Method for measuring halogen partial pressure, and method for manufacturing reference electrode and its diaphragm

The method using a concentration cell with a halide ion conductor and sintered halide ion conductor diaphragm addresses the challenge of measuring halogen partial pressure in molten salt systems, enabling precise evaluation and reducing precious metal losses.

JP7575744B2Active Publication Date: 2024-10-30IWATE UNIVERSITY +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021111300
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-06
Filing Date
2021-07-05
Publication Date
2024-10-30
Estimated Expiration
2041-07-05

AI Technical Summary

Technical Problem

There is no direct method to measure halogen partial pressure in systems containing high-temperature melts like molten salt, which hinders effective evaluation of molten salt use as a flux for metal recycling and leads to precious metal losses.

Method used

A method using a concentration cell with a halide ion conductor as a solid electrolyte to measure halogen partial pressure, employing a reference electrode and diaphragm made of a sintered halide ion conductor body, allowing measurement of halogen partial pressure through electromotive force.

Benefits of technology

Enables accurate measurement of halogen partial pressure in molten salt systems, even in multi-component environments, facilitating the evaluation of molten salt use as a flux and reducing precious metal losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575744000006
    Figure 0007575744000006
  • Figure 0007575744000007
    Figure 0007575744000007
  • Figure 0007575744000008
    Figure 0007575744000008
Patent Text Reader

Abstract

To provide a method for measuring halogen partial pressure of a system containing a halide-based molten salt phase by an electromotive force method using a concentration cell using a halide ion conductor as a solid electrolyte, and a manufacturing method of a reference electrode of the concentration cell used therefor and a diaphragm of the halide ion conductor.SOLUTION: In a method for measuring halogen partial pressure using a concentration cell equipped with a diaphragm, a solid electrolyte composed of a sintered compact of a halide ion conductor is provided as the diaphragm between a molten salt to be measured and a reference material composed of a metal and a halide, and the halogen partial pressure determined by chemical equilibria of a plurality of chemical species or molten salt and molten metal in a molten salt phase is measured by an electromotive force method.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for measuring halogen partial pressure in a system containing a molten salt, and a method for producing a reference electrode and a diaphragm thereof used therein. [Background technology]

[0002] Molten salts are salts consisting of cations and anions such as sodium chloride in a molten state, and are melts that play an important role in smelting and recycling processes. Industrially, they are used to produce metals that cannot be electrolytically won from aqueous solutions, such as aluminum, magnesium, and rare earth metals (Non-Patent Document 1). In addition, its use as a flux for extracting unnecessary components from spent aluminum alloy scrap and its application to the treatment of spent nuclear fuel material generated from nuclear power plants are being considered (Non-Patent Documents 2 and 3).

[0003] On the other hand, in the smelting and recycling process of nonferrous metals, the input amount of waste electronic substrates has increased in recent years, and the generation of molten salts containing halides in the dry process has been confirmed. It has been pointed out that the presence of molten salts in the furnace may change the distribution behavior of precious metals, leading to losses (Non-Patent Document 4).

[0004] The molten salts used in the nonferrous smelting and recycling fields are generally multi-component melts consisting of multiple halides. To evaluate the process and minimize the loss of precious metals such as silver due to the formation of the molten salt phase, thermodynamic data on the components that make up the molten salt phase are important. In other words, it is important to clarify the conditions under which the molten salt phase becomes stable and the amount of precious metals distributed in the molten salt phase from the perspective of equilibrium theory, such as the distribution of silver between the slag phase and the molten salt phase, the slag composition, and the relationship with the partial pressures of oxygen, chlorine, and bromine in the smelting furnace. Such thermodynamic data in the melt can be obtained by measuring the distribution ratio of the target components between the molten salt and the liquid metal and the partial pressure of the halogens in the system. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Sato, N. and Waseda, Y. (Eds.), Wet Process Solutions, Solvents, and Wastewater Treatment, 4.3 Molten Salt Electrolysis, (2018 Uchida Rokakuho, Tokyo) 178-193. [Non-Patent Document 2] T. Hiraki, T. Miki, K. Nakajima, K. Matsubae, S. Nakamura, T. Nagasaka: Thermodynamic analysis for the refining ability of salt flux for aluminum recycling, Materials, 7 (2014), 5543-5553. [Non-Patent Document 3] Reiko Fujita, Hitoshi Nakamura, Koji Mizuguchi, Kazuhiro Utsunomiya: Development of electrochemical techniques for the treatment of radioactive waste generated from nuclear fuel cycle facilities [Non-Patent Document 4] Akane Kawamura, Nina Iwabuchi, Hidehiro Sekimoto, Tsutomu Yamaguchi: Partition ratio of silver between PbBr2-KCl molten salt and molten lead, Lectures on Resources and Materials Vol.2 (2015) No.2 (Autumn Matsuyama), PY-07 Summary of the Invention [Problem to be solved by the invention]

