Polycrystalline silicon raw material
A polycrystalline silicon raw material with controlled bulk and surface dopant concentrations addresses the challenge of achieving high resistivity in single crystal silicon, ensuring consistent p-type conductivity and resistivity of 10,000 Ωcm or more without additional dopants.
Patent Information
- Application Number
- JP2021512310
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-05
- Filing Date
- 2020-04-02
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-04-02
AI Technical Summary
Existing methods for producing single crystal silicon with high resistivity, such as the CZ method, face challenges in controlling the concentration of dopant elements, particularly surface dopant elements, leading to inconsistent conductivity type and resistivity, making it difficult to achieve resistivities of 10,000 Ωcm or more without adding dopants.
A polycrystalline silicon raw material is developed with controlled bulk and surface dopant concentrations, where the total concentration of donor and acceptor elements satisfy the relationship 5[ppta]≦(Ca1+Ca2)-(Cd1+Cd2)≦26[ppta], ensuring accurate high resistivity and desired conductivity type without adding dopants.
The solution allows for the production of single crystal silicon with p-type conductivity and resistivity of 10,000 Ωcm or more by precisely balancing bulk and surface dopant concentrations, thereby stabilizing the conductivity type and resistivity.
Smart Images

Figure 0007572352000016 
Figure 0007572352000001 
Figure 0007572352000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polycrystalline silicon raw material, in particular to a polycrystalline silicon raw material for producing single crystal silicon having high resistivity. [Background technology]
[0002] Single crystal silicon is an extremely important material industrially, and is used as a substrate for various elements such as semiconductor wafers, solar cells, high frequency devices, and sensors. When used as a substrate for various elements, the substrate is required to be single crystal silicon with high resistivity in order to suppress the movement of charges within the substrate. For example, as described in Patent Document 1, a substrate with a resistivity of about several thousand Ωcm is required.
[0003] Single crystal silicon is obtained as a single crystal silicon ingot by contacting a seed crystal with the silicon melt obtained by melting polycrystalline silicon raw material. Known methods for obtaining single crystal silicon ingots are the CZ (Czochralski) method and the FZ (Floating Zone) method.
[0004] Conventionally, single crystal silicon with high resistivity has been produced by the FZ method, but it is difficult to produce large-diameter ingots using the FZ method, and this method is disadvantageous in terms of cost.
[0005] Therefore, attempts have been made to produce single crystal silicon having high resistivity by the CZ method, which allows the comparatively easy production of large-diameter ingots of φ300 mm or more and is less expensive than the FZ method.
[0006] For example, Patent Document 2 discloses that single crystal silicon having high resistivity can be obtained by using a polycrystalline silicon raw material in which the difference in impurity concentration (the difference between the donor concentration and the acceptor concentration) in the polycrystalline silicon raw material is controlled within a specific range.
[0007] However, the surface of the polycrystalline silicon raw material is usually contaminated, and various impurity elements are present on the surface. Such impurity elements include dopant elements (donor elements and acceptor elements). A distinction is made between dopant elements present on the surface of the polycrystalline silicon raw material (surface dopant elements) and dopant elements present in the bulk of the polycrystalline silicon raw material (bulk dopant elements).
[0008] However, when the polycrystalline silicon raw material is melted, the surface dopant element is included in the silicon melt together with the bulk dopant element. Therefore, when the single crystal silicon is pulled up, the surface dopant element is incorporated into the single crystal silicon as a bulk dopant element. As a result, the surface dopant element of the polycrystalline silicon raw material affects the resistivity of the single crystal silicon.
[0009] In particular, the polycrystalline silicon raw material used in the CZ method is a fragmented raw material (polycrystalline silicon chunks) obtained by crushing a polycrystalline silicon rod. Therefore, the surface area of the polycrystalline silicon raw material consisting of the polycrystalline silicon chunks is much larger than the surface area of the rod-shaped polycrystalline silicon raw material used in the FZ method. Since the amount of surface dopant elements is proportional to the surface area, in the CZ method, the effect of the surface dopant elements on the resistivity of single crystal silicon is extremely large.
[0010] Furthermore, the size of the polycrystalline silicon chunks in the polycrystalline silicon raw material is not constant, but has a certain particle size distribution. Since the surface area of the polycrystalline silicon chunks corresponds to the size of the polycrystalline silicon chunks, the amount of surface dopant elements varies depending on the size of the polycrystalline silicon chunks.
[0011] Therefore, when producing single crystal silicon having high resistivity, a technique is known that focuses on not only the bulk dopant element of the polycrystalline silicon raw material but also the surface dopant element. For example, Patent Document 3 discloses that the concentration of the surface dopant element and the concentration of the bulk dopant element in the polycrystalline silicon raw material are set within a predetermined range. In addition, Patent Document 4 and Patent Document 5 disclose that the concentration of the surface dopant element and the concentration of the bulk dopant element in the polycrystalline silicon raw material are measured, and dopants are added to obtain a desired resistivity based on the measurement results. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2017-69240 A [Patent Document 2] JP 2004-315336 A [Patent Document 3] JP 2013-151413 A [Patent Document 4] JP 2014-156376 A [Patent Document 5] JP 2018-90466 A Summary of the Invention [Problem to be solved by the invention]
[0013] In recent years, there has been a demand for single crystal silicon having a higher resistivity, for example, a resistivity of 10,000 Ωcm or more. In order to obtain single crystal silicon having such a very high resistivity, it is preferable to adjust the amount of dopant element contained in the polycrystalline silicon raw material without adding a dopant.
[0014] However, Patent Document 2 does not suggest controlling the concentration of the bulk dopant element in the polycrystalline silicon raw material, but simply uses a raw material in which the difference between the donor concentration and the acceptor concentration in the raw material is controlled within a specific range by combining various polycrystalline silicon raw materials, and does not pay any attention to the concentration of the surface dopant element in the polycrystalline silicon raw material.
[0015] Therefore, depending on the concentration of the surface dopant element, there is a problem that single crystal silicon having a conductivity type opposite to the desired conductivity type is obtained, or even if single crystal silicon has the desired conductivity type, there is a problem that the desired resistivity is not obtained.
[0016] In the first place, Patent Document 2 aims to produce single crystal silicon having a resistivity of about 2000 Ωcm, and even if the difference between the donor concentration and the acceptor concentration in the polycrystalline silicon raw material is within the range described in Patent Document 2, it is not possible to produce single crystal silicon having a resistivity of, for example, 10000 Ωcm or more.
[0017] In Patent Document 3, although the concentration of the surface dopant element and the concentration of the bulk dopant element are focused on, the concentration range of each is merely specified. Therefore, depending on the magnitude relationship between the donor concentration and the acceptor concentration in the surface dopant element and the donor concentration and the acceptor concentration in the bulk dopant element, there is a problem that a single crystal silicon having a conductivity type opposite to the desired conductivity type is obtained. Or, even if the single crystal silicon has a desired conductivity type, there is a problem that the desired resistivity cannot be obtained.
[0018] Similarly to Patent Document 2, Patent Documents 4 and 5 do not suggest controlling the concentrations of surface dopant elements and bulk dopant elements of the polycrystalline silicon raw material, but add dopants to adjust the resistivity of the single crystal silicon based on the measurement results of the concentrations of the surface dopant elements and bulk dopant elements.
[0019] However, both Patent Document 4 and Patent Document 5, like Patent Document 2, aim to produce single crystal silicon with a resistivity of about several thousand Ωcm. Therefore, when attempting to obtain single crystal silicon with a resistivity of, for example, 10,000 Ωcm or more by the method disclosed in Patent Document 4, the amount of dopant added must be extremely small. There is a problem in that the error in measuring such an extremely small amount of dopant added is large, making it difficult to obtain the desired resistivity.
[0020] Moreover, in these patent documents, the intended dopant elements are, specifically, only phosphorus (P) as a donor element and only boron (B) as an acceptor element. For these reasons, the resistivity of single crystal silicon obtained without adding dopants cannot be set to the desired value, and as a result, it is difficult to control the conductivity type and also the resistivity to a desired high value unless the above-mentioned dopants are added and adjusted.
[0021] The present invention has been made in view of the above circumstances, and has an object to provide a polycrystalline silicon raw material for producing single crystal silicon that has a p-type conductivity without the addition of a dopant and can accurately exhibit a targeted high resistivity. [Means for solving the problem]
[0022] The inventors have discovered that by taking into consideration all acceptors and donors that affect resistivity in a polycrystalline silicon raw material and keeping the balance of these within a specified range, it is possible to obtain single crystal silicon that has a targeted conductivity type and can accurately exhibit the targeted resistivity, even if the targeted resistivity is high.
