Compound semiconductor polishing pad and method for manufacturing porous resin body

The porous resin body with PES or PVDF-HFP resin and fine pores addresses the issues of resin deterioration and scratches in polishing pads, ensuring long-lasting performance and effective polishing of compound semiconductor wafers.

JP7571326B1Active Publication Date: 2024-10-22NORITAKE MACHINE TECHNO CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024052458
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-10-22
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Existing compound semiconductor polishing pads suffer from short service life due to resin deterioration when using permanganate-based strong oxidizing agents, leading to surface roughness issues and scratches during polishing of difficult-to-polish wafers.

Method used

A porous resin body made of PES (polyethersulfone) resin or PVDF-HFP (copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) with fine pores of 2 to 20 μm, manufactured by dissolving the resin in a high melting point organic solvent like 2-pyrrolidone or DMSO, precipitating solids in cold water, and replacing them with hot water to form a polishing pad with high oxidant resistance and abrasion resistance.

Benefits of technology

The polishing pad maintains a high polishing rate and surface roughness for an extended period without scratches, effectively polishing difficult-to-polish wafers using a permanganate-based strong oxidizing agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571326000001_ABST
    Figure 0007571326000001_ABST
Patent Text Reader

Abstract

A porous resin body having fine pores, a compound semiconductor polishing pad, and a method for producing the porous resin body are provided. [Solution] The method for producing a resin porous body includes a melt preparation process P1 in which a base resin is melted in a high-melting point organic solvent having a melting point at room temperature to obtain a melt; a molding process P2 in which the melt is molded into a thin plate to obtain a thin plate-like molded body; a precipitation process P3 in which the thin plate-like molded body is left in cold water that is lower in temperature than the melting point of the high-melting point organic solvent to finely precipitate the high-melting point organic solvent in the thin plate-like molded body; a replacement process P4 in which the thin plate-like molded body that has undergone the precipitation process P3 is left in warm water that is higher in temperature than both the cold water and the melting point of the high-melting point organic solvent to replace the solid of the high-melting point organic solvent precipitated in the thin plate-like molded body with water; and a drying process P5 in which the thin plate-like molded body is dried until all moisture is removed from it.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous resin body, a compound semiconductor polishing pad using the porous resin body, and a method for producing the porous resin body. [Background technology]

[0002] There is a demand for resin porous bodies that are highly chemical-resistant and have fine pores for use in compound semiconductor polishing pads for polishing compound semiconductor wafers, water-adhesive pads for fixing compound semiconductor wafers on polishing disks, synthetic leather, vibration-proof sheets, soundproofing materials, water-absorbing and water-retaining bodies, separators and separation membranes for fuel cells, and the like.

[0003] For example, semiconductor wafers such as SiC wafers, GaN wafers, Si wafers, and Si oxide wafers are known to be difficult to polish. A polishing method based on the CMP method has been proposed for polishing such semiconductor wafers using a resin polishing pad that mechanically promotes polishing and a polishing solution that chemically promotes polishing. For example, the polishing method described in Patent Document 1 is one such method. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-057368 Summary of the Invention [Problem to be solved by the invention]

[0005] However, when the hard-to-polish wafer is polished on a polishing pad using a polishing solution containing a strong oxidizing agent such as potassium permanganate, if the resin constituting the polishing pad is a resin with low resistance to the oxidizing agent, such as a foamed polyurethane resin, the resin deteriorates, and the surface roughness and shape of the polishing material are easily deteriorated, resulting in a short service life of the polishing pad. On the other hand, when a polishing pad with a high proportion of polyurethane resin in the polishing pad and fewer pores is used, the service life is longer, but there is a problem that scratches are easily caused due to the small number of pores.

[0006] The present invention has been made against the background of the above circumstances, and an object of the present invention is to provide a resin porous body which, when used in a compound semiconductor polishing pad, causes no scratches when polishing difficult-to-polish wafers and can maintain the polishing rate and surface roughness for a long period of time, a compound semiconductor polishing pad using this resin porous body, and a manufacturing method for obtaining them.