[0006] However, currently there is no method to directly measure the partial pressures of chlorine and bromine in systems in which high-temperature melts such as molten salts coexist, and it is not possible to obtain data that is useful for formulating operational guidelines to reduce the loss of precious metals or for evaluating whether molten salts can be used as fluxes for metal recycling.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for measuring a halogen partial pressure, which is determined by the chemical equilibrium between a plurality of chemical species in a halide-based molten salt phase or between a halide-based molten salt and a molten metal, by an electromotive force method using a concentration cell in which a halide ion conductor is used as a solid electrolyte, and to provide a method for manufacturing a reference electrode for the concentration cell and a diaphragm of a halide ion conductor to be used therein. [Means for solving the problem]

[0008] The method for measuring halogen partial pressure and the method for producing a reference electrode and a diaphragm thereof according to the present invention have been made in order to solve the above technical problems, and are characterized as follows.

[0009] First, the method for measuring halogen partial pressure of the present invention is a method for measuring halogen partial pressure using a concentration cell equipped with a diaphragm, characterized in that a solid electrolyte made of a sintered body of a halide ion conductor is provided as the diaphragm between the molten salt to be measured and a reference substance consisting of a metal and a halide, and the halogen partial pressure in an equilibrium state of a system containing the molten salt is measured by an electromotive force method. Secondly, in the method for measuring halogen partial pressure according to the first aspect of the present invention, it is preferable that the halogen partial pressure is a chlorine partial pressure, and the reference substance is a combination of a metal of an element whose chloride of a single oxidation number is stable, and the chloride. Thirdly, in the method for measuring a halogen partial pressure according to the first or second aspect of the present invention, it is preferable that the reference substance is any one of a combination of a metal of Ag and a chloride of AgCl, a combination of a metal of Ni and a chloride of NiCl2, or a combination of a metal of Mg and a chloride of MgCl2, and that the solid electrolyte is a solid solution of LaOCl-CaO. Fourthly, in the method for measuring halogen partial pressure according to the first aspect of the present invention, it is preferable that the halogen partial pressure is bromine partial pressure, and the reference substance is a combination of a metal of an element whose bromide of a single oxidation number is stable, and the bromide. Fifth, in the method for measuring halogen partial pressure according to the first or fourth aspect of the present invention, it is preferable that the reference substance is any one of a combination of a metal of Ag and a bromide of AgBr, a combination of a metal of Ni and a chloride of NiBr2, or a combination of a metal of Mg and a bromide of MgBr2, and the solid electrolyte is a solid solution of LaOBr-SrO. Sixthly, the reference electrode of the present invention is a reference electrode of a concentration cell used in the method for measuring halogen partial pressure of any one of the first to third inventions, characterized in that a heat-resistant tube in which a reference substance is placed and a diaphragm are bonded with a ceramic bond, and the bonded portion is covered with a glass-based sealant. Seventh, a method for producing a diaphragm of the present invention is a method for producing a diaphragm of a reference electrode used in a method for measuring a partial pressure of chlorine, and is characterized by comprising the steps of: mixing LaOCl and CaCO3 in a molar ratio of 80:20 to 95:5, adding ethanol to form a slurry, and pulverizing and mixing the slurry in a ball mill; distilling and separating the ethanol, calcining the slurry in air, and doping CaO into LaOCl; grinding and classifying the CaO-doped LaOCl, and then compression-molding the resulting mixture into pellets; and embedding the pellets in a powder of CaO-doped LaOCl having the same composition as the CaO-doped LaOCl in a crucible, and sintering the resulting mixture in an inert gas atmosphere. Eighth, a method for producing a diaphragm of the present invention is a method for producing a diaphragm of a reference electrode used in a method for measuring bromine partial pressure, comprising the steps of: mixing LaOBr and SrCO3 in a molar ratio of 80:20 to 95:5, adding ethanol to form a slurry, and grinding and mixing the slurry in a ball mill; distilling and separating the ethanol, calcining the slurry in air, and doping SrO into LaOBr; grinding and classifying the SrO-doped LaOBr, and then compression-molding the resulting mixture into pellets; and embedding the pellets in a powder of SrO-doped LaOBr having the same composition as the SrO-doped LaOBr in a crucible, and sintering the resulting mixture in an inert gas atmosphere. Ninthly, in the method for producing a diaphragm according to the seventh or eighth aspect of the present invention, it is considered preferable that the sintering temperature of the pellets is in the range of 1200 to 1400°C. Effect of the Invention

