Laminated polyester film, laminated film with cured resin layer, and metal laminated film

The laminated polyester film with PBN layers and a cured resin layer addresses transparency and dielectric challenges, providing low dielectric properties and reduced transmission loss for high-speed communication circuits and transparent antenna films.

JP7574733B2Active Publication Date: 2024-10-29MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021078738
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-06
Publication Date
2024-10-29
Estimated Expiration
2041-05-06

AI Technical Summary

Technical Problem

Existing laminated biaxially stretched polyester films with cavities for low dielectric properties face challenges in controlling cavity size and material dispersion, leading to inadequate transparency and dielectric performance, with issues like light refraction at cavity interfaces and high transmission loss.

Method used

A laminated polyester film with two or more layers, including a layer A composed of polybutylene naphthalate (PBN) for low dielectric properties, and optionally a cured resin layer for improved adhesion and transparency, ensuring a dielectric loss tangent of 0.0060 or less and a dielectric constant of 3.0 or less at 28 GHz.

Benefits of technology

The film achieves excellent low dielectric properties and transparency, suitable for high-speed communication circuits and transparent antenna films, with reduced transmission loss and improved heat resistance, mechanical strength, and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574733000006
    Figure 0007574733000006
  • Figure 0007574733000007
    Figure 0007574733000007
  • Figure 0007574733000001
    Figure 0007574733000001
Patent Text Reader

Abstract

To provide a laminated polyester film that supports high-speed communication and has low dielectric properties and superior transparency, and a laminated film with a cured resin layer and a laminated metal film.SOLUTION: A laminated polyester film has two or more polyester layers. The film has, as at least one surface layer, at least one layer A of the polyester layers. The layer A contains polybutylene naphthalate, with the dielectric loss tangent at 28 GHz being 0.0060 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated polyester film, a laminated film with a cured resin layer, and a metal laminated film. [Background technology]

[0002] In recent years, the increasing performance and functionality of electrical and electronic devices has created a need for high-speed information communication. For example, with the launch of 5G (fifth generation mobile communication system) high-speed smartphone communication services, high-speed communication services are becoming widespread not only in the consumer sector but also in the industrial sector (factories, automobiles and other vehicles, etc.). 5G's high-speed, large-volume data communications will use radio waves in the "millimeter wave" band (wavelength 1-10 mm, frequency 30-300 GHz). Advantages of millimeter waves include the large amount of data that can be transmitted at one time and the high-resolution images that can be obtained.

[0003] On the other hand, when a high-frequency digital signal such as the above-mentioned millimeter wave is transmitted to a circuit board, a dielectric loss occurs in which a part of the transmitted digital signal is consumed as heat on the wiring of the circuit board, and the attenuated digital signal arrives at the receiving side, resulting in a so-called "transmission loss." Therefore, measures to reduce the transmission loss are also required for the materials used. The transmission loss is the sum of the dielectric loss and the conductor loss, and the dielectric loss α d is calculated from the following formula (1).

[0004]

number

[0005] Here, f is frequency, c is the speed of light, and ε r is the relative dielectric constant, and tan δ is the dielectric tangent.

[0006] For example, in flexible printed circuits (FPCs), which are flexible circuit boards made of resin film and copper foil, the resin film has a dielectric loss αd More specifically, the reduction of ε r Attempts have been made to reduce the viscosity and tan δ, particularly to reduce tan δ. Specifically, compared to polyimide (PI) used as a material for FPCs, examples of such fluororesins include liquid crystal polymer (LCP), which has a dielectric loss of approximately 1 / 10; cycloolefin polymer (COP), which has a dielectric loss of approximately 1 / 50; and polytetrafluoroethylene (PTFE), which has a dielectric loss of approximately 1 / 100 (Non-Patent Document 1).

[0007] However, LCP and COP have problems of low heat resistance, and fluororesin has problems of low adhesion strength with other materials such as copper foil and difficulty in drilling holes with UV laser due to UV absorption. Furthermore, fluororesin is expensive. Therefore, there is a demand for a resin film with low dielectric loss and versatility.

[0008] A polyester film is an example of a versatile resin film. Polyester films are excellent in heat resistance, weather resistance, mechanical strength, transparency, etc., and are also readily available at low cost, so they are used in various applications such as packaging materials and optical applications, but their low dielectric properties have not been studied much.

[0009] For example, Patent Document 1 discloses a laminated biaxially oriented polyester film containing 5 to 45% by volume of voids therein as a polyester film having excellent low dielectric properties. The inclusion of voids allows voids (air) to be dispersed, achieving a low dielectric constant and a low dielectric loss tangent.

[0010] Recently, a "transparent antenna film" in which invisible ultrafine metal mesh wiring is formed on a transparent film has been studied, and there is a demand for reducing the dielectric loss of the film, more specifically, for reducing the dielectric constant and dielectric dissipation factor of the film. Compared to conventional microwaves, the above-mentioned millimeter waves are more susceptible to the influence of nearby products, which limits the freedom in where antennas can be installed. In addition, because radio waves have a strong tendency to travel in a straight line, it is necessary to increase the number of antennas installed in order to ensure a better communication environment than before. The transparent antenna film being considered to address these issues does not impair design, and can be attached not only to mobile devices, but also to buildings such as window glass and car glass to receive 5G radio waves. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2006-352470 A [Non-patent literature]

[0012] [Non-Patent Document 1] "Development trends of high-frequency compatible materials and their application to 5G and millimeter wave radar", Technical Information Association, Chapter 3, Section 2, p.77-84 "Development trends of high-speed, high-frequency compatible FPCs and low transmission loss" Summary of the Invention [Problem to be solved by the invention]

[0013] The void-containing laminated biaxially stretched polyester film described in Patent Document 1 above is formed by mixing different materials to form the voids. In such a case, it is difficult to control the size of the voids or the dispersion state of the different materials. For example, if the dispersion state of the different materials is insufficient, the desired low dielectric properties may not be obtained. Furthermore, depending on the different materials used, the inherent transparency of polyester film may not be obtained, and in addition, the transparency may be reduced due to light refraction at the interface of the cavity.

[0014] The problem to be solved by the present invention is to solve the above problems and provide a laminated polyester film which is highly versatile and yet has excellent low dielectric properties and transparency. [Means for solving the problem]

[0015] The present inventors have conducted extensive research to achieve the above object, and as a result have completed the present invention. In one aspect, the present invention is summarized as follows [1] to

[23] . [1] A laminated polyester film having two or more polyester layers, comprising at least one layer A of the polyester layers on at least one surface layer, the layer A containing polybutylene naphthalate, and having a dielectric loss tangent at 28 GHz of 0.0060 or less. [2] The laminated polyester film according to the above [1], wherein the layer A has a relative dielectric constant of 3.0 or less at 28 GHz. [3] The laminated polyester film according to the above [1] or [2], wherein the dielectric tangent of the layer A at 28 GHz is 0.0050 or less. [4] The laminated polyester film according to any one of the above [1] to [3], which has a hysteresis loss rate of 60% or less in both a longitudinal direction (MD) and a transverse direction (TD) when subjected to a tensile cycle test up to 5% tensile strain. [5] The laminated polyester film according to any one of the above [1] to [4], wherein the Layer A further contains an amorphous polyester. [6] The laminated polyester film according to the above [5], wherein the amorphous polyester has a glass transition temperature higher than that of the polybutylene naphthalate. [7] The laminated polyester film according to [5] or [6] above, comprising the amorphous polyester in an amount of 1 part by mass or more and 100 parts by mass or less per 100 parts by mass of the polybutylene naphthalate. [8] The laminated polyester film according to any one of the above [5] to [7], wherein the amorphous polyester is a polyarylate. [9] The laminated polyester film according to any one of the above [1] to [8], wherein a layer other than the Layer A contains polyethylene terephthalate.

[10] The laminated polyester film according to any one of the above [1] to [9], which has a haze of 4.0% or less.

[11] The laminated polyester film according to any one of the above [1] to

[10] , which has a total thickness of 1 to 300 μm.

[12] The laminated polyester film according to any one of the above [1] to

[11] , wherein the thickness of the Layer A is 10 to 70% of the total thickness of the laminated polyester film.

[13] A laminate film with a cured resin layer, comprising the laminate polyester film according to any one of the above [1] to

[12] , and a cured resin layer on at least one surface layer, the cured resin layer being formed from a resin composition containing a crosslinking agent in an amount of 70 mass% or more relative to the non-volatile components.

