Lithium composite oxide single crystal, lithium composite oxide polycrystal, lithium composite oxide material, solid electrolyte material, all-solid-state lithium ion secondary battery, and method for producing solid electrolyte material

Lithium composite oxide single crystals and polycrystals with a garnet-type structure, produced via a melting method, address the conductivity challenges of existing batteries by achieving high relative densities and improved lithium ion conductivity, suitable for all-solid lithium ion secondary batteries.

JP7573308B2Active Publication Date: 2024-10-25NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022563721
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-17
Filing Date
2021-11-12
Publication Date
2024-10-25
Estimated Expiration
2041-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion secondary batteries face challenges in achieving high lithium ion conductivity due to difficulties in producing high-density molded bodies of polycrystalline materials with cubic garnet structures, which are difficult to sinter, leading to issues with grain boundary resistance and interfacial resistance.

Method used

The development of lithium composite oxide single crystals and polycrystals with a garnet-type structure, specifically Li7-3x-w-vGa x La3Zr2-w-vTaW Nb vO12, which are produced through a melting method to achieve high relative densities and improved lithium ion conductivity, utilizing methods like the floating zone and Czochralski techniques.

Benefits of technology

The resulting lithium composite oxides exhibit lithium ion conductivity of 1.0×10−3 S/cm or more, with relative densities of 90% or higher, reducing grain boundary resistance and enabling the production of high-quality solid electrolyte materials for all-solid lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573308000001
    Figure 0007573308000001
  • Figure 0007573308000002
    Figure 0007573308000002
  • Figure 0007573308000003
    Figure 0007573308000003
Patent Text Reader

Abstract

This lithium composite oxide single crystal has a chemical composition represented by Li7-3x-w-vGaxLa3Zr2-w-vTawNbvO12 (wherein 0.02 ≤ x < 0.5, 0 ≤ W ≤ 1.0, 0 ≤ V ≤ 1.0 and 0.05 ≤ W + V ≤ 1.0), while belonging to the cubic space group I-43d and having a garnet structure.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium composite oxide single crystal, a lithium composite oxide polycrystal, a lithium composite oxide material, a solid electrolyte material, an all-solid-state lithium ion secondary battery, and a method for producing a solid electrolyte material. This application claims priority based on Japanese Patent Application No. 2020-191100, filed on November 17, 2020, the contents of which are incorporated herein by reference. [Background technology]

[0002] Lithium-ion secondary batteries have a higher energy density than secondary batteries such as nickel-cadmium batteries and nickel-metal hydride batteries, and can be operated at a high potential, so they are widely used in small information devices such as mobile phones and laptops. In addition, lithium-ion secondary batteries are easy to make small and lightweight, so in recent years, there has been an increasing demand for them as secondary batteries for hybrid and electric vehicles. In consideration of safety, research and development is being conducted on all-solid-state lithium-ion secondary batteries that do not use flammable electrolytes. The solid electrolyte used in all-solid-state lithium-ion secondary batteries is required to have high ionic conductivity.

[0003] It has been reported that materials having a cubic garnet structure have high ionic conductivity (see Patent Document 1), and research and development of materials having this structure is underway. 7-x La3Zr 2-x Ta x O 12 , Li 7-x La3Zr 2-x Nb x O 12It has been reported that materials represented by the formula (1) have high ionic conductivity when the composition ratio x is close to 0.5 (see Non-Patent Documents 1 and 2). To achieve high ionic conductivity, it is necessary to reduce grain boundary resistance and interface resistance as much as possible, so a solid material that is a high-density molded body is desirable. A solid material that is a high-density molded body can prevent short circuits between the positive and negative electrodes during charging and discharging and can be made into thin pieces, which makes it possible to miniaturize all-solid-state lithium-ion secondary batteries in the future. However, it is known that these polycrystalline materials with a cubic garnet structure are difficult to sinter, and it is difficult to prepare a high-density molded body.

[0004] Recently, the garnet-type Li 7-x La3Zr 2-x Ta x O 12 Single crystals and Li 7-x La3Zr 2-x Nb x O 12 There have been reports of growing single crystals of this compound (see Patent Documents 2 and 3).

[0005] Recently, gallium-substituted cubic garnet-type Li 7-3x Ga x La3Zr2O 12 There are reports of sintered bodies of Li2O3 produced by melting and showing high lithium ion conductivity (see Non-Patent Documents 3 and 4). 7-3x Ga x La3Zr2O 12 It has been reported that single crystals have higher ionic conductivity than sintered bodies.

[0006] To achieve high ionic conductivity, it is necessary to minimize grain boundary and interface resistance, so a high-density molded solid material is desirable. In particular, a high-density molded single crystal is expected to have high lithium ion conductivity because it is not affected by grain boundaries. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-195373 A [Patent Document 2] International Publication No. 2016 / 068040 [Patent Document 3] International Publication No. 2017 / 130622 [Non-patent literature]

[0008] [Non-Patent Document 1] Scientific reports, 8, 9965(2018) [Non-Patent Document 2] Chemelectrochem, 5, 2551(2018) [Non-Patent Document 3] Chemistry Materials, 28, 1861-1871(2016) [Non-Patent Document 4] Crystallographic Communications, E72, 287-289, (2016) [Non-Patent Document 5] Applied Materials Interfaces, 12, 25709-25717(2020) Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in view of the above circumstances, and has an object to provide a lithium composite oxide single crystal, a lithium composite oxide polycrystal, a lithium composite oxide material, a solid electrolyte material, an all-solid-state lithium ion secondary battery, and a method for producing the solid electrolyte material, all of which have improved lithium ion conductivity. [Means for solving the problem]

[0010] The present inventors have conducted extensive research into a method for melting a mixed raw material containing an excess of lithium and gallium compared to the composition ratio of the target solid electrolyte material at a high temperature and then cooling it. As a result, they have found that Li 7-3x-w-v Ga x La3Zr 2-w-v Ta W Nb v O 12 The inventors discovered that it was possible to produce a single crystal with the following formula: (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0) and confirmed that this single crystal could be mechanically sliced ​​to form a thin slice, thereby completing the present invention. In order to solve the above problems, the present invention employs the following means.

[0011] (1) The lithium composite oxide single crystal according to one embodiment of the present invention has a chemical composition of Li 7-3x-w-v Ga x La3Zr 2-w-v Ta W Nb v O 12 (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0), it belongs to the cubic crystal system, space group I-43d, and has a garnet-type structure.

[0012] (2) The lithium composite oxide polycrystal according to one embodiment of the present invention has a chemical composition of Li 7-3x―w-v Ga x La3Zr 2-w―v Ta W Nb v O 12 (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0), it belongs to the cubic crystal system, space group I-43d, and has a garnet-type structure.

[0013] (3) In the lithium composite oxide polycrystal according to the above aspect, the relative density is preferably 90% or more.

[0014] (4) In the lithium composite oxide polycrystal according to the above aspect, the relative density is preferably 95% or more.

[0015] (5) A lithium composite oxide material according to one embodiment of the present invention includes the lithium composite oxide single crystal according to the above embodiment or the lithium composite oxide polycrystal according to the above embodiment.

[0016] (6) A solid electrolyte material according to an embodiment of the present invention includes the lithium composite oxide single crystal according to the above embodiment or the lithium composite oxide polycrystal according to the above embodiment.

[0017] (7) In the solid electrolyte material according to the above aspect, the lithium ion conductivity is 1.0×10 -3 It is preferable that the viscosity is S / cm or more.

[0018] (8) An all-solid-state lithium-ion secondary battery according to an aspect of the present invention includes a positive electrode, a negative electrode, and the solid electrolyte material according to the above aspect.

