Manufacturing method of grain-oriented electrical steel sheet
By controlling ignition loss and carbon dioxide concentration during storage, the method addresses carbon content issues at the coil edge, ensuring uniform magnetic properties and reducing manufacturing costs in grain-oriented electrical steel sheets.
Patent Information
- Application Number
- JP2022571890
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-26
- Filing Date
- 2022-05-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-05-24
AI Technical Summary
Existing methods for manufacturing grain-oriented electrical steel sheets fail to sufficiently reduce carbon content near the sheet width end portion, leading to magnetic aging issues and increased manufacturing costs due to the use of specialized Ti composite oxides.
A method that stabilizes carbon content at the coil edge portion by controlling ignition loss, storage time, and carbon dioxide concentration during the storage of cold-rolled steel sheets, using a formula (A×IGLOSS≦-1500×Ln(T)+9000) to ensure uniform magnetic properties without increasing costs.
Manufactures grain-oriented electrical steel sheets with excellent uniformity of magnetic properties across the sheet width direction at a lower cost by effectively managing carbon content through controlled storage conditions.
Smart Images

Figure 0007578146000004 
Figure 0007578146000001 
Figure 0007578146000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a grain-oriented electrical steel sheet. [Background technology]
[0002] Grain-oriented electrical steel sheets are generally manufactured by subjecting a steel slab adjusted to a prescribed composition to hot rolling, annealing, and cold rolling, followed by primary recrystallization annealing and decarburization annealing, followed by finish annealing. Of the above steps, the finish annealing process requires heat treatment at a high temperature of 1000°C or higher. Therefore, in the finish annealing process, an annealing separator mainly composed of magnesium oxide (hereinafter also referred to as MgO) powder is generally applied to the surface of the cold-rolled steel sheet to prevent coil seizure.
[0003] In addition to preventing seizure, MgO also plays a role in forming a forsterite film during final annealing by reacting with an oxide layer mainly composed of silica (SiO2) (hereinafter also referred to as the SiO2 oxide layer). Here, the SiO2 oxide layer is formed on the surface of the cold-rolled steel sheet during decarburization annealing performed before the final annealing. MgO also plays a role in removing and purifying the steel sheet after the final annealing, by removing precipitates (e.g., some of AlN, MnS, MnSe, Si3N4, TiN, TiC, etc.) that control the growth of iron crystal grains, called inhibitors.
[0004] Carbon in steel is an essential element for improving, for example, the primary recrystallization texture. However, if a large amount of carbon remains in the final product, it may precipitate as carbides inside the steel sheet over time. These carbides cause a problem of deteriorating magnetic properties, a problem known as magnetic aging.
[0005] As a technique for solving such a problem, for example, Patent Document 1 describes: "A method for producing grain-oriented silicon steel sheet, which comprises subjecting a hot-rolled sheet for grain-oriented silicon steel to one or more cold rolling processes with intermediate annealing therebetween, followed by decarburization annealing, coating the sheet with an annealing separator mainly composed of MgO containing a Ti compound, and then performing final annealing, characterized in that the total carbon content in the steel and in the annealing separator of the steel sheet coated with the annealing separator just before the final annealing is set to 0.0015 wt% or less, thereby producing grain-oriented silicon steel sheet with little iron loss degradation associated with strain relief annealing." has been disclosed.
