Method for manufacturing an interposer substrate and a device using the interposer substrate
The interposer substrate with small-diameter through electrodes and fired metal powder body addresses thermal stress issues in high-current devices, enhancing durability and enabling efficient mounting of power devices.
Patent Information
- Application Number
- JP2020216194
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-12-25
AI Technical Summary
Conventional interposer substrates are not suitable for high-current and high-temperature semiconductor devices like power devices due to thermal stress and thermal cycle effects, which can cause damage or poor connections in through electrodes.
An interposer substrate with a base material having through holes and through electrodes made of a fired metal powder body, composed of gold, silver, or copper with a purity of 99.9% and a particle size of 0.005 μm to 2.0 μm, dispersed to alleviate thermal stress by forming a plurality of small-diameter through electrodes and bumps for improved durability.
The substrate provides enhanced durability against thermal cycles, allowing for system-in-packaging and three-dimensional stacked mounting of semiconductor devices, particularly power devices, with improved electrical characteristics and increased layer count.
Smart Images

Figure 0007576976000002 
Figure 0007576976000003 
Figure 0007576976000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an interposer substrate, and in particular to an interposer substrate that is useful for packaging high-output semiconductor devices such as power devices in a system-in-package or stacked packaging technique and has durability against heat stress caused by heat generation and thermal cycles of the devices. [Background technology]
[0002] In order to meet the demand for miniaturization and high integration of semiconductor devices, 2.5-dimensional packaging using interposer substrates has been put into practical use as a packaging technology for semiconductor chips. In this packaging method, semiconductor chips and circuit boards are connected in the thickness direction via the interposer substrate, achieving high integration of semiconductor chips and high-speed transmission of signals between chips.
[0003] An interposer substrate is an intermediate substrate in which through electrodes are formed in a base material such as silicon or glass at positions corresponding to the connection parts of the bumps of a semiconductor chip. The through electrodes of the interposer substrate are manufactured by forming a conductor inside a through hole formed in the base material. Known types of through electrodes include those in which the through hole is filled with a conductive metal such as copper (Cu) by plating (via filling), and those in which the inner surface of the hole is coated with a conductive metal film without filling the entire hole.
[0004] Meanwhile, the range of semiconductor devices that require miniaturization and high integration continues to expand, and the demand for high current, high load semiconductor devices such as power devices and LED devices is also growing. In recent years, the demand for power devices and the like has increased against the backdrop of the spread of EVs, PHEVs, HEVs and their quick chargers in the automotive field, and the spread of photovoltaic power generation systems and mega solar systems in the energy field, and the demand for miniaturization and high integration of these devices is also growing. Therefore, application of the above-mentioned mounting technology using interposer substrates is considered as a response to the miniaturization of power devices and the like. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-342888 A [Patent Document 2] JP 2000-151060 A [Patent Document 3] JP 2000-228566 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the above-mentioned mounting technology using interposer substrates has been mainly applied to semiconductor devices that are driven by relatively low current and generate little heat, such as memory (stack memory) and PCs for servers and graphics. And, there are many negative views on the applicability of interposer substrates to power devices. This is because semiconductor devices for power conversion and control, such as power devices, tend to be driven by large currents and have high operating temperatures. In particular, it is predicted that the thermal cycle caused by turning the device on and off will have a large impact on the interposer substrate. In semiconductor devices, the bonded members such as semiconductor chips and the base material and through electrodes that make up the interposer substrate have different thermal conductivities and thermal expansion coefficients. And, the thermal stress caused by these differences may cause damage to the through electrodes or cause connection failures. It is predicted that the impact will be particularly large in semiconductor devices that generate a large amount of heat, such as power devices. Therefore, there have been few reports of the application of interposer substrates that can be used with power devices, and the mounting method has had to rely on conventional surface mounting.
[0007] Therefore, the present invention aims to provide an interposer substrate that enables system-in-packaging and three-dimensional stacking mounting of semiconductor devices, particularly active devices such as power devices, and has excellent durability under high temperatures and severe thermal cycle conditions. Also disclosed is a device manufacturing method that applies the mounting method using this interposer substrate. [Means for solving the problem]
[0008] The present invention, which solves the above-mentioned problems, provides an interposer substrate that is bonded in an overlapping state to one or more bonded members having one or more connection parts and is electrically connected to the bonded members, the interposer substrate comprising a base material having one or more connection regions corresponding to the connection parts of the bonded members, the base material having a plurality of through holes formed in the connection regions thereof, the plurality of through holes being formed adjacent to one another to form a segment that serves as one unit for the connection, one or more of the segments being formed within the connection regions, the through holes each having a through electrode penetrating the through hole, and a bump formed at at least one end of the through electrode and having a cross-sectional shape wider than the through electrode, the through electrode and the bump each being made of a metal powder sintered body obtained by sintering one or more metal powders selected from gold, silver, and copper having a purity of 99.9% by mass or more and an average particle size of 0.005 μm to 2.0 μm.
[0009] The present inventors have imparted durability to the interposer substrate by suppressing the effect of thermal stress on the through electrodes caused by the thermal cycle of the semiconductor device using two means. As a first means, in the present invention, the through electrodes are composed of a plurality of small-diameter through electrodes. In a conventional interposer substrate, one or a plurality of through electrodes are formed according to the structure, area, etc. of the connection part of the joined member such as a semiconductor element. In the present invention, the one through electrode in the conventional technology is referred to as one unit of electrical connection. In the interposer substrate in the present invention, a plurality of small-diameter through electrodes are set and constitute one unit of electrical connection. In other words, in the conventional technology, one unit of electrical connection is constituted by one through electrode, but in the present invention, a plurality of through electrodes constitute one unit of electrical connection. By distributing the through electrodes in this way, the thermal stress is divided and the effect of the thermal stress is alleviated.
[0010] The second means for improving the durability of the interposer substrate in the present invention is to improve the constituent material of the through electrode. In conventional interposer substrates, the through electrode is generally formed by plating or the like. Metal formed by plating or the like is dense and bulky and hard, and may break due to repeated stress. In the present invention, the through electrode is formed from a sintered body of metal powder with a specified particle size and purity. The sintered body of metal powder is a material with a different material structure and organization from bulk metal, has flexibility, and is thought to have an effect of relaxing stress caused by thermal cycles. In this way, in the present invention, durability against thermal cycles is imparted from the structural aspect of the through electrode.