[0023] In order to achieve the above object, the present invention provides: [1] A polycrystalline silicon raw material for producing single crystal silicon, comprising a plurality of polycrystalline silicon chunks, When the total concentration of donor elements present in the bulk of the polycrystalline silicon raw material is Cd1 [ppta], the total concentration of acceptor elements present in the bulk of the polycrystalline silicon raw material is Ca1 [ppta], the total concentration of donor elements present on the surface of the polycrystalline silicon raw material is Cd2 [ppta], and the total concentration of acceptor elements present on the surface of the polycrystalline silicon raw material is Ca2 [ppta], The polycrystalline silicon raw material is characterized in that Cd1, Ca1, Cd2 and Ca2 satisfy the relationship 5 [ppta] ≦ (Ca1 + Ca2) - (Cd1 + Cd2) ≦ 26 [ppta].
[0024] [2] The polycrystalline silicon raw material according to [1], characterized in that, when the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material is taken as 100%, the weight of the polycrystalline silicon chunks having a maximum side length of 10 mm or more and 45 mm or less is 90% or more.
[0025] [3] The polycrystalline silicon raw material according to [1], characterized in that, when the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material is taken as 100%, the weight of the polycrystalline silicon chunks having a maximum side length of 20 mm or more and 70 mm or less is 90% or more.
[0026] [4] The polycrystalline silicon raw material according to [1], characterized in that, when the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material is taken as 100%, the weight of the polycrystalline silicon chunks having a maximum side length of 60 mm or more and 100 mm or less is 90% or more. Effect of the Invention
[0027] According to the present invention, it is possible to provide a polycrystalline silicon raw material for producing single crystal silicon that has a p-type conductivity without adding a dopant and can accurately exhibit a targeted high resistivity. [Brief description of the drawings]
[0028] [Figure 1]FIG. 1 is a process diagram of a method for producing polycrystalline silicon raw material according to the present embodiment and a method for producing single crystal silicon using the polycrystalline silicon raw material according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The present invention will now be described in detail based on specific embodiments in the following order. 1. Polycrystalline silicon raw material 2. Method for producing polycrystalline silicon raw material 2.1. Production of polycrystalline silicon rods 2.2. Crushing of polycrystalline silicon rods 2.3. Cleaning of crushed polycrystalline silicon 2.4. Polycrystalline silicon raw materials 3. Controlling the dopant concentration of polycrystalline silicon raw material 3.1. Control of bulk dopant concentration in polycrystalline silicon raw material 3.1.1. Measurement of bulk dopant concentration 3.2. Control of surface dopant concentration in polycrystalline silicon raw material 3.2.1. Measurement of surface dopant concentration 4. Summary of this embodiment
[0030] (1. Polycrystalline silicon raw material) The polycrystalline silicon raw material according to the present embodiment includes a plurality of polycrystalline silicon chunks. The polycrystalline silicon chunks are obtained by crushing a polycrystalline silicon rod produced by a known method and cleaning the crushed polycrystalline silicon.
[0031] The polycrystalline silicon raw material according to the present embodiment is suitable for use in the production of single-crystalline silicon having a p-type conductivity. When the carriers present in the single-crystalline silicon are holes, the conductivity type is p-type, and when the carriers are free electrons, the conductivity type is n-type.
[0032] In single crystal silicon, acceptor elements that supply holes include boron (B), aluminum (Al), gallium (Ga), and indium (In). On the other hand, donor elements that supply free electrons include phosphorus (P), arsenic (As), and antimony (Sb). Therefore, in single crystal silicon with p-type conductivity, holes are the majority carriers that carry electric charges.
[0033] Therefore, in order to produce single crystal silicon having a p-type conductivity, in this embodiment, taking into consideration all dopants (acceptor elements and donor elements) present in the polycrystalline silicon raw material used as the raw material for the single crystal silicon, the acceptor element concentration is made higher than the donor element concentration, and holes are made the majority carriers, thereby making it possible to easily obtain single crystal silicon having a p-type conductivity.
[0034] On the other hand, the resistivity of single crystal silicon with p-type conductivity corresponds to the acceptor element concentration, i.e., the number of carriers in the single crystal silicon. If the acceptor element concentration is high, the number of carrier holes is large, and the resistivity is low. Therefore, to obtain single crystal silicon with high resistivity, it is necessary to reduce the acceptor element concentration.
[0035] However, the present inventors have noticed that this acceptor element concentration does not need to be the total concentration of the acceptor elements present in the single crystal silicon, but only needs to be the effective acceptor element concentration that actually contributes to the resistivity. When an acceptor element and a donor element are present in the single crystal silicon, carriers (holes) derived from the acceptor element and carriers (free electrons) derived from the donor element cancel each other out, so that from the viewpoint of the number of carriers, the difference between the acceptor element concentration and the donor element concentration becomes the effective acceptor element concentration, and the number of effective carriers corresponding to the effective acceptor element concentration is reflected in the resistivity.
[0036] In other words, by setting the effective acceptor element concentration within a predetermined range, the resistivity of single crystal silicon having p-type conductivity can be set within a predetermined range.
[0037] Here, in the single crystal silicon pulling process, dopant contamination caused by external factors other than the polycrystalline silicon raw material can be suppressed to an extremely small amount. Therefore, to control the effective acceptor element concentration in the single crystal silicon, as described above, it is sufficient to control the concentration taking into consideration all dopants (acceptor elements and donor elements) present in the polycrystalline silicon raw material used as the raw material for single crystal silicon. The acceptor elements and donor elements present in the polycrystalline silicon raw material consist of dopants present in the bulk of the polycrystalline silicon raw material (bulk dopants) and dopants present on the surface of the polycrystalline silicon raw material (surface dopants).
[0038] Therefore, in this embodiment, the difference between the total concentration of acceptor elements present in the bulk and on the surface of the polycrystalline silicon source and the total concentration of donor elements present in the bulk and on the surface of the polycrystalline silicon source is controlled to be within a specific range.
[0039] Specifically, if the total concentration of donor elements present in the bulk of the polycrystalline silicon raw material is Cd1 [ppta], the total concentration of acceptor elements present in the bulk of the polycrystalline silicon raw material is Ca1 [ppta], the total concentration of donor elements present on the surface of the polycrystalline silicon raw material is Cd2 [ppta], and the total concentration of acceptor elements present on the surface of the polycrystalline silicon raw material is Ca2 [ppta], Cd1, Ca1, Cd2 and Ca2 satisfy the following relationship. 5[ppta]≦(Ca1+Ca2)-(Cd1+Cd2)≦26[ppta]
[0040] Here, the total concentration of donor elements (Cd2) and the total concentration of acceptor elements (Ca2) present on the surface of the polycrystalline silicon raw material do not indicate the amount of these donor elements and acceptor elements present on the surface of the polycrystalline silicon raw material as values relative to the surface of the polycrystalline silicon raw material, but as will be apparent from the calculation formula described later, are values indicating the amount of each of these surface dopant elements as a value relative to the elemental quantity of silicon in the polycrystalline silicon raw material.
[0041] By using a polycrystalline silicon raw material in which the acceptor element concentration and the donor element concentration are controlled within the above ranges, the dopant concentration in the bulk of the produced single crystal silicon almost reflects the concentration derived from the polycrystalline silicon raw material. Therefore, by controlling the acceptor element concentration and the donor element concentration in the polycrystalline silicon raw material as described above, the produced single crystal silicon has a targeted conductivity type and can accurately exhibit a targeted resistivity.
[0042] The upper limit in the above relationship, 26 [ppta], corresponds to the theoretical acceptor element concentration in single crystal silicon that exhibits a resistivity of approximately 10,000 [Ωcm]. In other words, in the above relationship, by setting the upper limit of the effective acceptor element concentration in the polycrystalline silicon raw material to 26 [ppta], it is possible to obtain single crystal silicon that is p-type conductive and has a resistivity of approximately 10,000 [Ωcm].
[0043] On the other hand, the lower limit of the above relationship, 5 [ppta], corresponds to the theoretical acceptor element concentration in single crystal silicon that exhibits a resistivity of approximately 50,000 [Ωcm]. Single crystal silicon with a resistivity exceeding 50,000 [Ωcm] exhibits a dopant concentration close to that of an intrinsic semiconductor, so that even a very slight change in the acceptor element concentration or donor element concentration can reverse the magnitude relationship between the acceptor element concentration and the donor element concentration, resulting in single crystal silicon of the opposite conductivity type to the desired conductivity type, i.e., n-type.
[0044] From the viewpoint of more reliably obtaining P-type single crystal silicon having a resistivity of 10,000 [Ωcm] or more, it is more preferable that Cd1, Ca1, Cd2 and Ca2 satisfy the following relationship. 10[ppta]≦(Ca1+Ca2)-(Cd1+Cd2)≦20[ppta]
[0045] During the pulling of the single crystal silicon, phosphorus, which is a donor element, and boron, which is an acceptor element, are incorporated into the single crystal silicon. Phosphorus and boron have different segregation coefficients, and boron, which has a segregation coefficient of 0.8, hardly segregates in the single crystal silicon, so the boron concentration in the single crystal silicon does not change much between the early and later stages of pulling. On the other hand, phosphorus, which has a segregation coefficient of 0.35, segregates more easily than boron, and the phosphorus concentration in the single crystal silicon is low in the early stage of pulling, but increases as the pulling progresses. As a result, in the pulled single crystal silicon, the magnitude relationship between the acceptor element concentration and the donor element concentration is reversed between the part obtained in the early stage of pulling and the part obtained in the later stage of pulling, and the conductivity type may be inverted. To prevent this, in this embodiment, the lower limit of the above relationship is set to 5 [ppta].