[0007] The inventor of the present invention has conducted various studies in the light of the above circumstances. As a result, when a PES (polyethersulfone) resin, which is highly resistant to a strong oxidizing agent such as permanganate, is dissolved in a solvent having a melting point at room temperature, the resulting melt is molded into a predetermined shape, and the molded body is cooled to a temperature lower than the melting point of the solvent, the solvent precipitates as a fine solid in the melt, and when the precipitated solid is replaced with water, a resin porous body having fine pores with an average diameter of about 2 to 20 μm is obtained. Then, the inventor has found that when polishing is performed with a polishing pad using the resin porous body, the action of the fine pores prevents scratches, and the polishing rate and surface roughness can be maintained for a long time. The present invention is based on this finding. [Means for solving the problem]

[0008] That is, the gist of the first invention is a resin porous body having (1) a base resin which is a PES (polyethersulfone) resin or a PVDF-HFP (copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin, and (2) micropores formed in the base resin, the size of the micropores being 2 to 20 μm. A compound semiconductor polishing pad made of a resin porous body, (3) the compound semiconductor polishing pad is used to polish a hard-to-polish compound semiconductor wafer using a polishing solution containing a permanganate-based strong oxidizing agent, and (4) the compound semiconductor polishing pad has 54.3 to 65.1 volume % pores, 34.9 to 45.7 volume % PES resin, and a durometer hardness (Type-D) of 34.0 to 54.0. The point is...

[0010] No. 2 The gist of the invention is (1) a method for producing a resin porous body having high resistance to oxidizing agents and abrasion resistance and fine pores, comprising: (2) a melt preparation step in which a base resin having high resistance to oxidizing agents and abrasion resistance is melted in a high-melting-point organic solvent that has a melting point at room temperature (10 to 30°C) and is soluble in water to obtain a melt; (3) a molding step in which the melt is molded into a thin plate to obtain a thin plate-like molded body; and (4) a process in which the thin plate-like molded body is molded at a temperature lower than the melting point of the high-melting-point organic solvent. (5) a replacement step of leaving the thin plate-shaped body after the precipitation step in hot water having a temperature higher than the temperature of the cold water and the melting point of the high-melting point organic solvent to replace the solid of the high-melting point organic solvent finely precipitated in the thin plate-shaped body with water; and (6) a drying step of drying the thin plate-shaped body until no moisture remains in the thin plate-shaped body. (7) The base resin is PES (polyethersulfone) resin or PVDF-HFP (a copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin. The point is...

[0012] No. 3 The gist of the invention is as follows: 2 In the present invention, the high melting point organic solvent is 2-pyrrolidone having a melting point of 24.6° C. or DMSO (dimethyl sulfoxide) having a melting point of 18.4° C. If room temperature is defined as 10° C. to 30° C., 2-pyrrolidone and DMSO have melting points at room temperature and are solvents that dissolve PES (polyethersulfone) resin and PVDF-HFP resin.

[0013] No. 4 The gist of the invention is as follows: 2In the present invention, the high melting point organic solvent is a solvent that disperses in water and dissolves the PES (polyethersulfone) resin and the PVDF-HFP (a copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin.

[0014] No. 5 The gist of the invention is as follows: 2 In the present invention, the precipitation step involves leaving the thin plate-shaped body in the cold water at 5 to 10°C, and the replacement step involves leaving the thin plate-shaped body that has undergone the precipitation step in the warm water at 40 to 60°C.

[0015] No. 6 The gist of the invention is as follows: 2 In the present invention, the resin porous body has fine pores with an average diameter of 2 to 20 μm, preferably 2 to 10 μm. Effect of the Invention

[0017] The first invention Compound semiconductor polishing pads It is a resin porous body made of PES (polyethersulfone) resin or PVDF-HFP (a copolymer of 80% polyvinylidene fluoride and 20% hexafluoropropylene) resin, which has high resistance to oxidizing agents and abrasion, and the size of the micropores formed in the base resin is 2 to 20 μm. A compound semiconductor polishing pad made of a resin porous body, the compound semiconductor polishing pad is used to polish a difficult-to-polish compound semiconductor wafer using a polishing solution containing a permanganic acid-based strong oxidizing agent, and the compound semiconductor polishing pad has 54.3 to 65.1 volume % of pores, 34.9 to 45.7 volume % of PES resin, and a durometer hardness (Type-D) of 34.0 to 54.0. Therefore, when the resin is used as the base resin of a compound semiconductor polishing pad used in CMP polishing of difficult-to-polish wafers, which is performed using a polishing liquid that mechanically promotes polishing while also chemically promoting polishing, a compound semiconductor polishing pad that is free of scratches and can maintain the polishing rate and surface roughness for a long period of time can be obtained. In addition, since the compound semiconductor polishing pad has 54.3 to 65.1 volume % pores, 34.9 to 45.7 volume % PES resin, and a durometer hardness of 34.0 to 54.0, when it is used to polish difficult-to-polish compound semiconductor wafers by the CMP method using a polishing liquid containing a permanganate-based strong oxidizing agent, there are no scratches and the polishing rate and surface roughness can be maintained for a long time.