[0011] The configuration of the interposer substrate according to the present invention, its manufacturing method, and mounting technology to which the interposer substrate according to the present invention is applied are described below. The basic configuration of the interposer substrate according to the present invention is a base material, through holes and through electrodes formed in the base material, and bumps. To facilitate understanding of the following description, Fig. 1 and Fig. 2 show an example of the interposer substrate according to the present invention and an example of the state in which the interposer substrate is bonded to a bonded member (such as a power module).
[0012] A. Interposer substrate according to the present invention (I) Joining object (joined parts) The interposer substrate according to the present invention is bonded to one or more bonded members and electrically connected to the bonded members. The bonded members are semiconductor elements, integrated circuits, power modules, multi-chip modules, circuit boards, etc. that constitute a semiconductor device. When bonding to one bonded member, the bonded member is placed on one of the surfaces of the interposer substrate and bonded. When bonding to two or more bonded members, the interposer substrate is sandwiched between a pair of bonded members and bonded. At this time, electrical connection between the bonded members is possible via the interposer substrate. Also, multiple bonded members may be bonded to one surface of the interposer substrate.
[0013] The members to be joined have one or more connection parts for electrical connection (see Fig. 1). A connection part is a conductor for electrical connection such as an electrode, electrode pad (bump), wiring, or terminal that is set and formed on the members to be joined, such as a semiconductor element, an integrated circuit, a multi-chip module, or a circuit board, and its shape and dimensions are not particularly limited.
[0014] (II) Base material The substrate is a main component of the interposer substrate on which one or more bonded members are mounted three-dimensionally. The substrate has connection areas set on its surface at positions corresponding to the connection parts of the bonded members described above (see FIG. 1). The connection areas on the substrate are designed to overlap the connection parts of the bonded members when the substrate and the bonded members are superimposed during mounting (see FIG. 2). This connection area includes one or more segments each composed of a plurality of through holes, which will be described later. The bonding area is an area virtually set on the substrate, and does not need to be defined by lines or irregularities that can be visually recognized and understood in the appearance of the substrate. This bonding area may be a virtual area for determining the arrangement of segments (through holes and through electrodes) in the design of the interposer substrate.
[0015] The constituent material of the substrate is silicon with an oxide film, glass, ceramic, resin, etc., as in the case of conventional interposer substrates. The substrate may be composed of a single layer, or may have a structure in which multiple layers are laminated. In addition, the substrate may contain passive elements, logic circuits, and analog circuits in addition to the first and second bonded members.
[0016] (III) Through hole A plurality of through holes are formed in the bonding area of the base material (see FIG. 1). In a conventional interposer substrate, one through hole is formed for one unit of electrical connection with the connection part of the bonded member, whereas in the interposer substrate of the present invention, one unit of electrical connection is formed by a plurality of through electrodes provided in a plurality of small diameter through holes. As described above, this is to disperse and alleviate thermal stress by the plurality of through electrodes. In the present invention, a set of a plurality of through holes and through electrodes forming one unit of electrical connection is called a segment. One or more segments are formed in the bonding area of the base material, and one or more segments are bonded to one connection part of the bonded member. The number and arrangement pattern of the segments formed in one bonding area are not particularly limited and can be set arbitrarily. The number and arrangement pattern of the through holes (through electrodes) formed in one segment can also be set arbitrarily.
[0017] The diameter of the through hole is preferably 10 μm or more and 100 μm or less. This diameter can be said to be sufficiently fine considering that the diameter of the through hole in a conventional general interposer substrate is 200 μm or more. Furthermore, the number of through holes (through electrodes) formed in one segment is not particularly specified. It can be set arbitrarily based on the bonding area required for the connection part of the joined members and the area of the through hole. Furthermore, although a plurality of through holes are mutually adjacent to form a segment, the interval between the through holes in one segment is not particularly limited as long as it is shorter than the distance between adjacent segments.
[0018] (IV) Through electrode A through electrode is formed inside the through hole (see FIG. 2). This through electrode is formed from a metal powder sintered body obtained by sintering one or more metal powders selected from gold, silver, and copper, which have a purity of 99.9% by mass or more and an average particle size of 0.005 μm to 2.0 μm. The through electrode formed from the metal powder sintered body of the present invention is a molded body formed by tightly bonding minute metal powders while plastically deforming, and effectively acts as an electrode. Although the metal powder sintered body is relatively dense, it has minute pores, so that it can relieve the applied stress. Therefore, compared with a through electrode made of a completely bulk-like metal, it has flexibility and durability against thermal stress. In the present invention, durability against thermal stress is ensured by the setting of the above-mentioned multiple minute through electrodes and the structure of the through electrodes.
[0019] The purity and particle size of the metal powder forming the metal powder sintered body are set within the above ranges because low purity of the powder increases the hardness of the powder, and the powder deformation and recrystallization during the formation of the sintered body are difficult to proceed, resulting in a decrease in density. In addition, with respect to particle size, powder with a coarse particle size will have a decrease in density after sintering. The through electrode in the present invention aims to relieve stress by forming a porous structure having pores, but denseness is necessary. If the pores of the through electrode become coarse and the denseness is poor, not only will the conductivity decrease, but there is also a risk of an insufficient strength. In order to obtain a metal powder sintered body having a stress relaxation effect while ensuring the strength and conductivity required for a through electrode, the purity and average particle size of the metal powder described above are necessary. In addition, the metal species of the metal powder, which is the constituent metal of the electrode, are gold, silver, and copper because these metals are suitable as electrode materials and have good plastic deformability when formed into a sintered body.
[0020] As described above, the metal powder sintered body constituting the through electrode of the present invention has appropriate pores to obtain a stress relaxation effect while ensuring strength. As a specific standard, the porosity (void ratio) of the metal powder sintered body is preferably 7% or more and 35% or less. This porosity is defined as the area ratio of pores in the through electrode in an arbitrary cross section. It can be measured, for example, by observing an arbitrary cross section of the through electrode with a microscope or an electron microscope, and measuring the area ratio of the pore portion in the observation area based on the captured photograph. In measuring the area ratio, software for image analysis can be used as appropriate.