[0006] In addition, Patent Document 2 states: "A method for producing grain-oriented electrical steel sheet comprising a series of steps of hot rolling a silicon steel slab containing 1.0 to 5.0 mass% Si, followed by cold rolling once or twice or more times including annealing treatment to obtain a final sheet thickness, subjecting the slab to primary recrystallization annealing, applying an annealing separator to the steel sheet surface, and then subjecting the steel sheet to final annealing, A method for manufacturing a grain-oriented electrical steel sheet coil, comprising using an annealing separator as a main component, the main component containing at least 50% magnesia and, as a trace component, a titanate compound having the following composition, in an amount of 1 to 10 parts by mass per 100 parts by mass of magnesia. Note (M + a,M 2+ b,M 3+ c) TixOy However, 0≦a≦4, 0≦b≦2, 0≦c≦2 1≦x≦4, 2≦y≦9 M + :One of the following: Li, Na, or K M 2+ : One of the following selected from Mg, Ca, Sr, Ba, Cr, Co, Mn, Zn, and Fe M 3+ : One of the following selected from Fe, Al, Cr, and Mn has been disclosed. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2-93021 [Patent Document 2] JP 2007-169755 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, the technology of Patent Document 1 has a problem in that the carbon content in the steel near the width ends (hereinafter also referred to as the coil edge portions) of the coil-shaped steel sheet obtained after finish annealing is not sufficiently reduced, and magnetic aging is not sufficiently improved in the coil edge portions.
[0009] Furthermore, the technique of Patent Document 2 requires the use of the Ti composite oxide having the above-mentioned special composition, which results in a problem of high production costs.
[0010] The present invention has been developed to solve the above problems, and has an object to provide a method for producing a grain-oriented electrical steel sheet in which the carbon content in the coil edge portion after final annealing is stabilized at a low level without increasing production costs, thereby improving magnetic aging throughout the entire width direction of the coil (hereinafter also referred to as "excellent uniformity of magnetic properties in the width direction"). [Means for solving the problem]
[0011] The inventors have conducted extensive research from the standpoint of improving production management in order to achieve the above object without increasing manufacturing costs. As a result, the inventors found that the reason why the carbon content in steel at the coil edges is not sufficiently reduced in the technology of Patent Document 1 is that the annealing separator applied to the coil edges carbonates and carburizes during the period from when the annealing separator is applied and wound into a coil until the start of finish annealing, i.e., during standby in the coil yard.
[0012] Based on the above findings, the inventors conducted further research and found that by satisfying the relationship of the following formula (1) for the ignition loss of the annealing separator after drying: IGLOSS (mass %), the storage time of the cold-rolled steel sheet: T (hr), and the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet: A (mass ppm), the carbon content of the coil edge after finish annealing can be stabilized at a low level, thereby improving magnetic aging throughout the entire width direction of the coil. A×IGLOSS≦-1500×Ln(T)+9000 (1) The present invention was completed based on the above findings and through further investigation.
[0013] That is, the gist and configuration of the present invention are as follows. 1. A method for producing a grain-oriented electrical steel sheet, comprising the steps of: A step of preparing a cold-rolled steel sheet having a composition of C: 0.0100 mass% or more and Si: 1.0 mass% or more; A step of subjecting the cold-rolled steel sheet to decarburization annealing; applying an annealing separator mainly composed of MgO to a surface of the cold-rolled steel sheet and drying the annealing separator; A step of storing the cold-rolled steel sheet after winding the cold-rolled steel sheet into a coil; A step of subjecting the cold rolled steel sheet to finish annealing; A method for producing a grain-oriented electrical steel sheet, in which the ignition loss of the annealing separator after drying: IGLOSS (mass %), the storage time of the cold-rolled steel sheet: T (hr), and the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet: A (mass ppm) satisfy the relationship of the following formula (1). A×IGLOSS≦-1500×Ln(T)+9000 (1) Effect of the Invention
[0014] According to the present invention, it is possible to manufacture, at low cost, a grain-oriented electrical steel sheet having excellent uniformity in magnetic properties in the sheet width direction. [Brief description of the drawings]
[0015] [Figure 1]FIG. 1 is a schematic diagram showing sample collection positions for evaluating magnetic aging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described based on the following embodiments. A method for producing a grain-oriented electrical steel sheet according to an embodiment of the present invention includes the steps of: A step of preparing a cold-rolled steel sheet having a composition of C: 0.0100 mass% or more and Si: 1.0 mass% or more (hereinafter also referred to as a preparation step); A step of subjecting the cold-rolled steel sheet to decarburization annealing (hereinafter also referred to as a decarburization annealing step); A process of applying an annealing separator mainly composed of MgO to the surface of the cold-rolled steel sheet and drying the annealing separator (hereinafter also referred to as a coating and drying process); A process of storing the cold-rolled steel sheet after winding the cold-rolled steel sheet into a coil (hereinafter also referred to as a storage process); A process for subjecting the cold-rolled steel sheet to finish annealing (hereinafter also referred to as a finish annealing process), The ignition loss of the annealing separator after drying: IGLOSS (mass %), the storage time of the cold-rolled steel sheet: T (hr), and the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet: A (mass ppm) satisfy the relationship of the following formula (1). A×IGLOSS≦-1500×Ln(T)+9000 (1) Each step will be described below.