[0010] According to the method for measuring halogen partial pressure of the present invention, it is possible to provide a method for measuring halogen partial pressure in a system in which two chemical species of the same metal element but different valences are in equilibrium in a halide-based molten salt phase or in a system in which a halide-based molten salt phase and a molten metal are in equilibrium, by an electromotive force method using a concentration cell with a halide ion conductor as a solid electrolyte. In addition, by using a reference electrode of the concentration cell of the present invention and a diaphragm of a halide ion conductor obtained by the manufacturing method of the present invention, it is also possible to measure the concentration of halogen dissolved in a metal or the concentration of halide ions dissolved in a molten salt. In addition, it is possible to measure even if the molten salt is a multi-component system (a system consisting of multiple halides). [Brief description of the drawings]

[0011] [Figure 1] The sintered body was bonded to a mullite tube using ceramic bond, and AgCl was poured inside. The change in appearance after heating and holding is shown in Fig. 1. (a) shows the state immediately after bonding, (b) shows the state after 10 minutes, and (c) shows the state after 20 minutes. [Diagram 2] FIG. 2 is a schematic explanatory diagram showing a method for joining a mullite tube and a sintered body using a ceramic bond. [Diagram 3] (a) is a schematic diagram showing the bonded state of a sintered body and a mullite tube, which are bonded using a ceramic bond and coated with a glass-based sealant, and (b) is a photograph of the actual product (a). [Figure 4] This is a backscattered electron image and element map of the bonded portion and the cross section of the sintered compact after AgCl was poured into the inside of a mullite tube that was bonded to a sintered compact using a ceramic bond and coated with a glass-based sealant and then held at high temperature. [Diagram 5] FIG. 2 is a process diagram showing a manufacturing process of a LaOCl-CaO sintered body. [Figure 6] FIG. 1 is a process diagram showing a manufacturing process of a LaOBr-SrO sintered body. [Figure 7] FIG. 1 is a schematic diagram showing a chlorine concentration cell. [Figure 8]1 is a graph showing changes in electromotive force and sample temperature over time during an electromotive force measurement test. [Figure 9] 1 shows a backscattered electron image and an element map of a cross section of a sintered body after an electromotive force measurement test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The method for measuring halogen partial pressure of the present invention is characterized in that a concentration cell is used in which a solid electrolyte made of a sintered body of a halide ion conductor is provided as a diaphragm between the molten salt to be measured and a reference substance made of a metal and a halide, and the halogen partial pressure in the equilibrium state of the molten salt is measured by an electromotive force method.

[0013] The halogen partial pressure in the present invention is a value as a potential determined by the equilibrium between a chemical species and a metal in the molten salt, or between a plurality of chemical species with different valences in the molten salt. Therefore, the halogen molecules to be measured do not necessarily need to be present in the molten salt.

[0014] An example of the chlorine partial pressure determined by the equilibrium between chemical species and metals in the molten salt is the chlorine partial pressure determined by the equilibrium between lead chloride (PbCl2) and lead (Pb) shown in the following formula (1). Pb + Cl2 = PbCl2 (1)

[0015] In addition to the above-mentioned equilibrium between PbCl2 and lead (Pb), the chlorine partial pressure determined by the equilibrium between NiCl2 and Ni and the equilibrium between MgCl2 and Mg can also be mentioned.