[14] The laminated polyester film has the cured resin layers on both surface layers, and the amount of oligomer precipitation on the surface of at least one of the cured resin layers is 0.40 mg / m 2 The cured resin layer-attached laminate film according to the above item

[13] , which is as follows:

[15] A metal laminated film comprising a cured resin layer-attached laminated film according to

[13] or

[14] above, and a metal layer on the cured resin layer.

[16] The metal laminated film according to

[15] above, wherein the metal layer is patterned.

[17] The metal laminated film according to

[15] or

[16] above, wherein the metal layer is made of copper or silver.

[18] The laminated polyester film according to any one of the above [1] to

[12] , which is for use in a high-speed communication circuit.

[19] The laminated polyester film according to

[18] above, which is used for a transparent antenna film.

[20] A laminate film with a cured resin layer according to the above

[13] or

[14] , which is for use in high-speed communication circuits.

[21] The laminate film having a cured resin layer according to

[20] above, which is used for a transparent antenna film.

[22] The metal laminated film according to any one of the above

[15] to

[17] , which is for use in a high-speed communication circuit.

[23] The metal laminated film according to

[22] above, which is used for a transparent antenna film. Effect of the Invention

[0016] The laminated polyester film, the laminated film with a cured resin layer, and the metal laminated film of the present invention have excellent low dielectric properties that enable high-speed communication. Furthermore, the laminated polyester film, the laminated film with a cured resin layer, and the metal laminated film of the present invention are excellent in transparency and can be suitably used, particularly, as a transparent antenna film. [Brief description of the drawings]

[0017] [Figure 1] 1 is a profile of a stress-strain curve. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a microstrip line. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The inventors considered that when a high-frequency electrical signal is passed through a circuit board such as that used for high-speed communication circuits, the electric field strength is greatest directly below the conductor wiring of the circuit board. Therefore, by making layer A, which is placed directly below the conductor wiring, have low dielectric properties, in particular a low dielectric tangent, it is possible to efficiently reduce transmission loss. Furthermore, by effectively reducing transmission loss by lowering the dielectric properties of Layer A directly below the conductor wiring, it is believed possible to provide a highly versatile laminated polyester film without compromising the excellent heat resistance, weather resistance, mechanical strength, and cost performance that are characteristic of polyester films such as polyethylene terephthalate films. The present invention will be described in detail below. However, the content of the present invention is not limited to the embodiments described below.

[0019] <<Laminated polyester film>> A laminated polyester film according to one embodiment of the present invention (hereinafter also referred to as "the present laminated polyester film") is a laminated polyester film having two or more polyester layers, and is characterized in that it has at least one layer A of the polyester layers on at least one surface layer, the layer A containing polybutylene naphthalate, and has a dielectric tangent at 28 GHz of 0.0060 or less. In the present invention, the laminated polyester film means a laminated polyester film having two or more polyester layers, and the surface layer means a layer disposed on the most surface side of the laminated polyester film. A cured resin layer, a metal layer, etc., which will be described later, can be disposed on the surface layer, and the laminated polyester film having a cured resin layer, a metal layer, etc., disposed thereon is called a laminated film with a cured resin layer, and a metal laminated film, respectively, and is distinguished from a laminated polyester film.

[0020] In the present laminated polyester film, the number of laminated polyester layers is preferably 10 or less. If it is 10 or less, the thickness of each layer is sufficient, so that lamination during film formation is sufficient, flow marks and the like are unlikely to occur, and the quality of the film is sufficiently maintained. Among them, from the viewpoint of suppressing production costs, 2 to 3 layers is the most preferable.

[0021] The present laminated polyester film has two or more polyester layers, and at least one of the polyester layers has at least one layer A on the surface thereof. For example, when a polyester layer other than the layer A is designated as layer B, the present laminated polyester film may have layers other than the layers A and B. However, from the viewpoints of film formability and interlayer adhesion, it is preferable that the present laminated polyester film is composed of only the layers A and B.

[0022] Furthermore, for the purpose of efficiently reducing transmission loss, a two-layer structure of layer A / layer B is sufficient, but if versatility of the equipment is important, a three-layer structure of layer A / layer B / layer A or layer A / layer B / layer B is preferable.

[0023] The polyester layers constituting the present laminated polyester film will be described in detail below. As an example of the embodiment according to the present invention, a polyester layer on at least one surface layer is designated as Layer A, and a polyester layer other than Layer A is designated as Layer B, and the laminated polyester film will be described as being composed only of Layer A and Layer B. Layer A and Layer B may be made of the same polyester or different polyesters.

[0024] <Layer A> Layer A is a polyester layer for imparting low dielectric properties to the laminated polyester film, and contains polybutylene naphthalate (hereinafter also referred to as "PBN") having 2,6-naphthalenedicarboxylic acid units as the dicarboxylic acid component (a-1) and 1,4-butanediol units as the diol component (a-2).

[0025] From the viewpoint of imparting low dielectric properties, the dielectric loss tangent of layer A at 28 GHz is preferably 0.0050 or less. If the dielectric loss tangent of layer A is 0.0050 or less, the dielectric loss tangent of the entire laminated polyester film can be reduced, and a sufficient effect of reducing transmission loss can be obtained. From the above viewpoints, the dielectric loss tangent of layer A is more preferably 0.0045 or less, even more preferably 0.0040 or less, particularly preferably 0.0035 or less, and especially preferably 0.0030 or less. The lower limit is not particularly limited, but is 0.001 or more. From the same viewpoint, the relative dielectric constant of layer A at 28 GHz is preferably 3.0 or less, more preferably 2.9 or less, and even more preferably 2.8 or less. The lower limit is not particularly limited, but is 2.0 or more. The dielectric loss tangent and the relative dielectric constant of Layer A are values ​​measured by the method described in the Examples.

[0026] Although the mechanism by which layer A, which contains PBN, has excellent low dielectric properties is unclear, it is assumed that this is because dipole motion is suppressed by aromatic stacking. Generally, when a dielectric material is placed in an electric field, the dipoles are oriented. The dipoles then rotate and flip to follow the phase of the AC electric field. This rotation and flip motion of the dipoles creates friction, which causes dielectric loss. Therefore, it is presumed that suppressing the dipole motion leads to excellent low dielectric properties.

[0027] The PBN preferably contains 2,6-naphthalenedicarboxylic acid and 1,4-butanediol as its main components, i.e., it contains 50 mol % or more of 2,6-naphthalenedicarboxylic acid units as the dicarboxylic acid component (a-1) and 50 mol % or more of 1,4-butanediol units as the diol component (a-2). In particular, the PBN used in the present invention more preferably contains 90 mol % or more of 2,6-naphthalenedicarboxylic acid units as the dicarboxylic acid component (a-1) and 90 mol % or more of 1,4-butanediol units as the diol component (a-2).

[0028] The dicarboxylic acid component (a-1) constituting the PBN contains 2,6-naphthalenedicarboxylic acid units, and of the dicarboxylic acid component (a-1), the 2,6-naphthalenedicarboxylic acid units preferably account for 92 mol % or more, more preferably 94 mol % or more, particularly preferably 96 mol % or more, and particularly preferably 98 mol % or more. It is most preferable that all of the dicarboxylic acid component (a-1) (100 mol %) is 2,6-naphthalenedicarboxylic acid. By containing 90 mol % or more of 2,6-naphthalenedicarboxylic acid units as the dicarboxylic acid component (a-1), the low dielectric properties and heat resistance of Layer A are improved.

[0029] The PBN may be copolymerized with a dicarboxylic acid component other than 2,6-naphthalenedicarboxylic acid for the purpose of improving moldability and heat resistance. Specifically, aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenylether dicarboxylic acid; and aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid; among these, isophthalic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, and 3,4-furandicarboxylic acid are preferred from the viewpoint of moldability. These dicarboxylic acid components may be used alone or in combination of two or more. The content of the dicarboxylic acid components other than 2,6-naphthalenedicarboxylic acid is preferably 10 mol % or less of the total dicarboxylic acid components including 2,6-naphthalenedicarboxylic acid.

[0030] The diol component (a-2) constituting the PBN contains 1,4-butanediol units, and in the diol component (a-2), the 1,4-butanediol units preferably account for 92 mol % or more, even more preferably 94 mol % or more, particularly preferably 96 mol % or more, and especially preferably 98 mol % or more. It is most preferable that all of the diol component (a-2) (100 mol %) is 1,4-butanediol. By making the diol component (a-2) contain 90 mol % or more of 1,4-butanediol units, the low dielectric properties and heat resistance of Layer A are improved.

