Finger joint cutter, wood processed product and its manufacturing method

The innovative finger joint cutter and wood product design with specific geometric parameters and manufacturing method enhance joint strength, addressing the trade-off between finger length and strength in laminated wood products, achieving superior tensile and bending strengths.

JP7575010B2Active Publication Date: 2024-10-29KANEFUSA HAMONO KOUGIYOU KK +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021528269
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-27
Filing Date
2020-06-16
Publication Date
2024-10-29
Estimated Expiration
2040-06-16

AI Technical Summary

Technical Problem

Existing finger joint cutters and laminated wood products face a trade-off between shortening finger length to reduce machining costs and energy consumption, which compromises joint strength.

Method used

A finger joint cutter and wood product design with specific geometric parameters (finger length < 12.0 mm, scarf slope ratio ≤ 1/8.8, and unit cross-sectional area of 1 mm²) and a complementary blade configuration to form high-strength finger joints, along with a manufacturing method using a feed amount of 0.5 to 1.75 mm per blade.

Benefits of technology

The solution enables the production of high-strength laminated wood products, exceeding standard tensile and bending strengths, suitable for applications under large external forces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575010000002
    Figure 0007575010000002
  • Figure 0007575010000003
    Figure 0007575010000003
  • Figure 0007575010000004
    Figure 0007575010000004
Patent Text Reader

Abstract

The present invention addresses the problem of providing a finger joint which exhibits high strength even when the finger length is made short. This finger joint has a finger length L of 12.0 mm or less, a scarf inclination ratio tanθ of 1 / 8.8 or less, and an adhesive area s per unit cross-sectional area (1 mm2) in a butting direction of 4.67 mm2 or more. This wood product is formed by vertical joining using this finger joint. The wood product is any one of a structural laminated wood laminar, a cross laminated timber (CLT) laminar, and a vertical joining material for a framework wall construction method structure. These are all supposed to be used for parts on which large external force will be applied, and thus are required to be of high strength.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a finger joint cutter, a wood processed product, and a method for manufacturing the same. [Background technology]

[0002] Laminated timber is manufactured by stacking lamina formed by joining finger joints formed by cutting zigzags at the ends of multiple plate materials together vertically (Non-Patent Document 1). It is desirable to make the length of the finger joint (finger length) as short as possible from the viewpoints of reducing processing costs and energy, reducing cutting chips, etc., but shortening the finger length results in a relative decrease in joint strength. For example, fingers shorter than those used in structural laminated timber are used in structural laminated timber.

[0003] Here, the finger joints are generally formed by cutting using a blade called a finger joint cutter (Non-Patent Document 2, etc.). [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Japanese Agricultural Standards for Laminated Timber (Ministry of Agriculture, Forestry and Fisheries Notification No. 683, March 29, 2018) [Non-Patent Document 2] Kanefusa Co., Ltd., product information on chip saws, bits, drills, etc., wood (wood material) processing: replaceable blade finger cutter, http: / / www.kanefusa.co.jp / products / 001980.html Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention was completed in consideration of the above-mentioned circumstances, and aims to provide a finger joint cutter that can form finger joints having a shape that can achieve high strength even if the finger length is shortened. Another aim is to provide a wood processed product having a finger joint having a shape that can achieve higher strength than conventional products, and a manufacturing method thereof. [Means for solving the problem]

[0006] In order to solve the above problems, the present inventors conducted various studies on the shape of the finger joint. As a result, they discovered that a high joint strength can be achieved even if the finger length is shortened by forming the finger joint in a specific shape, and completed the following invention.

[0007] The wooden product of the present invention, which solves the above problems, has a finger length L of less than 12.0 mm, a scarf slope ratio tan θ of 1 / 8.8 or less, and a unit cross-sectional area (1 mm 2 ) adhesive area s is 4.67 mm 2 The finger joint is made of wood joined vertically at this finger joint.

[0008] The wood product of the present invention is any one of lamina for structural laminated timber, lamina for cross-laminated timber (CLT), and vertical joint material for wood-frame construction. All of these are expected to be used in areas where a large external force may be applied, and therefore require high strength.

[0009] The finger joint cutter of the present invention, which solves the above problems, is a finger joint cutter that cuts an object to be cut by rotating about a rotation axis.