[0019] (9) A method for producing a solid electrolyte material according to one aspect of the present invention is a method for producing a solid electrolyte material according to the above aspect, (7-3x-W)y Ga xz La3Zr 2-W Ta W Nb v O 12 The method includes a molten portion forming step of forming a molten portion by melting at least a portion of a rod-shaped substrate (first substrate) containing a raw material represented by the formula (0.02≦x<0.5, 1.1≦y≦1.4, 1.6≦z≦3.3, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0, 1.1≦y≦1.5, 1.5≦z≦3.5), and a molten portion moving step of moving the molten portion at an average speed of 8 mm / h or more.

[0020] (10) In the method for producing a solid electrolyte material according to the above aspect, the average speed is preferably 8 mm / h or more and 19 mm / h or less.

[0021] (11) In the molten portion forming step of the method for producing a solid electrolyte material according to the above aspect, the substrate is preferably rotated together with the molten portion in a plane perpendicular to the longitudinal direction at a rotation speed of 30 rpm or more.

[0022] (12) In the method for producing a solid electrolyte material according to the above aspect, the molten portion moving step may be performed in a state in which a seed crystal of the solid electrolyte is attached to the molten portion.

[0023] (13) In the molten portion moving step of the method for producing a solid electrolyte material according to the above aspect, the molten portion is preferably rotated at a rotation speed of 2 rpm or more and 8 rpm or less on a plane perpendicular to a longitudinal direction of the substrate.

[0024] (14) A method for producing a solid electrolyte material according to another aspect of the present invention is a method for producing a solid electrolyte material according to the above aspect, the method comprising the steps of: (7-3x-W)y Ga xz La3Zr 2-W Ta W Nb v O 12 The method includes a melt forming step of melting a raw material represented by (0.02≦x<0.5, 1.1≦y≦1.4, 1.6≦z≦3.3, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0, 1.1≦y≦1.5, 1.5≦z≦3.5) in a crucible to form a melt of the raw material, a melt adhering step of immersing a substrate (second substrate) in the melt in the crucible to allow the melt to adhere to the substrate, and a melt moving step of moving the melt adhering to the substrate together with the substrate out of the crucible at an average speed of 8 mm / h or more.

[0025] (15) In the method for producing a solid electrolyte material according to the above aspect, the average speed is preferably 8 mm / h or more and 19 mm / h or less.

[0026] (16) In the method for producing a solid electrolyte material according to the above aspect, the melt transferring step may be performed in a state where a seed crystal of the solid electrolyte is attached to the substrate.

[0027] (17) In the melt portion moving step of the method for producing a solid electrolyte material according to the above aspect, the rod-shaped substrate is preferably rotated in a plane perpendicular to the longitudinal direction relative to the melt at a rotation speed of 2 rpm or more and 8 rpm or less. Effect of the Invention

[0028] According to the present invention, it is possible to provide a lithium composite oxide single crystal, a lithium composite oxide polycrystal, a lithium composite oxide material, a solid electrolyte material, an all-solid-state lithium ion secondary battery, and a method for producing a solid electrolyte material, all of which have improved lithium ion conductivity. [Brief description of the drawings]

[0029] [Figure 1] 1 is a photograph showing the appearance of a Li6Ga0.25La3Zr1.75Ta0.25O12 single crystal grown by the FZ method in Example 1. [Diagram 2] FIG. 1 shows a single crystal X-ray diffraction pattern obtained for the Li6Ga0.25La3Zr1.75Ta0.25O12 single crystal. [Diagram 3] 2 is a schematic diagram showing the garnet-type structure of the Li6Ga0.25La3Zr1.75Ta0.25O12 single crystal of FIG. 1. [Figure 4] This is a Nyquist plot obtained by using the AC impedance method for the Li6Ga0.25La3Zr1.75Ta0.25O12 single crystal in Figure 1. [Diagram 5] FIG. 1 shows a powder X-ray diffraction pattern obtained for the Li6Ga0.25La3Zr1.75Ta0.25O12 single crystal. [Figure 6] FIG. 2 is a schematic diagram of an evaluation device for an all-solid-state lithium-ion secondary battery produced using the Li6Ga0.25La3Zr1.75Ta0.25O12 of FIG. 1. [Figure 7] 1 is a photograph showing the appearance of a Li6Ga0.25La3Zr1.75Nb0.25O12 crystal grown by the FZ method in Example 3. [Figure 8] FIG. 7 shows a single crystal X-ray diffraction pattern obtained for the Li6Ga0.25La3Zr1.75Nb0.25O12 single crystal. [Figure 9] 8 is a schematic diagram showing the garnet-type structure of the Li6Ga0.25La3Zr1.75Nb0.25O12 single crystal of FIG. [Figure 10] 1 is a photograph showing the appearance of a Li6Ga0.25La3Zr1.75Ta0.125Nb0.125O12 crystal grown by the FZ method in Example 4. [Figure 11] FIG. 10 shows a single crystal X-ray diffraction pattern obtained for the Li6Ga0.25La3Zr1.75Ta0.125Nb0.125O12 single crystal. [Figure 12] 12 is a schematic diagram showing the garnet-type structure of the Li6Ga0.25La3Zr1.75Ta0.125Nb0.125O12 single crystal of FIG. [Figure 13] 1 is a photograph showing the appearance of a Li6.125Ga0.125La3Zr1.5Ta0.25Nb0.25O12 crystal grown by the Cz method in Example 5. [Figure 14] FIG. 13 shows a single crystal X-ray diffraction pattern obtained for the LiGaLaZrTaNbO single crystal. [Figure 15] 14 is a schematic diagram showing the garnet-type structure of the Li6.125Ga0.125La3Zr1.5Ta0.25Nb0.25O12 single crystal of FIG. [Figure 16] 1 is a photograph showing the appearance of a Li5.55Ga0.4La3Zr1.75Ta0.125Nb0.125O12 crystal grown by the FZ method in Example 6. [Figure 17] FIG. 16 shows a single crystal X-ray diffraction pattern obtained for the Li5.55Ga0.4La3Zr1.75Ta0.125Nb0.125O12 single crystal. [Figure 18] 17 is a schematic diagram showing the garnet-type structure of the Li5.55Ga0.4La3Zr1.75Ta0.125Nb0.125O12 single crystal of FIG. [Figure 19] 1 is a photograph showing the appearance of the lithium composite oxide polycrystal prepared in Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, the lithium composite oxide single crystal, lithium composite oxide polycrystal, lithium composite oxide material, solid electrolyte material, all-solid-state lithium ion secondary battery, and manufacturing method of the solid electrolyte material according to the embodiment of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged manner for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality. In addition, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and can be appropriately modified and implemented within the scope of the present invention.

[0031] (Solid electrolyte materials, lithium composite oxide single crystals, lithium composite oxide polycrystals) The solid electrolyte material according to one embodiment of the present invention has a chemical composition of Li 7-3x-w-v Ga x La3Zr 2-w-v Ta W Nb v O 12 The lithium composite oxide material includes at least one of a lithium composite oxide single crystal and a lithium composite oxide polycrystal represented by (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0). Here, the solid electrolyte material is a type of lithium composite oxide material. The application of the lithium composite oxide material is not limited to the application as a solid electrolyte for an all-solid-state battery, and can be applied to various applications.

[0032] The lithium composite oxide single crystal contained in the solid electrolyte material is a cubic crystal belonging to space group I-43d and has a garnet-type structure. The lithium composite oxide polycrystal contained in the solid electrolyte material is a cubic crystal belonging to space group I-43d and has a garnet-type structure.

[0033] In this embodiment, a lithium composite oxide having a relative density of 99% or more is defined as a lithium composite oxide single crystal, and a lithium composite oxide having a relative density of 90% or more and less than 99%, preferably 95% or more and less than 99%, is defined as a lithium composite oxide polycrystal. In the manufacturing process of the lithium composite oxide single crystal described below, volatile materials are used, and air is generated when the single crystal is manufactured by a melting method, which may cause voids inside the single crystal. In such cases, the single crystal has a relative density of less than 100%.