[0031] The PBN may be copolymerized with a diol component other than 1,4-butanediol for the purpose of improving moldability and heat resistance.Specific examples of the diol component include 1,2-propanediol, 1,3-propanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, ethylene glycol, diethylene glycol, triethylene glycol, polyalkylene glycol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, hydroquinone, bisphenol, spiroglycol, 2,2,4,4,-tetramethylcyclobutane-1,3-diol, and isosorbide.Of these, ethylene glycol, diethylene glycol, 1,3-propanediol, 1,3-cyclohexanedimethanol, and 1,4-cyclohexanedimethanol are preferred from the viewpoint of moldability.These diol components may be used alone or in combination of two or more. The content of the diol components other than 1,4-butanediol is preferably 10 mol % or less of the total diol components including 1,4-butanediol.

[0032] It is preferable that a polyester other than the PBN is mixed in the layer A. By using a mixed polyester containing PBN in the layer A, the crystallization rate can be controlled, and extrusion moldability and stretch processability can be improved. The polyester other than PBN is not particularly limited, but is preferably an amorphous polyester, and more preferably the amorphous polyester has a higher glass transition temperature than the PBN. By mixing the PBN with an amorphous polyester, the crystallinity of the PBN itself can be alleviated, breakage during stretching can be suppressed, and handling properties during processing can be improved. In addition, since the amorphous polyester has a higher glass transition temperature than PBN, a resin composition having a higher glass transition temperature than PBN alone can be obtained, resulting in good heat resistance.

[0033] The amorphous polyester preferably has a structure obtained by polycondensation of at least three or more dicarboxylic acid components and diol components. Examples of the dicarboxylic acid component include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenonedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid; aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid; and oxycarboxylic acids such as p-oxybenzoic acid. Examples of the diol component include ethylene glycol, diethylene glycol, propylene glycol, 1,2-propanediol, 1,3-butanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 1,5-pentanediol, neopentyl glycol, polytetramethylene ether glycol, dimer diol, polyalkylene glycol, 2,2-bis(4'-β-hydroxyethoxyphenyl)propane, isosorbite, spiroglycol, and bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, bisphenol S, and bisphenol TMC, or derivatives thereof, or ethylene oxide adducts thereof). Among the amorphous polyesters, from the viewpoint of heat resistance, wholly aromatic polyesters are preferred, and among them, polyarylates (hereinafter also referred to as "PAR") are more preferred.

[0034] The PAR is a polycondensation product of a dicarboxylic acid component and a dihydric phenol component. The dicarboxylic acid component constituting the PAR is not particularly limited as long as it is a divalent aromatic carboxylic acid, and is preferably a mixture of a terephthalic acid component and an isophthalic acid component. The mixing ratio (molar ratio) of the terephthalic acid component and the isophthalic acid component is preferably terephthalic acid / isophthalic acid=99 / 1 to 1 / 99, more preferably 90 / 10 to 10 / 90, further preferably 80 / 20 to 20 / 80, particularly preferably 70 / 30 to 30 / 70, and particularly preferably 60 / 40 to 40 / 60. When the mixing ratio of terephthalic acid and isophthalic acid as the dicarboxylic acid components is within the above range, the PAR has excellent heat resistance and extrusion moldability.

[0035] The PAR may be copolymerized with an acid component other than terephthalic acid and isophthalic acid as the dicarboxylic acid component. Specifically, aromatic dicarboxylic acids such as phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenylether dicarboxylic acid are preferred. In order not to impair the heat resistance of the PAR, the copolymerization ratio of the acid component other than terephthalic acid and isophthalic acid is preferably less than 10 mol %.

[0036] The dihydric phenol component constituting the PAR is not particularly limited as long as it is a dihydric phenol, but it is preferable that the PAR contains either a bisphenol A (2,2-bis(4-hydroxyphenyl)propane) component or a bisphenol TMC (1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane) component, or both bisphenol A and bisphenol TMC.

[0037] In general, the inclusion of bisphenol A results in PAR with excellent extrusion moldability (fluidity). On the other hand, the inclusion of bisphenol TMC component increases the glass transition temperature, resulting in PAR with excellent heat resistance. When it is desired to balance extrusion moldability and heat resistance, it is preferable to use both the bisphenol A component and the bisphenol TMC component. In this case, the ratio (mol %) of the bisphenol A component and the bisphenol TMC component is preferably bisphenol A / bisphenol TMC=99 / 1 to 1 / 99, more preferably 90 / 10 to 10 / 90, further preferably 80 / 20 to 20 / 80, particularly preferably 70 / 30 to 30 / 70, and particularly preferably 60 / 40 to 40 / 60. By setting the ratio of the bisphenol A component and the bisphenol TMC component within this range, a PAR having an excellent balance between heat resistance and extrusion moldability can be obtained.

[0038] The PAR may be copolymerized with bisphenols other than bisphenol A and bisphenol TMC as the dihydric phenol component. Specifically, bisphenol AP (1,1-bis(4-hydroxyphenyl)-1-phenylethane), bisphenol AF (2,2-bis(4-hydroxyphenyl)hexafluoropropane), bisphenol B (2,2-bis(4-hydroxyphenyl)butane), bisphenol BP (bis(4-hydroxyphenyl)diphenylmethane), bisphenol C (2,2-bis(3-methyl-4-hydroxyphenyl)propane), bisphenol E (1,1-bis(4-hydroxyphenyl)ethane), bisphenol F (bis(4-hydroxyphenyl)methane), bisphenol Examples of such bisphenols include phenol G (2,2-bis(4-hydroxy-3-isopropylphenyl)propane), bisphenol M (1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene), bisphenol S (bis(4-hydroxyphenyl)sulfone), bisphenol P (1,4-bis(2-(4-hydroxyphenyl)-2-propyl)benzene), bisphenol PH (5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane), and bisphenol Z (1,1-bis(4-hydroxyphenyl)cyclohexane). In order not to impair the heat resistance of PAR, the copolymerization ratio of the above compound is preferably less than 10 mol %.

[0039] In order to enhance compatibility with the PBN, it is preferable to select a mixture of a terephthalic acid component and an isophthalic acid component as the dicarboxylic acid component, and a bisphenol A component, a bisphenol TMC component, or a mixture of bisphenol A and bisphenol TMC as the dihydric phenol component.

[0040] The PAR may be mixed with a polycarbonate resin for the purpose of improving extrusion moldability. Since the PAR and the polycarbonate resin are compatible with each other, by mixing the PAR with the polycarbonate resin, the glass transition temperature of the PAR can be lowered while maintaining the transparency and mechanical properties, and as a result, the extrusion moldability can be improved. When PAR and polycarbonate are mixed, the mixing ratio (mass ratio) of PAR / polycarbonate is preferably 99 / 1 to 50 / 50, more preferably 98 / 2 to 60 / 40, further preferably 97 / 3 to 70 / 30, and particularly preferably 96 / 4 to 80 / 20. When the mixing ratio of PAR and polycarbonate is within this range, the extrusion moldability can be improved while maintaining the heat resistance of PAR.

[0041] When Layer A contains an amorphous polyester such as PBN and PAR, it preferably contains the amorphous polyester in a ratio of 1 part by mass to 100 parts by mass per 100 parts by mass of PBN. The content of the amorphous polyester is more preferably 5 parts by mass or more and 90 parts by mass or less, further preferably 10 parts by mass or more and 80 parts by mass or less, and particularly preferably 20 parts by mass or more and 70 parts by mass or less, relative to 100 parts by mass of PBN. When the content of the amorphous polyester is 1 part by mass or more, the heat resistance and extrusion moldability are improved, whereas when the content of the amorphous polyester is 100 parts by mass or less, the low dielectric properties are sufficient.

[0042] The polyester polymerization catalyst is not particularly limited, and any conventionally known compound can be used, such as titanium compounds, germanium compounds, antimony compounds, manganese compounds, aluminum compounds, magnesium compounds, and calcium compounds.

[0043] In order to suppress the amount of precipitation of oligomer components, the film may be produced using a polyester having a low content of oligomer components as the raw material. As a method for producing a polyester having a low content of oligomer components, various known methods can be used, such as a method of performing solid phase polymerization after the production of a polyester. The polyester may also be obtained by carrying out esterification or transesterification, followed by melt polycondensation at a higher reaction temperature under reduced pressure.