[0010] The finger joint cutter of the present invention has a cross-sectional shape on a plane including the rotation axis of a solid formed by rotating the blade portion once around the rotation axis, the cross-sectional shape of which is approximately complementary to a cross-sectional shape on a plane including the pitch direction and length direction of the fingers of the finger joint in the processed wood product of the present invention. A typical example of the finger joint cutter has a cylindrical main body with a plurality of blade portions formed on the outer peripheral surface of the cylinder, which is rotated around the central axis of the cylinder constituting the main body as the rotation axis for use as a finger joint cutter.

[0011] The method for manufacturing a processed wood product of the present invention for solving the above problems includes a finger forming step of cutting the workpiece with the finger joint cutter of the present invention to form the fingers. In this case, the feed amount per blade is 0.5 mm or more and 1.75 mm or less. Effect of the Invention

[0012] The wood product of the present invention has high strength despite the presence of vertical joints made by finger joints because of the above-mentioned configuration. The finger joint cutter of the present invention and the manufacturing method of the wood product of the present invention have the above-mentioned configuration, and therefore it is possible to efficiently manufacture the wood product of the present invention. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic diagram of a wood product according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a finger joint cutter according to the present embodiment. [Figure 3A] FIG. 2 is a schematic diagram of a finger joint cutter according to the present embodiment. [Figure 3B] FIG. 2 is a schematic diagram of a finger joint cutter according to the present embodiment. [Figure 4] 1 is a graph showing the relationship between adhesive area s per unit area and tensile strength in a test sample in this example. [Diagram 5]1 is a graph showing the relationship between adhesive area s per unit area and bending strength in a test sample in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the wood product, its manufacturing method, and finger joint cutter of the present invention will be described in detail based on the embodiment. The wood product of this embodiment is any one of lamina for structural laminated timber, lamina for cross-laminated timber (CLT), and vertical joint material for frame wall construction structure. All of these are made by joining board materials such as sawn boards by vertical joints (jointing in the direction of the wood fibers). The vertical joints are made by butting finger joints formed on the joint surfaces. Laminas for structural laminated timber and lamina for cross-laminated timber (CLT) are made by stacking multiple sheets in the thickness direction to form laminated timber and CLT. The drawings used for explanation in this embodiment are schematic diagrams, and individual dimensions, relative positions, the number of individual elements, etc. can be changed as appropriate. In this specification, unless otherwise specified, the unit of length is mm, and the unit of area is mm. 2 Use.

[0015] (Wood processed products) The wood product of this embodiment will be described with reference to FIG. 1. As shown in FIG. 1, the wood product of this embodiment is joined between a first member 10 and a second member 20 by a finger joint. The illustration of both ends in the width direction of the figure (the direction of the arrow corresponding to P in the figure: hereinafter referred to as "P direction") is omitted. In addition, in FIG. 1, there are fingers that are not engaged by butting together (fingers 13, 14), but this is for convenience, and such unengaged fingers may or may not exist. From the viewpoint of improving strength, it is preferable to have fewer fingers that are not involved in the joint. For example, it is preferable that the number of fingers formed on each of the first member 10 and the second member 20 is the same, or the number of fingers on one side is the number of fingers on the other side + 1.

[0016] The first member 10 and the second member 20 are oriented in such a way that the vertical direction in the drawing (the direction of the arrow corresponding to L in the drawing: hereinafter referred to as "L direction") is approximately the direction of the wood fibers. There are no particular limitations on the type of wood constituting the first member 10 and the second member 20. The type is appropriately selected depending on the strength, appearance, etc. required for the application in which the wood product is used.

[0017] The first member 10 is manufactured by cutting a sawn board, and has fingers 11 to 14. The fingers 11 to 14 have a constant cross-sectional shape in the vertical direction of the plane of the drawing, and the cross-sectional shape is preferably a trapezoid whose width narrows toward the top of the drawing, and is a substantially isosceles trapezoid.

[0018] Here, the shape of the sawn board is specified in three directions: the grain direction (longitudinal direction) of the wood, the width direction which is the longer direction among the directions perpendicular to the grain direction of the wood, and the thickness direction which is perpendicular to the grain direction and the width direction of the wood and is shorter than the width direction. The direction in which the fingers 11-14 are formed on the sawn board may be such that the width direction and the P direction coincide with each other, or the thickness direction and the P direction coincide with each other. Also, the fingers may be obliquely aligned with both the width direction and the thickness direction, not aligned with each other.

[0019] The tip thickness of the trapezoid (finger tip thickness) is t1 (mm). Fingers 11-14 are arranged with a gap (finger bottom width) t2 (mm) between adjacent fingers. In other words, fingers 11-14 are arranged at a finger pitch P (mm) calculated by (the lower thickness of fingers 11-14 in the L direction) + (finger bottom width t2).