[0046] In this embodiment, as long as the effective acceptor element concentration satisfies the above relationship, the values of Cd1, Ca1, Cd2 and Ca2 are not particularly limited. That is, it is not so important to control the absolute values of the bulk dopant concentration and the surface dopant concentration in the polycrystalline silicon raw material, but it is important to control the bulk dopant concentration and the surface dopant concentration in cooperation with each other.
[0047] In addition, Ca1 is usually in the range of 1 to 10 [ppta], and from the viewpoint of stably obtaining P-type single crystal silicon of 10000 [Ωcm] or more, Ca1 is preferably in the range of 1 to 4 [ppta]. Ca2 is usually in the range of 1 to 100 [ppta], and for the same reason as above, Ca2 is preferably in the range of 10 to 90 [ppta]. On the other hand, Cd1 is usually in the range of 1 to 80 [ppta], and from the viewpoint of stably obtaining P-type single crystal silicon of 10000 [Ωcm] or more, Cd1 is preferably in the range of 10 to 60 [ppta]. Cd2 is usually in the range of 1 to 50 [ppta], and for the same reason as above, Cd2 is preferably in the range of 1 to 30 [ppta].
[0048] (2. Method for producing polycrystalline silicon raw material) The method for producing the polycrystalline silicon raw material according to this embodiment is not particularly limited, and may be a known method such as the Siemens method, the fluidized bed method, etc. In this embodiment, the method for producing the polycrystalline silicon raw material by the Siemens method will be described with reference to the process diagram shown in FIG.
[0049] (2.1. Production of polycrystalline silicon rods) In the Siemens process, first, a silicon core wire connected to a carbon electrode is placed inside a reaction vessel, and electricity is passed through the silicon core wire to heat it to a temperature above the silicon deposition temperature. As shown in Figure 1, a silane compound gas and a reducing gas are supplied as raw material gases to the heated silicon core wire, and polycrystalline silicon is deposited on the silicon core wire by chemical vapor deposition to obtain a polycrystalline silicon rod.
[0050] Examples of the silane compound include monosilane, trichlorosilane, silicon tetrachloride, monochlorosilane, dichlorosilane, etc., and in this embodiment, trichlorosilane is preferred. As the reducing gas, hydrogen gas is usually used.
[0051] The resulting polycrystalline silicon rod contains impurity elements resulting from the source gas (trichlorosilane and hydrogen) and the electrodes. Such impurity elements include dopant elements such as boron (B), aluminum (Al), phosphorus (P), and arsenic (As). In other words, such dopant elements are bulk dopant elements contained in the bulk of the polycrystalline silicon rod.
[0052] In this embodiment, bulk dopant concentration control, which will be described later, is performed to control the concentrations of the bulk dopant elements (Cd1 and Ca1) in the polycrystalline silicon rod within a predetermined range.
[0053] (2.2. Crushing of polycrystalline silicon rods) As shown in Fig. 1, the obtained polycrystalline silicon rod is cut and crushed to a predetermined size to obtain polycrystalline silicon fragments in the form of chunks. Specifically, the polycrystalline silicon rod is crushed into chunks by a hammer made of a hard metal such as tungsten carbide, a crusher such as a jaw crusher, etc. After crushing, impurity elements resulting from the materials of the hammer and crusher, the environment during crushing, etc. adhere to the surface of the polycrystalline silicon fragments, and the surface becomes contaminated.
[0054] Such impurity elements may include the above-mentioned dopant elements. That is, surface dopant elements may exist on the surface of the polycrystalline silicon fragments. If surface dopant elements exist, when producing single crystal silicon from silicon melt obtained by melting the polycrystalline silicon fragments, the surface dopant elements of the polycrystalline silicon fragments are taken into the single crystal silicon and exist as bulk dopant elements in the single crystal silicon, which significantly affects the conductivity type and resistivity of the single crystal silicon.
[0055] (2.3. Cleaning of crushed polycrystalline silicon) Therefore, in this embodiment, as shown in Fig. 1, in order to reduce surface contamination of the polycrystalline silicon fragments caused by the crushing of the polycrystalline silicon rod, the polycrystalline silicon fragments are washed (wet treatment). Specifically, the polycrystalline silicon fragments are first brought into contact with a solution containing hydrofluoric acid, nitric acid, etc., and the surface portion of the polycrystalline silicon fragments is eluted by etching. By carrying out such a treatment, the surface dopant element attached during crushing can be separated from the polycrystalline silicon fragments. After etching, the polycrystalline silicon fragments are rinsed with ultrapure water or the like and dried.
[0056] (2.4. Polycrystalline silicon raw materials) In this embodiment, as shown in FIG. 1, the surface dopant concentration of the washed crushed polycrystalline silicon is controlled as described below to obtain polycrystalline silicon raw material.
[0057] In this embodiment, when the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material satisfying the above-mentioned effective acceptor element concentration is taken as 100%, it is preferable that the weight of the polycrystalline silicon chunks having a maximum side length of 10 mm to 45 mm is 90% or more. It is also preferable that the weight of the polycrystalline silicon chunks having a maximum side length of 20 mm to 70 mm is 90% or more when the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material satisfying the above-mentioned effective acceptor element concentration is taken as 100%. It is also preferable that the weight of the polycrystalline silicon chunks having a maximum side length of 60 mm to 100 mm is 90% or more when the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material satisfying the above-mentioned effective acceptor element concentration is taken as 100%.
[0058] The above-mentioned effective acceptor element concentration takes into consideration the surface dopant element concentration. This surface dopant element concentration depends on the surface area of the polycrystalline silicon raw material. For example, when the grain size of the polycrystalline silicon chunks constituting the polycrystalline silicon raw material is small and when the grain size of the polycrystalline silicon chunks is large, the surface area of the polycrystalline silicon raw material (total surface area of the polycrystalline silicon chunks) is larger when the grain size of the polycrystalline silicon chunks is small, assuming that the weight of the polycrystalline silicon raw material is the same. In other words, even when the weight of the polycrystalline silicon raw material is the same, the surface dopant concentration is larger when the grain size is small than when the grain size is large, and it becomes more difficult to control the p-type conductivity and accurately achieve the desired high resistivity.
[0059] However, in this embodiment, as described later, the surface dopant concentration is controlled in consideration of the grain size of the polycrystalline silicon raw material. As a result, even if the grain size of the polycrystalline silicon chunks constituting the polycrystalline silicon raw material is different as described above, the effective acceptor element concentration in the polycrystalline silicon raw material satisfies the above relationship. From the viewpoint of achieving this effect more significantly, it is more preferable that the polycrystalline silicon raw material is a chunk having a small grain size and a large surface area. Specifically, among those with the above grain sizes, it is particularly preferable that the weight of the polycrystalline silicon chunks having a maximum side length of 10 mm to 45 mm is 90% or more, with the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material being 100%.
[0060] By etching the crushed polycrystalline silicon, the effects of surface contamination at the time of crushing the polycrystalline silicon rods can be removed. However, the surface of the polycrystalline silicon raw material may become contaminated again with dopant elements due to the storage environment, etc. until the polycrystalline silicon raw material is used.
[0061] Therefore, in order to reduce such surface contamination, the cleaned polycrystalline silicon raw material is usually filled by a predetermined amount into a packaging bag made of a resin such as polyethylene, and the packaging bag is sealed, as shown in Fig. 1. After being stored in a sealed state, the packaging bag is transported to a clean room in which the single crystal silicon manufacturing equipment is installed, the packaging bag is opened, the polycrystalline silicon raw material is taken out, and is filled into a crucible or a recharge tube.
[0062] (3. Controlling the dopant concentration of polycrystalline silicon raw material) In this embodiment, the bulk dopant concentrations (Cd1 and Ca1) and the surface dopant concentrations (Cd2 and Ca2) in the polycrystalline silicon raw material are controlled so as to satisfy the above relationship.
[0063] In this embodiment, the bulk dopant concentration in the polycrystalline silicon raw material is the dopant concentration contained in the bulk of the polycrystalline silicon rod after the bulk dopant concentration control, as shown in Fig. 1. The surface dopant concentration in the polycrystalline silicon raw material is the dopant concentration after the surface dopant concentration control for the polycrystalline silicon crushed material (polycrystalline silicon raw material) after cleaning, as shown in Fig. 1. After the surface dopant concentration control, the polycrystalline silicon raw material is promptly filled into a packaging bag and sealed, so that the surface dopant concentration after the surface dopant concentration control is maintained until the polycrystalline silicon raw material is used.