[0019] No. 2The method for producing a resin porous body having micropores and high resistance to oxidizing agents and abrasion is provided by the present invention, which includes a melt preparation step of melting a base resin having high resistance to oxidizing agents and abrasion in a high-melting-point organic solvent having a melting point at room temperature (10 to 30°C) and soluble in water to obtain a melt; a molding step of molding the melt into a thin plate to obtain a thin plate-like molded body; a precipitation step of leaving the thin plate-like molded body in cold water at a temperature lower than the melting point of the high-melting-point organic solvent to finely precipitate a solid of the high-melting-point organic solvent in the thin plate-like molded body; a replacement step of leaving the thin plate-like molded body that has been subjected to the precipitation step in hot water at a temperature higher than the cold water and the melting point of the high-melting-point organic solvent to replace the solid of the high-melting-point organic solvent finely precipitated in the thin plate-like molded body with water; and a drying step of drying the thin plate-like molded body until no moisture remains in the thin plate-like molded body. The base resin is PES (polyethersulfone) resin or PVDF-HFP (copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin. As a result, minute pores are formed in the resin, which has high resistance to oxidizing agents and abrasion, and this makes it possible to obtain a compound semiconductor polishing pad that is free from scratches when polishing difficult-to-polish wafers and that can maintain the polishing rate and surface roughness for a long period of time. In addition, since the base resin is PES (polyethersulfone) resin or PVDF-HFP (a copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin, a resin porous body with high resistance to oxidizing agents and abrasion is obtained.

[0021] No. 3 In the invention, the high melting point organic solvent is 2-pyrrolidone having a melting point of 24.6° C. or DMSO (dimethyl sulfoxide) having a melting point of 18.4° C. Thus, in the precipitation step, the thin plate-shaped body is left in cold water at a temperature lower than the melting point of the high melting point organic solvent, whereby the solid of the high melting point organic solvent can be finely precipitated in the thin plate-shaped body.

[0022] No. 4 In the present invention, the high-melting organic solvent is a solvent that diffuses in water and dissolves PES (polyethersulfone) resin and PVDF-HFP resin. This allows the thin plate-shaped molded body that has been subjected to the precipitation step to be left in hot water that is higher than the temperature of the cold water and the melting point of the high-melting organic solvent, so that the solid of the high-melting organic solvent that has precipitated finely in the thin plate-shaped molded body can be replaced with water.

[0023] No. 5In the present invention, the precipitation step involves leaving the thin plate-like molded body in cold water at 5 to 10° C., and the replacement step involves leaving the thin plate-like molded body that has been subjected to the precipitation step in warm water at 40 to 60° C., which is sufficiently higher than the melting point of the high-melting-point organic solvent. This allows the high-melting-point organic solvent solid to be finely precipitated in the thin plate-like molded body, and then the high-melting-point organic solvent solid precipitated in the thin plate-like molded body is replaced with water in the warm water.

[0024] No. 6 In the present invention, the resin porous body has micropores with an average diameter of 2 to 20 μm, preferably 2 to 10 μm, which has the advantage that when a compound semiconductor wafer that is difficult to polish is polished with a compound semiconductor polishing pad made of the resin porous body, the edges of the many micropores contribute to the polishing mechanism, making it difficult for scratches to occur, and thus a favorable polishing rate and surface roughness can be obtained. [Brief description of the drawings]

[0026] [Figure 1] 1 is a perspective view showing a schematic diagram of a surface polishing apparatus used for polishing by a CMP method in which a polishing pad according to an embodiment of the present invention is used. [Diagram 2] 2 is a plan view for explaining a rotation mechanism of an application disk of the surface polishing apparatus of FIG. 1. FIG. [Diagram 3] 2 is a process diagram illustrating a manufacturing process for manufacturing a resin porous body constituting the polishing pad of FIG. 1. [Figure 4] FIG. 2 is a diagram showing the chemical structure of a PES resin (polyethersulfone resin), which is an example of a resin constituting the polishing pad of FIG. [Diagram 5] FIG. 2 is a diagram showing the chemical structure of PVDF-HFP resin (polyvinylidene fluoride 80% + hexafluoropropylene 20% copolymer resin), which is another example of the resin constituting the polishing pad of FIG. [Figure 6] 1 is a table showing samples used in polishing test 1 and the results of the polishing test. [Figure 7] 1 is a table showing the resin proportion, pore proportion, and durometer hardness of Examples 1 to 4 in the samples used in Polishing Test 1. [Figure 8] FIG. 2 is a SEM photograph of a cross section of Example Product 3 in the sample used in Polishing Test 1, showing pores in Example Product 3. [Figure 9] FIG. 2 is a SEM photograph of a cross section of Comparative Example 1 in a sample used in Polishing Test 1, showing pores in Comparative Example 1. [Figure 10] FIG. 2 is a SEM photograph of a cross section of Comparative Example 2 in the sample used in Polishing Test 1, showing pores in Comparative Example 2. [Figure 11] 1 is a graph showing the polishing rate PR, surface roughness Sa, and number of scratches obtained using Example 3 in Polishing Test 2 over time. [Figure 12] 12 is a line graph showing the change in the polishing rate PR in FIG. 11. [Figure 13] 12 is a line graph showing the change in surface roughness Sa in FIG. 11. [Figure 14] 12 is a line graph showing the change in the number of scratches in FIG. 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] An embodiment of the present invention will now be described with reference to the drawings. Note that in the following embodiment, the drawings are appropriately simplified or modified, and the dimensional ratios and shapes of the various parts are not necessarily drawn accurately. EXAMPLES