[0044] Furthermore, Layer A may contain resins other than polyester as long as the effects of the present invention are not impaired. Examples of the other resins include polystyrene-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, chlorinated polyethylene-based resins, polylactic acid-based resins, polybutylene succinate-based resins, polycarbonate-based resins, polyamide-based resins (including aramid-based resins), polyacetal-based resins, acrylic-based resins, ethylene-vinyl acetate copolymers, polymethylpentene-based resins, polyvinyl alcohol-based resins, cyclic olefin-based resins, polyacrylonitrile-based resins, polyethylene oxide-based resins, cellulose-based resins, polyimide-based resins, polyurethane-based resins, polyphenylene sulfide-based resins, polyphenylene ether-based resins, polyvinyl acetal-based resins, polybutadiene-based resins, polybutene-based resins, polyamideimide-based resins, polyamide bismaleimide-based resins, polyetherimide-based resins, polyetheretherketone-based resins, polyetherketone-based resins, polyethersulfone-based resins, polyketone-based resins, polysulfone-based resins, and fluorine-based resins.

[0045] Layer A may contain particles for the main purpose of imparting lubricity and preventing scratches during each process. The type of particles is not particularly limited as long as they are particles capable of imparting lubricity, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.

[0046] On the other hand, the shape of the particles to be used is not particularly limited, and any of spherical, block, rod-like, flat, etc. may be used. There is also no particular restriction on the hardness, specific gravity, color, etc. These particles may be used alone or in combination of two or more kinds, if necessary.

[0047] The average particle size of the particles used is usually preferably 5 μm or less, more preferably in the range of 0.01 to 3 μm. If it is 5 μm or less, the surface roughness of the film will not be too rough, and no problems will occur when various surface functional layers are formed in a post-process. In addition, the transparency of the film will be sufficient, which is preferable. The average particle size of the particles is calculated from the particle size at an integrated volume fraction of 50% (d50) in an equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device.

[0048] Furthermore, the particle content in layer A is usually preferably less than 5% by mass, more preferably in the range of 0.0003 to 3% by mass. When there are no particles or only a small amount of particles, the film becomes highly transparent and is good in terms of transparency, but the slipperiness may be insufficient, so it may be necessary to take measures such as adding particles to the coating layer to improve the slipperiness. On the other hand, when the particle content is less than 5% by mass, the film has good transparency.

[0049] The method of adding particles to Layer A is not particularly limited, and any conventionally known method may be used. For example, the particles may be added at any stage in the production of the polyester constituting each layer, but it is preferable to add the particles after the completion of the esterification or transesterification reaction.

[0050] In addition to the above-mentioned particles, conventionally known ultraviolet absorbents, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added to Layer A as necessary.

[0051] <Layer B> The polyester constituting the layer B is not particularly limited, and examples thereof include those composed of a dicarboxylic acid component (b-1) and a diol component (b-2) as shown below. Examples of the dicarboxylic acid component (b-1) include terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, p-hydroxybenzoic acid, trimellitic acid monopotassium salt, and ester-forming derivatives thereof.

[0052] Examples of the diol component (b-2) include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. One or more of the above compounds may be appropriately selected and subjected to a conventional polycondensation reaction to synthesize a polyester.

[0053] The polyester constituting Layer B may be the same as or different from the polyester constituting Layer A.

[0054] Among the above polyesters, from the viewpoint of improving versatility and a balance between heat resistance, weather resistance, mechanical strength, cost, etc., it is preferable to use polyethylene terephthalate having terephthalic acid units as the dicarboxylic acid component (b-1) and ethylene glycol units as the diol component (b-2). From the viewpoint of crystallinity and heat resistance, it is more preferable that the dicarboxylic acid component (b-1) contains 60 mol % or more of terephthalic acid units, even more preferably 80 mol % or more, particularly preferably 90 mol % or more, and particularly preferably all (100 mol %) of the dicarboxylic acid component (b-1) is terephthalic acid units. From the same viewpoint, it is more preferable that the diol component (b-2) contains 60 mol % or more of ethylene glycol units, even more preferably 80 mol % or more, particularly preferably 90 mol % or more, and particularly preferably all of the diol component (b-2) (100 mol %) is an ethylene glycol unit.

[0055] The polyester polymerization catalyst is not particularly limited, and any conventionally known compound can be used, such as titanium compounds, germanium compounds, antimony compounds, manganese compounds, aluminum compounds, magnesium compounds, and calcium compounds.

[0056] In order to suppress the amount of precipitation of oligomer components, the film may be produced using a polyester having a low content of oligomer components as the raw material. As a method for producing a polyester having a low content of oligomer components, various known methods can be used, such as a method of performing solid phase polymerization after the production of a polyester. The polyester may also be obtained by carrying out esterification or transesterification, followed by melt polycondensation at a higher reaction temperature under reduced pressure.

[0057] Like Layer A, Layer B may also contain particles, ultraviolet absorbers, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc.

[0058] <Method of manufacturing laminated polyester film> A method for producing the laminated polyester film will be described. However, the following description is merely an example of the method for producing the laminated polyester film, and the laminated polyester film of the present invention is not limited to the laminated polyester film produced by the above-mentioned method.

[0059] For example, when producing a biaxially stretched film, a method is preferred in which the above-mentioned raw material polyester is extruded as a molten sheet from a die using multiple extruders, and then cooled and solidified on a rotating cooling drum to obtain an unstretched laminate sheet. In this case, it is preferred to increase the adhesion between the laminate sheet and the rotating cooling drum in order to improve the flatness of the laminate sheet, and an electrostatic application adhesion method and / or a liquid application adhesion method are preferably used. In this way, an unstretched laminate sheet is obtained. The polyester raw material may be fed to the extruder in the form of pellets or the like after being appropriately dried. Also, particles, an ultraviolet absorbing agent, and other additives may be appropriately mixed into the pellets.

[0060] Next, the unstretched laminate sheet obtained by the above method is stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120° C., preferably 80 to 110° C., and the stretching ratio is usually 2.5 to 7 times, preferably 3.0 to 6 times. Then, the film is stretched in a direction perpendicular to the first-stage stretching direction. In this case, the stretching temperature is usually 70 to 170° C., and the stretch ratio is usually 3.0 to 7 times, preferably 3.5 to 6 times.

[0061] Then, the film is subsequently heat-treated at a temperature of 180 to 270° C. under tension or relaxation of 30% or less to obtain a biaxially stretched film. In the above stretching, a method of stretching in one direction in two or more stages can be adopted. In that case, it is preferable to perform the stretching so that the final stretch ratios in both directions are each within the above range.

[0062] A simultaneous biaxial stretching method can also be used to produce the laminated polyester film. The simultaneous biaxial stretching method involves simultaneously stretching and orienting the unstretched sheet in the longitudinal and transverse directions under a temperature controlled condition usually at 70 to 120° C., preferably 80 to 110° C., and the stretching ratio is 4 to 50 times, preferably 7 to 35 times, and more preferably 10 to 25 times in terms of area ratio. The film is then heat-treated under tension or relaxation of 30% or less at a temperature of 170 to 250° C. to obtain a stretched and oriented film. Regarding the simultaneous biaxial stretching device employing the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, or a linear drive method can be employed.

[0063] The machine direction (MD) of the film is the direction in which the film advances during the film production process, i.e., the winding direction of the film roll, and the transverse direction (TD) is the direction parallel to the film surface and perpendicular to the machine direction, i.e., the direction parallel to the central axis of the roll when the film is rolled.

[0064] The total thickness of the present laminated polyester film is preferably from 1 to 300 μm, more preferably from 30 to 250 μm, and further preferably from 50 to 200 μm. If the total thickness is 1 μm or more, the film strength remains within a practical range, while if the total thickness is 300 μm or less, it is easy to incorporate into mobile devices and the like. The total thickness of this laminated polyester film was determined by cutting a roughly square sample piece with sides of 40 mm from the laminated polyester film, measuring the thickness at any five points on the film surface with a dial gauge with a graduation of 1 / 1000 mm, and calculating the average value.