[0020] The fingers 11 to 14 have scarves b which are parts b corresponding to the legs of the isosceles trapezoid formed by the fingers 11 to 14. The shape of the scarf b is determined by the "scarf inclination ratio: tan θ" which is expressed as the angle θ with the L direction. It is preferable that the surface of the scarf b is smooth.

[0021] The finger joint in the wood product of this embodiment has the following configuration: Finger length L is less than 12 mm, scarf slope ratio tan θ is 1 / 8.8 or less, and unit cross-sectional area (1 mm 2 ) adhesive area s is 4.67 mm 2 As for L, preferred upper limit values ​​include 11 mm, 10.5 mm, 10 mm, 9 mm, 8 mm, 7 mm, 6.5 mm, 6.0 mm, 5.5 mm, and 5.0 mm. Preferred lower limit values ​​include 4 mm.

[0022] As for tan θ, preferred upper limits include 1 / 9, 1 / 10, 1 / 11, and 1 / 12. 2 The preferred lower limit for the adhesive area per 2 , 5.5mm 2 , 6.0mm 2 , 6.5mm 2 , 7.0mm 2 , 7.5mm 2 Examples include:

[0023] Here, the cross-sectional area in the butt direction is the cross-sectional area in the P direction of the first member 10 in Fig. 1. Usually, the first member 10 and the second member 20 are members having the same cross-sectional shape in the butt direction. However, when joining the first member 10 and the second member 20 to manufacture a processed wood product, it is not necessarily necessary that the cross-sectional shapes of both members in the butt direction are the same. Even if the two members do not have the same cross-sectional shape, the cross-sectional shape can be changed (for example, made to be the same cross-sectional shape) by processing them with a planer or the like after joining.

[0024] The adhesive area s is the area of ​​the part that contacts the finger of the second member 20 that is to be butted. In other words, it is the sum of the areas of the parts that are adhered in the direction in which the first member 10 is butted against the second member 20. For example, it is the area excluding the area of ​​part A that is not involved in adhesion among the scarf surfaces of the fingers 11-14. Note that if butt parts are formed on both ends where the fingers 11-14 are arranged, the butt parts are not included in the adhesive area.

[0025] To increase the adhesive area s, increase L, decrease P, and decrease the finger tip thickness t1 and finger bottom width t2. To increase the number of fingers, decrease the scarf slope ratio tan θ. When P is the same, the scarf slope ratio tan θ should be as large as possible within one pitch in order to increase the adhesive area (the scarf slope ratio tan θ can be increased even if P is the same by decreasing t1 and t2). Increasing the adhesive area s can improve the strength of the joint.

[0026] The relationship between the finger length L and the finger pitch P is not particularly limited, but L / P is preferably greater than 2.19, more preferably 3.0 or greater, and even more preferably 3.2 or greater. The relationship between the finger tip thickness t1 and the finger pitch P is also not particularly limited, but t1 / P is preferably 0.28 or less, and even more preferably 0.18 or less.

[0027] The second member 20 also has fingers formed similar to those of the first member 10. In particular, since it is desirable that the finger joints of the first member 10 and the second member 20 have complementary shapes, the preferred shape of the second member 20 is the same as that described for the first member 10.

[0028] (Finger joint cutter) The finger joint cutter of this embodiment can form a finger joint by cutting the workpiece by rotation. For example, as shown in Fig. 2, it can be composed of a cylindrical main body 30 (the central axis of the cylinder is the axis of rotation) and a blade part 40 arranged on the outer circumferential surface of the main body 30.

[0029] 2 and 3B show perspective views of an example of a finger joint cutter in which a plurality of blade portions 40 are arranged in a single row on the outer circumferential surface of the main body portion 30 in the axial direction of the main body portion 30, and Fig. 3A and Fig. 3B show perspective views of an example of a finger joint cutter in which a plurality of blade portions 40 are arranged in double rows in the axial direction of the main body portion 30. Note that the finger joint cutters shown in Figs. 2 and 3 have different configurations, but are given the same reference numerals as the main body portion 30 and the blade portions 40.

[0030] There is no particular limitation on the rotation diameter (cutting arc diameter) of the path of the tip of the blade portion 40 when the finger joint cutter is used (rotated). For example, in consideration of the reuse of conventional equipment (equipment using conventional finger joint cutters), it is preferable to set it to the same as that of conventional finger joint cutters (for example, about φ150 mm to φ280 mm). In addition, it is preferable to subtract from the radius of the diameter of the cutting arc diameter of about 8 mm to 15 mm, which is the radial length of the blade portion 40, for the diameter of the main body portion 30.