[0028] Fig. 1 conceptually shows the main part of a surface polishing apparatus 10 for polishing hard-to-polish compound semiconductor wafers such as SiC wafers, GaN wafers, and InP wafers, as an example of the present invention, with the guide roller fixing table removed. In Fig. 1, the surface polishing apparatus 10 is provided with a circular polishing platen (rotary table) 12 rotatably supported about its vertical rotation axis C1, and the polishing platen 12 is rotated at a constant speed in one rotation direction indicated by an arrow in the figure by a platen driving motor 14. A compound semiconductor polishing pad (hereinafter referred to as polishing pad) 18 made of a sheet-like resin porous body 17 is attached to the upper surface of the polishing platen 12, i.e., the surface against which a workpiece (hard-to-polish compound semiconductor wafer) 16 is pressed.

[0029] The workpiece 16 is held on the lower surface of the application disc 20, i.e., the surface facing the polishing pad 18, and the application disc 20 presses the workpiece 16 against the polishing pad 18 with a predetermined load. A drip nozzle 22 is provided near the application disc 20 of the surface polishing device 10, and a strongly acidic polishing solution PF containing a strong oxidizing agent of permanganate such as potassium permanganate (KMnO4) added thereto is supplied onto the polishing table 12 from a tank (not shown).

[0030] The surface polishing apparatus 10 is provided, as required, with an adjustment tool holding member (not shown) that is arranged rotatable about the rotation axis C1 of the polishing table 12 and movable in the direction of the rotation axis C1 and in the radial direction of the polishing table 12, and an abrasive body adjustment tool (dresser or conditioner) such as a diamond wheel (not shown) that is attached to the lower surface of the adjustment tool holding member, i.e., the surface facing the polishing pad 18. The adjustment tool holding member and the abrasive body adjustment tool attached thereto are pressed against the polishing pad 18 while being rotated and driven by an adjustment tool drive motor (not shown), and are moved back and forth in the radial direction of the polishing table 12, thereby adjusting the polishing surface of the polishing pad 18 and constantly maintaining the surface state of the polishing pad 18 in a state suitable for polishing.

[0031] 2, at a position eccentric from the rotation axis C1 on the polishing table 12, the outer peripheral surface of a short cylindrical attachment disk 20, which holds the workpiece 16 to be polished on its underside by suction, adhesion, or a holding frame, is received by a pair of rotatable guide rollers 30 and a drive guide roller 32 provided on a guide roller fixing base 28, which is fixed in a position and fixed to a frame (not shown), so that the attachment disk 20 can rotate about the rotation axis C2. The attachment disk 20 is rotated about the rotation axis C2 by a rotation force based on the difference in peripheral speed between the polishing table 12 or the polishing pad 18, and the attachment disk 20 is pressed against the polishing pad 18 on the polishing table 12 by the load of, for example, a weight 34, thereby polishing the workpiece 16.

[0032] The following polishing method is applied during polishing by the surface polishing device 10. That is, while the polishing pad 18 attached to the polishing table 12, the attachment disk 20, and the workpiece 16 held on its lower surface are rotated around the rotation axis C1 and the rotation axis C2 by the table drive motor 14 and the drive guide roller 32, the polishing liquid PF not containing abrasive grains is supplied from the drip nozzle 22 onto the surface of the polishing pad 18, while the workpiece 16 held on the attachment disk 20 is pressed against the polishing pad 18. As a result, the surface to be polished of the workpiece 16, i.e., the surface facing the polishing pad 18, is polished flat by the chemical polishing action of the polishing liquid PF.