[0065] The thickness of the layer A is preferably 10 to 70% of the total thickness of the laminated polyester film, more preferably 15 to 60%, and further preferably 20 to 50%. When the thickness of the layer A is 10% or more, the laminated polyester film has good low dielectric properties. On the other hand, when the thickness of the layer A is 70% or less, the balance of heat resistance, weather resistance, mechanical strength, cost, etc. and versatility are good. The thickness of the layer A can be adjusted by the ratio of the discharge rates when the polyester raw material is extruded during the production of the laminated polyester film. The thickness of layer A can be determined by creating an oblique cut surface of the film using SAICAS (registered trademark) and using a time-of-flight secondary ion mass spectrometer (TоF-SIMS) to determine the layer thickness from the ion peak intensity data.

[0066] <Physical properties of laminated polyester film> The dielectric loss tangent of the laminated polyester film at 28 GHz is 0.0060 or less. If the dielectric loss tangent exceeds 0.0060, a sufficient effect of reducing transmission loss cannot be obtained. From the above viewpoints, the dielectric loss tangent of the laminated polyester film is more preferably 0.0058 or less, even more preferably 0.0056 or less, particularly preferably 0.0054 or less, particularly preferably 0.0052 or less, and most preferably 0.0050 or less. The lower limit is not particularly limited, but is 0.001 or more. When the dielectric loss tangent of the present laminated polyester film is within this range, the present laminated polyester film has good low dielectric properties and can be suitably used for high-speed communication circuits. The dielectric loss tangent can be adjusted by the polyesters used in Layer A and Layer B and the film-forming and stretching conditions of the laminated polyester film.

[0067] The relative dielectric constant of the present laminated polyester film at 28 GHz is preferably 3.5 or less, more preferably 3.3 or less, and even more preferably 3.1 or less. The lower limit is not particularly limited, but is 2.0 or more. When the dielectric constant of the present laminated polyester film is within this range, the present laminated polyester film has good low dielectric properties and can be suitably used for high-speed communication circuits. The dielectric loss tangent and the relative dielectric constant of the laminated polyester film are values ​​measured by the method described in the examples.

[0068] The hysteresis loss rate of the present laminated polyester film when subjected to a tensile cycle test up to 5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) is preferably 60% or less. The lower limit is not particularly limited, and is 0.1% or more. The smaller the hysteresis loss rate, the greater the restoring force of the film, and the easier it is to return to its original state, i.e., the better the flex resistance. If the hysteresis loss rate of the present laminated polyester film is 60% or less, the film has a greater restoring force and a good flex resistance. From this viewpoint, it is more preferably 58% or less, even more preferably 56% or less, and particularly preferably 54% or less. The hysteresis loss rate can be adjusted by the polyesters used in Layer A and Layer B, and the film-forming and stretching conditions of the laminated polyester film.

[0069] The haze of the present laminated polyester film is preferably 4.0% or less, more preferably 3.0% or less, even more preferably 2.5% or less, particularly preferably 2.0% or less, particularly preferably 1.5% or less, and most preferably 1.0% or less. The lower limit is not particularly limited, but is 0.1% or more. When the haze is within this range, it can be said that the present laminated polyester film has good transparency, and can be suitably used, particularly, as a transparent antenna film. The haze is a value measured by the method described in the examples.

[0070] The heat shrinkage of the laminated polyester film after heat treatment at 150°C for 30 minutes is preferably -5 to 5%, more preferably -3 to 3%, and even more preferably -2 to 2% in both the machine direction (MD) and the transverse direction (TD). If the heat shrinkage is within this range, the film has sufficient flatness and heat resistance. The heat shrinkage is measured by the method described in the examples, and a positive value is the shrinkage rate and a negative value is the expansion rate.

[0071] (Transmission loss reduction rate (%)) The transmission loss reduction rate (%) when the present laminated polyester film was used was calculated as follows using the transmission loss (dB) obtained from the simulation described in the Examples. [Transmission loss reduction rate (%)] = (1 - [Transmission loss when using this laminated polyester film (dB)] / [Transmission loss when using polyethylene terephthalate film (dB)]) x 100 The transmission loss reduction rate is preferably 5% or more, more preferably 7% or more, and even more preferably 10% or more. The higher the transmission loss reduction rate, the better, but if it is 5% or more, it can be said that the transmission loss can be effectively reduced by using the present laminated polyester film in which Layer A arranged directly under the conductor wiring has low dielectric properties.

[0072] <<Laminated film with cured resin layer>> The laminated polyester film of the present invention may have a cured resin layer on at least one surface layer of the laminated polyester film as necessary for the purpose of improving adhesion to the metal layer, and the cured resin layer is preferably formed from a resin composition containing 70% by mass or more of a crosslinking agent based on the non-volatile components. In particular, it is more preferable to provide a cured resin layer on both surface layers of the laminated polyester film. Here, the laminated polyester film having a cured resin layer is called a laminated film with a cured resin layer, as described above. Incidentally, another layer may be present between the laminated polyester film and the cured resin layer.

[0073] As the crosslinking agent, various known crosslinking agents can be used, and examples thereof include oxazoline compounds, melamine compounds, epoxy compounds, isocyanate compounds, carbodiimide compounds, and silane coupling compounds. Among these, when a metal layer is provided on a cured resin layer, oxazoline compounds are preferably used from the viewpoint of improving durable adhesion. From the viewpoints of preventing the precipitation of oligomers on the film surface due to heating and improving the durability of the cured resin layer, a melamine compound is preferably used.

[0074] (Oxazoline compounds) The oxazoline compound is a compound having an oxazoline group in the molecule, and in particular, a polymer containing an oxazoline group is preferred, and can be prepared by polymerization of an addition polymerizable oxazoline group-containing monomer alone or with other monomers. Examples of the addition polymerizable oxazoline group-containing monomer include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline, and one or a mixture of two or more of these can be used. Among these, 2-isopropenyl-2-oxazoline is suitable because it is easily available industrially. The other monomer is not limited as long as it is a monomer that can be copolymerized with the addition-polymerizable oxazoline group-containing monomer, and examples thereof include (meth)acrylic acid esters such as alkyl (meth)acrylates (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, styrenesulfonic acid, and salts thereof (sodium salts, potassium salts, ammonium salts, tertiary amine salts, etc.); unsaturated nitriles such as acrylonitrile and methacrylonitrile; (meth)acrylamide, N-alkyl ( Examples of the monomer include unsaturated amides such as (meth)acrylamide and N,N-dialkyl(meth)acrylamide (alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); vinyl esters such as vinyl acetate and vinyl propionate; vinyl ethers such as methyl vinyl ether and ethyl vinyl ether; α-olefins such as ethylene and propylene; halogen-containing α,β-unsaturated monomers such as vinyl chloride and vinylidene chloride; and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. One or more of these monomers can be used. From the viewpoint of improving the durability of the coating film, the amount of oxazoline groups in the oxazoline compound is preferably in the range of 0.5 to 10 mmol / g, more preferably 3 to 9 mmol / g, and even more preferably 5 to 8 mmol / g.

[0075] (Melamine compounds) The melamine compound is a compound having a melamine skeleton in the compound, and for example, an alkylolated melamine derivative, a compound partially or completely etherified by reacting an alkylolated melamine derivative with an alcohol, and a mixture thereof can be used. As the alcohol used for etherification, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, isobutanol, etc. can be suitably used. The melamine compound may be either a monomer or a dimer or higher polymer, or a mixture of these. Furthermore, melamine may be partially co-condensed with urea or the like, and a catalyst may be used to increase the reactivity of the melamine compound.

[0076] (Epoxy compounds) The epoxy compound is a compound having an epoxy group in the molecule, and examples thereof include condensations of epichlorohydrin, ethylene glycol, polyethylene glycol, glycerin, polyglycerin, bisphenol A, etc. with a hydroxyl group or an amino group, polyepoxy compounds, diepoxy compounds, monoepoxy compounds, glycidylamine compounds, etc. Examples of polyepoxy compounds include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, triglycidyl tris(2-hydroxyethyl)isocyanate, glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, etc. Examples of diepoxy compounds include neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, resorcinol diglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polytetramethylene glycol diglycidyl ether, etc. Examples of the monoepoxy compound include allyl glycidyl ether, 2-ethylhexyl glycidyl ether, and phenyl glycidyl ether, and examples of the glycidylamine compound include N,N,N',N'-tetraglycidyl-m-xylylenediamine and 1,3-bis(N,N-diglycidylamino)cyclohexane.