[0021] (V) Bump at the end of the through electrode In the present invention, at least one end of the through electrode is provided with a bump made of a sintered metal powder that is wider than the through electrode (see FIG. 2). The bump is a connection member for achieving a stable electrical connection with the joined member, such as a semiconductor chip, an integrated circuit, a power module, or a multi-chip module. Furthermore, the sintered metal powder becomes dense when pressurized and heated, and has the effect of joining to the contacting material while diffusing the metal elements. In other words, the bump also functions as a joining material that joins the interposer substrate and the joined member.
[0022] The bump is made of a sintered metal powder made of the same metal as the through electrode. By using the same metal as the through electrode, mutual distortion (thermal distortion) is prevented when the bump and the member to be joined are joined. The particle size and purity of the metal powder of the sintered metal powder making up the bump are the same as those of the through electrode. The porosity of the bump is preferably 7% or more and 35% or less, the same as that of the through electrode.
[0023] As described later, the bumps and through electrodes are formed by firing a metal paste containing metal powder. Here, the range of firing temperatures that can be set for forming the bumps is preferably lower than the range of firing temperatures that can be set for forming the through electrodes. This is because the function of the bumps as a bonding material is taken into consideration. In firing the metal paste, the firing temperature is set to a high temperature, which promotes contact between the metal powders and bonding and growth of the pores. In firing at a low temperature, the pores do not grow and are maintained in a small state. In order to ensure the bonding of the bumps, especially the bonding at a relatively low temperature, it is preferable to make the pore diameter small and increase the number of contact points between the metal powders. Therefore, the firing temperature of the bumps is set to a relatively low temperature to ensure low-temperature bonding. Therefore, the material structure of the bumps and the material structure of the through electrodes may differ in terms of the pore diameter and the state of the metal powder. In addition, the preferred range of the porosity of the bumps is the same as that of the through electrodes, but the porosity of the bumps and the porosity of the through electrodes may differ depending on the manufacturing method of the interposer substrate.
[0024] The appearance of the bump and through electrode in the present invention will be described with reference to FIG. 3. The bump needs to be wider than the through electrode at the surface in contact with the through electrode. The through electrode has a porous structure with fine pores. When joining the member to be joined and the interposer substrate, it is preferable to make the bump width larger than the end diameter of the through electrode in order to transmit the load evenly to the entire end face of the through electrode. Note that the width of the through electrode and bump here is determined with respect to the cross-sectional shape in the vertical direction to the substrate. The cross-sectional area of the bump (the horizontal cross-sectional area at the boundary surface between the through electrode and the bump) is preferably 1.2 to 9 times the horizontal cross-sectional area of the end of the through electrode.
[0025] There are no particular limitations on the vertical and horizontal shapes of the bump. In vertical cross section, it may be a square with a uniform width, or a trapezoid, inverted trapezoid, or arc shape with a variable width. In planar cross section, it may be a circle, or may be another shape.
[0026] (VI) Segment A segment is formed by gathering a plurality of through electrodes having the through holes and bumps described above. The arrangement pattern of the through holes (through electrodes) formed in one segment can be set arbitrarily. Figure 4(a) shows an example of the arrangement pattern of the through holes in one segment. As shown in Figure 4(a), the through holes can be arranged so that the outline of the through holes roughly describes a figure such as a circle or a polygon, or a linear shape (straight line, curve, spiral). In addition, since the multiple through electrodes and bumps that make up the segment form one unit of electrical connection, adjacent bumps may be connected (Figure 4(b)).
[0027] (VII) Other optional configurations (VII-1) Metallized film When forming the above-mentioned bump, it is preferable to form a metallized film made of metal on the region of the substrate surface where the substrate and the bump contact each other. As described above, the sintered metal powder constituting the bump acts as a bonding material for bonding the substrate and the member to be bonded. This bonding action occurs due to contact of the metal powder by pressure and heat and diffusion of the metal element at the contact portion. By forming a metallized film on the contact surface between the substrate and the bump, high adhesion occurs due to thermal diffusion at the bonding interface between the sintered metal powder and the metallized film, and the bonding action can be enhanced. In addition, the metallized film also has the effect of suppressing diffusion of the constituent metal of the bump (gold, etc.) to the substrate, and when there is a base film described later, the effect of suppressing diffusion of the constituent metal of the base film (titanium, etc.) to the bump. In consideration of these effects, the metallized film may be formed by forming two or more layers of metal films made of different metals.
[0028] The metallized film is preferably made of any of gold, silver, copper, palladium, platinum, and nickel with a purity of 99.9% by mass or more. The reason why the metallized film has a metal purity of 99.9% by mass or more is that impurities in a metal with a low purity may become an oxide film and diffuse to the metallized film surface, hindering bonding. The metallized film is more preferably made of a metal of the same material as the metal powder constituting the bump and the through electrode. In addition, the thickness of the single-layer or multi-layer metallized film is preferably 10 nm to 1000 nm.
[0029] The metallization film is preferably made of a bulk metal to ensure adhesion to the bumps, and is preferably formed by plating (electrolytic plating, electroless plating), sputtering, vapor deposition, CVD, or the like. The metallization film may consist of only one layer, but may have a multi-layer structure. For example, a platinum film may be formed on the substrate side, and a gold film may be formed on top of that (on the bump side). In the case of a multi-layer structure, the metallization film on the bump side is preferably formed of the same material as the metal of the metal powder that constitutes the through electrode.
[0030] The metallized film may be formed directly on the substrate, or may be formed via an undercoat film. The undercoat film is formed to improve the adhesion between the metallized film and the substrate. The undercoat film is preferably made of titanium, chromium, tungsten, a titanium-tungsten alloy, or nickel. The undercoat film is also preferably formed by plating, sputtering, vapor deposition, CVD, or the like, and is preferably 10 nm to 1000 nm thick.
[0031] The metallized film and the undercoat film may be formed at least on the contact surface between the bump and the substrate. As described above, the metallized film is intended to enhance the bonding between the bump and the substrate. However, the metallized film may be formed over a wide area beyond the contact surface between the bump and the substrate, except for the area where electrical insulation is required. For example, the metallized film may be formed in the area that will become the segment. The metallized film and the undercoat film may also be formed on the inner surface of the through hole. As described above, these metal thin films may be formed by sputtering or CVD, and may be formed on the inner surface of the through hole at the same time as forming the film on the contact surface with the bump. Even when the metallized film and the undercoat film are formed in an area other than the contact surface between the bump and the substrate, the thickness of each metal film is within the range described above. The thickness of the metallized film and the undercoat film can be confirmed and measured by observing the cross section of the interposer substrate with a microscope (SEM, etc.).