[0033] The polishing pad 18 is composed of a resin porous body 17 including fine pores with an average diameter of 2 to 20 μm, preferably 2 to 10 μm. The resin porous body 17 functions as a base resin of the polishing pad 18. The resin porous body 17 is made of PES (polyethersulfone) resin that does not contain abrasive grains, or PVDF-HFP resin (polyvinylidene fluoride 80% + propylene hexafluoride 20% copolymer resin) and is formed into a sheet shape with a thickness of about 2 to 3 mm. PES resin and PVDF-HFP resin have high resistance to the strong oxidizing agent of permanganate in the polishing liquid PF and abrasion resistance that allows a high polishing rate PR to be obtained. The PES resin is shown in the chemical structure of FIG. 4, and the PVDF-HFP resin is shown in the chemical structure of FIG. 5.

[0034] Polishing pad 18 preferably has 54.3 to 65.1 volume % pores, 34.9 to 45.7 volume % PES resin, and a durometer hardness (Type-D) of 34.0 to 54.0.

[0035] The resin porous body 17 constituting the polishing pad 18 is manufactured by the manufacturing steps P1 to P5 shown in Fig. 3. In Fig. 3, in the melt preparation step P1, PES resin or PVDF-HFP resin is heated and stirred at a temperature of 50°C or higher together with 2-pyrrolidone or DMSO (dimethyl sulfoxide), which is a high melting point organic solvent having a melting point at room temperature (10 to 30°C), to prepare a melt. Next, in the molding step P2, the melt is molded into a thin plate shape of about 2 to 3 mm by slip casting or blade casting to obtain a thin plate-like molded body. Next, in the precipitation step P3, the thin plate-like molded body is left in cold water at a temperature of, for example, 5 to 10°C lower than the melting point of 2-pyrrolidone for about 5 hours, so that a solid of the high melting point organic solvent (2-pyrrolidone or DMSO) is finely precipitated in the thin plate-like molded body. The fine precipitates (crystals) of 2-pyrrolidone form fine pores in the PES resin after the drying step P5 described below. The size of the fine pores is adjusted by the temperature of the cold water and the standing time, but the average diameter is preferably 2 to 20 μm, and more preferably 2 to 10 μm.

[0036] In the subsequent substitution step P4, the thin plate-shaped molded body that has been subjected to the precipitation step P3 is left in hot water, for example, at 40 to 60°C, which is higher than the temperature of the cold water and the melting point of 2-pyrrolidone, for about 5 hours, so that the solid of the high melting point organic solvent (2-pyrrolidone or DMSO) that has precipitated finely in the thin plate-shaped molded body is replaced with water and the thin plate-shaped molded body is hardened. Then, in the drying step P5, the thin plate-shaped molded body is dried until all moisture is removed from the thin plate-shaped molded body. This results in a thin plate-shaped resin porous body (base resin of polishing pad 18) 17 made of PES resin or PVDF-HFP resin having micropores of about 3 to 20 μm.

[0037] 2-pyrrolidone has a chemical formula of C4H7NO, a melting point of 24.6°C and a boiling point of 245°C, is soluble in water, and is capable of dissolving the base resin (PES resin or PVDF-HFP resin). DMSO (dimethyl sulfoxide) has a chemical formula of C2H6OS, a melting point of 18.4°C and a boiling point of 189°C, is soluble or diffusible in water, and is capable of dissolving the base resin (PES resin or PVDF-HFP resin). As described in the melt preparation step P1, the precipitation step P3, and the replacement step P4, other organic solvents other than 2-pyrrolidone and DMSO may be used as long as they can melt the PES resin, precipitate at the temperature of cold water, and replace it with water at the temperature of hot water.

[0038] [Polishing test 1] The present inventors have conducted a polishing test 1 for semiconductor wafers as follows. In the polishing test 1, comparative examples 1-2 and examples 1-5 shown in FIG. 6 were applied to an apparatus configured similarly to the surface polishing apparatus 10 shown in FIG. 1, and a 4-inch diameter SiC wafer was polished under the test conditions of the polishing test 1 described below. Examples 1-4 were produced using the manufacturing process shown in FIG. 3 so that the ratio of PES resin to 2-pyrrolidone was different from one another. FIG. 7 shows the volume ratio of PES resin, the volume ratio of pores, and durometer hardness (Type-D) of the examples 1-4. FIG. 8 shows an SEM photograph of example 3, which represents examples 1-5. From the SEM photograph in FIG. 8, fine pores of about 2-20 μm or 2-10 μm are observed. Comparative example 1 is made of a hard polyurethane resin in which pores of 20-40 μm are formed by a pore-forming agent. FIG. 9 shows an SEM photograph of comparative example 1. Pores of about 20 to 40 μm are observed in the SEM photograph of Fig. 9. Comparative Example 2 is a nonwoven fabric in which intertwined polyester fibers are bonded with polyurethane resin, and gaps of about 100 μm are formed between the fibers. Fig. 10 shows an SEM photograph of Comparative Example 2. Large pores of about 100 μm are observed in the SEM photograph of Fig. 10.