[0077] (Isocyanate compounds) The isocyanate compound is a compound having an isocyanate or an isocyanate derivative structure, such as a blocked isocyanate. Examples of the isocyanate include aromatic isocyanates such as tolylene diisocyanate, xylylene diisocyanate, methylene diphenyl diisocyanate, phenylene diisocyanate, and naphthalene diisocyanate; aliphatic isocyanates having an aromatic ring such as α,α,α',α'-tetramethyl xylylene diisocyanate; aliphatic isocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate; and alicyclic isocyanates such as cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate), and isopropylidenedicyclohexyl diisocyanate. In addition, polymers and derivatives such as biuretized products, isocyanurate products, uretdione products, and carbodiimide modified products of these isocyanates are also included. These may be used alone or in combination. Among the above isocyanates, aliphatic isocyanates or alicyclic isocyanates are more preferable than aromatic isocyanates in order to prevent yellowing due to ultraviolet rays.

[0078] When used in the form of a blocked isocyanate, examples of the blocking agent include phenolic compounds such as bisulfites, phenol, cresol, and ethylphenol; alcohol compounds such as propylene glycol monomethyl ether, ethylene glycol, benzyl alcohol, methanol, and ethanol; active methylene compounds such as methyl isobutanoylacetate, dimethyl malonate, diethyl malonate, methyl acetoacetate, ethyl acetoacetate, and acetylacetone; mercaptan compounds such as butyl mercaptan and dodecyl mercaptan; lactam compounds such as ε-caprolactam and δ-valerolactam; amine compounds such as diphenylaniline, aniline, and ethyleneimine; acid amide compounds such as acetanilide and acetic acid amide; and oxime compounds such as formaldehyde, acetaldoxime, acetoneoxime, methyl ethyl ketoneoxime, and cyclohexanoneoxime, which may be used alone or in combination of two or more.

[0079] The isocyanate compound may be used alone or as a mixture or bond with various polymers. In terms of improving the dispersibility and crosslinking property of the isocyanate compound, it is preferable to use a mixture or bond with a polyester resin or a urethane resin.

[0080] (Carbodiimide compounds) A carbodiimide compound is a compound having a carbodiimide structure, and is a compound having one or more carbodiimide structures in the molecule. For better adhesion, etc., a polycarbodiimide compound having two or more carbodiimide structures in the molecule is more preferred.

[0081] Carbodiimide compounds can be synthesized by conventionally known techniques, and generally, condensation reaction of diisocyanate compounds is used. The diisocyanate compounds are not particularly limited, and both aromatic and aliphatic compounds can be used, and specific examples thereof include tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, phenylene diisocyanate, naphthalene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, cyclohexane diisocyanate, methylcyclohexane diisocyanate, isophorone diisocyanate, dicyclohexyl diisocyanate, and dicyclohexylmethane diisocyanate.

[0082] The content of carbodiimide groups contained in the carbodiimide compound, in terms of carbodiimide equivalent (weight [g] of the carbodiimide compound required to give 1 mol of carbodiimide groups), is usually in the range of 100 to 1000, preferably 250 to 700, and more preferably 300 to 500. By using within the above range, the durability of the coating film is improved.

[0083] Furthermore, within the scope of the present invention, in order to improve the water solubility or water dispersibility of the polycarbodiimide compound, a surfactant may be added, or a hydrophilic monomer such as a polyalkylene oxide, a quaternary ammonium salt of a dialkylamino alcohol, or a hydroxyalkylsulfonate may be added.

[0084] (Silane coupling compound) A silane coupling compound is an organosilicon compound that has an organic functional group and a hydrolyzable group such as an alkoxy group in one molecule. For example, epoxy group-containing compounds such as 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; vinyl group-containing compounds such as vinyltrimethoxysilane and vinyltriethoxysilane; styryl group-containing compounds such as p-styryltrimethoxysilane and p-styryltriethoxysilane; (meth)acrylic group-containing compounds such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane; 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)- Amino group-containing compounds such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-phenyl-3-aminopropyltriethoxysilane; isocyanurate group-containing compounds such as tris(trimethoxysilylpropyl)isocyanurate and tris(triethoxysilylpropyl)isocyanurate; mercapto group-containing compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropylmethyldiethoxysilane.

[0085] These crosslinking agents may be used alone or in combination of two or more, but by using two or more in combination, it is possible to improve the adhesion to the metal layer provided on the cured resin layer and the prevention of oligomer precipitation after heating. Among them, a combination of an oxazoline compound that can improve the adhesion to the metal layer on the cured resin layer and a melamine compound that has good prevention of oligomer precipitation after heating is particularly preferred.

[0086] In order to further improve the adhesion between the cured resin layer and the metal layer, it is more preferable to combine three or more types of crosslinking agents. When combining three or more types of crosslinking agents, it is preferable to select a melamine compound as one of the crosslinking agents. As the counterpart crosslinking agent to be combined with the melamine compound, an oxazoline compound and an epoxy compound, or a carbodiimide compound and an epoxy compound are further preferable.

[0087] The crosslinking agent is preferably present in an amount of 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total non-volatile components in the resin composition forming the cured resin layer according to the present invention. If the amount is 70% by mass or more, the adhesion to the metal layer provided on the cured resin layer and the prevention of oligomer precipitation after heating are good.

[0088] The resin composition may contain a binder resin in order to improve the appearance of the cured resin layer and to improve adhesion to a metal layer provided on the cured resin layer, within the scope of the present invention. As the binder resin, any of the conventionally known resins can be used, but from the viewpoint of improving adhesion with a layer provided on the cured resin layer, it is preferable to use a polyester resin, an acrylic resin, or a urethane resin.

[0089] The resin composition may also contain particles for the purpose of preventing blocking and improving slippage. The average particle size is preferably 1.0 μm or less, more preferably 0.5 μm or less, and even more preferably 0.2 μm or less, from the viewpoint of film transparency. On the other hand, in order to more effectively improve slippage, the average particle size is preferably 0.01 μm or more, more preferably 0.03 μm or more, and particularly preferably in a range larger than the film thickness of the cured resin layer. Specific examples of particles include silica, alumina, kaolin, calcium carbonate, and organic particles.

[0090] Furthermore, within the scope of the present invention, the resin composition may be used in combination with a crosslinking catalyst, an antifoaming agent, a coatability improving agent, a thickener, an organic lubricant, an antistatic agent, an ultraviolet absorber, an antioxidant, a foaming agent, a dye, a pigment, etc., as necessary.

[0091] The thickness of the cured resin layer (after drying) is preferably 0.003 to 1.0 μm, more preferably 0.005 to 0.5 μm, and even more preferably 0.01 to 0.2 μm. If the thickness is 1.0 μm or less, the appearance and blocking resistance of the cured resin layer are sufficient. On the other hand, if the thickness is 0.003 μm or more, the amount of oligomer precipitated from the film is small and good.

[0092] The resin composition is generally preferably diluted with water, an organic solvent, or a mixture thereof, and the cured resin layer may be formed by coating the diluted resin composition as a coating liquid on the surface of the laminated polyester film and drying it.

[0093] A coating may be applied to the surface of the laminated polyester film as necessary, and the cured resin layer may be formed by coating. Methods for forming the cured resin layer include in-line coating and off-line coating, and in-line coating is preferred. In-line coating is a method for coating within the process of manufacturing the laminated polyester film, and specifically, a method for coating at any stage from melt extrusion of the raw material polyester to stretching, heat setting, and winding up. Usually, coating is performed on any of the following: an unstretched laminated sheet obtained by melting and quenching, a stretched uniaxially stretched film, a biaxially stretched film before heat setting, and a laminated polyester film after heat setting and before winding up. In particular, a method of coating a uniaxially stretched film stretched in the longitudinal direction (lengthwise direction) and then stretching in the width direction (transverse direction) is preferred.

[0094] <Physical properties of laminated film with cured resin layer> The cured resin layer according to the present invention is effective not only in improving adhesion to the metal layer, but also in preventing oligomer precipitation on the film surface due to heating. By reducing oligomer precipitation, it is possible to suppress the decrease in visibility caused by whitening of the film appearance due to oligomer precipitation and whitening. In the laminated film with a cured resin layer of the present invention, in an embodiment in which the laminated polyester film has cured resin layers on both surface layers, the amount of oligomer (cyclic ester trimer) precipitated on the surface of at least one of the cured resin layers is 0.40 mg / m 2 Preferably, it is 0.35 mg / m or less. 2 More preferably, it is 0.30 mg / m or less. 2 More preferably, it is 0.25 mg / m or less. 2 It is particularly preferable that the amount of oligomer precipitation is 0.40 mg / m or less. 2 If the content is less than this, there is no decrease in visibility due to whitening of the film appearance caused by precipitation and crystallization of oligomers on the surface, and there is no occurrence of defects in post-processing and no contamination of the process or parts, which is preferable. The lower limit is not particularly limited, but it is preferably 0.01 mg / m 2 That's all. The amount of oligomer precipitated on the surface of the cured resin layer can be adjusted by the polyester used and the layer structure of the laminated polyester film. Furthermore, when the amount of oligomer precipitation on the surface of the cured resin layer on Layer A is smaller than the amount of oligomer precipitation on the surface of the cured resin layer on Layer B, from the viewpoint of suppressing a decrease in visibility, a three-layer structure of Layer A / Layer B / Layer A is preferable to a two-layer structure of Layer A / Layer B or a three-layer structure of Layer A / Layer B / Layer B. The amount of oligomer precipitation is a value obtained by the method described in the Examples.