[0016] Furthermore, an example of the chlorine partial pressure determined by the equilibrium between multiple chemical species with different oxidation numbers in a molten salt is the chlorine partial pressure determined by the equilibrium with ferrous chloride (FeCl2) and ferric chloride (FeCl3) shown in the following formula (2). 2FeCl2+Cl2=2FeCl3 (2)

[0017] Further, examples of the bromine partial pressure determined by the equilibrium between chemical species and metals in the molten salt include the equilibrium between AgBr and Ag, the equilibrium between NiBr2 and Ni, and the equilibrium between MgBr2 and Mg. Furthermore, an example of the bromine partial pressure determined by the equilibrium between a plurality of chemical species with different oxidation numbers in the molten salt is the bromine partial pressure determined by the equilibrium between ferrous bromide (FeBr2) and ferric bromide (FeBr3).

[0018] In the method for measuring halogen partial pressure of the present invention, a concentration cell is used in which a solid electrolyte made of a sintered body of a halide ion conductor is provided as a diaphragm between the molten salt to be measured and a reference substance made of a metal and a halide.

[0019] For example, in a chlorine concentration cell used to measure chlorine partial pressure, when a solid electrolyte having suitable chloride ion conductivity is used for the diaphragm, and Ag that is in equilibrium with AgCl is used as the reference electrode, a chlorine concentration cell having a structure shown in the following formula (3) can be exemplified.

[0020]

number

[0021] Here, PCl2(I) is the chlorine partial pressure of the reference electrode, and its value is determined by the equilibrium between Ag and AgCl. PCl2(II) is the chlorine partial pressure of the sample electrode. In the above formula (3), when the transference number of the chloride ion is considered to be 1, the electromotive force of this battery can be expressed as the following formula (4).

[0022]

number

[0023] In equation (4), PCl2(I) is the standard Gibbs energy of formation of AgCl, ΔG f (AgCl), so if you can measure the emf, you can determine the chlorine partial pressure logPCl2. Also, ΔV thermois a thermoelectromotive force correction term, which varies depending on the type of metal used for the electrode inserted into the molten salt and the reference material. For example, when a Mo wire is inserted into the molten salt as a lead wire and an Ag wire is used as the reference material, it is 3 to 8 mV in the temperature range of 400 to 900°C. E m is a correction term for the electromotive force generated in the diaphragm when the chloride in the reference electrode is molten, and is 20 to 30 mV when AgCl is used as the reference substance and PbCl2 is used as the sample electrode. Here, chloride ion conductors are required to have a high transport number of about 0.98 to 1, not to react with chloride-based molten salts, and to be stable even at high temperatures.

[0024] The reference electrode of the concentration cell used in the present invention is composed of a heat-resistant tube for containing a reference substance and a diaphragm made of a sintered body of a halide ion conductor provided so as to close the lower end of the heat-resistant tube. Here, the heat-resistant tube may be a dense body such as a mullite tube, a quartz tube, or a magnesia tube. On the other hand, the bonding between the end of the heat-resistant tube and the diaphragm is important from the viewpoint of the fragility and permeability of the adhesive joint.

[0025] For example, as shown in Figure 1(a), a diaphragm made of a sintered body sintered at 900°C was bonded to a mullite tube with a ceramic bond (Toagosei Co., Ltd. Aron Ceramic D type), and AgCl was placed inside and held at 600°C. After 10 minutes, the ceramic bond at the bonded part changed color from white to ochre, as shown in Figure 1(b). After 20 minutes, droplets of molten salt were observed adhering to the surface of the sintered body, as shown in Figure 1(c). This is thought to be due to the AgCl molten salt penetrating into the ceramic bond.

[0026] Therefore, in the reference electrode of the present invention, the heat-resistant tube in which the reference substance is placed and the diaphragm are bonded with a ceramic bond, and the bonded portion is further covered with a glass-based sealing material.

[0027] In order to confirm the coating effect of the glass-based sealant on the reference electrode, a ceramic bond (Aron Ceramic D type, Toagosei Co., Ltd.) was applied to one end of the mullite tube, and a diaphragm made of a sintered LaOCl-CaO solid solution was pressed onto it, as shown in Figure 2. Then, ceramic bond was applied to the side near the interface between the mullite tube and the sintered body, and a glass-based sealant (Aremco, Aremcoseal 617) was applied and coated onto the ceramic bond, the side of the sintered body, and the side of the mullite tube, as shown in the schematic diagram in Figure 3. The diaphragm was made of LaOCl-CaO solid solution sintered at 900°C.