[0064] The bulk dopant concentration can be controlled by the purity of the raw material gas during the production of the polycrystalline silicon rod, the purity of the material constituting the electrodes, the material of the deposition reactor, the temperature, etc. The bulk dopant concentration does not change until the polycrystalline silicon raw material is obtained from the polycrystalline silicon rod. Therefore, by first controlling the bulk dopant concentration and determining it to a predetermined value, and then controlling the surface dopant concentration, it becomes easy to make the bulk dopant concentration and the surface dopant concentration in the polycrystalline silicon raw material satisfy the above-mentioned relationship.
[0065] (3.1. Bulk dopant concentration control of polycrystalline silicon raw material) The acceptor elements in silicon are boron (B), aluminum (Al), gallium (Ga), and indium (In), but since gallium and indium are hardly present in the bulk of the polycrystalline silicon rod, there is no need to consider their concentrations. Therefore, in this embodiment, the bulk B concentration and bulk Al concentration are considered as the bulk acceptor concentration.
[0066] The donor elements in silicon are phosphorus (P), arsenic (As), and antimony (Sb), but antimony is hardly present in the bulk of the polycrystalline silicon rod, so there is no need to consider its concentration. Therefore, in this embodiment, the bulk P concentration and bulk As concentration are considered as the bulk donor concentration.
[0067] The bulk P concentration of the polycrystalline silicon rod can be controlled by adjusting the dichlorosilane concentration in the raw material gas trichlorosilane, as described in JP 10-316413 A. Also, for example, as described in JP 2004-250317 A, JP 2005-67979 A, JP 2012-91960 A, etc., it can be controlled by distilling chlorosilanes in the presence of liquid alkoxysilanes or in the presence of an aldehyde compound having a predetermined structure.
[0068] The phosphorus concentration in the polycrystalline silicon raw material can be controlled by the bulk P concentration. However, if the desired phosphorus concentration cannot be achieved by the bulk P concentration alone, the surface P concentration may be controlled by the method described below.
[0069] In order to control the bulk B concentration and bulk Al concentration of the polycrystalline silicon rod, it is necessary to control the purity of trichlorosilane, which is the raw material gas of the polycrystalline silicon rod. However, when attempting to control the bulk B concentration and bulk Al concentration, the bulk carbon (C) concentration and bulk phosphorus (P) concentration also fluctuate. Therefore, in this embodiment, the bulk B concentration and bulk Al concentration are reduced as much as possible, and the acceptor element concentration in the polycrystalline silicon raw material is controlled by controlling the surface B concentration and surface Al concentration.
[0070] The bulk B concentration, bulk Al concentration, and bulk As concentration of the polycrystalline silicon rod, like the bulk P concentration, can be controlled by using purified chlorosilanes obtained by distilling chlorosilanes in the presence of liquid alkoxysilanes, or purified chlorosilanes obtained by distilling chlorosilanes in the presence of an aldehyde compound having a predetermined structure, as described in, for example, JP 2013-129592 A, JP 2004-250317 A, JP 2005-67979 A, and JP 2012-91960 A.
[0071] (3.1.1. Measurement of Bulk Dopant Concentration) In this embodiment, the bulk dopant concentration is measured according to JIS H0615. Specifically, a coring rod with an inner diameter of 19 mm is cut out with a drill in the diameter direction including the silicon core wire at an arbitrary position of the straight body of the polycrystalline silicon rod to obtain a polycrystalline silicon rod for FZ. The obtained polycrystalline silicon rod for FZ is tapered, degreased, washed, and etched with fluoronitric acid. The etched polycrystalline silicon rod for FZ is single-crystallized by the FZ method.
[0072] The resistance value of the obtained single crystal in the long axis direction of the single crystal is measured at 10 mm intervals, and the average resistivity is calculated. Next, the single crystal is cut out from the position that shows the same resistivity as the calculated average resistivity. The cut single crystal is polished and then etched with fluoronitric acid to obtain a sample for photoluminescence (PL) measurement. The bulk dopant concentration of the obtained PL measurement sample is measured using a PL device while immersed in liquid helium.
[0073] (3.2. Control of surface dopant concentration in polycrystalline silicon raw material) Next, a method for controlling the concentration of the surface dopant element will be described. The concentration of the surface dopant element can be controlled by controlling the adhesion of the dopant element to the surface of the polycrystalline silicon raw material, and various methods can be adopted. The method shown below is one example of a method for controlling the concentration of the surface dopant element, and the concentration may be controlled by a method other than the method shown below.
[0074] In this embodiment, the surface donor element is considered to be the surface P concentration, and the surface acceptor element is considered to be the surface B concentration and the surface Al concentration. In consideration of the safety of the workers, the impact on the environment, various laws and regulations, etc., the surface As concentration is not controlled. In addition, antimony, gallium, and indium are not usually present on the surface of the polycrystalline silicon raw material, and the surface dopant concentration can be controlled by other dopant elements, so the surface concentrations of these elements are not considered as well as the bulk concentrations. As described above, the attachment of dopant elements to the surface of the polycrystalline silicon raw material is likely to occur when the polycrystalline silicon rod is crushed, but the surface dopant elements attached during such crushing can be easily removed by cleaning the polycrystalline silicon crushed material. For this reason, in this embodiment, as shown in FIG. 1, the control of the surface dopant concentration is performed on the polycrystalline silicon crushed material after cleaning.
[0075] The surface B concentration of the polycrystalline silicon raw material is proportional to the boron concentration in the air that the polycrystalline silicon raw material is in contact with, the amount of air supplied, and the exposure time. The surface B concentration is also inversely proportional to the grain size of the polycrystalline silicon chunks that make up the polycrystalline silicon raw material, and proportional to the surface area of the polycrystalline silicon chunks.
[0076] Therefore, for the washed polycrystalline silicon crushed material (polycrystalline silicon raw material) W [kg] with an average particle size L [mm], the B concentration is Q _B [ng / m 3 ] is the air V [m 3 / min], the surface B concentration of the polycrystalline silicon raw material when the polycrystalline silicon raw material is exposed to the environment for t [min] is Ca2 _B [ppta] can be expressed by the following formula.
number
[0077] The control of the surface B concentration is usually performed in a clean room, so the amount of air V supplied to the clean room is constant. The B concentration in the air can be measured by a known method, for example, the impinger analysis specified in JACA No. 35A.
[0078] The surface Al concentration and the surface P concentration are controlled by utilizing polyethylene resin, which is a resin constituting a packaging bag in which the polycrystalline silicon raw material is filled. For example, Japanese Patent Application Laid-Open No. 2017-56959 describes lowering the concentration of a predetermined dopant element contained in a polyethylene packaging bag used for storing or transporting the polycrystalline silicon raw material in order to keep the surface of the polycrystalline silicon raw material clean. In contrast, in this embodiment, the surface contamination of Al and P from the polyethylene resin is actively utilized to control the surface Al concentration and the surface P concentration to predetermined values.
[0079] The surface Al concentration of the polycrystalline silicon raw material is proportional to the Al concentration in the polyethylene film and the contact area of the polycrystalline silicon raw material with the polyethylene film per unit weight. The surface P concentration of the polycrystalline silicon raw material is proportional to the amount of phosphate in the polyethylene film and the contact area of the polycrystalline silicon raw material with the polyethylene film per unit weight.
[0080] Therefore, in this embodiment, the polycrystalline silicon raw material is brought into contact with the polyethylene film in a clean room environment for controlling the surface B concentration. At this time, in order to prevent the surface of the polycrystalline silicon raw material from being contaminated by elements other than Al and P, it is preferable to cover and cure the bottom and side surfaces of the polycrystalline silicon raw material with a polyethylene film.
[0081] The present inventors have found that the influence of the average particle size of the polycrystalline silicon raw material and the contact time with the polyethylene film on the surface Al concentration and surface P concentration can be neglected.
[0082] Polyethylene resin often contains Al derived from catalysts such as organoaluminum, aluminoxane, and aluminum chloride, and when the polycrystalline silicon raw material comes into contact with the polyethylene resin, the Al contained in the polyethylene resin adheres to the surface of the polycrystalline silicon raw material.
[0083] Since the content of Al in the polyethylene resin depends on the raw material polyethylene pellets, it is possible to control the Al concentration in the polyethylene resin. _Al [ng / cm 2 When polycrystalline silicon raw material W [kg] is placed on a polyethylene film having a thickness of 100 mm, the contact area between the polyethylene film and the polycrystalline silicon raw material is defined as S [cm 2 ], the surface Al concentration of the polycrystalline silicon raw material is Ca2 _Al [pptw] can be expressed by the following formula.
number
[0084] In addition, phosphate esters are added as additives to polyethylene resins for use as plasticizers, antioxidants, etc. When the polycrystalline silicon raw material comes into contact with the polyethylene resin, phosphorus originating from the phosphate esters adheres to the surface of the polycrystalline silicon raw material. Since the amount of phosphorus in the polyethylene resin depends on the amount of the phosphate esters, the amount of phosphorus contained in the polyethylene resin can be controlled.