[0032] (VII-2) Gap between the through electrode and the inner surface of the through hole The through electrode and the inner surface of the through hole may be in close contact with each other, but there may be a gap between the inner surface of the through hole and the through electrode (see FIG. 3). The gap may mitigate the effect of the difference in thermal expansion coefficient between the substrate and the through electrode. Specifically, it is permitted to have a gap of 1 / 1000 to 1 / 10 of the diameter of the through hole. The gap does not need to be completely constant along the length of the through hole, and it is sufficient that the gap is within the above range. In this case, the inner surface of the through hole is the outermost surface of the inside of the through hole, and if a metal film is formed on the inner wall of the through hole, the distance between the surface of the metal film and the through electrode must be within the above range. In addition, the hole diameter is the diameter of the through hole itself, and does not include the thickness of a metallized film or a base film formed on the inner wall of the through hole.
[0033] B. Manufacturing method of interposer substrate according to the present invention Next, a method for manufacturing an interposer substrate according to the present invention will be described. As described above, the interposer substrate according to the present invention is characterized in that a plurality of through electrodes are formed for one electrical connection, and that the constituent material of the through electrodes and the bumps at their ends is a sintered body of metal powder. In this respect, the method for forming the through holes is the same as the method for forming the through holes of conventional interposer substrates. In other words, the method for manufacturing an interposer substrate according to the present invention is characterized by the method for forming the through electrodes and bumps. Other steps are basically the same as those of a normal interposer substrate.
[0034] The through electrode formation process involves applying and filling a metal paste containing metal powder onto a substrate having through holes, and then drying and firing the metal powder paste. In addition, to form bumps at the ends of the through electrodes, a metal paste is applied to the end faces of the through electrodes simultaneously with or after the formation of the through electrodes, and the metal powder paste is dried and fired. In the following explanation, the composition of the metal paste is explained, and then a specific method for manufacturing an interposer substrate to which the metal paste is applied is explained.
[0035] (1) Composition of metal paste for through-hole and bump formation The metal paste for forming the through electrodes and bumps is basically composed of one or more metal powders selected from gold, silver, and copper, which have a purity of 99.9% by mass or more and an average particle size of 0.005 μm to 2.0 μm, and an organic solvent. The purity of the metal powder is set to 99.9% or more, as described above, in consideration of the deformability and sinterability when the powder is fired, as well as ensuring electrical conductivity. The average particle size of the metal powder is set to 0.005 μm to 2.0 μm because metal powders with a particle size exceeding 2.0 μm have a large distance between large metal powder particles when filled into minute through holes, making it difficult to ensure the final required electrical conductivity. In addition, if the distance between the metal powder particles is large, it is difficult to ensure the bonding strength. On the other hand, metal powders with a particle size of less than 0.005 μm aggregate in the paste and are difficult to disperse, and the shrinkage rate during firing is large, making it difficult to fill the through holes. In the present invention, the average particle size of a metal powder can be obtained by calculating the 50% cumulative particle size in the particle size distribution measured by a laser diffraction / scattering method, or by observing multiple metal powders under a microscope (SEM) and calculating the average particle size measured by a biaxial method.
[0036] As the organic solvent used in the metal paste, ester alcohol, terpineol, pine oil, butyl carbitol acetate, butyl carbitol, carbitol, perchlorate, and menthanol are preferable. These solvents are less aggressive to the resist and can be volatilized at relatively low temperatures (less than 50°C), making it easy to dry the metal paste after application. In particular, perchlorate is particularly preferable because it can be dried at room temperature.
[0037] The mixing ratio of the metal powder and the organic solvent in the metal paste is preferably 60 to 99% by mass of the metal powder and 1 to 20% by mass of the organic solvent. The reason for this ratio is to prevent the aggregation of the metal powder and to supply enough metal powder to form the electrode. The mixing ratio of the metal powder affects the volume difference of the through electrode before and after firing. The above-mentioned gap between the inner surface of the through hole and the through electrode affects the mixing ratio of the metal powder in the metal paste and the firing conditions. In order to form a suitable gap, the mixing ratio of the metal powder is more preferably 70 to 98% by mass.
[0038] The metal paste used in the present invention may contain an additive. The additive may be one or more selected from acrylic resins, cellulose resins, and alkyd resins. For example, the acrylic resin may be methyl methacrylate polymer, the cellulose resin may be ethyl cellulose, and the alkyd resin may be phthalic anhydride resin. These additives have the effect of suppressing the aggregation of metal powder in the metal paste, and make the metal paste homogeneous. The amount of additive added is preferably 2% by mass or less relative to the metal paste. The metal powder content can be kept within a range sufficient for filling the through holes while maintaining a stable aggregation suppression effect.
[0039] However, the metal paste used in the present invention is different from general metal pastes widely used for forming wiring electrodes and wiring patterns on the surface of a substrate, and does not contain glass frit. The reason why glass frit is not mixed into the metal paste is to form a dense through electrode and not to leave impurities that may inhibit recrystallization in the electrode. In addition, components other than the metal powder, such as the organic solvent that constitutes the metal paste and the above-mentioned additives that are added arbitrarily, disappear during the drying and firing process after filling, so they do not become an inhibiting factor like glass frit.
[0040] (2) A manufacturing method of the interposer substrate according to the present invention using a metal paste Here, two specific and preferred embodiments of the manufacturing process for the interposer substrate using the above-mentioned metal paste will be described.
[0041] (2-1) First aspect of the method for manufacturing an interposer substrate according to the present invention In this manufacturing process, after the through holes are formed (drilled) in the substrate, the through electrodes and the bumps are formed at the same time. Figures 5(a) to 5(e) are diagrams for explaining the outline of this manufacturing process. This process will be explained together with the preferable application method and firing conditions of the above-mentioned metal paste.