[0028] Next, AgCl was poured into the mullite tube with the diaphragm attached, the temperature was raised to 600°C, and the temperature was maintained for a certain period of time to observe the changes in the adhesive joint. In addition, the tip of the mullite tube after the holding period was cut and embedded in epoxy resin, and the cross section was analyzed by SEM-EDS to observe the penetration of the molten salt.

[0029] FIG. 4 shows backscattered electron images and element maps of the ceramic bond, glass-based coating material, and sintered body near the interface. The dark gray particles with strong Al characteristic X-ray intensity are the particles that make up the ceramic bond, and the dark gray phase is the glass-based coating material in which Si, Na, and Ca are found. The light gray area in which La is found is the sintered body of LaOCl-CaO solid solution. From FIG. 4, it was confirmed that AgCl does not penetrate into the glass-based coating material. Furthermore, the presence of Ag was found inside the sintered body of LaOCl-CaO solid solution sintered at 900°C, and it was revealed that known sintering methods (for example, the sintering method described in Japanese Patent No. 379380) cannot be used as a diaphragm in a system containing a molten salt phase because molten salt penetrates it.

[0030] An embodiment of the method for producing a diaphragm made of a sintered body of a chloride ion conductor used in the reference electrode of the present invention will be described in detail below. Fig. 5 shows an outline of the manufacturing process of the method for producing a diaphragm made of a chloride ion conductor (LaOCl-CaO) of the present invention.

[0031] The diaphragm made of a sintered body of a chloride ion conductor is a diaphragm of a reference electrode used in a method for measuring chlorine partial pressure, and in the manufacturing method thereof, LaOCl and CaCO3 are first mixed in a predetermined molar ratio, ethanol is added to form a slurry, and the mixture is ground and mixed in a ball mill. The predetermined molar ratio of LaOCl and CaCO3 is considered to be La:Ca=80:20 to 95:5, preferably 85:15. In addition, when alumina balls are used in the grinding and mixing by the ball mill, aluminum derived from the alumina balls may be detected in the sintered body, so it is preferable to use zirconia balls.

[0032] Next, ethanol is separated by distillation, and the mixture is ground, sieved, and then calcined in air to dope CaO into LaOCl. The calcination conditions are considered to be in the range of 800°C to 1000°C and 6 hours to 12 hours. Next, the CaO-doped LaOCl is ground and classified, compressed and molded into pellets, and the pellets are embedded in powder of CaO-doped LaOCl having the same composition as the CaO-doped LaOCl in a crucible, and sintered in an inert gas atmosphere. Argon can be used as the inert gas. The sintering conditions are 1100°C to 1600°C, preferably 1200°C to 1400°C, and 12 hours to 24 hours. The diaphragm produced by the method of the present invention is a dense sintered body, and can be a diaphragm into which molten salt does not penetrate.

[0033] In the case of producing a diaphragm made of a sintered body of a bromide ion conductor used in a method for measuring bromine partial pressure, for example, when producing a diaphragm made of a LaOBr-SrO sintered body using LaOBr and SrCO3, LaOBr and SrCO3 can be weighed out so that the molar ratio of La:Sr is 80:20 to 95:5, preferably 90:10, and then the diaphragm can be produced according to the production process for the LaOBr-SrO sintered body shown in FIG. 6. EXAMPLES

[0034] Hereinafter, a method for measuring the chlorine partial pressure as the halogen partial pressure in the present invention will be described in more detail with reference to examples, although the present invention is not limited to these examples.

[0035] [Example 1] (Production of diaphragms made of sintered chloride ion conductors) According to the manufacturing process of the LaOCl-CaO sintered body of the present invention shown in Fig. 5, LaOCl and CaCO3 were mixed in a molar ratio of La:Ca = 85:15, ethanol was added to make a slurry, and the mixture was ground and mixed for 12 hours at a rotation speed of 270 rpm using zirconia balls in a ball mill stand. The ethanol was distilled off, and the mixture was calcined in air at a temperature of 800 °C for 6 hours to dope CaO into LaOCl.