[0039] The polishing rate PR, surface roughness Sa, and number of scratches of the SiC wafer after the polishing test of Polishing Test 1 and the polishing test of Polishing Test 2 described below were measured by the following methods.

[0040] [Test conditions for polishing test 1] Workpiece: 4-inch diameter SiC wafer (0001) Si surface, tilt angle 4° Workpiece rotation speed: 60 rpm Polishing pad diameter: 300mmφ Polishing pad rotation speed: 60 rpm Polishing pressure: 42kPa Polishing liquid: KMnO4 (0.25mol / l) pH=3.2 (Abrasive grains not included) Polishing liquid flow rate: 10ml / min Polishing time: [Comparative example 1] 200 hours [Comparative Example 2] 70 hours [Example 1] 2 hours [Example 2] 2 hours [Example 3] 200 hours [Example 4] 2 hours [Example 5] 2 hours

[0041] [Method for measuring polishing rate PR] The difference in mass of the SiC wafer before and after the polishing test was determined using an analytical balance, and the amount of polishing (wear thickness) was calculated from the known density of the SiC wafer and the surface area of ​​the polished surface. The polishing rate PR (nm / h) was calculated by dividing the amount of polishing by the polishing time.

[0042] [Surface roughness Sa measurement method] The surface roughness Sa of the surface profile of the polished surface of the SiC wafer after the polishing test was measured using a white light interference microscope (Hitachi High-Tech VS-1330), and the arithmetic mean surface roughness Sa specified in ISO25178 was calculated.

[0043] [Method of measuring the number of scratches] The polished surface of the SiC wafer was observed using a confocal differential contrast microscope (Lasertec Corporation, OPTELICS HYBRID), and scratches detected using the included scratch assessment software were counted as one.

[0044] FIG. 6 shows the polishing test results (polishing rate PR (nm / h) and surface roughness Sa (nm) of the polished surface) and the number of scratches (count) when using Example products 1 to 5 and Comparative examples 1 to 2, respectively. The polishing results show that Example products 1 to 5 have a higher polishing rate PR (nm / h) than Comparative examples 1 to 2. Also, Example products 1 to 5 have a better surface roughness Sa than Comparative examples 1 to 2. SiC wafers are polished while supported by the edges of bubbles, but Example products 1 to 5 have fine pores and are supported by many edges, which is thought to be the reason for the above polishing results.

[0045] [Polishing test 2] Example product 3 in Figure 7 was applied to an apparatus configured similarly to surface polishing apparatus 10 shown in Figure 1, and a 4-inch φ SiC wafer was polished under the same conditions as those in Polishing Test 1 except for the polishing time. The polishing rate PR (nm / h), surface roughness Sa (nm) of the polished surface, and the number of scratches (count) were measured 22 times each time the polishing time elapsed until 200 hours had elapsed.

[0046] FIG. 11 shows the polishing rate PR (nm / h), the surface roughness Sa (nm) of the polished surface, and the number of scratches (count) obtained from the 22 measurements. FIG. 12 is a line graph showing the change in the polishing rate PR during polishing of the SiC wafer. FIG. 13 is a line graph showing the change in the surface roughness Sa during polishing of the SiC wafer. FIG. 14 is a line graph showing the change in the number of scratches during polishing of the SiC wafer. In FIG. 12 to FIG. 14, the circle marks indicate the values ​​of Example 3, the triangle marks indicate the values ​​of Comparative Example 1, and the square marks indicate the values ​​of Comparative Example 2.

[0047] As shown in Fig. 12, Example Product 3 exhibits a higher polishing rate PR than Comparative Example Product 1, and remains at a substantially constant value. The polishing rate PR of Comparative Example Product 2 is generally low and decreases with polishing time, and after 70 hours, fluffing occurs and the periphery of the pad is chipped, making polishing impossible. The polyester fiber (nonwoven fabric) of Comparative Example Product 2 is considered to have low resistance to strong oxidizing agents.

[0048] 13, Example 3 exhibits a lower surface roughness Sa than Comparative Example 1, and remains at a substantially constant value. The surface roughness Sa of Comparative Example 1 changes periodically, while the surface roughness Sa of Comparative Example 2 increases with the polishing time, becoming unpolishable after 70 hours.