[0034] The relative density is calculated by measuring the external shape of the prepared lithium composite oxide sample (such as a thin piece) to calculate the apparent volume, and dividing the apparent density calculated from the measured mass by the true density obtained from the results of single crystal X-ray structure analysis. The solid electrolyte material of the present embodiment has a high density, and therefore can be easily cut to any thickness using a diamond cutter or the like.

[0035] In solid electrolyte materials, the lithium ion conductivity is set to 1.0×10 -3 S / cm or more, and by making the relative density almost 100%, the -3 The higher the relative density, the stronger the adhesion between particles and the fewer the grain boundaries, which can improve the ionic conductivity.

[0036] (Method of manufacturing solid electrolyte material) The method for producing a solid electrolyte material of this embodiment mainly includes a step of forming a molten part of the raw material of the solid electrolyte material (molten part forming step) and a step of moving the molten part (molten part moving step). The formation and movement of the molten zone is carried out using one of the melting methods such as the floating zone (FZ) method, the Czochralski (Cz) method, the Bridgman method, the pedestal method, etc., depending on the size, shape, etc. of the crystal to be produced.

[0037] [FZ method] When a solid electrolyte material is manufactured using the FZ method, the following procedure is taken as a specific example. First, considering that lithium volatilizes at high temperatures, lithium compounds, gallium compounds, lanthanum compounds, zirconium compounds, tantalum compounds, and niobium compounds are weighed out. This weighing is performed so that the molar ratio of Li:Ga:La:Zr:Ta:Nb in the final solid electrolyte material is (7-3x-wv)y:xz:3:2-wv:w:v (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0, 1.1≦y≦1.5, 1.5≦z≦3.5).

[0038] The lithium compound is not particularly limited as long as it contains lithium, and examples thereof include oxides such as Li2O and carbonates such as Li2CO3. The gallium compound is not particularly limited as long as it contains gallium, and examples thereof include oxides such as Ga2O3 and nitrates such as Ga(NO3)3. The lanthanum compound is not particularly limited as long as it contains lanthanum, and examples thereof include oxides such as La2O3 and hydroxides such as La(OH)3. The zirconium compound is not particularly limited as long as it contains zirconium, and examples thereof include oxides such as ZrO2 and chlorides such as ZrCl4. The tantalum compound is not particularly limited as long as it contains tantalum, and examples thereof include oxides such as Ta2O5 and chlorides such as TaCl5. The niobium compound is not particularly limited as long as it contains niobium, and examples thereof include oxides such as Nb2O5 and chlorides such as NbCl5.

[0039] Alternatively, a compound consisting of two or more kinds selected from lithium, gallium, lanthanum, zirconium, and tantalum or niobium or both may be used and weighed out so that the molar ratio of Li:Ga:La:Zr:Ta:Nb is (7-3x-wv)y:xz:3:(2-wv):w:v (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0, 1.1≦y≦1.5, 1.5≦z≦3.5). Examples of such a compound consisting of two or more kinds include lanthanum zirconium oxide such as La2Zr2O7, gallium lanthanum oxide such as GaLaO6, lithium gallium oxide such as Li5GaO4, lithium zirconium oxide such as Li2ZrO3, lanthanum tantalum compound such as LaTaO4, and lanthanum niobium compound such as LaNbO4.

[0040] Next, the weighed compounds are mixed. The mixing method is not particularly limited as long as the compounds can be mixed uniformly, and may be mixed wet or dry using a mixer such as a mixer. The mixture obtained is then filled into a crucible with a lid, and pre-fired at 600°C to 900°C, preferably 850°C, to obtain a powder that serves as a raw material. It is more preferable to crush, mix, and fire the raw material once pre-fired.

[0041] Next, the obtained raw material powder is pulverized to reduce the particle size so as to facilitate molding. The pulverization method is not particularly limited as long as the particles can be made fine, and for example, pulverization may be performed in a wet or dry manner using a pulverizing device such as a planetary ball mill, a pot mill, or a bead mill. The pulverized material obtained is then filled into a rubber tube, and is then molded into a rod shape by isostatic pressing.

[0042] Next, the obtained rod-shaped molded body is sintered at about 700°C to 1300°C, preferably 800°C to 1150°C, for about 4 hours to obtain a rod-shaped first substrate. At this point, the chemical composition of the raw material is Li (7-3x-w-v)y Ga xz La3Zr2 -W Ta W Nb v O12 (0.02≦x<0.5, 1.1≦y≦1.4, 1.6≦z≦3.3, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0). In this manner, a rod-shaped first substrate can be manufactured.

[0043] Then, the rod-shaped first base material is placed in an infrared ray collecting heating furnace, and at least a part of the first base material is melted (melted portion forming process). (7-3x-w-v)y Ga xz La3Zr 2-w Ta W Nb v O 12 At least a part of a rod-shaped first base material containing a raw material represented by (0.02≦x<0.5, 1.1≦y≦1.4, 1.6≦z≦3.3, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0) is heated using a predetermined heating means (such as an infrared focusing heating device) to form a molten part. Here, the molten part forming step may be performed while rotating on a plane perpendicular to the longitudinal direction, i.e., while rotating the first base material about its axis along the longitudinal direction.

[0044] Subsequently, or together with the molten part forming step, the raw material with the molten part formed therein is moved in its longitudinal direction (molten part moving step). In the molten part moving step, for example, the raw material with the above-mentioned chemical composition is moved parallel to the longitudinal direction, i.e., along the longitudinal direction, at an average speed of 8 mm / h or more (preferably, 8 mm / h or more and 19 mm / h or less). From the viewpoint of efficient growth of the lithium composite oxide crystal, the molten part moving step may be performed in a state where a seed crystal of a solid electrolyte is attached to the molten part. In this case, the seed crystal also forms a molten part and starts moving within a few minutes after being combined with the molten part of the raw material. The molten part is rapidly cooled during the movement.

[0045] After quenching, it is a cubic crystal with a relative density of 90% or more, belongs to the space group I-43d, and has a garnet-type structure. 7-3x-w-v GaxLa3Zr 2-w-v Ta W Nb v O 12A solid electrolyte material containing a lithium composite oxide with (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0) can be obtained. This manufacturing method produces a solid electrolyte material with a length (maximum diameter) of 2 cm or more, which can be easily cut into multiple pieces to produce thin pieces of solid electrolyte material with the same quality.

[0046] In the molten part moving step, the molten part of the rod-shaped first substrate is rotated in a plane perpendicular to the longitudinal direction at a predetermined rotation speed, preferably 30 rpm or more, more preferably 30 rpm or more and 60 rpm or less. Furthermore, when a seed crystal is used, it is attached to the tip of the rod-shaped first substrate, melted together with the first substrate, a part of which becomes the molten part, and rotated together with the molten part at approximately the same rotation speed.

[0047] When manufacturing by the FZ method, bubbles are generated in the molten part as highly volatile lithium tries to volatilize. In this way, bubbles originating from the raw material are generated during the manufacturing process, and voids may occur in the lithium composite oxide single crystal as a finished product. In this case, the relative density is less than 100%. However, by increasing the rotation speed of the rod-shaped raw material (first substrate) to 30 rpm or more, the bubbles can be easily removed. Therefore, the relative density of the lithium composite oxide single crystal as a finished product can be increased. In addition, when an infrared light collecting heating device is used, if a highly volatile gas is stagnated, the infrared light may be blocked by the highly volatile gas, and from the viewpoint of efficiently carrying out the FZ method, it is required to reduce the volatile components or to discharge them outside the device. From this viewpoint, it is preferable to carry out the molten part forming process and the molten part moving process in a dry gas atmosphere. The FZ method can be carried out while flowing a dry gas such as oxygen, nitrogen, argon, or air.

[0048] [Cz method] When a solid electrolyte material is manufactured using the Cz method, the following procedure is taken as a specific example: First, the same raw material as the first substrate is melted in a crucible in the same procedure as in the FZ method to form a melt of the raw material (melt formation process).