[0031] In addition, the main body 30 is made up of multiple members, which improves maintainability. For example, it can be divided in the axial direction of the cylinder, in the circumferential direction, in the radial direction, or in a combination of these division directions. In the finger joint cutter shown in Figures 2 and 3, the blade 40 is fastened by a blade fastening bolt 41 so that it can be freely removed.

[0032] The cross-sectional shape of the blade portion 40 in a plane including the axis of rotation of the path formed by rotating the finger joint cutter of this embodiment once as in the usage state has a shape that is approximately complementary to the cross-sectional shape in a plane including the length direction L and pitch direction P of the finger in the woodworked product of this embodiment described above.

[0033] In other words, when there is one blade, the shape of the blade is generally complementary to the shape of the finger joint. When there are multiple blades, the combined shape of the multiple blades can be generally complementary to the finger joint. Even if the shapes of all the blades of the finger joint cutter are not generally complementary to the finger joint, it is sufficient that the partial shape of the part that comes into contact with the workpiece for cutting is generally complementary.

[0034] When a plurality of blade portions are provided, for example, they can be distributed in the circumferential direction on the outer circumferential surface of the main body portion 30 or in the direction of the rotation axis. The blade portions 40 are fixed to the main body portion 30, and the fixing method may be either an easily detachable method or a method that does not easily detach, such as welding.

[0035] The material constituting the blade portion can be a material for a general woodworking blade. For example, the blade portion can be made of a matrix high-speed steel or a base material made of a cemented carbide containing 0.5% to 0.8% C, 4% to 6% Cr, 0% to 2% W, 2% to 6% Mo, 1% to 2% V, and Fe as a main component based on the total mass. Furthermore, a hard film can be formed on the surface of the base material. The hard film can be formed by PVD, containing at least Cr and N. The surface roughness of the cutting edge of the blade portion is preferably Ra 0.30 μm or less, more preferably Ra 0.10 μm or less.

[0036] (Manufacturing methods for wood products) The method for manufacturing a processed wood product of this embodiment includes a finger forming step of cutting a workpiece with the finger joint cutter of this embodiment to form a finger joint consisting of fingers in the processed wood product of this embodiment. The processed wood product of this embodiment can be manufactured without using the method for manufacturing a processed wood product of this embodiment, but it is preferable to use the method for manufacturing a processed wood product of this embodiment. Here, the feed amount per blade is 0.5 mm or more and 1.75 mm or less.

[0037] The two components are bonded and joined by butting and meshing the finger joints formed in the finger forming process. An appropriate adhesive is used for bonding. Examples of adhesives include water-based polymer-isocyanate adhesives, resorcinol resin adhesives, resorcinol-phenol co-condensation resin adhesives, melamine resin adhesives, melamine-urea co-condensation resin adhesives, one-liquid polyurethane adhesives, and vinyl acetate resin emulsion adhesives. It is desirable to apply an appropriate pressure during bonding, and an example of the pressure is 4 MPa or more, with 8 MPa or more being preferable. EXAMPLES

[0038] Test 1 The wood product and its manufacturing method of the present invention will be described based on examples using two cedar materials, grades L50 and L80.

[0039] -Preparation of test samples For each of the cedars (grades L50 and L80), the finger length L, finger pitch P, finger tip thickness t1, finger bottom width t2, and unit cross-sectional area (1 mm 2 A pair of test pieces (each 125 mm wide, 33 mm thick, and 435 mm long) with finger joints with the adhesive area s per unit area (s) shown in Table 1 were prepared, and the finger joints were butted together and glued. Resorcinol resin was used as the adhesive, and the pieces were pressed for 10 seconds while applying an external force of 5 to 10 MPa in the butting direction, and then kept for one month in an atmosphere of 20°C and relative humidity of 55 to 60%. Then, the four sides were processed with a planer to produce test samples with a width of 120 mm, a thickness of 29 mm, and a length of approximately 840 mm. In producing the test samples, a finger joint cutter having a shape complementary to the shape of the formed fingers was manufactured and cut (finger forming process). The tensile strength and bending strength of each of the obtained test samples were measured. The results are also shown in Table 1. The strength of the wood itself is shown as test sample 0.