[0095] <<Metal laminated film>> In the metal laminated film of the present invention, a metal layer may be provided on the cured resin layer, and another layer may be provided between the cured resin layer and the metal layer. The metal layer is a layer containing a metal as a main component, which means that the metal occupies 50% by mass or more of the metal layer, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. Metals that can be used include copper, copper alloys, silver, stainless steel, nickel, nickel alloys, aluminum, aluminum alloys, titanium, titanium alloys, etc., but from the viewpoint of electromagnetic wave shielding properties, copper or silver is preferred, and from the viewpoint of flexibility, copper is more preferred.

[0096] From the viewpoint of maintaining the transparency of the laminated polyester film and the laminated film with a cured resin layer, the metal layer is preferably patterned, for example, in a mesh shape or wire shape.

[0097] The thickness of the metal layer is preferably 2 to 30 μm, and more preferably 3 to 25 μm. When the thickness of the metal layer is equal to or more than the lower limit, the electrical conductivity is sufficiently ensured, whereas when the thickness is equal to or less than the upper limit, the visibility of the metal layer can be reduced. The thickness of the metal layer can be measured by observing a cross section of a sample with an electron microscope.

[0098] <<Applications>> The laminated polyester film, the laminated film with a cured resin layer, and the metal laminated film of the present invention have excellent low dielectric properties without impairing transparency. Therefore, it can be suitably used for high-speed communication circuits. Examples of high-speed communication circuit applications include FPCs (Flexible Printed Circuits), which are flexible circuit boards formed of resin films and copper foils, and transparent antenna films in which invisible ultrafine metal mesh wiring is formed on a transparent film. In particular, it can be suitably used for transparent antenna films, which require high transparency.

[0099] In addition, when the laminated polyester film has excellent bending resistance, it can be suitably used for a flexible display equipped with a high-speed communication circuit. The flexible display is a general term for displays that are required to have excellent restoring properties and to be resistant to repeated bending, and examples of such displays include bendable, rollable, stretchable, and foldable. Examples of displays include mobile phones, smartphones, digital cameras, and personal computers, and the type of display is not particularly limited and may include liquid crystal displays, plasma displays, and organic electroluminescence displays.

[0100] <<Explanation of terms, etc.>> In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0101] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to the examples described below.

[0102] <Evaluation method> (1) Intrinsic viscosity of polyester 1 g of polyester was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and measured at 30°C.

[0103] (2) Dielectric tangent and relative dielectric constant of laminated polyester film The dielectric loss tangent and relative dielectric constant of the laminated polyester films obtained in the examples and comparative examples were measured at a frequency of 28 GHz in accordance with JIS R1641 using a dielectric constant measurement system (cavity resonator (TE mode), control software, vector network analyzer MS46122B (manufactured by Anritsu Corporation)) manufactured by AET Corporation.

[0104] (3) Dielectric tangent and relative dielectric constant of layer A The raw material of layer A was put into a small twin screw extruder and melt extruded at 300°C to obtain an unstretched sheet having a thickness of 200 μm. The obtained unstretched sheet was stretched at 100°C at a ratio of 3.0 × 3.0 by a batch type small biaxial stretching machine to obtain a biaxially stretched film sample. The dielectric loss tangent and relative dielectric constant of layer A at a frequency of 28 GHz were measured for the obtained film sample using the same method as above.

[0105] (4) Hysteresis loss rate The hysteresis loss rate at 23° C. was determined by the following method in accordance with JIS K 7312:1996. The measuring device used was a tensile tester (Autograph AG-I manufactured by Shimadzu Corporation). The test specimen was cut from an arbitrary position of the polyester film into a rectangle with a length of 100 mm and a width of 10 mm in the measurement direction. Both ends of the test specimen in the length direction were chucked with a chuck distance of 50 mm, and the test specimen was raised to a strain of 5% at a crosshead speed of 0.5 mm / min, and then lowered to the initial position at the same speed to obtain a stress-strain curve from one cycle of tensile cycle test. The stress-strain curve had a profile as shown in Figure 1, and the hysteresis loss rate was calculated from the obtained stress-strain curve using the area A1 (abcda) of the curve obtained in the ascending operation and the area A2 (abcef) which is the difference between the area A1 and the area of ​​the curve obtained in the descending operation, using the following formula (2). The test was performed three times, and the average value was calculated. The above tensile cycle test was performed in the longitudinal direction (MD) and the axial direction (TD) of the film, respectively. Hysteresis loss rate = A2 / A1 × 100 Formula (2)

[0106] (5) Haze The measurement was performed using a haze meter DH-2000 manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K7136.

[0107] (6) Heat shrinkage rate A sample film of 1.5 cm x 15 cm was heat-treated for 30 minutes in a hot air oven maintained at a specified temperature (150°C) in an untensioned state, and the length of the sample film was measured before and after the treatment, and the elastic modulus was calculated using the following formula. The measurements were taken in both the machine direction (MD) and the cross direction (TD) of the film. Heat shrinkage rate (%) = {(sample length before heat treatment) - (sample length after heat treatment)} ÷ (sample length before heat treatment) x 100

[0108] (7) Evaluation of transmission loss by simulation An electromagnetic field simulation was performed on a film circuit board using a microstrip line as a pattern to determine the appropriate line width (50 Ω line width) for a characteristic impedance of 50 Ω and the transmission loss (insertion loss, S21). As a simulation model, the thickness of the polyester film (substrate) was set to 125 μm. The relative dielectric constant and dielectric loss tangent at 28 GHz of each polyester layer used in the simulation are as shown in Table 1. In addition, a simulation model was created in which a metal layer (copper foil, thickness 18 μm, surface roughness (Rz) 1.0 μm, line length 100 mm) was laminated on a substrate. The electromagnetic field simulation was performed under the conditions of a characteristic impedance of 50 Ω and a frequency of 28 GHz.

[0109] 2 is a cross-sectional view showing an example of a microstrip line 10. The microstrip line 10 has a substrate 11, a microstrip line 12 made of a metal layer, and a ground plane 13 made of a metal layer.

[0110] [Table 1]

[0111] (8) Amount of oligomer (cyclic ester trimer) precipitated on the surface of the cured resin layer due to heating The laminated films with the cured resin layer obtained in the Examples and Comparative Examples were cut into sample pieces measuring 300 mm in length and 225 mm in width, and were subjected to heat treatment for 120 minutes in a hot air oven maintained at a prescribed temperature (180° C.). After the heat treatment, a box-shaped sample was made with the measurement surface as the inner surface, measuring 200 mm in length and 125 mm in width, and open at the top. Next, 10 mL of DMF (dimethylformamide) was placed in the box-shaped container and allowed to stand for 3 minutes, after which the DMF was collected and fed to a liquid chromatograph (Shimadzu Corporation: LC-7A, mobile phase A: acetonitrile, mobile phase B: 2% aqueous acetic acid solution, column: Mitsubishi Chemical Corporation "MCI GEL ODS 1HU", column temperature: 40°C, flow rate: 1 mL / min, detection wavelength: 254 nm) to determine the amount of ester cyclic trimer in the DMF, and this value was divided by the area of ​​the film in contact with the DMF to determine the amount of oligomer (ester cyclic trimer) (mg / m) on the surface of the cured resin layer. 2The amount of cyclic ester trimers in DMF was determined from the peak area ratio between the standard sample peak area and the measured sample peak area (absolute calibration curve method). The standard sample was prepared by accurately weighing a previously separated ester cyclic trimer and dissolving it in an accurately weighed amount of DMF.