[0049] Next, a second substrate for growing a crystal of a lithium composite oxide is immersed in the melt in the crucible, and the melt is attached to the second substrate (melt attachment step). The shape of the second substrate is not particularly limited. Next, the melt attached to the second substrate together with the second substrate is moved (pulled up) out of the crucible at an average speed of 8 mm / h or more (preferably 8 mm / h or more and 19 mm / h or less) (melt transfer step). By increasing the lifting speed (transfer speed) of the melt to 8 mm / h or more, the volatilization of lithium and gallium is suppressed, and high-density Li 7-3x-w-v Ga x La3Zr 2-w-v Ta W Nb v O 12 (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0) crystals are obtained.

[0050] For example, when the second substrate is rod-shaped, the growth of crystals of the lithium composite oxide can be promoted by rotating the second substrate in a plane perpendicular to the longitudinal direction of the second substrate relative to the melt at a rotation speed of 2 rpm or more and 8 rpm or less in the melt portion moving step.

[0051] When the melt attachment step is performed in a state in which a seed crystal of a solid electrolyte is attached to the second substrate, the melt is attached onto the seed crystal, which can promote the growth of a crystal of a lithium composite oxide in the melt transfer step.

[0052] As described above, the lithium composite oxide Li grown by the melting method of this embodiment 7-3x-w-v Ga x La3Zr 2-w-v Ta W Nb v O 12 (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0) has a different space group from lithium composite oxides synthesized by the solid-state method so far. That is, the lithium composite oxides synthesized by the solid-state method have a space group of Ia-3d, whereas the lithium composite oxides grown by the melt method have a space group of I-43d.

[0053] In addition, the lithium composite oxide grown by the melting method has a crystal structure with a relative density of 90% or more and has few grain boundaries, and therefore has excellent lithium ion conductivity. Therefore, for example, in an all-solid-state lithium ion secondary battery including a positive electrode, a negative electrode, and a solid electrolyte, a solid electrolyte material containing the lithium composite oxide of this embodiment (lithium composite oxide single crystal, lithium composite oxide polycrystal) can be used as the solid electrolyte.

[0054] The relative density of the grown lithium composite oxide can be adjusted by changing the production conditions. For example, the higher the heating temperature in the molten part (melt) forming step, the longer the heating time, the higher the relative density can be. EXAMPLES

[0055] The effects of the present invention will be more clearly understood by the following examples. Note that the present invention is not limited to the following examples, and can be modified as appropriate without departing from the spirit and scope of the present invention.

[0056] <Example 1> The lithium composite oxide single crystal of the present invention was produced by the following procedure.

[0057] (Li6Ga 0.25 La3Zr 1.75 Ta 0.25 O 12 Mixing of raw materials) First, 28.024g of lithium carbonate Li2CO3 (made by Rare Metallic, purity 99.99%), 3.385g of gallium oxide Ga2O3 (made by Rare Metallic, purity 99.99%), 44.131g of lanthanum oxide La2O3 (made by Rare Metallic, purity 99.99%), 19.472g of zirconium oxide ZrO2 (made by Rare Metallic, purity 99.99%), and 4.988g of tantalum oxide Ta2O5 (made by Rare Metallic, purity 99.99%) were placed in an agate mortar and mixed uniformly by a wet method using ethanol. The lanthanum oxide was pre-calcined at 900°C. The molar ratio of metals contained in these mixtures, Li:Ga:La:Zr:Ta, was 0.001 g, which was the target Li6Ga 0.25 La3Zr 1.75 Ta 0.25 O 12 The amount of lithium was 1.4 times the target composition, and the amount of gallium was 1.6 times the target composition. In other words, the chemical composition of the metals contained in the mixture was Li 8.4 Ga 0.4 La3Zr 1.75 Ta 0.25 O 12 It was decided.

[0058] Next, 100 g of this mixture was filled into an alumina crucible with a lid (Nikkato, C3 type). Then, this was placed in a box-type electric furnace (Yamato Scientific, FP100 type) and pre-fired at 850 °C for 6 hours to obtain a powder (first powder). Next, the obtained first powder was pulverized. More specifically, 100 g of the first powder, 300 g of zirconia balls with a diameter of 5 mm, and 50 g of isopropanol were filled into a zirconia pulverization container with a capacity of 250 mL, and pulverized by rotating at a revolution speed of 200 rpm for a total of 300 minutes using a planetary ball mill (Fritsch, Germany, model P-6). The powder after pulverization (second powder) was dried at 100 °C for 24 hours and classified using a sieve with 250 μm openings. Hereinafter, the powder that passed through the sieve with 250 μm openings is referred to as the third powder.

[0059] (Preparation of rod-shaped compacts) Using the third powder (raw material) that passed through the sieve in the above process, a rod-shaped molded body (first substrate) was produced in the following procedure. First, about 34 g of the third powder was filled into a cylindrical rubber mold and degassed. Next, this mold was sealed and placed in water, and the water pressure was kept at 40 MPa for 5 minutes. Then, after the water pressure was reduced, the molded body (first molded body) was removed from the mold. The first molded body was cylindrical, with a bottom diameter of about 1.0 cm and a height of about 12.0 cm. Next, the first cylindrical molded body was fired at 1150°C for 4 hours using a box-type electric furnace (manufactured by Denken, model number KDF009). The fired molded body, which was the second molded body (first substrate), was rod-shaped with a bottom diameter of about 0.9 cm and a height of about 11 cm.

[0060] (Li6Ga 0.25 La3Zr 1.75 Ta 0.25 O 12 (Crystal Growth) First, the rod-shaped second compact obtained in the above process was placed inside a four-ellipse infrared condensing heating furnace (FZ furnace) (Crystal System, FZ-T-10000H type) equipped with a 1kW halogen lamp, and the internal space was made into a dry air atmosphere. Next, the rod-shaped second compact was heated at 24.4% of the output around the extension direction of the second compact while rotating at a rotation speed of 40 rpm on a plane perpendicular to the longitudinal direction, i.e., with the direction in which the second compact extends as the axis. After a while, a part of the second compact (first substrate), which is a polycrystalline sample, melted to form a molten part. Then, while maintaining the heating of the first substrate, the installation table of the rod-shaped second compact was lowered along the longitudinal direction at a moving speed of 10 mm / h to obtain high-density Li6Ga 0.25 La3Zr 1.75 Ta 0.25 O 12 A crystal of the above (hereinafter sometimes referred to as "sample 1") was grown.

[0061] The chemical composition of the grown sample 1 was analyzed by ICP-AES and single crystal X-ray crystal structure analysis. The analysis results showed that the chemical composition by ICP-AES was Li:Ga:La:Zr:Ta=6.0:0.25:3.0:1.75:0.25. Figure 1 is a photograph of the appearance of sample 1 grown along the longitudinal direction of first substrate B. As shown in Figure 1, the length of sample 1 is approximately 7 cm.

[0062] (High density Li6Ga 0.25 La3Zr 1.75 Ta 0.25 O 12 Evaluation of crystals A single crystal X-ray diffractometer equipped with a two-dimensional IP detector (Rigaku Corporation, R-AXIS RAPID-II) was used to investigate the structure of sample 1. Figure 2 shows an image showing the X-ray diffraction pattern obtained for sample 1, and the diffraction point D, which is specific to the single crystal structure, can be clearly confirmed from this image.

[0063] Diffraction intensity data for sample 1 was collected, and the crystal structure was examined using the crystal structure analysis program Jana2006. It was found that sample 1 is a cubic crystal and belongs to the space group I-43d. Four slices with a thickness of 0.1 cm were cut out from sample 1 using a diamond cutter, and their relative densities were calculated using the method described above. As a result, the relative densities were 99.8%, 99.9%, 100%, and 100%, respectively.