[0049] 14, Example Product 3 has fewer scratches than Comparative Example Product 1, and the number of scratches remains constant (value "0"). Comparative Example Product 1 has a periodic increase in the number of scratches, while Comparative Example Product 2 has an increase in the number of scratches with the passage of polishing time, and becomes unpolishable after 70 hours.

[0050] As described above, according to the resin porous body 17 of this embodiment, the base resin is PES (polyethersulfone) resin or PVDF-HFP (a copolymer of 80% polyvinylidene fluoride and 20% hexafluoropropylene) resin, which has high resistance to oxidizing agents and abrasion, and the size of the micropores formed in the base resin is 2 to 20 μm. Therefore, since the resin porous body 17 is used as the base resin of a compound semiconductor polishing pad used in polishing by the CMP method, which uses a resin polishing pad that mechanically promotes polishing and a polishing liquid that chemically promotes polishing when polishing a difficult-to-polish wafer by the CMP method, a compound semiconductor polishing pad that is free of scratches and can maintain the polishing rate and surface roughness for a long time can be obtained.

[0051] Since the resin porous body 17 of this embodiment has fine pores with a size of 2 to 20 μm, when the polishing pad 18 to which this resin porous body 17 is applied is used for polishing a hard-to-polish compound semiconductor wafer by the CMP method using a polishing liquid containing a permanganate-based strong oxidizing agent, there are no scratches and the polishing rate and surface roughness can be maintained for a long time.

[0052] As described above, the manufacturing method of the resin porous body 17 constituting the polishing pad 18 of this embodiment includes a melt preparation process P1 in which a base resin having high resistance to oxidizing agents and wear resistance is melted in a high-melting-point organic solvent that has a melting point at room temperature (10 to 30°C) and is soluble in water to obtain a melt, a molding process P2 in which the melt is molded into a thin plate to obtain a thin plate-like molded body, a precipitation process P3 in which the thin plate-like molded body is left in cold water that is lower than the melting point of the high-melting-point organic solvent to finely precipitate the high-melting-point organic solvent in the thin plate-like molded body, a replacement process P4 in which the thin plate-like molded body that has undergone the precipitation process P3 is left in hot water that is higher than the temperature of the cold water and the melting point of the high-melting-point organic solvent to replace the solid of the high-melting-point organic solvent that has finely precipitated in the thin plate-like molded body with water, and a drying process P5 in which the thin plate-like molded body is dried until all moisture is removed from the thin plate-like molded body. As a result, the resin porous body constituting the polishing pad 18 is made of PES resin, which is highly resistant to strong oxidizing agents, and fine pores are formed within the PES resin, so that when polishing difficult-to-polish wafers, there are no scratches and the polishing rate PR and surface roughness Sa can be maintained for a long period of time.

[0053] The base resin in this embodiment is PES (polyethersulfone) resin or PVDF-HFP (a copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin, so that a resin porous body having high resistance to oxidizing agents and abrasion is obtained.

[0054] The high melting point organic solvent in this embodiment is 2-pyrrolidone having a melting point of 24.6° C. or DMSO (dimethyl sulfoxide) having a melting point of 18.4° C. Thus, in the precipitation step P3, the thin plate-shaped body is left in cold water at a temperature lower than the melting point of the high melting point organic solvent, so that the solid of the high melting point organic solvent can be finely precipitated in the thin plate-shaped body.

[0055] The high melting point organic solvent in this embodiment is a solvent that disperses in water and dissolves PES (polyethersulfone) resin and PVDF-HFP resin. This allows the thin plate-shaped molded body that has been subjected to the precipitation step P3 to be left in hot water that is higher than the temperature of the cold water and the melting point of the high melting point organic solvent, so that the solid of the high melting point organic solvent that has precipitated finely in the thin plate-shaped molded body can be replaced with water.

[0056] In this embodiment, the precipitation step P3 is to leave the thin plate-shaped body in cold water at 5 to 10° C., and the replacement step P4 is to leave the thin plate-shaped body that has been subjected to the precipitation step P3 in warm water at 40 to 60° C., which is sufficiently higher than the melting point of the high-melting point organic solvent. As a result, the solid of the high-melting point organic solvent can be finely precipitated in the thin plate-shaped body, and then the solid of the high-melting point organic solvent precipitated in the thin plate-shaped body is replaced with water in the warm water.

[0057] The resin porous body of this embodiment has micropores with an average diameter of 2 to 20 μm, preferably 2 to 10 μm. This has the advantage that when the workpiece 16 is polished with the polishing pad 18 made of the resin porous body, the edges of the many micropores contribute to the polishing mechanism, making it difficult for scratches to occur, and thus making it possible to obtain a favorable polishing rate PR and surface roughness Sa.