[0112] <Materials used> [Polyester raw materials] Raw material A: Homopolybutylene naphthalate Raw material B: Polyarylate (dicarboxylic acid component: terephthalic acid / isophthalic acid (molar ratio) = 50 / 50, dihydric phenol component: bisphenol A 100 mol%) Raw material C: homopolyethylene terephthalate (intrinsic viscosity = 0.64 dL / g)

[0113] [Cured resin layer] The following resin composition was used for forming the cured resin layer. (A1): Hexamethoxymethylolmelamine (A2): Epocross, an oxazoline compound (manufactured by Nippon Shokubai Co., Ltd.), with an oxazoline group content of 7.7 mmol / g (A3): Polyglycerol polyglycidyl ether (B1): Silica particles with an average particle size of 0.07 μm The compositions of the coating solutions used in the examples are shown in Table 2.

[0114] [Table 2]

[0115] Example 1 A mixture of raw materials A and B in a mass ratio of 70:30 was used as the raw material for layer A, and raw material C was used as the raw material for layer B. Raw materials A and B were mixed in a mass ratio of 70:30 as the raw materials for both surface layers, and raw material C was used as the raw material for the middle layer, and these were separately fed into a twin-screw extruder, and layer A was co-extruded at 285°C and layer B was co-extruded at 280°C, and cooled and solidified on a cooling roll set at 50°C to obtain an unstretched laminated sheet with two types and three layers, layer A / layer B / layer A. The unstretched laminated sheet was then stretched 3.0 times in the machine direction (MD) at 100° C. using a roll stretching machine. It was then preheated in a tenter at 115° C., and stretched 3.8 times in the transverse direction (TD) at 125° C. Finally, it was heat-treated at 210° C. to obtain a biaxially stretched laminated polyester film with a thickness of 125 μm (Layer A / Layer B / Layer A=25 / 75 / 25 (μm)). The properties of the obtained laminated polyester film were evaluated by the above-mentioned methods. The evaluation results are shown in Table 3.

[0116] Example 2 After the longitudinal direction (MD) stretching of Example 1 and before the transverse direction (TD) stretching, the above-mentioned coating liquid was applied to both sides of the uniaxially stretched laminated polyester film to obtain a biaxially stretched laminated polyester film (laminated film with a cured resin layer) having a film thickness (after drying) of 0.04 μm. The evaluation results of the resulting laminate film with a cured resin layer are shown in Table 4 below.

[0117] Comparative Example 1 Raw material C was fed into a twin-screw extruder, extruded at 280°C, and cooled and solidified on a cooling roll set at 20°C to obtain an unstretched sheet. The unstretched sheet was then stretched 3.2 times in the machine direction (MD) at 85° C. using a roll stretching machine. It was then preheated in a tenter at 110° C., and stretched 4.3 times in the transverse direction (TD) at 140° C. Finally, it was heat-treated at 240° C. to obtain a biaxially stretched polyester film having a thickness of 125 μm. The properties of the obtained polyester film were evaluated by the above-mentioned methods, and the evaluation results are shown in Table 3.

[0118] Comparative Example 2 After the longitudinal (MD) stretching of Comparative Example 1 and before the transverse (TD) stretching, the above coating liquid was applied to both sides of the uniaxially stretched polyester film to obtain a biaxially stretched polyester film having a cured resin layer with a thickness (after drying) of 0.04 μm. The evaluation results of the obtained film with a cured resin layer are shown in Table 4 below.

[0119] In Tables 3 and 4, the upper surface refers to the surface on which the microstrip line is provided, and the lower surface refers to the surface on which the ground plane is provided.

[0120] [Table 3]

[0121] [Table 4]

[0122] From the results of Example 1, the laminated polyester film of the present invention has a small transmission loss and a high transmission loss reduction rate, and even if the film is made of polyethylene terephthalate, a general-purpose resin, the results suggest the possibility of it being a low dielectric property film. In addition, since the hysteresis loss rate is small, the film has excellent recovery and repeated bending resistance, and can be suitably used for flexible displays equipped with high-speed communication circuits. Furthermore, the film has low haze and excellent transparency. Furthermore, since the film is made of polyethylene terephthalate, the film has excellent heat resistance, weather resistance, mechanical properties, and processability, and is also advantageous in terms of cost. Furthermore, in the laminate film with a cured resin layer, the amount of oligomer precipitation on the surface of the cured resin layer can be reduced by having a cured resin layer on Layer A, as shown in the results of Example 2. Therefore, the laminated polyester film and the laminate film with a cured resin layer of the present invention have good visibility and are particularly suitable for use as a transparent antenna film. [Industrial Applicability]

[0123] The laminated polyester film and the laminated film with a cured resin layer of the present invention have excellent low dielectric properties and transparency, and are therefore extremely useful for high-speed communication circuits, in particular as a transparent antenna film which requires high transparency. [Explanation of symbols]

[0124] 10 Microstrip Line 11 Substrate 12 Microstrip Lines 13 Ground Plane

Claims

1. A laminated polyester film having two or more polyester layers, the laminate having at least one layer A of the polyester layers on at least one surface layer, the layer A comprises polybutylene naphthalate, A laminated polyester film having a dielectric loss tangent of 0.0060 or less at 28 GHz.

2. 2. The laminated polyester film according to claim 1, wherein the layer A has a relative dielectric constant of 3.0 or less at 28 GHz.

3. 3. The laminated polyester film according to claim 1, wherein the layer A has a dielectric loss tangent at 28 GHz of 0.0050 or less.

4. The laminated polyester film according to any one of claims 1 to 3, which has a hysteresis loss rate of 60% or less when subjected to a tensile cycle test up to 5% tensile strain in both the machine direction (MD) and the transverse direction (TD).

5. The laminated polyester film according to any one of claims 1 to 4, wherein the layer A further contains an amorphous polyester.

6. The laminated polyester film according to claim 5 , wherein the amorphous polyester has a glass transition temperature higher than that of the polybutylene naphthalate.

7. The laminated polyester film according to claim 5 or 6, comprising the amorphous polyester in an amount of 1 part by mass or more and 100 parts by mass or less per 100 parts by mass of the polybutylene naphthalate.

8. The laminated polyester film according to any one of claims 5 to 7, wherein the amorphous polyester is a polyarylate.

9. The laminated polyester film according to any one of claims 1 to 8, wherein a layer other than the layer A contains polyethylene terephthalate.

10. The laminated polyester film according to any one of claims 1 to 9, having a haze of 4.0% or less.

11. The laminated polyester film according to any one of claims 1 to 10, having a total thickness of 1 to 300 µm.

12. The laminated polyester film according to any one of claims 1 to 11, wherein the thickness of the layer A is 10 to 70% of the total thickness of the laminated polyester film.

13. A laminated film with a cured resin layer, comprising the laminated polyester film according to any one of claims 1 to 12, and a cured resin layer on at least one surface layer of the laminated polyester film, the cured resin layer being formed from a resin composition containing a crosslinking agent in an amount of 70 mass% or more relative to the non-volatile components.

14. The laminated polyester film has the cured resin layers on both surface layers, and the amount of oligomer precipitation on the surface of at least one of the cured resin layers is 0.40 mg / m 2 The cured resin layer-attached laminate film according to claim 13, wherein:

15. A metal laminated film comprising the cured resin layer-attached laminated film according to claim 13 or 14, and a metal layer on the cured resin layer.

16. 16. The metal laminate film of claim 15, wherein the metal layer is patterned.

17. 17. The metal laminated film according to claim 15 or 16, wherein the metal layer is made of copper or silver.

18. The laminated polyester film according to any one of claims 1 to 12, which is for use in high-speed communication circuits.

19. The laminated polyester film according to claim 18, which is used for a transparent antenna film.

20. The laminate film with a cured resin layer according to claim 13 or 14, which is for use in a high-speed communication circuit.

21. The cured resin layer-attached laminate film according to claim 20, which is used as a transparent antenna film.

22. The metal laminated film according to any one of claims 15 to 17, which is for use in high-speed communication circuits.

23. 23. The metal laminated film of claim 22, which is for use as a transparent antenna film.

Citation Information

Patent Citations

  • Electronic part for high frequency

    JP2006352470A

  • Copper alloy article containing polyester resin and method for producing the same

    JP2017222089A

  • Composite material of metal and resin

    JP2019025859A

  • 28GHz Vivaldi Step Tapered Antenna using LCP Substrate

    KR1020200075277A

  • Low dielectric coverlay film and coverlay film composition for the same

    KR1020200080612A