[0064] Figure 3 shows a schematic diagram of the structure of sample 1. As is generally known, the method for producing a solid electrolyte is to sinter polycrystalline lithium composite oxide raw material, which is a cubic garnet-type Li 7-3x-y Ga x La3Zr 2-y Nb y O 12belongs to the space group Ia-3d (for example, Non-Patent Document 5). In contrast, the sample 1 grown by the melting method according to the above embodiment belongs to the space group I-43d, and the 24c site (coordinates x=0.25, y=0.125, Z=0) in the crystal structure is occupied by lanthanum, the 16a site (x=0, y=0, z=0) is occupied by zirconium and tantalum, the 12a site (coordinates x=0.75, y=0.625, z=0), the 12b site (coordinates x=0.75, y=0.125, z=0), and two types of 48e sites (coordinates x=0.6803, y=0.5651, z=0.1452, coordinates x=0.6905, y=0.5895, z=0.0818) are lithium sites, and the 12a site and the 12b site are gallium sites. Thus, it is clear that Sample 1 obtained by the melting method has a space group that is clearly different from that produced by the sintering method disclosed in Non-Patent Document 5, and is a new substance with a different crystal structure. Since the R factor, which indicates the reliability of the crystal structure analysis here, was 2.33%, it can be determined that the results of this crystal structure analysis are valid.

[0065] In sample 1, which has a gallium-substituted cubic garnet structure, the lithium ions are arranged at the closest distance to each other, and there is a moderate lack of lithium ion sites. Therefore, it is considered that the lithium ion conductivity of sample 1 is higher than that of other cubic garnet structure compounds. Sample 1 was cut to prepare a cylindrical flake (bottom diameter approximately 0.50 cm, thickness approximately 0.20 cm). Gold was sputtered on the two bottom surfaces (front and back) of this flake to form cylindrical electrodes (bottom diameter 0.40 cm, thickness 40 nm).

[0066] The impedance of Sample 1 was measured for each AC frequency by an AC impedance method (measuring device: Solarton, 1260) in a nitrogen atmosphere at 25°C. Figure 4 is a graph of a Nyquist plot obtained from the measurement results. The horizontal axis of the graph indicates the real part of the impedance Z' (Ωcm), and the vertical axis of the graph indicates the imaginary part of the impedance Z'' (Ωcm). From this graph, it was found that the lithium ion conductivity was 4.62×10 -3 It is calculated as S / cm.

[0067] The lattice constant a of sample 1 was calculated by the least squares method using the reflections observed in the single crystal X-ray diffraction measurement, and was found to be a = 1.29646 nm ± 0.00003 nm. From this lattice constant, it was found that sample 1 is a lithium composite oxide having a garnet-type structure. Figure 5 shows the powder X-ray diffraction pattern obtained by crushing sample 1 and performing powder X-ray diffraction measurement. The powder X-ray diffraction pattern of sample 1 was similar to the diffraction pattern of a single phase of a cubic garnet-type structure. The lattice constant a calculated from the result of powder X-ray structure analysis was a = 1.29691 nm ± 0.00001 nm. Combining the results of single crystal X-ray diffraction measurement and powder X-ray structure analysis, it is found that the lattice constant of sample 1 is 1.29646 nm ≦ a ≦ 1.29691 nm.

[0068] <Example 2> (Creating all-solid-state lithium-ion secondary batteries) An all-solid-state lithium ion secondary battery including Sample 1 obtained in Example 1 as a solid electrolyte material was manufactured by the following procedure.

[0069] First, 0.0105 mol of lithium acetate dihydrate (Sigma-Aldrich) and 0.01 mol of cobalt acetate tetrahydrate (Wako Pure Chemical Industries) were dissolved in 100 g of ethylene glycol (Wako Pure Chemical Industries). 10 g of polyvinylpyrrolidone K-30 (Wako Pure Chemical Industries) was further added and dissolved to prepare a 0.1 mol / kg lithium cobaltate precursor solution. The amount of lithium acetate was 5% more than the amount of cobalt acetate in molar ratio because the amount of lithium evaporated during firing was taken into consideration.

[0070] Next, sample 1 was cut to prepare a cylindrical flake with a bottom diameter of about 0.6 cm and a thickness of about 0.10 cm, and 10 μl of the above solution was dropped onto the flake and pre-baked for 20 minutes at 400° C. Then, it was baked for 10 minutes at 850° C. Lithium cobalt oxide was synthesized as a positive electrode on the front surface of sample 1, and metallic lithium was attached as a negative electrode to the back surface of sample 1 to obtain an all-solid-state lithium-ion secondary battery (hereinafter sometimes referred to as “sample 2”).

[0071] FIG. 6 is a diagram showing a schematic configuration of an evaluation device 10 for the sample 2. For the sake of explanation, each component of the evaluation device 10 is shown disassembled. The evaluation device 10 is mainly composed of a battery evaluation cell 11 and a support means 12 for the sample 2 placed therein. The battery evaluation cell 11 is composed of an evaluation cell body 11A that houses and supports the support means 12, and an evaluation cell lid 11B that covers the side opposite to the evaluation cell body 11A. The evaluation cell body 11A and the evaluation cell lid 11B are connected via a silicone rubber O-ring 13 and a fluororesin O-ring 14, and are configured to fix the sample 1. The support means 12 is composed of a base 12A on which the sample 1 is placed with a metal lithium plate (negative electrode) 15 sandwiched therebetween, a spring 12B that adjusts the height of the base 12A, and a spring guide 12C that fixes the spring 12B.

[0072] In this evaluation device 10, sample 1 was used as a solid electrolyte material, and a positive electrode and a negative electrode were synthesized thereon to form sample 2, which was subjected to voltage measurement. Specifically, sample 2 and a disk-shaped metallic lithium plate (diameter 4 mm, thickness 1 mm) 15 were placed in a commercially available HS cell for battery evaluation (manufactured by Hohsen Co., Ltd.) 11 in a glove box, and the voltage was measured, showing an open circuit voltage of 2.9 V. This confirmed that sample 2 functioned as a battery.

[0073] <Example 3> Example 3 differs from Example 1 in that a sample containing niobium but not tantalum was formed, and in the mixing ratio of the raw materials. (Li6Ga 0.25 La3Zr 1.75 Nb 0.25 O 12 Mixing of raw materials) First, 28.5922g of lithium carbonate Li2CO3 (made by Rare Metallic, purity 99.99%), 3.4539g of gallium oxide Ga2O3 (made by Rare Metallic, purity 99.99%), 45.0257g of lanthanum oxide La2O3 (made by Rare Metallic, purity 99.99%), 19.8671g of zirconium oxide ZrO2 (made by Rare Metallic, purity 99.99%), and 3.0612g of niobium oxide Nb2O5 (made by Rare Metallic, purity 99.99%) were placed in an agate mortar and mixed uniformly by a wet method using ethanol. The lanthanum oxide was pre-calcined at 900°C. The molar ratio of metals contained in these mixtures, Li:Ga:La:Zr:Ta, was 0.0001g, which was the target Li6Ga 0.25 La3Zr 1.75 Nb 0.25 O 12 The amount of lithium was 1.4 times the target composition, and the amount of gallium was 1.6 times the target composition. In other words, the chemical composition of the metals contained in the mixture was Li 8.4 Ga 0.4 La3Zr 1.75 Nb 0.25 O 12 It was decided.

[0074] Next, a high density Li6Ga was grown using the mixture in the same manner as in Example 1, in which sample 1 was grown using the mixture. 0.25 La3Zr 1.75 Nb 0.25 O 12 Sample 3, which is a crystal of The chemical composition of the grown sample 3 was analyzed in the same manner as in Example 1. As a result of the analysis, the chemical composition by ICP-AES was Li:Ga:La:Zr:Nb=6.0:0.25:3.0:1.75:0.25. Figure 7 is a photograph of the appearance of sample 3. As shown in Figure 7, the length of sample 3 is about 7 cm.