[0017] [Preparation process] First, a cold-rolled steel sheet having a chemical composition of C: 0.0100 mass % or more and Si: 1.0 mass % or more is prepared. Here, the method for preparing the cold-rolled steel sheet is not particularly limited. For example, a steel slab having a composition of C: 0.0100 mass% or more and Si: 1.0 mass% or more is hot-rolled to obtain a hot-rolled steel sheet. The hot-rolled steel sheet is annealed as necessary, and then cold-rolled once or twice or more with intermediate annealing to obtain a cold-rolled steel sheet. In this way, a cold-rolled steel sheet having the above-mentioned composition can be prepared.
[0018] The conditions for the hot rolling, hot-rolled sheet annealing, intermediate annealing, and cold rolling are not particularly limited, and may be in accordance with conventional methods.
[0019] The reasons for limiting the chemical composition of the cold-rolled steel sheet to be prepared are as follows.
[0020] C: 0.0100% by mass or more C is a component useful for generating crystal grains of the Goss orientation. To effectively exert this effect, the C content is set to 0.0100 mass% or more. On the other hand, if the C content is too high, decarburization failure may occur even after decarburization annealing. Therefore, the C content is preferably 0.1000 mass% or less.
[0021] Si: 1.0% by mass or more Silicon is an element that increases electrical resistance and reduces iron loss. Silicon is also an element that stabilizes the BCC structure of iron, making high-temperature heat treatment possible. Therefore, the silicon content is set to 1.0 mass% or more. The silicon content is preferably 2.0 mass% or more. On the other hand, if the silicon content is too high, cold rolling may become difficult. Therefore, the silicon content is preferably 5.0 mass% or less.
[0022] In addition to the above elements, the composition of the cold-rolled steel sheet to be prepared may further include, in mass%, (a) Mn: 0.01-1.0%, (b) sol.Al: 0.003-0.050%, (c) N: 0.001 to 0.020%, and (d) at least one selected from the group consisting of S: 0.001 to 0.05% and Se: 0.001 to 0.05%; Among these, (a) to (d) can be contained alone or in combination.
[0023] Mn effectively contributes to improving the hot brittleness of steel. In addition, Mn forms precipitates such as MnS and MnSe with S and Se, and functions as an inhibitor. From the viewpoint of fully obtaining this effect, the Mn content is preferably 0.01 mass% or more. On the other hand, if the Mn content is too high, the grain size of precipitates such as MnSe becomes coarse. This may cause the inhibitor effect to be lost. Therefore, the Mn content is preferably 1.0 mass% or less.
[0024] Sol. Al is a useful component that forms AlN in steel and acts as an inhibitor as a dispersed second phase. If the amount of Al is too small, the amount of AlN precipitated may not be sufficient. On the other hand, if the amount of Al is too much, AlN may precipitate coarsely and lose its inhibitory effect. For this reason, the sol. Al content is preferably 0.003 to 0.050 mass%.
[0025] Like Al, N is a component for forming AlN. If the N content is too low, the precipitation of AlN may be insufficient. On the other hand, if the N content is too high, swelling may occur during heating of the slab. For this reason, the N content is preferably 0.001 to 0.020 mass%.