[0042] (a) Forming through holes in a substrate A bonding region and a segment are set for the substrate, and a plurality of through holes are formed for each segment. As in the case of conventional interposer substrates, the through holes can be formed by laser processing, dry etching, wet etching, ultrasonic processing, drilling, sandblasting, or the like. In the present invention, since it is necessary to form a plurality of minute through holes close to each other in a substrate made of silicon or glass, laser processing, dry etching, and wet etching are preferred. In addition, when a silicon substrate is used as the substrate, it is preferred to form an insulating layer such as a thermal oxide film after the through holes are formed.
[0043] (b) Mask pattern formation for bump formation After the through-holes are formed, a metallized film is formed on the substrate as necessary. The metallized film can be formed by plating, sputtering, vapor deposition, CVD, etc. At this stage, a metal film may be formed on the inner wall of the through-holes as well as on the substrate surface.
[0044] In this first embodiment, a pattern is formed by masking for bump formation. The mask pattern is preferably formed by applying a photosensitive masking material such as a photosensitive film or photoresist, followed by photoetching.
[0045] (c) Metal paste application Next, the metal paste containing the above-mentioned metal powder is applied onto the substrate, and the metal paste is filled into the inside of the through-hole and the recesses corresponding to the bumps of the mask pattern. The metal paste is applied by supplying an appropriate amount of the metal paste onto the substrate. Methods of applying the paste by spin coating, screen printing, inkjet, etc., and methods of supplying an appropriate amount of the metal paste and then spreading it with a spatula, etc., can be applied. In addition, in order to suitably fill the through-hole, mechanical vibrations of a predetermined frequency may be applied to the metal paste after supplying an appropriate amount of the metal paste. The metal paste applied in the present invention is basically in the form of only metal powder dispersed in an organic solvent, and may have poor fluidity. Therefore, in order to fill the through-hole with the metal paste without gaps, it is preferable to apply mechanical vibrations. The frequency of the mechanical vibrations applied to the metal paste is preferably 60 Hz to 300 kHz. Vibrations within this range can improve the fluidity of the metal paste.
[0046] A specific method for applying the metal paste while applying mechanical vibrations is to spread the metal paste over the entire substrate while contacting the metal paste with a blade (spatula) vibrated at the above frequency after or while supplying the metal paste to the substrate. By applying mechanical vibrations directly to the metal paste, the metal powder in the metal paste is subjected to vibrations, improving the fluidity.
[0047] Furthermore, as a more preferred embodiment for completely penetrating the metal paste into the through-hole, the pressure in the through-hole may be reduced. As a method for reducing the pressure in the through-hole, it is preferable to carry out the coating in a reduced pressure chamber or to reduce the pressure on the back surface of the substrate (opposite the surface to which the metal paste is coated), and it is preferable to make the pressure inside the through-hole -10 kPa to -90 kPa. By mechanically vibrating the metal paste and reducing the pressure in the through-hole, the metal paste can be sufficiently filled into the through-hole.
[0048] (d) Sintering of metal powder After applying the metal paste, the metal paste can be dried as desired. If firing is performed immediately after applying and filling the metal paste, voids may be generated due to the sudden generation of gas caused by the evaporation of the organic solvent, which may affect the shape of the fired body. In addition, by drying once, the metal powder in the through holes can be temporarily fixed. When drying is performed, the drying temperature is preferably less than 80°C, but room temperature is also possible.
[0049] The heating temperature when firing the metal paste is preferably 80°C or more and 100°C or less. The reason for setting such a temperature range is that the firing of the metal powder does not proceed at temperatures below 80°C, and it is not possible to form a through electrode and a bump having a certain degree of density. The firing step of the first embodiment is a step of simultaneously firing the through electrode and the bump. If the firing temperature in this firing step is set to more than 100°C, the above-mentioned growth of pores occurs in the fired body that will become the bump, and the bonding property is impaired. In addition, there is a concern that high-temperature firing may damage the mask pattern such as the resist. In consideration of these, the upper limit of the firing temperature in the first embodiment is set to 100°C. The firing time in this firing step is preferably set to more than 10 minutes and less than 2 hours.
[0050] (e) Other processes The metal powder is fired and solidified by the firing process described above, forming the through electrodes and bumps. The mask pattern is then removed to form the basic form of the interposer substrate. If the bumps are formed on only one side, a metallized film may be formed on the other side. The manufactured interposer substrate may also be subjected to a hermetic sealing process using a resin or the like.
[0051] (2-2) Second aspect of the method for manufacturing an interposer substrate according to the present invention In this manufacturing process, the formation of the through electrodes and the formation of the bumps are performed separately. Therefore, the firing process of the metal paste is performed twice. Figures 6(a) to 6(e) are diagrams for explaining the outline of this manufacturing process. Each step will be explained below.
[0052] (a) Forming through holes in a substrate In the second embodiment, the through holes are formed in the substrate first, and then a metallized film is formed as necessary. Suitable steps for the method of forming the through holes are the same as those in the first embodiment.
[0053] (b) Coating and firing of metal paste (first firing process) In this second process, after forming through holes and, if necessary, an insulating layer in the substrate, a metal paste is applied onto the substrate and the through holes are filled with the metal paste. In addition, when forming a metallized film on the substrate, a film formation process is performed before applying the metal paste. The method of applying the metal paste and the preferred specific conditions are the same as those in the first embodiment.
[0054] Then, after filling the through hole with the metal paste, firing is performed to form the through electrode. In this second embodiment, firing is performed for each of the through electrode formation and the bump formation, and this firing process is the first firing process. The firing temperature of the metal powder in this first firing process may be in the same temperature range (80°C to 100°C) as in the first embodiment, but firing at a higher temperature is also possible. In the second embodiment, the through electrode and the bump are manufactured separately, and only the through electrode is fired in the first firing process, so there is no need to consider the deterioration of the bonding property of the bump. In addition, since there is no mask pattern made of resist or the like on the base material at this stage, there is no need to consider the damage. Therefore, the firing temperature in the first firing process can be relatively high. Specifically, the firing temperature can be set to 100°C or higher and 300°C or lower. By setting the firing temperature to a high temperature in this manner, the firing of the metal powder can proceed to a deeper depth, and a through electrode with strength can be formed.