[0085] Therefore, the contact area between the polyethylene film and the polycrystalline silicon raw material when polycrystalline silicon raw material W3 [kg] is placed on a polyethylene film to which phosphate ester W2 [kg] is added per polyethylene pellet W1 [kg] is defined as S [cm 2 ], the surface P concentration of the polycrystalline silicon raw material (Ca2 _P ) [ppta] can be expressed by the following formula:
number
[0086] After the surface dopant concentration is controlled as described above, the polycrystalline silicon raw material is promptly filled into a packaging bag that is substantially free of Al and P and sealed, so that the surface dopant concentration after the control of the surface dopant concentration is maintained until the polycrystalline silicon raw material is used. An example of the packaging bag that is substantially free of Al and P is a packaging bag made of low-density polyethylene (LDPE) that does not contain phosphate esters as a plasticizer or antioxidant. This is because LDPE can be synthesized by radical polymerization without using a catalyst that contains Al.
[0087] (3.2.1. Measurement of surface dopant concentration) The surface B concentration, surface Al concentration, and surface P concentration in the polycrystalline silicon raw material after controlling the surface dopant concentration by the above-mentioned method can be measured by the method shown below.
[0088] First, in order to improve the lower limit of determination, a complexing agent for preventing the volatilization of boron is dissolved in a nitric acid / hydrofluoric acid solution containing high-purity nitric acid and high-purity hydrofluoric acid. Examples of the complexing agent include expensive alcohols.
[0089] A predetermined amount of polycrystalline silicon chunk is immersed in a fluoronitric acid solution, and the surface layer is eluted by etching to a depth of 1 μm or more, preferably 20 to 30 μm, and then the polycrystalline silicon chunk is taken out. After that, the fluoronitric acid solution containing the eluted part is evaporated to dryness at 100° C. or more, and the residue is dissolved and recovered with high-purity nitric acid. The surface B concentration, surface Al concentration, and surface P concentration can be calculated using the actual measured values quantified by double-focusing ICP-MS for the recovered residue.
[0090] The surface As concentration can be measured by the following method. For example, as described in JP 2005-172512 A, a predetermined amount of polycrystalline silicon chunks is filled into a fluororesin container with a lid having an outlet for collecting impurity gas, and then a predetermined amount of high-purity hydrofluoric acid is poured through the outlet, and the polycrystalline silicon chunks are immersed in the high-purity hydrofluoric acid and sealed. After removing the natural oxide film on the surface, the generated arsenic-containing gas is collected through the outlet, and the collected gas is quantified using a double-focusing ICP-MS equipped with a gas sample introduction system, and the surface As concentration in the polycrystalline silicon raw material is calculated using the actual measurement value.
[0091] The surface B concentration, surface Al concentration, surface P concentration, and surface As concentration are calculated by the following formula using the actual measured values of the concentration of each dopant element quantified using a double focusing ICP-MS.
number
[0092] From the surface B concentration, surface Al concentration, surface P concentration, and surface As concentration obtained above, the surface dopant concentration (Ca2 and Cd2) [ppta] can be obtained.
[0093] (4. Summary of the present embodiment) In this embodiment, attention is paid to the fact that the total concentration of bulk dopant elements present in single crystal silicon depends approximately on the total concentration of all dopant elements present in the polycrystalline silicon raw material used to produce the single crystal silicon.
[0094] The conductivity type of single crystal silicon is determined by whether the majority carriers are free electrons or holes, and the resistivity of single crystal silicon corresponds to the difference between the number of majority carriers and the number of minority carriers.
[0095] Therefore, in the polycrystalline silicon raw material used to produce single crystal silicon, the bulk concentration and surface concentration of the acceptor element and the bulk concentration and surface concentration of the donor element in the polycrystalline silicon raw material are controlled so as to satisfy the above-mentioned relationship.
[0096] As a method for producing single crystal silicon, for example, as shown in Fig. 1, a method for producing a single crystal silicon ingot using the above polycrystalline silicon raw material is exemplified. As a method for obtaining a single crystal silicon ingot, the CZ method is preferable. In the CZ method, a polycrystalline silicon raw material contained in a crucible is heated to form a silicon melt, and a seed crystal is brought into contact with the silicon melt to obtain a single crystal silicon ingot, which is then grown while being pulled up.
[0097] The obtained single crystal silicon ingot is usually rod-shaped, and is often composed of a straight body portion having a constant diameter, which is stably grown as a crystal, and a top portion (expanded diameter portion) and a tail portion (reduced diameter portion) located at both ends of the straight body portion. The length of the straight body portion of a single crystal silicon ingot produced by the CZ method is usually 900 to 1800 mm, and the diameter is usually φ200 to 300 mm.
[0098] Although a dopant may be added when melting the polycrystalline silicon raw material to control resistivity, etc., by using the polycrystalline silicon raw material according to this embodiment, a single crystal silicon ingot with high resistance can be obtained without adding a dopant when melting the polycrystalline silicon raw material. Even when single crystal silicon is produced using the polycrystalline silicon raw material according to this embodiment, a dopant may be added when melting the polycrystalline silicon raw material in order to control the properties of the single crystal silicon.
[0099] In the polycrystalline silicon raw material, when the effective acceptor element concentration (the difference between the sum of the bulk concentration and surface concentration of the acceptor element and the sum of the bulk concentration and surface concentration of the donor element) satisfies the above-mentioned relationship, the conductivity type of the obtained single crystal silicon ingot is P-type, and the resistivity exhibits a value corresponding to the effective acceptor element concentration of the polycrystalline silicon raw material.
[0100] In this embodiment, the concentrations of all of the acceptor elements and donor elements that affect the conductivity type of the single crystal silicon ingot are taken into consideration, so that a desired conductivity type is obtained and an ingot of a conductivity type different from the desired conductivity type is not obtained.
[0101] Furthermore, since the value calculated from the above-mentioned relationship for the polycrystalline silicon raw material corresponds to the resistivity in the single crystal silicon ingot, the target resistivity can be achieved with high precision.
[0102] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES
[0103] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0104] Example 1 The polycrystalline silicon raw material was produced by the Siemens process. Highly purified trichlorosilane and hydrogen were used as raw material gases.
[0105] The refined trichlorosilane used was produced by the following method: First, low-purity metallurgical-grade silicon, known as metallic silicon, was reacted with hydrogen chloride, and then metallic silicon was reacted with tetrachlorosilane and hydrogen to obtain crude trichlorosilane of low purity.
[0106] Silicon metal, which is the raw material for crude trichlorosilane, is contaminated with B, Al, P, and As at a ratio of several hundred ppb to several hundred ppm each, and during the reaction between silicon metal and hydrogen chloride, and between silicon metal, tetrachlorosilane, and hydrogen, each dopant component is also chlorinated and becomes mixed into the crude trichlorosilane.
[0107] The crude trichlorosilane was then purified by distillation to separate and remove B, P, Al, and As from the crude trichlorosilane, yielding purified trichlorosilane. The impurity concentrations in the purified trichlorosilane were measured by ICP-MS, and the concentrations of B, P, Al, and As were each 1 ppba or less.
[0108] In the polycrystalline silicon deposition process, the purified trichlorosilane was supplied to the reaction vessel, and unreacted trichlorosilane was recovered, purified by distillation, and then supplied back to the reaction vessel. In the trichlorosilane recovery and purification process, dichlorosilane and SiH3PH3, which has a boiling point close to that of dichlorosilane, were discharged outside the system to reduce the P concentration in the recovered and purified trichlorosilane.
[0109] The concentrations of B, P, Al, and As in the recovered and purified trichlorosilane were measured by ICP-MS and were each found to be less than 1 [ppba], while the dichlorosilane concentration was measured by gas chromatography and was found to be 800 [ppmw].
[0110] The hydrogen used was high-purity hydrogen with a dew point of -70°C or less, and recovered and purified hydrogen, which was made by purifying the unreacted hydrogen recovered after the high-purity hydrogen was supplied to the reaction vessel. The high-purity hydrogen and the recovered and purified hydrogen were mixed, and the amount of dopant components in the hydrogen immediately before being supplied to the reaction vessel was measured using the impinger method. The results showed that B, Al, P, and As were all below the lower limit of quantification of 0.05 [ppbv].
[0111] The silicon core wire on which polycrystalline silicon was precipitated was cut out from the polycrystalline silicon rod, and then etched using fluoronitric acid to dissolve the surface layer to a depth of 5 μm or more, thereby removing the effects of heavy metal contamination and dopant contamination that occurred during cutting.