[0026] Both S and Se are useful components that exert inhibitor effects. That is, S and Se combine with Mn and Cu to form MnSe, MnS, and Cu. 2-x Se, Cu 2-x S and Se form compounds such as S. These compounds act as a dispersed second phase in the steel and act as inhibitors. If the amount of S and Se is too small, the effect of adding them may be insufficient. On the other hand, if the amount of S and Se is too large, the solid solution may be incomplete when the slab is heated. In addition, it may cause defects on the product surface. For this reason, the S and Se contents are preferably 0.001 to 0.05 mass%, respectively.
[0027] In addition to the above elements, the composition of the cold-rolled steel sheet to be prepared may further include, in mass%, At least one selected from the group consisting of Cu: 0.01-0.2%, Ni: 0.01-0.5%, Cr: 0.01-0.5%, Sb: 0.01-0.1%, Sn: 0.01-0.5%, Mo: 0.01-0.5%, and Bi: 0.001-0.1% may be contained. Cu, Ni, Cr, Sb, Sn, Mo and Bi are all elements that act as auxiliary inhibitors and contribute to improving magnetic properties. If the content of any of the elements is less than the above-mentioned amount, it is difficult to obtain the effect. On the other hand, if the content exceeds the above-mentioned amount, the appearance of the coating may be poor and secondary recrystallization may be easily caused. Therefore, the content of these elements is preferably within the above-mentioned range.
[0028] In addition to the above elements, the composition of the cold-rolled steel sheet to be prepared may further include, in mass%, At least one element selected from the group consisting of B: 0.001-0.01%, Ge: 0.001-0.1%, As: 0.005-0.1%, P: 0.005-0.1%, Te: 0.005-0.1%, Nb: 0.005-0.1%, Ti: 0.005-0.1%, and V: 0.005-0.1% may be contained. This further strengthens the suppression force, and a higher magnetic flux density can be stably obtained.
[0029] The balance other than the above elements in the chemical composition of the prepared cold-rolled steel sheet is Fe and inevitable impurities. Note that, when the content of any of the above optional elements is less than the lower limit, the optional element is included as an inevitable impurity.
[0030] The thickness of the cold rolled steel sheet to be prepared is not particularly limited, but is preferably 0.14 to 0.50 mm. The width (width in the direction perpendicular to the rolling direction) of the cold rolled steel sheet to be prepared is not particularly limited, but is preferably 900 to 1500 mm. The same applies to the preferred ranges of the thickness and width of the cold rolled steel sheet wound into a coil.
[0031] [Decarburization annealing process] Next, the cold-rolled steel sheet prepared in the above preparation step is subjected to decarburization annealing. The conditions of the decarburization annealing are not particularly limited, and may be performed according to a conventional method. For example, the atmosphere in the decarburization annealing is preferably a wet hydrogen atmosphere from the viewpoint of ensuring decarburization and forming a SiO2 oxide layer. As described above, the SiO2 oxide layer reacts with MgO in the annealing separator during the finish annealing to form a forsterite film.
[0032] Here, the wet hydrogen atmosphere is an atmosphere with a hydrogen concentration of 50% by volume or more and a dew point of 40°C to 65°C. The decarburization annealing temperature is preferably 800°C to 900°C. By setting the hydrogen concentration in the wet hydrogen atmosphere to 50% by volume or more, it is possible to stably control the decarburization rate and the oxidation rate. If the decarburization annealing temperature is too low or the dew point is too low, decarburization failure may occur. On the other hand, if the decarburization annealing temperature is too high or the dew point is too high, the internal oxide layer may be overformed, resulting in product failure. In the wet hydrogen atmosphere, the remainder other than hydrogen is not particularly limited, but examples include neutral gases such as nitrogen and argon. In particular, it is preferable that the remainder other than hydrogen in the wet hydrogen atmosphere is nitrogen (i.e., a mixed atmosphere of hydrogen and nitrogen is adopted as the wet hydrogen atmosphere).
[0033] In addition, decarburization annealing generally serves as primary recrystallization annealing, but decarburization annealing and primary recrystallization annealing may be performed separately. The conditions other than those described above are not particularly limited and may be in accordance with conventional methods. For example, the annealing time is preferably 30 to 180 seconds.