[0055] (c) Bump formation (mask pattern formation and metal paste filling) After the through electrodes are formed, bumps are formed on them. After patterning with a resist or the like on the substrate on which the through electrodes are formed in the same manner as in the first embodiment, a metal paste is applied. In this case, the metal paste can also be applied under reduced pressure or with mechanical vibration.
[0056] (d) Firing the bumps (second firing step) After applying the metal paste to the mask pattern, it is dried appropriately and a second firing step is performed to form bumps. As described above, in firing the bumps, firing at a relatively low temperature is preferable to ensure bonding (low-temperature bonding). Therefore, the firing temperature in this second firing step is preferably 80°C or higher and 100°C or lower, the same as the firing temperature of the bumps in the first embodiment. The firing time is preferably the same as in the first embodiment.
[0057] (e) Other processes The above steps result in the metal powder of the bumps being sintered. The mask pattern is then removed to provide the basic form of the interposer substrate. In this embodiment as well, a metallized film can be formed on one side of the substrate and a hermetic sealing process can be performed.
[0058] C. A method for manufacturing a semiconductor device using an interposer substrate according to the present invention The interposer substrate according to the present invention described above is suitable for manufacturing a semiconductor device using a semiconductor element, an integrated circuit, a multi-chip module, a circuit board, etc. as a bonded member. That is, the manufacturing method of this semiconductor device is a device manufacturing method including a step of overlapping and bonding one or more bonded members having one or more connection parts and one or more interposer substrates to electrically connect the bonded members and the interposer substrate, and includes a step of using the interposer substrate described above as the interposer substrate, overlapping the interposer substrate and the bonded members, pressurizing the interposer substrate and / or the bonded members from one or both directions at 1 MPa or more and 50 MPa or less, and heating the interposer substrate and the bonded members at 150°C or more and 250°C or less to electrically connect the interposer substrate and the bonded members.
[0059] The sintered metal powder constituting the bump of the interposer substrate according to the present invention is sintered by contact between the metal powders and diffusion of the metal elements when pressurized and heated, and is bonded to the contacting material by adhesion. This sintering and bonding of the metal powder is particularly effective in the outer periphery of the bump, which is preferentially compressed when pressurized. This bonding establishes an electrical connection between the connection part of the bonded member and the bump of the interposer substrate.
[0060] As described above, the conditions for pressure and heat during bonding are 1 MPa to 50 MPa and 150°C to 250°C. If the pressure is less than 1 MPa or less than 150°C, the sintered metal powder body is less likely to be sintered, the adhesion is poor, and the bonding strength may be insufficient. On the other hand, if pressure and heat are applied at more than 50 MPa or more than 250°C, there is a concern that mechanical and thermal damage may occur in the semiconductor element or the like that is the member to be bonded. The time required for this bonding process is preferably 1 minute to 60 minutes. The pressure in the above conditions refers to the pressure applied to all bumps formed on the interposer substrate and pressed in the bonding process. In other words, the area used as the basis for setting the pressure is the total area of the bumps to be pressed.
[0061] Through the above bonding process, the sintered metal powder that constitutes the bump is sufficiently compressed and deformed, and the interposer substrate and the member to be bonded are bonded. The bonding may be completed in this state, but in order to obtain stronger bonding strength, a post-heat treatment (post-sintering) may be performed to heat the bump after the bonding process. Post-sintering is a process that mainly aims to additionally sinter the metal powder. This process can substantially eliminate the pores in the bump, making it even more dense.
[0062] The heating temperature when performing post-sintering is preferably 100°C or more and 250°C or less. If it is less than 100°C, progress of sintering and densification cannot be expected. If it exceeds 250°C, there is a concern that the device may be damaged, and sintering may progress excessively, resulting in an excessively hard bump. The heating time for post-sintering is preferably 10 minutes or more and 120 minutes or less. Post-sintering may be performed without pressure or under pressure. If pressure is applied, it is preferable that the pressure is 10 MPa or less.
[0063] Post-sintering has the advantage of shortening the processing time in the bonding process in addition to improving the bonding strength between the bump and the bonded member. A certain amount of time is required for heating to sinter the metal powder in the bonding process. Pressure is also applied at the same time in the bonding process, but this does not require much time. If post-sintering is planned, pressure can be given priority in the bonding process and processed in a short time, and even if there is a shortage of heating, this can be compensated for.
[0064] Through the above bonding method and the optional post-sintering step, the interposer substrate and the member to be bonded can be firmly bonded, and an electrical connection is also established at the same time. Effect of the Invention
[0065] As described above, the interposer substrate according to the present invention has a plurality of small-diameter through electrodes made of sintered metal powder, which disperses and relieves thermal stress and improves durability. The present invention is particularly applicable to the mounting of semiconductor devices such as power devices that generate a lot of heat. Furthermore, the substrate configuration can be multi-layered and the wiring length of the elements can be shortened, allowing the electrical characteristics of the semiconductor elements to be effectively exhibited. [Brief description of the drawings]
[0066] [Figure 1] 1A and 1B are diagrams illustrating an example of an interposer substrate and a member to be joined according to the present invention. [Diagram 2] The interposer substrate is bonded to the bonded component (power module, etc.) [Diagram 3] 4A to 4C are diagrams illustrating the periphery of an end portion of a through electrode and the state of a bump of an interposer substrate according to the present invention. [Figure 4] 4A to 4C are diagrams showing examples of arrangement patterns of through holes and through electrodes and examples of other aspects of bumps in one segment of an interposer substrate according to the present invention. [Diagram 5] 1A to 1C are diagrams for explaining an outline of a first embodiment of a method for manufacturing an interposer substrate according to the present invention. [Figure 6] 5A to 5C are diagrams for explaining an outline of a second embodiment of the method for manufacturing an interposer substrate according to the present invention. [Figure 7] 4A to 4C are diagrams showing the arrangement pattern of segments and through holes of an interposer substrate manufactured in this embodiment. [Figure 8] 4 is a photograph of the cross-sectional structure of the through electrodes and bumps of the interposer substrate manufactured in this embodiment. [Figure 9] 13 is an enlarged photograph of the vicinity of the boundary between the inner surface of a through hole and a through electrode of an interposer substrate manufactured in this embodiment. [Figure 10] Photographs of the surfaces of the interposer substrate and semiconductor chip after thermal cycle testing. [Figure 11] An enlarged photograph of one segment of the surface of the interposer substrate and semiconductor chip after shear strength was measured following thermal cycle loading. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0067] First embodiment A preferred embodiment of the present invention will be described below. In this embodiment, a metal paste using gold powder as the metal powder was prepared, and an interposer substrate was manufactured based on the above-mentioned second embodiment (FIG. 6). Then, an evaluation test of the bonding strength of a semiconductor chip using this interposer substrate was performed.