[0040] [Table 1]

[0041] As is clear from Table 1, the tensile strength tends to increase as L / P and the bonding area per unit cross-sectional area s increase. It was found that even higher tensile strength can be achieved when L / P is greater than 2.19. The bonding area per unit cross-sectional area s is 4.4 mm 2 Above this, even higher tensile strength can be achieved, up to 7.09 mm. 2 The above results show high strength that meets both the L80 and L50 standards.

[0042] The smaller the t1 / P, the higher the tensile strength. It was found that even higher tensile strength could be achieved by making t1 / P less than 0.28, or even less than 0.20 or 0.18. High tensile strength could be obtained with tanθ less than 1 / 8.8.

[0043] Here, the average standard for the strength performance of structural laminated timber lamina in the JAS standard for laminated timber is 16.5N / mm for tensile strength L50. 2 , 21.5N / mm for L80 2 , bending strength is 27.0N / mm for L50 2 , L80 is 36.0N / mm 2 When compared with these average value standards, the underlined strength values ​​were exceeded, and test samples 1 to 3 and 6 made with L50, and test samples 1 and 2 made with L80 met the average value standards.

[0044] When manufacturing another finger joint cutter with reference to Table 1, the finger length L, finger pitch P, finger tip thickness t1, finger bottom width t2, and bonding area s shown in Table 1 can be increased or decreased by approximately 1%, 2%, 5%, or 10%.

[0045] An approximation curve (logarithmic approximation) showing the relationship between the adhesive area s per unit cross-sectional area and strength was derived from the experimental results. The derived results are shown in Figure 4 (tensile strength) and Figure 5 (flexural strength). In the figures, the solid line corresponds to grade L50 for structural laminated timber laminas in the JAS standards for laminated timber, and the dashed line corresponds to L80. Auxiliary lines are drawn so that it is possible to see the adhesive area that corresponds to the average standard strength for the strength performance of structural laminated timber laminas in the above-mentioned JAS standards for laminated timber.

[0046] As is clear from Figures 4 and 5, the adhesive area that satisfies the average value standard for the strength performance of structural laminated timber lamina in the JAS standard for laminated timber is 3.24 mm for tensile strength L50. 2 , L80 is 3.95mm 2 , bending strength L50 is 3.27mm 2 , L80 is 4.67mm 2 Therefore, in order to satisfy the L80 JAS standard for structural laminated timber lamina, the adhesive area per unit area s must be 4.67 mm 2 It has been found that the above is preferable. [Explanation of symbols]

[0047] 10: First member 11-14: Fingers 20: Second member 21-22: Fingers L: Finger length P: Finger pitch t1: Finger tip thickness t2: Finger bottom width s: Bonding area per unit cross-sectional area b: Finger scarf θ…Scarf inclination angle 30…Main body 40...Blade part

Claims

1. The finger length L is less than 10.5 mm, more than 4 mm, the scarf inclination ratio tanθ is 1 / 10 or less, and the unit cross-sectional area in the butting direction (1 mm 2 ) The adhesive area s per 2 The finger joint is made of wood joined vertically with a finger joint having a finger length L (mm) / finger pitch P (mm) of 3.0 or more. A wood product that is any of the following: lamina for structural laminated timber, lamina for cross-laminated timber (CLT), and vertical joint material for frame construction structures.

2. 2. The wood product according to claim 1, wherein the finger length L is 8 mm or less.

3. 3. The wood product according to claim 1, wherein the finger tip thickness t1 (mm) / finger pitch P (mm) is 0.18 or less.

4. A finger joint cutter that cuts a workpiece by rotating around a rotation axis, A finger joint cutter, wherein the outer shape of a cross-sectional shape of a solid formed by rotating the blade portion around the rotation axis has a shape that is approximately complementary to the cross-sectional shape of the finger joint of any one of claims 1 to 3, the cross-sectional shape being a plane including the rotation axis.

5. The blade portion is A base material made of matrix high speed steel or cemented carbide containing, based on the total mass, 0.5% or more and 0.8% or less of C, 4% or more and 6% or less of Cr, 0% or more and 2% or less of W, 2% or more and 6% or less of Mo, 1% or more and 2% or less of V, and Fe as a main component; A hard coating containing at least Cr and N and formed on the surface by PVD; The finger joint cutter according to claim 4, comprising:

6. The method includes a finger forming step of cutting the workpiece to form the fingers using the finger joint cutter according to claim 4 or 5, The feed amount per blade is 0.5 mm or more and 1.75 mm or less. Manufacturing method for wood products.

Citation Information

Patent Citations

  • JP1991036804U

  • Finger cutter

    JP1997099404A

  • Finger cutter

    JP2003048203A