[0036] Next, the CaO-doped LaOCl was ground, classified using a 300 mesh sieve, and compressed into a cylindrical pellet. This pellet was embedded in CaO-doped LaOCl powder of the same composition, and held at 1300°C for 12 hours in an argon gas inert atmosphere to obtain a sintered body. Analysis of this sintered body using XRD, SEM-EDS, and Archimedes method revealed that it was a dense sintered body consisting of a single phase of LaOCl, with La, O, Cl, and Ca distributed uniformly, and with a porosity of about 4%.

[0037] (Manufacturing of reference electrodes) A heat-resistant inorganic adhesive (Aron Ceramic D type) was applied to one end of the mullite tube, the diaphragm of the sintered body was attached, and the diaphragm was bonded by appropriate heat treatment. After this, a glass-based sealant (Alemco Seal 617) was applied to the joint, the ceramic tube, and the side of the sintered body, and the holes were sealed by appropriate heat treatment. Figure 3(b) shows a schematic diagram and a photograph after bonding.

[0038] (Measurement of chlorine partial pressure) Next, as shown in FIG. 7, the measurement system was placed in a quartz tube as PbCl2 molten salt and liquid Pb, and a reference electrode containing Ag and AgCl as reference materials was placed in the mullite tube of the reference electrode. Next, an Ag wire was immersed in the AgCl molten salt phase in the mullite tube for current flow, and an Mo wire was immersed in the AgCl molten salt phase for current flow with the metal phase on the measurement electrode side, and a chlorine concentration cell was constructed by immersing the reference electrode in the molten salt phase directly above the metal phase, and the electromotive force was measured. According to the chlorine concentration cell configured as above, since different metals are used for both electrodes, a thermoelectromotive force is generated. The temperature of the sample was measured with a K-type thermocouple installed near the sample outside the quartz tube. In this Example 1, a PbCl2 molten salt was used alone as the molten salt in the measurement system. However, the halogen partial pressure measurement method of the present invention can be applied to a multi-component molten salt, such as a mixed molten salt of PbCl2 and KCl.

[0039] FIG. 8 shows a graph of the changes in electromotive force and sample temperature over time during the electromotive force measurement test. The temperature became stable about 15 minutes after the start. It can also be seen that the electromotive force became stable after 15 minutes when the temperature became constant. The thermoelectric characteristics were measured in a preliminary experiment, and the thermoelectromotive force was corrected after the electromotive force measurement.

[0040] Figure 9 shows a backscattered electron image and elemental map of the cross section of a sintered body of CaO-doped LaOCl after it had been used in electromotive force measurements. The backscattered electron image and elemental map in Figure 9 show that this sintered body is a good dense body, and even after immersion in molten salt for about an hour, no penetration of molten salt components into the sintered body was observed. It was also confirmed that O, Cl, La, and Ca are uniformly distributed in the sample, and no second phase was precipitated. After the measurement, the E m The chlorine partial pressure calculated from the corrected electromotive force is shown in Table 1 in comparison with the literature value.

[0041] [Table 1]

[0042] Next, the chlorine partial pressure was measured by increasing the temperature from 500°C to 750°C using a system in which PbCl2 and liquid Pb coexist as the sample electrode. Below, we will use the electromotive force corrected for thermoelectromotive force, the chlorine partial pressure calculated from the electromotive force, and the liquid junction potential difference of 22 mV that occurs at the interface between AgCl and PbCl2 at 600°C to calculate E m The chlorine partial pressure calculated from the corrected electromotive force is shown in Table 2 in comparison with the literature value.

[0043] [Table 2]

[0044] From the results in Tables 1 and 2, the measured chlorine partial pressure values ​​and the literature values ​​showed good agreement, confirming that the chlorine partial pressure can be measured by the above method. m Even though the values ​​were not corrected for , the difference from the literature values ​​was within 1, and sufficient accuracy was obtained for evaluating the smelting and recycling process.