[0068] First, a Si wafer (dimensions: 4 inches, thickness: 300 μm) was prepared as a substrate, and through-holes were formed in a predetermined pattern (see Fig. 6(a)). Here, as shown in Fig. 7, seven through-holes were formed in one segment, and the pattern was made so that the outer contour of the through-holes was hexagonal. Then, the segments were formed in seven rows (number of segments per row: 3-4-3-4-3-4-3) and two independent segments were formed, and the joining region was assumed (number of through-electrodes: 182). The through-holes were formed by forming a pattern with photoresist and processing it with dry etching. The shape of the through-holes was a vertical hole, and the hole diameter was 50 μm. After the through-holes were formed, the silicon substrate was heat-treated in the air to form a thermal oxide film.
[0069] An undercoat film was formed on one side of the silicon substrate with the through-holes formed. As the undercoat film, a Ti (50 nm) film was formed by sputtering, and then a gold (300 nm) metallized film was formed (see Figure 6 (b)). At this time, these metal films were formed on the inner walls of the through-holes as well as on the substrate surface.
[0070] Then, the metal paste was applied to the base material to fill the through holes (see FIG. 6(c)). In this embodiment, a metal paste (gold powder content: 90% by mass) was used, which was made by mixing gold powder (average particle size measured by SEM observation: 0.3 μm) with a purity of 99.99% by mass produced by a wet reduction method with tetrachloroethylene (product name: Asahi Park Roll) as an organic solvent. The metal paste was applied by dropping the above metal paste onto the substrate and spreading the metal paste over the entire substrate surface with a urethane rubber blade (blade width: 30 mm) vibrating at a frequency of 200 Hz. In addition, in this metal paste application process, the back surface of the substrate was placed in a reduced pressure atmosphere (-10 kPa to -90 kPa) so that the paste on the substrate application surface was sucked into the through holes. After applying the metal paste, the entire substrate was dried at 70° C. for 1 hour, and then heated at 200° C. for 30 minutes to sinter the metal powder and form the through electrodes.
[0071] Next, bumps were formed on the through electrodes. Photoresist (40 μm) was applied to one side of the substrate, and then the area around the through electrodes was exposed (750 mJ / cm using a direct writing exposure machine with a wavelength of 405 nm). 2 ), developed and opened. At this time, the diameter of the bump was set to 80 μm. After this masking process, the same metal paste as for the through electrodes was applied. The application method was basically the same as above, but the application was done using a blade with a vibration frequency of 170 Hz in a chamber decompressed to -65 kPa. After the metal paste was filled into the gaps that would become the bumps, it was dried in the same way as for the through electrodes, and then baked at 100°C for 1 hour (see Figure 6(d)).
[0072] After forming bumps by baking, the photoresist is removed to obtain the interposer substrate according to this embodiment (see FIG. 6(e)). In this embodiment, a metal film is finally formed on the back surface of the base material by sputtering using Ti and Au.
[0073] FIG. 8 shows an SEM photograph of the cross-sectional structure of the through electrode and the bump of the interposer substrate manufactured in this embodiment. FIG. 9 shows an enlarged SEM photograph of the boundary between the inner surface of the through hole and the through electrode. From these, it can be seen that the through electrode and the bump have a material structure with fine pores. It was also confirmed that there was a gap of about 0.5 μm between the inner surface of the through hole and the through electrode. This gap is considered to be due to slight shrinkage caused by firing the metal powder in the two firing processes. Furthermore, the porosity of the through electrode and the bump was measured. This measurement was performed by processing the photographs (magnification 5000 times) of the through electrode and the bump with image analysis software (named ImageJ) and measuring the total area of the pores. As a result, the porosity of the through electrode was 15%, and the porosity of the bump was 11%. In this embodiment, the through electrode and the bump are formed separately, the through electrode is fired at a high temperature of 230° C., and the bump is fired at a low temperature of 100° C. It is believed that the difference in porosity and pore size is due to the difference in firing temperature.
[0074] [Cold-heat cycle test] A semiconductor chip was bonded to the interposer substrate manufactured as described above to manufacture an evaluation sample, and durability against thermal cycle load was evaluated. The manufactured interposer substrate was cut to prepare a sample (see Figure 7), and a semiconductor chip (Si wafer with Ti / Au metallized film: dimensions 10mm x 10mm) was placed on the bump-formed surface of the sample, and the semiconductor chip was bonded to the interposer substrate by heating and pressurization. The bonding conditions were a heating temperature of 250°C and loads of 3MPa, 5MPa, and 10MPa, and three types of samples were manufactured.
[0075] The manufactured samples were subjected to a thermal cycle tester with a temperature cycle of -50℃ and 150℃, and the bond strength after 1000 cycles was measured. The bond strength was measured as shear strength, which indicates shear stress. The samples were set in a shear strength tester (bond tester), and the shear strength was measured at a shear speed of 100μm / sec.
[0076] Figure 10 shows a photograph of the surface of the interposer substrate and the semiconductor chip after the shear strength measurement of each sample. Also, Figure 11 is an enlarged photograph of the interposer substrate and the semiconductor chip after the shear strength measurement. It can be seen from Figure 10 that as the pressure applied during bonding increases, the amount of metal powder that constitutes the bump that transfers to the semiconductor chip increases. Also, referring to the surface shape of the bump on the interposer substrate after the shear strength measurement in Figure 11 and the shape of the metal powder that transferred to the semiconductor chip side, it is estimated that bonding occurred mainly at the outer periphery of the bump.
[0077] Next, the bonding strength between the interposer substrate and the semiconductor chip was evaluated for each of the above samples (bonding loads: 3 MPa, 5 MPa, 10 MPa). In this evaluation, taking into consideration that the bonding between the interposer substrate and the semiconductor chip mainly occurred at the outer periphery of the bump as described above, the outer periphery area of the bump, calculated by subtracting the area of the through electrodes in the center from the area of the entire bump, was used as the bonding area that contributed to the bonding. The outer periphery area of the bump was then multiplied by the number of through electrodes (182) in the sample to obtain the area (0.54 mm 2The bonding strength between the interposer substrate and the semiconductor chip was determined by multiplying the measured value in the shear strength test by the bonding area.