[0075] (High density Li6Ga 0.25 La3Zr 1.75 Nb 0.25 O 12 Evaluation of crystals The structure of sample 3 was examined in the same manner as in Example 1. Figure 8 is an image showing the X-ray diffraction pattern obtained for sample 3, and from this image, diffraction point D, which is specific to a single crystal structure, can be clearly confirmed.

[0076] Diffraction intensity data of sample 3 was collected, and the crystal structure was examined in the same manner as in Example 1. It was found that sample 3 is a cubic crystal and belongs to space group I-43d. Four slices with a thickness of 0.1 cm were cut out from sample 3 using a diamond cutter, and the relative densities of these slices were calculated by the method described above. As a result, the relative densities of these slices were 99.7%, 99.8%, 100%, and 100%, respectively.

[0077] Figure 9 shows a schematic diagram of the structure of sample 3. As is generally known, the method for producing a solid electrolyte is to sinter polycrystals of a lithium composite oxide raw material, which is a cubic garnet-type Li 7-3x-y Ga x La3Zr 2-y Nb y O 12 is a related compound, Li 7-3x-y Ga x La3Zr 2-y Ta y O 12Similarly, it is considered that the space group belongs to Ia-3d (for example, Non-Patent Document 5). In contrast, the sample 3 grown by the melting method according to the above embodiment belongs to the space group I-43d, and the 24c site (coordinates x = 0.25, y = 0.125, Z = 0) in the crystal structure is occupied by lanthanum, the 16a site (x = 0, y = 0, z = 0) is occupied by zirconium and niobium, the 12a site (coordinates x = 0.75, y = 0.625, z = 0), the 12b site (coordinates x = 0.75, y = 0.125, z = 0), and two types of 48e sites (coordinates x = 0.6801, y = 0.5648, z = 0.1454, coordinates x = 0.6902, y = 0.5890, z = 0.0822) are lithium sites, and the 12a site and the 12b site are gallium sites. Thus, it is clear that Sample 3 obtained when produced by the melting method has a space group that is clearly different from that produced by the sintering method as disclosed in Non-Patent Document 5, and is a new substance with a different crystal structure. Since the R factor, which indicates the reliability of the crystal structure analysis here, was 2.13%, it can be determined that the results of this crystal structure analysis are valid.

[0078] <Example 4> Example 4 differs from Example 1 in that a sample containing niobium was formed and in the mixing ratio of the raw materials. (Li6Ga 0.25 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 Mixing of raw materials) First, 28.3052g of lithium carbonate Li2CO3 (made by Rare Metallic, purity 99.99%), 3.4192g of gallium oxide Ga2O3 (made by Rare Metallic, purity 99.99%), 44.5737g of lanthanum oxide La2O3 (made by Rare Metallic, purity 99.99%), 19.6677g of zirconium oxide ZrO2 (made by Rare Metallic, purity 99.99%), 2.5190g of tantalum oxide Ta2O5 (made by Rare Metallic, purity 99.99%), and 1.5152g of niobium oxide Nb2O5 (made by Rare Metallic, purity 99.99%) were placed in an agate mortar and mixed uniformly by a wet method using ethanol. The lanthanum oxide was pre-calcined at 900°C. The molar ratio of metals contained in these mixtures Li:Ga:La:Zr:Ta was 0.01 to 0.01, which is the molar ratio of the target Li6Ga 0.25 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 The amount of lithium was 1.4 times the target composition, and the amount of gallium was 1.6 times the target composition. In other words, the chemical composition of the metals contained in the mixture was Li 8.4 Ga 0.4 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 It was decided.

[0079] Next, a high density Li6Ga was grown using the mixture in the same manner as in Example 1, in which sample 1 was grown using the mixture. 0.25 La3Zr 1.75 Ta 0.25 O 12 Sample 4, which is a crystal of

[0080] The chemical composition of the grown sample 4 was analyzed in the same manner as in Example 1. As a result of the analysis, the chemical composition by ICP-AES was Li:Ga:La:Zr:Ta:Nb=6.0:0.25:3.0:1.75:0.125:0.125. Figure 10 is a photograph of the appearance of sample 4. As shown in Figure 10, the length of sample 10 is about 5 cm.

[0081] (High density Li6Ga 0.25 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 Evaluation of crystals The structure of Sample 4 was examined in the same manner as in Example 1. Figure 11 is an image showing the X-ray diffraction pattern obtained for Sample 4, and from this image, diffraction point D specific to a single crystal structure can be clearly confirmed.

[0082] Diffraction intensity data of sample 4 was collected, and the crystal structure was examined in the same manner as in Example 1. It was found that sample 4 is a cubic crystal and belongs to space group I-43d. Four slices with a thickness of 0.1 cm were cut out from sample 4 using a diamond cutter, and the relative densities of these slices were calculated by the method described above. As a result, the relative densities of these slices were 99.8%, 100%, 100%, and 100%, respectively.

[0083] FIG. 12 shows a schematic diagram of the structure of sample 4. As is generally known, the method for producing a solid electrolyte is to sinter polycrystals of a lithium composite oxide raw material, which is a cubic garnet-type Li 7-3x―w-v Ga x La3Zr 2-w―v Ta W Nb v O 12 is a related compound, Li 7-3x-y Ga x La3Zr 2-y Ta y O 12Similarly, it is considered that the space group belongs to Ia-3d (for example, Non-Patent Document 5). In contrast, the sample 3 grown by the melting method according to the above embodiment belongs to the space group I-43d, and the 24c site (coordinates x = 0.25, y = 0.125, Z = 0) in the crystal structure is occupied by lanthanum, the 16a site (x = 0, y = 0, z = 0) is occupied by zirconium and niobium, the 12a site (coordinates x = 0.75, y = 0.625, z = 0), the 12b site (coordinates x = 0.75, y = 0.125, z = 0), and two types of 48e sites (coordinates x = 0.6805, y = 0.5652, z = 0.1448, coordinates x = 0.6900, y = 0.5885, z = 0.0818) are lithium sites, and the 12a site and the 12b site are gallium sites. Thus, it is clear that sample 4 obtained by the melting method has a space group that is clearly different from that produced by the sintering method disclosed in Non-Patent Document 5, and is a new substance with a different crystal structure. Since the R factor, which indicates the reliability of the crystal structure analysis here, was 1.88%, it can be determined that the results of this crystal structure analysis are valid.

[0084] <Example 5> Example 5 differs from Example 1 in that a sample containing niobium was formed, the mixing ratio of the raw materials was different, and the crystal was grown using the Cz method. (Li 6.125 Ga 0.125 La3Zr 1.5 Ta 0.25 Nb 0.25 O 12 Mixing of raw materials) First, 28.8647g of lithium carbonate Li2CO3 (made by Rare Metallic, purity 99.99%), 1.7078g of gallium oxide Ga2O3 (made by Rare Metallic, purity 99.99%), 44.5271g of lanthanum oxide La2O3 (made by Rare Metallic, purity 99.99%), 16.8408g of zirconium oxide ZrO2 (made by Rare Metallic, purity 99.99%), 5.0327g of tantalum oxide Ta2O5 (made by Rare Metallic, purity 99.99%), and 3.0273g of niobium oxide Nb2O5 (made by Rare Metallic, purity 99.99%) were placed in an agate mortar and mixed uniformly by a wet method using ethanol. The lanthanum oxide was pre-calcined at 900°C. The molar ratio of metals contained in these mixtures Li:Ga:La:Zr:Ta was determined based on the target Li 6.125 Ga 0.125 La3ZrTa 0.25 Nb 0.25 O 12 The amount of lithium was 1.4 times the target composition, and the amount of gallium was 1.6 times the target composition. In other words, the chemical composition of the metals contained in the mixture was Li 8.575 Ga 0.2 La3Zr 1.5 Ta 0.25 Nb 0.25 O 12 It was decided.

[0085] Next, a rod-shaped compact was produced from the mixture in the same manner as in Example 1 for producing the rod-shaped compact.