[0034] [Coating and drying process] Next, an annealing separator mainly composed of MgO is applied to the surface of the cold-rolled steel sheet that has been subjected to the above-mentioned decarburization annealing step, and the annealing separator is dried.
[0035] For example, the annealing separator mainly composed of MgO is made into a water slurry and applied to the surface of the cold-rolled steel sheet using a roll coater or the like. At this time, it is preferable to control the slurry temperature within a certain range (±5°). In addition, since controlling the slurry temperature at a temperature that is too far from room temperature wastes energy, the median value of the control of the slurry temperature is preferably 5°C or more and 30°C or less. Then, the cold-rolled steel sheet coated with the annealing separator mainly composed of MgO is dried by means of an infrared heating furnace or a hot air furnace to remove excess moisture in the annealing separator. The final sheet temperature (hereinafter also referred to as the drying temperature) is preferably 350°C or more. This allows magnesium hydroxide (Mg(OH)2) generated by the hydration reaction to be returned to MgO. In addition, since the generated MgO is highly reactive, the forsterite film formed during the final annealing is also in a good condition.
[0036] Here, "mainly composed of MgO" means that the MgO content of the annealing separator is 50% by mass or more. If the MgO content is less than 50% by mass, the amount of forsterite film formed is insufficient. The MgO content of the annealing separator is preferably 60% by mass or more, more preferably 80% by mass or more. The remainder of the annealing separator other than MgO includes, for example, TiO2, and sulfides, sulfates, oxides, and hydroxides of alkaline earth metals.
[0037] The other conditions are not particularly limited and may be the same as those described above. For example, the weight of the annealing separator is 2.5 to 10 g / m2 per one side of the steel sheet after drying. 2 In addition, the drying time is preferably 1 to 5 minutes.
[0038] [Storage process] Next, the cold-rolled steel sheet that has been subjected to the above-mentioned coating and drying process is wound into a coil shape, and then the cold-rolled steel sheet is stored. Note that storage of the cold-rolled steel sheet is generally performed in a coil yard.
[0039] In the manufacturing method of grain-oriented electrical steel sheet according to one embodiment of the present invention, it is extremely important that in this storage step, the ignition loss of the annealing separator after drying: IGLOSS (mass %), the storage time of the cold-rolled steel sheet: T (hr), and the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet: A (mass ppm) satisfy the relationship of the following formula (1). A×IGLOSS≦-1500×Ln(T)+9000 (1) In addition, Ln in the formula means the natural logarithm.
[0040] That is, in order to reduce the carbon concentration in the final product of the grain-oriented electrical steel sheet, particularly to make it less than 40 mass ppm, (1) Sufficient carbon removal from the steel sheet during decarburization annealing. (2) Reducing the carbon concentration in the annealing separator; and (3) Suppression of carbonation caused by atmospheric CO2 during coil yard standby It is important to do so.
[0041] The conditions of this storage process are closely related to (3) suppressing carbonation during waiting in the coil yard. In other words, the mechanism of carbonation during standby in the coil yard in (3) is thought to be the production of basic magnesium carbonate by carbonation of magnesium hydroxide (Mg(OH)2), as shown in the following reaction equation. (m+1)Mg(OH)2+mCO2→mMgCO3·Mg(OH)2·mH2O ···(2) In the above reaction scheme, m is an integer of 3 to 5.
[0042] In addition, the above-mentioned Patent Document 2 describes that it is difficult to control the waiting time in the coil yard, which corresponds to the reaction time of the chemical reaction according to the above reaction formula, because the operating state of the finish annealing equipment is not stable. It also describes that it is unrealistic to control the CO2 concentration and humidity in the atmosphere because of the enormous cost involved.
[0043] Incidentally, Mg(OH)2 on the left side of the above formula (2) is generated by a series of processes in which an annealing separator mainly composed of MgO is applied to the steel sheet surface as a water slurry and then dried. The content of Mg(OH)2 in the annealing separator after drying is considered to be measurable as the loss on ignition (IGLOSS) specified in JIS K 0067:1992.