[0112] The silicon core wire was electrically heated to about 1000°C, and then the mixed gas of the purified trichlorosilane and high-purity hydrogen was supplied to the reaction vessel to precipitate polycrystalline silicon. When the diameter of the precipitated polycrystalline silicon reached about 130 mm, the supply of the mixed gas of the purified trichlorosilane and high-purity hydrogen and the supply of electricity were stopped to terminate the precipitation reaction. The polycrystalline silicon precipitate was then cut out to obtain a polycrystalline silicon rod.
[0113] The bulk dopant concentration of the obtained polycrystalline silicon rod was measured as follows. According to JIS H0615, the obtained polycrystalline silicon rod was cored through the silicon core to obtain a coring rod with a diameter of 19 mm. The obtained coring rod was etched with fluoronitric acid to remove contamination during coring, and then single crystallization was performed by the FZ method. The resistivity of the obtained single crystal was measured every 10 mm in the long axis direction with a four-point needle resistance meter (RT-80 manufactured by NAPSON), and the average resistivity was calculated. The average resistivity was 2200 [Ωcm].
[0114] Next, a photoluminescence sample was cut out from the position where the resistivity was 2200 [Ωcm], polished, and etched to obtain a mirror-finished sample. The obtained mirror-finished sample was immersed in liquid helium, and the amount of each dopant was measured using a photoluminescence measuring device (PL-82IGA manufactured by Seishin Shoji). As a result, the bulk B concentration was 2 [ppta], the bulk Al concentration was less than the lower limit of quantification of 1 [ppta], the bulk P concentration was 45 [ppta], and the bulk As concentration was 1 [ppta]. Therefore, the bulk acceptor concentration was 2 [ppta] and the bulk donor concentration was 46 [ppta]. Note that the measurement result of the bulk Al concentration was less than 1 [ppta] and no peak was confirmed, so the bulk Al concentration was calculated as 0 [ppta] for the bulk acceptor concentration.
[0115] The polycrystalline silicon rod remaining after the sample for measuring the bulk dopant concentration was obtained was crushed to obtain crushed polycrystalline silicon (polycrystalline silicon nuggets).
[0116] The obtained polycrystalline silicon nuggets were sorted into three sizes by a sorting device, and 30 kg of each of the sorted nuggets was taken out and the maximum side length of each piece was measured with a vernier caliper.
[0117] Small-size nugget S contained 93 wt% nuggets with a maximum side length of 10 mm or more and 45 mm or less, and the median diameter of nugget S was 31 mm.
[0118] The medium-sized nugget M contained 92 wt% nuggets with a maximum side length of 20 mm or more and 70 mm or less, and the median diameter of nugget M was 51 mm.
[0119] The large-size nugget L contained 92 wt% nuggets with a maximum side length of 60 mm or more and 100 mm or less, and the median diameter of nugget L was 83 mm.
[0120] Polycrystalline silicon nuggets sorted by size were etched with a mixture of electronics-grade nitric acid and electronics-grade hydrofluoric acid to dissolve the surface layer and remove surface contamination caused by crushing. Since the reactivity of the nugget to the etching solution differs depending on the size of the nugget, the etching time was adjusted according to the size of the nugget, and etching was performed so that the etch-off amount was 3 μm or more for all sizes of nuggets. After that, it was rinsed with ultrapure water with a resistivity of 18 MΩ cm, and three types of polycrystalline silicon raw material with different sizes were obtained. The bulk dopant concentration of the three types of polycrystalline silicon raw material was the same.
[0121] The surface dopant concentration of the obtained polycrystalline silicon raw material was controlled as follows.
[0122] First, the polycrystalline silicon raw material was transported to a clean room where the cleanliness was controlled according to ISO14644-1 Class 6, and then placed in containers lined with polyethylene sheets according to size, and air-dried.
[0123] Regardless of the size of the polycrystalline silicon raw material, 150 kg of polycrystalline silicon was placed in the container, and the contact area between the polycrystalline silicon raw material and the polyethylene sheet was 1.7 m. 2 The amount of air supplied to the polycrystalline silicon raw material during air drying was 40 m 3 / min.
[0124] The dopant concentration in the supplied air was measured according to the standard set by the Japan Air Cleaning Association (JACA No. 35A), and the B concentration was 31 ng / m 3 The Al, P, and As concentrations were all at the lower limit of quantification of 1 ng / m 3 The results were as follows.
[0125] A linear short-chain branched polyethylene (LLDPE) sheet that does not contain phosphate esters as an antioxidant was used as the polyethylene sheet for protection. This polyethylene sheet was immersed in a 5% dilute nitric acid solution, and the amount of dopant on the polyethylene sheet surface was investigated using ICP-MS. The Al concentration was 13 ng / cm 2 The B, P and As concentrations were all at the lower limit of quantification of 1 ng / cm 2 It was.
[0126] In order to control the surface dopant concentration, the air drying time was set to 6 hours for nugget S, 15 hours for nugget M, and 36 hours for nugget L. After air drying was completed, 5 kg of each size was packed into a polyethylene packaging bag, and the opening of the packaging bag was heat sealed. The polyethylene packaging bag was filled with 5% dilute nitric acid, and the extract was measured by ICP-MS to investigate the amount of dopant on the surface of the packaging bag that came into contact with the nugget. As a result, the B concentration, Al concentration, P concentration, and As concentration were all below the lower limit of quantification of 1 ng / cm. 2 It was.
[0127] As samples for measuring the surface dopant concentration, 5 kg of polycrystalline silicon nuggets were taken out of the sealed polyethylene packaging bags for each size. The surface dopant concentration was measured as follows.
[0128] After adding mannitol to high-purity nitric acid and high-purity hydrofluoric acid and dissolving it, approximately 100 g of polycrystalline silicon nuggets were removed from the bag with PFA tweezers and immersed in fluoronitric acid. After 20 to 30 μm of the nugget surface was dissolved, the polycrystalline silicon nuggets were removed from the fluoronitric acid.
[0129] After removing the polycrystalline silicon, the fluoronitric acid was heated and evaporated to dryness, and the residue was recovered and dissolved in 10 ml of nitric acid, and each surface dopant element was quantified using a double-focusing ICP-MS (Thermo Fischer Element2). From the obtained measured values, the concentration of each surface dopant element was calculated using the formula shown below, based on the number of silicon atoms contained in the polycrystalline silicon. The results are shown in Table 1.
number
[0130] For the surface As concentration, about 100 g of polycrystalline silicon nuggets were filled in a fluororesin container with an outlet for collecting impurity gas on the lid, and then 200 mL of high-purity hydrofluoric acid was poured from the outlet to immerse the polycrystalline silicon nuggets in. The gas containing As generated by this operation was quantified using a double-focusing ICP-MS equipped with a gas sample introduction system (manufactured by J-Science), and the actual measured value was used.
[0131] [Table 1]
[0132] The obtained polycrystalline silicon nuggets were used to grow single crystal silicon by the CZ method.
[0133] In order to prevent contamination when polycrystalline silicon is filled into the quartz crucible, the outside air is treated with an air washer, and the air that has passed through a low-boron glass fiber HEPA filter is then supplied to the clean room. The dopant concentration in the air is measured by the impinger method, and the B concentration is found to be 2 ng / m 3 The Al, P and As concentrations were all at the lower limit of quantification of 1 ng / m 3 The results were as follows.
[0134] In a clean room where cleanliness is controlled according to ISO14644-1 Class 6, the sealed polyethylene packaging bag was opened and 150 kg of polycrystalline silicon nuggets were loaded into a quartz crucible, and then single crystal silicon with a straight body length of 1600 mm and a diameter of 200 mm was obtained by the CZ method.
[0135] The resistivity values of the top side (solidification rate 0.05) and tail side (solidification rate 0.84) of the straight body of the obtained single crystal silicon were measured using a four-point probe resistance meter, and the results shown in Table 2 were obtained.
[0136] [Table 2]
[0137] From Table 2, it was confirmed that by controlling the bulk dopant concentration and the surface dopant concentration in the polycrystalline silicon raw material so as to satisfy the above relationship, single-crystalline silicon of the desired conductivity type, p-type, can be obtained.
[0138] In addition, the magnitude relationship of the resistivity of samples Nos. 1 to 3 is related to the effective acceptor element concentration (C* Therefore, by setting the effective acceptor element concentration of the polycrystalline silicon raw material to a predetermined value, it is possible to accurately achieve the target resistivity.
[0139] Example 2 Trichlorosilane was synthesized, purified by distillation, recovered and purified, and polycrystalline silicon was deposited in the same manner as in Example 1. The dichlorosilane concentration in the recovered and purified trichlorosilane was measured by gas chromatography and found to be 900 ppmw.