[0086] (Li 6.125 Ga 0.125 La3Zr 1.5 Ta 0.25 Nb 0.25 O 12 (Crystal Growth) After preparing a rod-shaped compact by sintering, the sintered rod-shaped compact was first cut to an appropriate size and loaded into an iridium crucible with an outer diameter of 30 mm, an inner diameter of 28 mm, and a depth of 30 mm. The iridium crucible was then placed in the center of the high-frequency induction heating coil of a single crystal pulling furnace (Cz furnace) (manufactured by Technosearch, TCH-3 type) equipped with a high-frequency induction heating coil. Next, the sintered compact in the iridium crucible was heated until it melted. Then, an iridium rod as a second substrate, which had been placed in the upper part of the Cz furnace in advance, was immersed in the melt, and the melt was attached to the iridium rod. After that, the rod was rotated at a rotation speed of 5 rpm in a plane perpendicular to the longitudinal direction, i.e., with the longitudinal direction of the iridium rod as the axis, and the iridium rod with the melt attached was raised outside the crucible at a moving speed of 8 mm / h in a direction away from the melt in the crucible, and high-density Li 6.125 Ga 0.125 La3Zr 1.5 Ta 0.25 Nb 0.25 O 12 A crystal of (hereinafter sometimes referred to as "sample 5") was grown.

[0087] The chemical composition of the grown sample 5 was analyzed in the same manner as in Example 1. As a result of the analysis, the chemical composition by ICP-AES was Li:Ga:La:Zr:Ta:Nb=6.1:0.125:3.0:1.5:0.25:0.25. Figure 13 is a photograph of the appearance of sample 5. As shown in Figure 13, the diameter of sample 5 is about 20 mm, and the length is about 20 mm.

[0088] (High density Li 6.125 Ga 0.125 La3Zr 1.5 Ta 0.25 Nb 0.25 O 12 Evaluation of crystals The structure of Sample 5 was examined in the same manner as in Example 1. Figure 14 is an image showing the X-ray diffraction pattern obtained for Sample 5, and from this image, diffraction point D specific to a single crystal structure can be clearly confirmed.

[0089] Diffraction intensity data of sample 5 was collected, and the crystal structure was examined in the same manner as in Example 1. It was found that sample 5 is a cubic crystal and belongs to space group I-43d. Four slices with a thickness of 0.1 cm were cut out from sample 3 using a diamond cutter, and their relative densities were calculated by the method described above. As a result, the relative densities were 99.9%, 100%, 100%, and 100%, respectively.

[0090] FIG. 15 shows a schematic diagram of the structure of sample 5. As is generally known as a method for producing a solid electrolyte, the sample 5 is a cubic garnet-type Li 7-3x―w-v Ga x La3Zr 2-w―v Ta W Nb v O 12 is a related compound, Li 7-3x-y Ga x La3Zr 2-y Ta y O 12 Similarly, it is considered that the space group belongs to Ia-3d (for example, Non-Patent Document 5). In contrast, the sample 5 grown by the melting method according to the above embodiment belongs to the space group I-43d, and the 24c site (coordinates x = 0.25, y = 0.125, Z = 0) in the crystal structure is occupied by lanthanum, the 16a site (x = 0, y = 0, z = 0) is occupied by zirconium and niobium, the 12a site (coordinates x = 0.75, y = 0.625, z = 0), the 12b site (coordinates x = 0.75, y = 0.125, z = 0), and two types of 48e sites (coordinates x = 0.6798, y = 0.5651, z = 0.1439, coordinates x = 0.6913, y = 0.5892, z = 0.0816) are lithium sites, and the 12a site and the 12b site are gallium sites. Thus, it is clear that Sample 5 produced by the melting method has a space group that is clearly different from that produced by the sintering method disclosed in Non-Patent Document 5, and is a new substance with a different crystal structure. Since the R factor, which indicates the reliability of the crystal structure analysis here, was 1.62%, it can be determined that the results of this crystal structure analysis are valid.

[0091] <Example 6> Example 6 is different from Example 1 in the mixing ratio of the raw materials. (Li 5.55 Ga 0.4 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 Mixing of raw materials) First, 26.2010g of lithium carbonate Li2CO3 (made by Rare Metallic, purity 99.99%), 5.4746g of gallium oxide Ga2O3 (made by Rare Metallic, purity 99.99%), 44.6055g of lanthanum oxide La2O3 (made by Rare Metallic, purity 99.99%), 19.6817g of zirconium oxide ZrO2 (made by Rare Metallic, purity 99.99%), 2.5208g of tantalum oxide Ta2O5 (made by Rare Metallic, purity 99.99%), and 1.5163g of niobium oxide Nb2O5 (made by Rare Metallic, purity 99.99%) were placed in an agate mortar and mixed uniformly by a wet method using ethanol. The lanthanum oxide was pre-calcined at 900°C. The molar ratio of metals contained in these mixtures Li:Ga:La:Zr:Ta was determined based on the target Li 5.55 Ga 0.4 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 The amount of lithium was 1.4 times the target composition, and the amount of gallium was 1.6 times the target composition. In other words, the chemical composition of the metals contained in the mixture was Li 7.77 Ga 0.64 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 It was decided.

[0092] Next, 100 g of this mixture was filled into an alumina crucible with a lid (Nikkato, C3 type). Then, this was placed in a box-type electric furnace (Yamato Scientific, FP100 type) and pre-fired at 850 °C for 6 hours to obtain a powder. The obtained powder was then pulverized. More specifically, 100 g of the powder, 300 g of zirconia balls with a diameter of 5 mm, and 50 g of isopropanol were filled into a zirconia pulverization vessel with a capacity of 250 mL, and pulverized by rotating at a revolution speed of 200 rpm for a total of 300 minutes using a planetary ball mill (Fritsch, Germany, model P-6). The pulverized powder was dried at 100 °C for 24 hours and classified using a sieve with 250 μm openings.

[0093] Next, high density Li was grown using the mixture in the same manner as in Example 1, in which sample 1 was grown using the mixture. 5.55 Ga 0.4 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 Sample 6, which is a crystal of

[0094] The chemical composition of the grown sample 6 was analyzed in the same manner as in Example 1. As a result of the analysis, the chemical composition by ICP-AES was Li:Ga:La:Zr:Ta:Nb=5.57:0.388:3.0:1.75:0.125:0.125. Figure 16 is a photograph of the appearance of sample 6. As shown in Figure 16, the diameter of sample 6 is about 9 mm, and the length is about 45 mm.

[0095] (High density Li 5.55 Ga 0.4 La3Zr 1.75 Ta 0.125 Nb 0.125 O 12 Evaluation of crystals The structure of Sample 6 was examined in the same manner as in Example 1. Figure 17 is an image showing the X-ray diffraction pattern obtained for Sample 6, and from this image, diffraction point D specific to a single crystal structure can be clearly confirmed.

[0096] Diffraction intensity data of sample 6 was collected, and the crystal structure was examined in the same manner as in Example 1. It was found that sample 6 is a cubic crystal and belongs to space group I-43d. Four slices with a thickness of 0.1 cm were cut out from sample 6 using a diamond cutter, and their relative densities were calculated by the method described above. As a result, the relative densities were 99.6%, 99.8%, 99.9%, and 100%, respectively.