[0078] For each of the above samples, the measured shear strengths for samples with bonding loads of 3 MPa, 5 MPa, and 10 MPa and the bond strengths calculated from the shear tests were 6.8 N (12.6 N / mm 2 ), 8.0N(14.8N / mm 2 ), 17.4N(32.2N / mm 2 The bonding strength between the interposer substrate and the semiconductor chip was 10N / mm 2 (10 MPa) or more can be said to be sufficient bonding strength. If this is used as the pass standard for evaluation, it can be said that all of the samples exhibited sufficient bonding strength. From the above test results, it was confirmed that the interposer substrate manufactured in this embodiment can maintain its bonding strength even when subjected to thermal cycle loads, and has good durability.
[0079] Second embodiment In this embodiment, the metal type and particle size of the metal powder forming the through electrodes and bumps were changed, and after producing a metal paste, an interposer substrate was produced based on the second aspect in the same manner as in the first embodiment. The conditions for producing the metal paste and the conditions for producing the through electrodes and bumps were basically the same as in the first embodiment. However, the configuration of the base film was changed appropriately. After producing the interposer substrate, a bonding strength test was performed after applying a thermal cycle (1000 times) in the same manner as in the first embodiment. In this bonding strength test, the bonding loads were set to 0.8 MPa, 1.0 MPa, and 10 MPa, and the bonding strength was measured before and after the thermal cycle load, and it was found that the bonding strength after the load was 10 N / mm 2 The test results are shown in Table 1.
[0080] [Table 1]
[0081] From Table 1, it can be seen that good bonding strength and durability can be obtained in an interposer substrate in which through electrodes and bumps are formed from gold, silver, and copper metal powders of appropriate particle size. When the particle size of the metal powder exceeds 2.0 μm, the bonding strength is 10 N / mm after the thermal cycle load. 2 The bonding strength was less than 1.0 MPa, and when the bonding load was low, some of the strength was insufficient even before the thermal cycle load (immediately after bonding). This is thought to be because when the particle size of the metal powder is too large, gaps are generated inside the sintered metal powder body, and these gaps remain even after bonding, reducing the strength of the bonded area. Furthermore, when the load for the bonding process is less than 1.0 MPa, even if some bonding strength is achieved, the overall bonding strength tends to be low. To obtain a stable bonding strength, it is necessary to set the bonding load to 1.0 MPa or more. [Industrial Applicability]
[0082] The present invention is an interposer substrate suitable for stacked mounting such as system-in-packaging of semiconductor devices and 2.5-dimensional mounting, and has excellent durability against thermal stress caused by thermal cycles. The present invention can meet the demand for miniaturization and high integration of semiconductor devices, particularly high-current, high-load semiconductor devices such as power devices and LED devices. Therefore, the present invention is expected to contribute to the automotive and energy fields where power devices and the like are used.
Claims
1. An interposer substrate that is bonded to one or more bonded members having one or more connection portions in an overlapping state and is electrically connected to the bonded members, the interposer substrate includes a base material having one or more connection regions corresponding to the connection portions of the joined members; a plurality of through holes penetrating the base material are formed in the connection region of the base material; The plurality of through holes are formed adjacent to each other to form a segment that is one unit for the connection, and one or more of the segments are formed within the connection region, Each of the through holes has a through electrode penetrating the through hole, and a bump formed at at least one end of the through electrode and having a cross-sectional shape wider than the through electrode, The through electrode and the bump are made of a sintered metal powder obtained by sintering one or more kinds of metal powder selected from gold, silver, and copper having a purity of 99.9 mass% or more and an average particle size of 0.005 μm to 2.0 μm, An interposer substrate, wherein the porosity of the through electrodes is different from the porosity of the bumps.
2. a metallized film made of a metal is provided in an area where the base material and the bumps contact each other; The metallized film is made of any one of gold, silver, copper, palladium, platinum, and nickel having a purity of 99.9% by mass or more, 2. The interposer substrate according to claim 1, wherein the thickness of the metallized film is not less than 10 nm and not more than 1000 nm.
3. Further, a base film is provided between the metallized film and the substrate, the undercoat film is made of any one of titanium, chromium, tungsten, a titanium-tungsten alloy, and nickel; 3. The interposer substrate according to claim 2, wherein the thickness of the undercoat film is 10 nm or more and 1000 nm or less.
4. 4. The interposer substrate according to claim 1, wherein a gap is provided between an inner surface of a through hole and a through electrode, the gap being 1 / 1000 or more and 1 / 10 or less of a diameter of the through hole.
5. 5. The interposer substrate according to claim 1, wherein the cross-sectional area of the bump is 1.2 to 9 times the cross-sectional area of the end of the through electrode.
6. Each segment is composed of 2 to 20 through electrodes, 6. The interposer substrate according to claim 1, wherein an outer shape formed by the arrangement of the 2 to 20 through electrodes is circular, polygonal, or linear.
7. 7. The interposer substrate according to claim 1, wherein the porosity of the through electrodes and bumps made of sintered metal powder is 35% or less.
8. 1. A method for manufacturing a device, comprising: stacking and bonding one or more bonded members having one or more connection portions and one or more interposer substrates, thereby electrically connecting the bonded members and the interposer substrates, The interposer substrate is an interposer substrate according to any one of claims 1 to 7, The interposer substrate and the member to be joined are arranged in an overlapping manner; A device manufacturing method comprising a step of pressurizing the interposer substrate and / or the joined member from one direction or both directions at a pressure of 1 MPa or more and 50 MPa or less, and heating the interposer substrate and the joined member at a temperature of 150°C or more and 250°C or less to electrically connect the interposer substrate and the joined member.
Citation Information
Patent Citations
Mounting structure for electronic parts
JP2000151060A
Aggregate printed-wiring board
JP2000228566A
Circuit board
JP2001007530A
Wiring board for multiple pattern and method of manufacturing the same
JP2003110203A
Circuit substrate and mounting structure of surface mounting connector
JP2004342888A