[0045] [Example 2] (Measurement of Bromine Partial Pressure) According to the manufacturing process of the SrO-LaOBr sintered body of the present invention shown in Figure 6, LaOBr and SrCO3 were mixed in a molar ratio of La:Sr = 90:10 (La / Sr = 9), and the powder of SrO-doped LaOBr was produced by holding it at a temperature of 1000 °C for 6 hours, and sintered in the same manner as in Example 1. A bromine concentration cell with the same configuration as in Example 1 was produced using the sintered body, and the bromine partial pressure of a system in which a PbBr2-based molten salt and liquid Pb are in equilibrium was measured. The electromotive force and bromine partial pressure measured by the bromine concentration cell are shown in Table 2, in comparison with the literature values.

[0046] [Table 3]

[0047] The results in Table 3 show good agreement between the measured bromine partial pressure and the literature value, confirming that the bromine partial pressure can be measured using the above method.

Claims

1. A method for measuring halogen partial pressure using a concentration cell equipped with a diaphragm, comprising the steps of: A method for measuring halogen partial pressure, comprising the steps of: providing a solid electrolyte made of a sintered body of a halide ion conductor as the diaphragm between a molten salt to be measured and a reference substance made of a metal and a halide; and measuring the halogen partial pressure in the equilibrium state of the molten salt by an electromotive force method.

2. 2. The method for measuring halogen partial pressure according to claim 1, wherein the halogen partial pressure is a chlorine partial pressure, and the reference substance is a combination of a metal of an element whose chloride of a single oxidation number is stable, and the chloride.

3. The metal of the reference material is Ag and the chloride is AgCl. The metal is Ni and the chloride is NiCl. 2 or a combination of Mg metal and MgCl 2 3. The method for measuring halogen partial pressure according to claim 1, wherein the solid electrolyte is a solid solution of LaOCl-CaO.

4. 2. The method for measuring halogen partial pressure according to claim 1, wherein the halogen partial pressure is bromine partial pressure, and the reference substance is a combination of a metal of an element whose bromide is stable in a single oxidation number, and the bromide.

5. The metal of the reference material is Ag, the bromide is AgBr, the metal is Ni, and the chloride is NiBr. 2 or a combination of Mg metal and MgBr 2 and the solid electrolyte is a solid solution of LaOBr-SrO.

6. 6. A reference electrode for a concentration cell used in the method for measuring halogen partial pressure according to any one of claims 1 to 5, characterized in that a heat-resistant tube in which a reference substance is placed and a diaphragm are bonded together with a ceramic bond, and the bonded portion is covered with a glass-based sealant.

7. A method for manufacturing a diaphragm of a reference electrode used in a method for measuring chlorine partial pressure, comprising the steps of: LaOCl and CaCO 3 a molar ratio of 80:20 to 95:5, ethanol is added to form a slurry, and the slurry is pulverized and mixed in a ball mill; A process of distilling off ethanol, grinding and classifying the product, and then calcining the product in air to dope CaO into LaOCl; grinding and classifying the CaO-doped LaOCl, and then compressing and molding it into pellets; a step of embedding the pellet in powder of CaO-doped LaOCl having the same composition as the CaO-doped LaOCl, followed by sintering in an inert gas atmosphere.

8. A method for manufacturing a diaphragm of a reference electrode used in a method for measuring bromine partial pressure, comprising the steps of: LaOBr and SrCO 3 a molar ratio of 80:20 to 95:5, ethanol is added to form a slurry, and the slurry is pulverized and mixed in a ball mill; A process of distilling off ethanol, grinding and classifying the product, and then calcining the product in air to dope SrO into LaOBr; grinding and classifying the SrO-doped LaOBr, and then compressing and molding the same into pellets; the pellet is embedded in a crucible in powder of SrO-doped LaOBr having the same composition as the SrO-doped LaOBr, and the resulting mixture is sintered in an inert gas atmosphere.

9. 9. The method for producing a diaphragm according to claim 7 or 8, characterized in that the sintering temperature of the pellets is in the range of 1200 to 1400°C.

Citation Information

Patent Citations

  • Electrode element for chloride gas detector and manufacture thereof

    JP1994273373A

  • Sensor for measuring amount of dissolved hydrogen in molten metal

    JP1996035946A

  • Chloride ion conductive solid electrolyte

    JP2003212541A

  • Solid electrolyte

    JP2003257241A

  • Hydrogen sensor

    JP2011174832A