[0097] FIG. 18 shows a schematic diagram of the structure of sample 6. As is generally known as a method for manufacturing a solid electrolyte, the sample 6 is a cubic garnet-type Li 7-3x―w-v Ga x La3Zr 2-w―v Ta W Nb v O 12 is a related compound, Li 7-3x-y Ga x La3Zr 2-y Ta y O 12 Similarly, it is considered that the space group belongs to Ia-3d (for example, Non-Patent Document 5). In contrast, the sample 3 grown by the melting method according to the above embodiment belongs to the space group I-43d, and the 24c site (coordinates x = 0.25, y = 0.125, Z = 0) in the crystal structure is occupied by lanthanum, the 16a site (x = 0, y = 0, z = 0) is occupied by zirconium and niobium, the 12a site (coordinates x = 0.75, y = 0.625, z = 0), the 12b site (coordinates x = 0.75, y = 0.125, z = 0), and two types of 48e sites (coordinates x = 0.6784, y = 0.5656, z = 0.1442, coordinates x = 0.6937, y = 0.5903, z = 0.0822) are lithium sites, and the 12a site and the 12b site are gallium sites. Thus, it is clear that sample 4 obtained by the melting method has a space group that is clearly different from that of sample 4 produced by the sintering method disclosed in Non-Patent Document 5, and is a new substance with a different crystal structure. Since the R factor, which indicates the reliability of the crystal structure analysis, was 2.92%, the results of this crystal structure analysis can be judged to be valid.

[0098] <Example 7> A lithium composite oxide single crystal prepared in the same manner as in Example 1 above was pulverized and fired in the following manner to prepare a lithium composite oxide polycrystal.

[0099] First, the lithium composite oxide single crystal was roughly crushed in an agate mortar, and then ground to a powder form to form a polycrystalline powder of the lithium composite oxide. Next, about 0.4 g of the powder was filled into a tablet molder with a diameter of about 10 mm, and then a compact was obtained by applying a pressure of about 60 MPa with a hydraulic press. Next, the compact was placed in a platinum crucible and fired at 1150°C for 4 hours using a box-type electric furnace (manufactured by Denken, model number KDF009). Figure 19 is a photograph of the appearance of the lithium composite oxide polycrystalline obtained by the firing. The lithium composite oxide polycrystalline produced in Example 7 had a diameter of about 10 mm and a thickness of about 1.5 mm. The single crystal before crushing (the same lithium composite oxide single crystal as in Example 1) used to prepare the lithium composite oxide polycrystal of Example 7 has a garnet-type structure belonging to the space group I-43d, and the polycrystal after crushing has a powder X-ray diffraction pattern showing a garnet-type structure as shown in FIG. 5. Therefore, the polycrystalline sintered body prepared in this example also has a similar crystal structure. In this way, a polycrystal sintered body can be produced by crushing a single crystal to produce a polycrystal, molding the polycrystal in a tablet molding machine, and then sintering the molded product. [Industrial Applicability]

[0100] The present invention's high-density Li 7-3x―w-v Ga x La3Zr 2-w―v Ta W Nb v O 12 (0.02≦x<0.5, 0≦W≦1.0, 0≦V≦1.0, 0.05≦W+V≦1.0) The crystal can be used as a solid electrolyte material for all-solid-state lithium-ion secondary batteries. [Explanation of symbols]

[0101] 10. Evaluation device 11 Battery evaluation cell 11A···Evaluation cell body 11B: Evaluation cell cover 12...Support means 12A···Base 12B Spring 12C···Spring guide 13 Silicone rubber O-ring 14...Fluororesin O-ring 15 Metallic lithium plate 1, 2: Sample 2. Sample B...Base material D... diffraction point

Claims

1. Chemical composition is Li 7-3x―w-v G x La 3 Zr 2-w―v T W Nb v O 12 (0.02≦x<0.5, 0≦W≦0.5, 0≦V≦0.5, 0.25≦W+V≦0.5), A lithium composite oxide single crystal having a cubic crystal system, belonging to the space group I-43d, and having a garnet-type structure.

2. Chemical composition is Li 7-3x―w-v G x La 3 Zr 2-w―v T W Nb v O 12 (0.02≦x<0.5, 0≦W≦0.5, 0≦V≦0.5, 0.25≦W+V≦0.5), A lithium composite oxide polycrystal which is a single crystal having a cubic crystal system, belongs to the space group I-43d, and has a garnet-type structure.

3. The lithium composite oxide polycrystal according to claim 2 , which has a relative density of 90% or more.

4. 4. The lithium composite oxide polycrystal according to claim 2, which has a relative density of 95% or more.

5. A lithium composite oxide material comprising the lithium composite oxide single crystal according to claim 1 or the lithium composite oxide polycrystal according to any one of claims 2 to 4.

6. A solid electrolyte material comprising the lithium composite oxide single crystal according to claim 1 or the lithium composite oxide polycrystal according to any one of claims 2 to 4.

7. Lithium ion conductivity is 1.0 x 10 -3 The solid electrolyte material according to claim 6, wherein the electrical conductivity is 1.0 S / cm or more.

8. An all-solid-state lithium ion secondary battery comprising a positive electrode, a negative electrode, and the solid electrolyte material according to claim 6 or 7.

9. A method for producing a solid electrolyte material, comprising the steps of: producing the solid electrolyte material according to claim 6 or 7; The chemical composition is Li(7-3x-W-V)yGa xz La 3 Zr 2-W T W Nb v O 12 A molten part forming process of melting at least a part of a rod-shaped base material containing a raw material represented by (0.02≦x<0.5, 1.1≦y≦1.4, 1.6≦z≦3.3, 0≦W≦0.5, 0≦V≦0.5, 0.25≦W+V≦0.5) to form a molten part; and a molten portion moving step of moving the molten portion at an average speed of 8 mm / h or more.

10. The method for producing a solid electrolyte material according to claim 9, wherein the average speed is 8 mm / h or more and 19 mm / h or less.

11. 11. The method for producing a solid electrolyte material according to claim 9, wherein in the molten portion forming step, the base material is rotated together with the molten portion in a plane perpendicular to a longitudinal direction at a rotational speed of 30 rpm or more.

12. The method for producing a solid electrolyte material according to any one of claims 9 to 11, characterized in that the molten part moving step is performed in a state in which a seed crystal of the solid electrolyte material is attached to the molten part.

13. The method for producing a solid electrolyte material according to any one of claims 9 to 12, characterized in that, in the molten portion moving step, the molten portion is rotated at a rotation speed of 2 rpm or more and 8 rpm or less on a plane perpendicular to a longitudinal direction of the base material.

14. A method for producing a solid electrolyte material according to claim 6 or 7, comprising the steps of: The chemical composition is Li(7-3x-W-V)yGa xz La 3 Zr 2-W T W Nb v O 12 a melt forming step of melting a raw material represented by (0.02≦x<0.5, 1.1≦y≦1.4, 1.6≦z≦3.3, 0≦W≦0.5, 0≦V≦0.5, 0.25≦W+V≦0.5, 1.1≦y≦1.5, 1.5≦z≦3.5) in a crucible to form a melt of the raw material; a melt applying step of immersing a substrate in the melt in the crucible and applying the melt to the substrate; and a melt transferring step of transferring the melt attached to the substrate together with the substrate to outside the crucible at an average speed of 8 mm / h or more.

15. The method for producing a solid electrolyte material according to claim 14, wherein the average speed is 8 mm / h or more and 19 mm / h or less.

16. 16. The method for producing a solid electrolyte material according to claim 14, wherein the melt transferring step is performed in a state where a seed crystal of the solid electrolyte material is attached to the substrate.

17. The method for producing a solid electrolyte material according to any one of claims 14 to 16, characterized in that in the melt moving step, the rod-shaped base material is rotated at a rotation speed of 2 rpm or more and 8 rpm or less relative to the melt on a plane perpendicular to a longitudinal direction.

Citation Information

Patent Citations

  • Lithium ion conductive oxide, method for producing the same, and electrochemical device using the same as member

    JP2011195373A

  • Gallium substitution type solid electrolyte material and all-solid lithium ion secondary battery

    JP2021046340A

  • Lithium-containing garnet crystal body, method for producing same, and all-solid-state lithium ion secondary battery

    WO2016017769A1

  • Lithium-containing garnet crystal and all-solid-state lithium ion secondary battery

    WO2016068040A1

  • Solid electrolyte material and all solid lithium ion secondary battery

    WO2017130622A1