[0044] Here, JIS K 0067:1992 specifies that the ignition temperature should be 650° C.±50° C. However, when the ignition loss of the annealing separator after drying was measured at an ignition temperature of 650° C.±50° C., it was found that the ignition loss included not only the loss of Mg(OH)2 but also the loss of MgCO3.
[0045] As a result of further investigation, the inventors have come to the following findings. To accurately measure the weight loss of Mg(OH)2, it is necessary to measure the weight loss on ignition of the annealing separator after drying at an ignition temperature of 500°C±10°C and a soaking time of 30 minutes. By satisfying the relationship of the following formula (1) between the ignition loss of the annealing separator after drying measured under these conditions: IGLOSS (mass%), the storage time of the cold-rolled steel sheet: T (hr), and the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet: A (mass ppm), carbonation of the annealing separator applied to the coil edge, and therefore carburization of the coil edge, is suppressed. As a result, it becomes possible to manufacture grain-oriented electrical steel sheet with excellent uniformity of magnetic properties in the sheet width direction.
[0046] Here, the ignition loss: IGLOSS (mass %) of the annealing separator after drying is measured as follows. That is, 2 g of the dried annealing separator is sampled in powder form from the surface of the cold-rolled steel sheet that has been subjected to the above-mentioned coating and drying process. The sampled dried annealing separator is used as a sample, and the weight loss (the amount of mass loss when the sample is ignited) is measured under conditions of an ignition temperature of 500°C and a soaking time of 30 minutes according to a method in accordance with JIS K 0067:1992. The measured weight loss expressed as a mass percentage is defined as the ignition loss of the dried annealing separator: IGLOSS (mass%).
[0047] The storage time T (hr) of the cold-rolled steel sheet is defined as the time from the completion of coiling the cold-rolled steel sheet to the start of finish annealing. Here, the completion time of winding the cold rolled steel sheet refers to the time when the continuous steel sheet is wound, then sheared and separated into a coil, and the start time of finish annealing refers to the time when the coil is placed on the coil support of the finish annealing furnace.
[0048] In addition, the carbon dioxide concentration: A (ppm by mass) in the storage environment of the cold-rolled steel sheet is measured as follows. That is, the carbon dioxide concentration in the atmosphere is measured at 0 minutes past the hour Coordinated Universal Time (UTC) during storage of the cold-rolled steel sheet. The arithmetic mean value of the carbon dioxide concentration in the atmosphere measured at 0 minutes past the hour Coordinated Universal Time (UTC) during storage of the cold-rolled steel sheet is defined as the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet: A.
[0049] In order to satisfy the above formula (1), if it is known in advance that T will be extended due to equipment maintenance or the like, it is effective to reduce IGLOSS by setting the drying temperature of the annealing separator to 400°C or higher or lengthening the drying time. In this case, the amount of magnesium hydroxide (Mg(OH)2) once generated that returns to magnesium oxide (MgO) increases, which is preferable because the appearance of the forsterite coating after final annealing becomes uniform.
[0050] In addition, if T becomes longer than expected due to equipment trouble, it is necessary to reduce the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet. For example, a method of purging with nitrogen can be used by placing a vinyl cover on the coil and supplying liquid nitrogen into the cover.
[0051] Although there are no particular limitations as long as the above formula (1) is satisfied, it is usually preferable that IGLOSS is 1.5 to 5.0 mass%, the storage time of the cold-rolled steel sheet: T is 4 to 240 hours, and the carbon dioxide concentration in the storage environment of the cold-rolled steel sheet: A is in the range of 200 to 800 mass ppm.
[0052] The other conditions than those mentioned above are not particularly limited and may be those according to conventional methods.
[0053] [Finish annealing process] Next, the cold-rolled steel sheet that has been subjected to the above-mentioned storage process is subjected to final annealing. The conditions of the final annealing are not particularly limited, and may be in accordance with a conventional method. For example, the annealing temperature is preferably 1100 to 1250°C, and the annealing time is preferably 5 to 20 hours.