[0140] The polycrystalline silicon obtained after deposition was analyzed in the same manner as in Example 1. The average resistivity was 1,700 [Ωcm]. The bulk B concentration was 2 [ppta], and the bulk Al concentration was less than the lower limit of quantification, 1 [ppta]. The bulk acceptor concentration was set to 2 [ppta], assuming that the bulk Al concentration was 0 [ppta]. The bulk P concentration was 51 [ppta], and the bulk As concentration was 3 [ppta]. Therefore, the bulk donor concentration was 54 [ppta].
[0141] Next, similarly to Example 1, the obtained polycrystalline silicon rod was crushed and sorted into nuggets S, nuggets M, and nuggets L, and then etched to obtain polycrystalline silicon raw material.
[0142] 30 kg of each size was sampled, and the maximum side length of each piece was measured. Nugget S contained 91 wt% nuggets with a maximum side length of 10 mm to 45 mm, and the median diameter of nugget S was 29 mm. Nugget M contained 94 wt% nuggets with a maximum side length of 20 mm to 70 mm, and the median diameter of nugget M was 51 mm. Nugget L contained 94 wt% nuggets with a maximum side length of 60 mm to 100 mm, and the median diameter of nugget L was 81 mm.
[0143] The polycrystalline silicon raw material obtained by etching in the same manner as in Example 1 was received in a container covered with a polyethylene sheet according to size and air-dried. The weight of the polycrystalline silicon raw material loaded in the container at this time was 150 kg for each size. The contact area between the polycrystalline silicon raw material and the polyethylene sheet was 1.7 m 2 The amount of air supplied to the polycrystalline silicon raw material during air drying was 40 m 3 The dopant concentration in the supplied air was measured and found to be 57 ng / m 3 The Al, P, and As concentrations were all at the lower limit of quantification of 1 ng / m 3 The results were as follows.
[0144] The polyethylene sheet used for protection was an LLDPE sheet containing phosphate esters. The amount of dopant on the surface of this sheet was measured, and the P concentration was 15 ng / cm 2 , Al concentration is 4ng / cm 2 The B and As concentrations were all at the lower limit of quantification of 1 ng / cm 2 It was.
[0145] The air-drying times for the nuggets were 3 hours for nuggets S, 7 hours for nuggets M, and 18 hours for nuggets L. After air-drying, the nuggets were packed in polyethylene packaging bags of 5 kg each, and the opening of the packaging bag was heat-sealed.
[0146] 5 kg of polycrystalline silicon nuggets were sampled for each size from the sealed polyethylene packaging bags, and the surface dopant concentrations were calculated in the same manner as in Example 1. The results are shown in Table 3.
[0147] [Table 3]
[0148] Using the obtained polycrystalline silicon nugget, single crystal silicon having a straight body length of 1600 mm and a diameter of φ200 mm was obtained by the CZ method in the same manner as in Example 1.
[0149] The conductivity type and resistivity of the obtained single crystal silicon were measured in the same manner as in Example 1. The results are shown in Table 4.
[0150] [Table 4]
[0151] From Table 4, it was confirmed that, similarly to Example 1, by controlling the relationship between the bulk dopant concentration and the surface dopant concentration in the polycrystalline silicon raw material within the above range, single crystal silicon having a desired conductivity type and a targeted resistivity can be obtained.
[0152] Example 3 Trichlorosilane synthesis, distillation purification, recovery and purification, and deposition of polycrystalline silicon were carried out in the same manner as in Example 1. The dichlorosilane concentration in the recovered and purified trichlorosilane was measured by gas chromatography and found to be 200 ppmw.
[0153] The polycrystalline silicon obtained after deposition was analyzed in the same manner as in Example 1. The average resistivity was 8,300 [Ωcm]. The bulk B concentration was 2 [ppta], and the bulk Al concentration was less than the lower limit of quantification, 1 [ppta]. The bulk acceptor concentration was set to 2 [ppta], assuming that the bulk Al concentration was 0 [ppta]. The bulk P concentration was 11 [ppta], and the bulk As concentration was 2 [ppta]. Therefore, the bulk donor concentration was 13 [ppta].
[0154] Next, similarly to Example 1, the obtained polycrystalline silicon rod was crushed and sorted into nuggets S, nuggets M, and nuggets L, and then etched to obtain polycrystalline silicon raw material.
[0155] 30 kg of each size was sampled, and the maximum side length of each piece was measured. Nugget S contained 92 wt% nuggets with a maximum side length of 10 mm to 45 mm, and the median diameter of nugget S was 31 mm. Nugget M contained 93 wt% nuggets with a maximum side length of 20 mm to 70 mm, and the median diameter of nugget M was 50 mm. Nugget L contained 92 wt% nuggets with a maximum side length of 60 mm to 100 mm, and the median diameter of nugget L was 81 mm.
[0156] The polycrystalline silicon raw material obtained by etching in the same manner as in Example 1 was received in a container covered with a polyethylene sheet according to size and air-dried. The weight of the polycrystalline silicon raw material loaded in the container at this time was 150 kg for each size. The contact area between the polycrystalline silicon raw material and the polyethylene sheet was 1.7 m 2 The amount of air supplied to the polycrystalline silicon raw material during air drying was 40 m 3 The dopant concentration in the supplied air was measured and found to be 30 ng / m 3 The Al, P, and As concentrations were all at the lower limit of quantification of 1 ng / m 3 The results were as follows.
[0157] The polyethylene sheet used for protection was an LDPE sheet that did not contain phosphate esters. The dopant amount on the surface of this sheet was measured, and the Al concentration was 2 ng / cm 2 The B, P and As concentrations were all at the lower limit of quantification of 1 ng / cm 2 It was.
[0158] The air-drying times for the nuggets were 3 hours for nuggets S, 7 hours for nuggets M, and 18 hours for nuggets L. After air-drying, the nuggets were packed in polyethylene packaging bags of 5 kg each, and the opening of the packaging bag was heat-sealed.
[0159] 5 kg of polycrystalline silicon nuggets were sampled for each size from the sealed polyethylene packaging bags, and the surface dopant concentrations were calculated in the same manner as in Example 1. The results are shown in Table 5.
[0160] [Table 5]
[0161] Using the obtained polycrystalline silicon nugget, single crystal silicon having a straight body length of 1600 mm and a diameter of φ200 mm was obtained by the CZ method in the same manner as in Example 1.
[0162] The conductivity type and resistivity of the obtained single crystal silicon were measured in the same manner as in Example 1. The results are shown in Table 6.
[0163] [Table 6]
[0164] From Table 6, it was confirmed that, similarly to Example 1, by controlling the relationship between the bulk dopant concentration and the surface dopant concentration in the polycrystalline silicon raw material within the above range, single crystal silicon having a desired conductivity type and a targeted resistivity can be obtained.
[0165] Comparative Example 1 Trichlorosilane synthesis, distillation purification, recovery and purification, and deposition of polycrystalline silicon were carried out in the same manner as in Example 1. The dichlorosilane concentration in the recovered and purified trichlorosilane was measured by gas chromatography and found to be 150 ppmw.
[0166] The polycrystalline silicon obtained after deposition was analyzed by the same method as in Example 1. The average resistivity was 10,100 [Ωcm]. The bulk B concentration was 2 [ppta], and the bulk Al concentration was less than the lower limit of quantification, 1 [ppta]. The bulk acceptor concentration was set to 2 [ppta], assuming that the bulk Al concentration was 0 [ppta]. The bulk P concentration was 9 [ppta], and the bulk As concentration was 1 [ppta]. Therefore, the bulk donor concentration was 10 [ppta].
[0167] Next, similarly to Example 1, the obtained polycrystalline silicon rod was crushed and sorted into nuggets S, nuggets M, and nuggets L, and then etched to obtain polycrystalline silicon raw material.
[0168] 30 kg of each size was sampled, and the maximum side length of each piece was measured. Nugget S contained 92 wt% nuggets with a maximum side length of 10 mm to 45 mm, and the median diameter of nugget S was 30 mm. Nugget M contained 92 wt% nuggets with a maximum side length of 20 mm to 70 mm, and the median diameter of nugget M was 49 mm. Nugget L contained 94 wt% nuggets with a maximum side length of 60 mm to 100 mm, and the median diameter of nugget L was 81 mm.
[0169] The polycrystalline silicon raw material obtained by etching in the same manner as in Example 1 was received in a container covered with a polyethylene sheet according to size and air-dried. The weight of the polycrystalline silicon raw material loaded in the container at this time was 150 kg for each size. The contact area between the polycrystalline silicon raw material and the polyethylene sheet was 1.7 m 2 The amount of air supplied to the polycrystalline silicon raw material during air drying was 40 m 3 The dopant concentration in the supplied air was measured and found to be 14 ng / m 3 The Al, P, and As concentrations were all at the lower limit of quantification of 1 ng / m 3 The results were as follows.
[0170] The polyethylene sheet used for protection was an LDPE sheet that did not contain phosphate esters. The dopant amount on the surface of this sheet was measured, and the Al concentration was 2 ng / cm 2 The B, P and As concentrations were all at the lower limit of quantification of 1 ng / cm 2 It was.
