Al-Mg hot-dip plated steel member according to claim 1, further comprising a chemical conversion treatment layer on a surface of the hot-dip plated layer.
3. The Zn-Al-Mg hot-dip plated steel member according to claim 2, wherein the chemical conversion coating layer has a metallic appearance.
4. The 60-degree specular gloss Gs(60°) of the surface of the hot-dip plating layer corresponding to the white pixel aggregation region is 150 or less, 2. The Zn-Al-Mg based hot-dip plated steel member according to claim 1, wherein a 60 degree specular gloss Gs (60°) of a surface of the hot-dip plated layer corresponding to a region where black pixels are gathered is 1.5 times or more a 60 degree specular gloss Gs (60°) of a surface of the hot-dip plated layer corresponding to a region where white pixels are gathered.
5. The 60-degree specular gloss Gs(60°) of the surface of the hot-dip plating layer corresponding to the white pixel aggregation region is 150 or less, 3. The Zn-Al-Mg based hot-dip plated steel member according to claim 2, wherein a 60 degree specular gloss Gs (60°) of a surface of the hot-dip plated layer corresponding to a region where black pixels are gathered is 1.5 times or more a 60 degree specular gloss Gs (60°) of a surface of the hot-dip plated layer corresponding to a region where white pixels are gathered.
6. The 60-degree specular gloss Gs(60°) of the surface of the hot-dip plating layer corresponding to the white pixel collection region is 70 or less, 2. The Zn-Al-Mg based hot-dip plated steel member according to claim 1, wherein a 60 degree specular gloss Gs (60°) of a surface of the hot-dip plated layer corresponding to a region where black pixels are gathered is 1.5 times or more a 60 degree specular gloss Gs (60°) of a surface of the hot-dip plated layer corresponding to a region where white pixels are gathered.
7. The Zn-Al-Mg hot-dip plated steel member according to any one of claims 1 to 6, wherein the average composition of the hot-dip plated layer contains one or more selected from the following Group A, Group B, or Group C: Group A: Si: 0.0001-2% Group B: Ni, Ti, Zr, Sr, or any one or more of them, 0.0001 to 2% in total Group C: Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, C, any one or more of these, 0.0001 to 2% in total
8. The Zn-Al-Mg hot-dip plated steel member according to claim 5, wherein the average composition of the hot-dip plated layer contains the Group A alloy.
9. The Zn-Al-Mg hot-dip plated steel member according to claim 5, wherein the average composition of the hot-dip plated layer contains the B group.
10. The Zn-Al-Mg hot-dip plated steel member according to claim 5, wherein the average composition of the hot-dip plated layer contains the C group.
Citation Information
Patent Citations
Zinc-based double layer-plated steel material and method for producing the same
JP2011241458A
Coated steel plate and mehtod for manufacturing the same
KR1020150135605A
Zn-Al-Mg HOT-DIP COATED STEEL SHEET AND PROCESS FOR PRODUCTION THEREOF
WO2011001662A1
Zn-Al-Mg-BASED HOT-DIP PLATED STEEL SHEET AND METHOD FOR PRODUCING SAME
WO2019230894A1
Hot dip plated steel sheet
WO2021199953A1