[0054] In addition, after the finish annealing step, planarization annealing may be optionally performed. The conditions for planarization annealing are not particularly limited, and may be performed according to a conventional method. EXAMPLES
[0055] Example 1 A steel slab containing, in mass%, C: 0.0400%, Si: 3.25%, Mn: 0.08%, S: 0.002%, sol.Al: 0.015%, N: 0.006%, Cu: 0.05%, and Sb: 0.01%, with the balance being Fe and unavoidable impurities, was heated under the conditions of a slab heating temperature of 1150°C and a holding time of 20 minutes. The steel slab was then hot rolled to obtain a hot-rolled steel sheet having a thickness of 2.4 mm. The obtained hot-rolled steel sheet was then subjected to hot-rolled sheet annealing under the conditions of an annealing temperature of 1000°C and an annealing time of 60 seconds (1 minute). The hot-rolled steel sheet was then cold-rolled to prepare a cold-rolled steel sheet having a thickness (final thickness): 0.27 mm. The chemical composition of the prepared cold rolled steel sheet was the same as that of the above-mentioned steel slab.
[0056] The prepared cold-rolled steel sheets were subjected to decarburization annealing, which also served as primary recrystallization annealing, under the conditions of an annealing temperature of 820°C and an annealing time of 60 seconds in a wet hydrogen atmosphere of 50 vol% hydrogen and 50 vol% nitrogen with a dew point of 50°C. The average heating rate from room temperature to 820°C was 100°C / s. The carbon content of the base steel of the cold-rolled steel sheets after decarburization annealing was 5 ppm by mass in all cases.
[0057] Next, an annealing separator mainly composed of MgO, specifically an annealing separator in which 100 parts by mass of MgO and 5 parts by mass of TiO2 were mixed, was made into a water slurry and subjected to a hydration treatment at 15°C for 2.0 hours. Next, the cold-rolled steel sheet after decarburization annealing was dried to have a basis weight of 6.5 g / m2 per side of the steel sheet. 2 The annealing separator was applied so as to obtain the following: Next, the annealing separator was dried under the conditions of a drying temperature of 350° C. and a drying time of 1 minute.
[0058] Next, the cold-rolled steel sheet was wound into a coil and then stored for a certain period of time under the conditions shown in Table 1. The ignition loss: IGLOSS (mass%) of the annealing separator after drying was measured by the above-mentioned method, and the value was 3.0 mass%. The carbon dioxide concentration: A in the storage environment of the cold-rolled steel sheet was controlled by the above-mentioned method.
[0059] Next, the cold-rolled steel sheet was subjected to finish annealing under the conditions of an annealing temperature of 1200°C and an annealing time of 5 hours. The temperature rise time from 300°C to 800°C was 100 hours, and the average temperature rise rate from 800°C to 1200°C was 50°C / hr. After the finish annealing, unreacted annealing separator was removed with a brush. Next, the cold-rolled steel sheet was subjected to flattening annealing in a non-oxidizing atmosphere of 98 vol% nitrogen and the remainder hydrogen under the conditions of an annealing temperature of 800°C and an annealing time of 30 seconds, to obtain a grain-oriented electrical steel sheet as the final product.
[0060] Next, the magnetic aging of the obtained grain-oriented electrical steel sheets was evaluated. That is, as shown in Fig. 1, samples with a length of 300 mm and a width (width direction) of 100 mm are taken from the coil center (width center) and the coil edge at a position 1000 m inward from the outer coil winding part of the obtained grain-oriented electrical steel sheet toward the center of the coil (a position 1000 m from the outermost part after the coil is unwound). Note that the center position in the width direction of the sample taken from the coil center (width center) is set to the width center position of the coil. Also, the center position in the width direction of the sample taken from the coil edge is set to a position 60 mm from the width end of the coil (i.e., the area up to 10 mm from the width end is cut off).