[0171] As in Example 1, the air-drying times for the nuggets were 2 hours for nugget S, 4 hours for nugget M, and 12 hours for nugget L. After air-drying, the nuggets were packed in polyethylene packaging bags of 5 kg each, and the opening of the packaging bag was sealed by heat sealing.
[0172] 5 kg of polycrystalline silicon nuggets were sampled for each size from the sealed polyethylene packaging bags, and the surface dopant concentrations were calculated in the same manner as in Example 1. The results are shown in Table 7.
[0173] [Table 7]
[0174] Using the obtained polycrystalline silicon nugget, single crystal silicon having a straight body length of 1600 mm and a diameter of φ200 mm was obtained by the CZ method in the same manner as in Example 1.
[0175] The conductivity type and resistivity of the obtained single crystal silicon were measured in the same manner as in Example 1. The results are shown in Table 8.
[0176] [Table 8]
[0177] As can be seen from Table 8, unlike Examples 1 to 3, for the single crystal silicon ingots of Samples 10 to 12, the conductivity type on the top side was n-type, which is opposite to the targeted conductivity type, and was inverted to p-type midway through the ingot.
[0178] Therefore, even if both the bulk dopant concentration and the surface dopant concentration are reduced in order to minimize contamination of the polycrystalline silicon raw material, unless the relationship between the bulk dopant concentration and the surface dopant concentration is controlled within a predetermined range, it has been confirmed that the conductivity type will be inverted during the process of producing a single crystal silicon ingot, and as a result, it has been confirmed that the yield of single crystal silicon will drop significantly.
[0179] The conductivity type was P-type, and the straight body length at the position showing a resistivity of 10,000 [Ωcm] or more was 600 mm for sample number 10, 150 mm for sample number 11, and 300 mm for sample number 12.
[0180] Comparative Example 2 Trichlorosilane synthesis, distillation purification, recovery and purification, and polycrystalline silicon deposition were performed in the same manner as in Example 1. The dichlorosilane concentration in the recovered and purified trichlorosilane was measured by gas chromatography and found to be 200 ppmw.
[0181] The polycrystalline silicon obtained after deposition was analyzed by the same method as in Example 1. The average resistivity was 7,600 [Ωcm]. The bulk B concentration was 3 [ppta], and the bulk Al concentration was less than the lower limit of quantification of 1 [ppta]. The bulk acceptor concentration was set to 3 [ppta], assuming that the bulk Al concentration was 0 [ppta]. The bulk P concentration was 12 [ppta], and the bulk As concentration was 1 [ppta]. Therefore, the bulk donor concentration was 13 [ppta].
[0182] Next, similarly to Example 1, the obtained polycrystalline silicon rod was crushed and sorted into nuggets S, nuggets M, and nuggets L, and then etched to obtain polycrystalline silicon raw material.
[0183] 30 kg of each size was sampled, and the maximum side length of each piece was measured. Nugget S contained 94 wt% nuggets with a maximum side length of 10 mm to 45 mm, and the median diameter of nugget S was 29 mm. Nugget M contained 92 wt% nuggets with a maximum side length of 20 mm to 70 mm, and the median diameter of nugget M was 49 mm. Nugget L contained 94 wt% nuggets with a maximum side length of 60 mm to 100 mm, and the median diameter of nugget L was 79 mm.
[0184] The polycrystalline silicon raw material obtained by etching in the same manner as in Example 1 was received in a container covered with a polyethylene sheet according to size and air-dried. The weight of the polycrystalline silicon raw material loaded in the container at this time was 150 kg for each size. The contact area between the polycrystalline silicon raw material and the polyethylene sheet was 1.7 m 2 The amount of air supplied to the polycrystalline silicon raw material during air drying was 40 m 3 The dopant concentration in the supplied air was measured and found to be 19 ng / m 3 The Al, P, and As concentrations were all at the lower limit of quantification of 1 ng / m 3 The results were as follows.
[0185] The polyethylene sheet used for protection was an LLDPE sheet containing phosphate esters. The amount of dopant on the surface of this sheet was measured, and the P concentration was 15 ng / cm 2 , Al concentration is 2ng / cm 2 The B and As concentrations were all at the lower limit of quantification of 1 ng / cm 2 It was.
[0186] As in Example 1, the air-drying times for the nuggets were 6 hours for nugget S, 15 hours for nugget M, and 36 hours for nugget L. After air-drying, the nuggets were packed in polyethylene packaging bags of 5 kg each, and the opening of the packaging bag was heat-sealed.
[0187] 5 kg of polycrystalline silicon nuggets were taken out for each size from the sealed polyethylene packaging bags, and the surface dopant concentrations were calculated in the same manner as in Example 1. The results are shown in Table 9.
[0188] [Table 9]
[0189] Using the obtained polycrystalline silicon nugget, single crystal silicon having a straight body length of 1600 mm and a diameter of φ200 mm was obtained by the CZ method in the same manner as in Example 1.
[0190] The conductivity type and resistivity of the obtained single crystal silicon were measured in the same manner as in Example 1. The results are shown in Table 10.
[0191] [Table 10]
[0192] From Table 10, the conductivity type of the single crystal silicon ingot of sample number 13 was p-type, and the resistivity on the top side was 10,000 [Ωcm] or more, but fell below 10,000 [Ωcm] from the position 750 mm from the top side. The conductivity type of the single crystal silicon ingots of sample numbers 14 and 15 was p-type, but the resistivity from the top side was 10,000 [Ωcm] or less.
[0193] Therefore, it was confirmed that when the relationship between the bulk dopant concentration and the surface dopant concentration is greater than the above range, the resistivity of the single crystal silicon ingot becomes smaller than 10,000 [Ωcm].
Claims
1. A polycrystalline silicon raw material for producing p-type single crystal silicon, comprising a plurality of polycrystalline silicon chunks, When the total concentration of donor elements present in the bulk of the polycrystalline silicon raw material is Cd1 [ppta], the total concentration of acceptor elements present in the bulk of the polycrystalline silicon raw material is Ca1 [ppta], the total concentration of donor elements present on the surface of the polycrystalline silicon raw material is Cd2 [ppta], and the total concentration of acceptor elements present on the surface of the polycrystalline silicon raw material is Ca2 [ppta], A polycrystalline silicon raw material, wherein Cd1, Ca1, Cd2 and Ca2 satisfy the relationship: 5 [ppta]≦(Ca1+Ca2)−(Cd1+Cd2)≦26 [ppta].
2. The polycrystalline silicon raw material described in claim 1, characterized in that if the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material is 100%, the weight of the polycrystalline silicon chunks having a maximum side length of 10 mm or more and 45 mm or less is 90% or more.
3. The polycrystalline silicon raw material described in claim 1, characterized in that if the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material is 100%, the weight of the polycrystalline silicon chunks having a maximum side length of 20 mm or more and 70 mm or less is 90% or more.
4. The polycrystalline silicon raw material described in claim 1, characterized in that if the total weight of the polycrystalline silicon chunks contained in the polycrystalline silicon raw material is 100%, the weight of the polycrystalline silicon chunks having a maximum side length of 60 mm or more and 100 mm or less is 90% or more.
5. A method for producing p-type single crystal silicon by melting a polycrystalline silicon raw material containing a plurality of polycrystalline silicon chunks, comprising: The method includes a step of producing p-type single crystal silicon having a resistivity of 10,000 Ωcm or more without adding a dopant when melting the polycrystalline silicon raw material, A method for producing p-type single crystal silicon using, as the polycrystalline silicon raw material, a polycrystalline silicon raw material in which Cd1, Ca1, Cd2, and Ca2 satisfy the relationship: 5 [ppta]≦(Ca1+Ca2)-(Cd1+Cd2)≦26 [ppta], where Cd1, Ca1, Cd2, and Ca2 are the total concentration of donor elements present in the bulk of the polycrystalline silicon raw material, Cd1 [ppta], the total concentration of acceptor elements present in the bulk of the polycrystalline silicon raw material, Ca1 [ppta], the total concentration of donor elements present on the surface of the polycrystalline silicon raw material, Cd2 [ppta], and the total concentration of acceptor elements present on the surface of the polycrystalline silicon raw material, Ca2 [ppta].
6. A method for producing p-type single crystal silicon as described in claim 5, wherein in the process of producing p-type single crystal silicon, the resistivity of the p-type single crystal silicon is 50,000 Ω cm or less.
Citation Information
Patent Citations
Method for manufacturing high resistivity silicon single crystal
JP2004315336A
Low dopant polycrystalline silicon lump
JP2013151413A
Method of producing silicon single crystal and method of producing silicon single crystal wafer
JP2014156376A
Growing method of silicon single crystal
JP2016108160A
Manufacturing method of bonded SOI wafer
JP2017069240A