[0058] The polishing pad 18 of this embodiment has 54.3 to 65.1 volume % pores, 34.9 to 45.7 volume % PES resin, and a durometer hardness of 34.0 to 54.0, so it is free of scratches and can maintain the polishing rate PR and surface roughness Sa for a long time.

[0059] Although the preferred embodiment of the present invention has been described in detail above with reference to the drawings, the present invention is not limited to this embodiment and may be carried out in other embodiments.

[0060] For example, the polishing liquid PF in the above-described embodiment does not contain abrasive grains, but it may contain abrasive grains.

[0061] Further, the polishing solution PF in the above-mentioned embodiment contains a permanganate-based strong oxidizing agent such as potassium permanganate (KMnO4), but other strong oxidizing agents may be added.

[0062] Furthermore, the polishing pad 18 in the above embodiment does not contain abrasive grains, but it may contain abrasive grains.

[0063] Furthermore, although the resin porous body in the above-mentioned embodiment was used as the polishing pad 18, it may also be used for other purposes, such as a water-adhesive pad for fixing a compound semiconductor wafer on a polishing table, synthetic leather, an anti-vibration sheet, a sound-absorbing material, a water-absorbing and water-retaining body, a separator or separation membrane for a fuel cell, etc.

[0064] Note that the above is merely one embodiment, and other examples are not provided, but the present invention can be implemented in various forms with various modifications and improvements based on the knowledge of those skilled in the art without departing from the spirit of the present invention. [Explanation of symbols]

[0065] 16: Workpiece (hard-to-polish compound semiconductor wafer) 17: Porous resin 18: Polishing pad (compound semiconductor polishing pad made of resin porous body) PF: Polishing fluid

Claims

1. A compound semiconductor polishing pad comprising a resin porous body having a base resin which is a PES (polyethersulfone) resin or a PVDF-HFP (copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin, and micropores formed in the base resin, the size of the micropores being 2 to 20 μm, The compound semiconductor polishing pad is used to polish a hard-to-polish compound semiconductor wafer using a polishing solution containing a permanganic acid-based strong oxidizing agent, The compound semiconductor polishing pad has 54.3 to 65.1 volume % of pores, 34.9 to 45.7 volume % of PES resin, and a durometer hardness (Type-D) of 34.0 to 54.

0.

1. A compound semiconductor polishing pad comprising:

2. A method for producing a resin porous body having high oxidant resistance and abrasion resistance and fine pores, comprising the steps of: a melt preparation step of melting a base resin having high resistance to oxidizing agents and wear resistance in a high-melting-point organic solvent having a melting point at room temperature and soluble in water to obtain a melt; a molding step of molding the molten material into a thin plate to obtain a thin plate-shaped body; a precipitation step of leaving the thin plate-like molded body in cold water at a temperature lower than the melting point of the high-melting point organic solvent to finely precipitate a solid of the high-melting point organic solvent in the thin plate-like molded body; a replacement step in which the thin plate-shaped body having been subjected to the precipitation step is left in hot water having a temperature higher than the temperature of the cold water and the melting point of the high-melting point organic solvent, thereby replacing the solid of the high-melting point organic solvent finely precipitated in the thin plate-shaped body with water; A drying step of drying the thin plate-like molded body until all moisture is removed from the thin plate-like molded body, The base resin is a PES (polyethersulfone) resin or a PVDF-HFP (copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin. The present invention relates to a method for producing a porous resin body.

3. The high melting point organic solvent is 2-pyrrolidone having a melting point of 24.6° C. or DMSO (dimethyl sulfoxide) having a melting point of 18.4° C. The method for producing a resin porous body according to claim 2 .

4. The high melting point organic solvent is a solvent that disperses in water and dissolves the PES (polyethersulfone) resin and the PVDF-HFP (copolymer of 80% polyvinylidene fluoride and 20% propylene hexafluoride) resin. The method for producing a resin porous body according to claim 2 .

5. The precipitation step is a step of leaving the thin plate-shaped body in the cold water at 5 to 10°C, and the replacement step is a step of leaving the thin plate-shaped body having been subjected to the precipitation step in the warm water at 40 to 60°C. The method for producing a resin porous body according to claim 2 .

6. The resin porous body has fine pores with an average diameter of 2 to 20 μm.

3. The compound semiconductor polishing pad according to claim 2.

Citation Information

Patent Citations

  • Production of polymeric porous material

    JP1990208332A

  • Polishing pad with groove

    JP2000349053A

  • Porous membrane and production thereof

    JP2001164029A

  • Porous film

    JP2016147966A

  • New method for manufacturing network-like high polymer porous particle