[0061] Next, the iron loss (W 17 / 50 The measurement results are shown in Table 1. The W of the samples taken from the coil center (width center) and the coil edge (before stress relief annealing) was 17 / 50 All of the B8 values for the samples taken from the coil center (widthwise center) and coil edge (before stress relief annealing) were within the range of 1.895 to 1.905 T.
[0062] Next, the samples were subjected to stress relief annealing in a nitrogen atmosphere at an annealing temperature of 800°C for 3 hours. The iron loss and carbon content of the base steel were measured for the samples after stress relief annealing. The iron loss ratio before and after stress relief annealing (=[iron loss measured in the sample after stress relief annealing] / [iron loss measured in the sample before stress relief annealing]) was calculated for each sample collected from the center of the coil (center of the sheet width) and the coil edge, and the uniformity of the magnetic properties in the sheet width direction was evaluated according to the following criteria. Pass (Excellent): The iron loss ratio before and after stress relief annealing is 1.05 or less in both samples taken from the center of the coil (center of the sheet width) and the coil edge. Rejected: In at least one of the samples taken from the center of the coil (center of the sheet width) and the coil edge, the iron loss ratio before and after stress relief annealing is more than 1.05. The results are shown in Table 1.
[0063] [Table 1] TIFF0007578146000002.tif233166
[0064] As shown in Table 1, all of the inventive examples had excellent uniformity in magnetic properties in the sheet width direction. In addition, in all of the inventive examples, the carbon content of the base steel at the coil edge was suppressed to less than 40 ppm by mass. Furthermore, all of the inventive examples had a good coating appearance. On the other hand, in the comparative example, sufficient uniformity of the magnetic properties in the sheet width direction was not obtained.
[0065] Example 2 A steel slab containing, in mass%, C: 0.0100%, Si: 2.00%, Mn: 0.07%, S: 0.015%, Sb: 0.015%, and Cr: 0.03%, with the balance being Fe and unavoidable impurities, was heated under the conditions of a slab heating temperature of 1350°C and a holding time of 40 minutes. The steel slab was then hot rolled to obtain a hot-rolled steel sheet having a thickness of 2.6 mm. The obtained hot-rolled steel sheet was then subjected to hot-rolled sheet annealing under the conditions of an annealing temperature of 900°C and an annealing time of 60 seconds. The hot-rolled steel sheet was then subjected to intermediate annealing under the conditions of an annealing temperature of 1050°C and an annealing time of 60 seconds, and then cold-rolled to prepare a cold-rolled steel sheet having a thickness (final thickness): 0.30 mm. The chemical composition of the prepared cold rolled steel sheet was the same as that of the above-mentioned steel slab.
[0066] The prepared cold-rolled steel sheets were subjected to decarburization annealing, which also served as primary recrystallization annealing, under the conditions of an annealing temperature of 840°C and an annealing time of 60 seconds in a wet hydrogen atmosphere of 60 vol% hydrogen and 40 vol% nitrogen with a dew point of 55°C. The average heating rate from room temperature to 820°C was 700°C / s. The carbon content of the base steel of the cold-rolled steel sheets after decarburization annealing was 4 ppm by mass in all cases.
[0067] Next, an annealing separator mainly composed of MgO, specifically an annealing separator in which 3 parts by mass of TiO2 was mixed with 100 parts by mass of MgO, was made into a water slurry and subjected to a hydration treatment for 1.0 hour at the temperature shown in Table 2. Next, the cold-rolled steel sheet after decarburization annealing was coated with a 6.5 g / m2 coating solution after drying on one side of the steel sheet. 2 The annealing separator was then dried at the drying temperature shown in Table 2 for a drying time of 1 minute.
[0068] Next, the cold-rolled steel sheet was wound into a coil and then stored for a certain period of time under the conditions shown in Table 2. In addition, the ignition loss: IGLOSS (mass%) of the annealing separator after drying was measured by the method described above. The measurement results are also shown in Table 2. In addition, the carbon dioxide concentration: A in the storage environment of the cold-rolled steel sheet was controlled by the method described above.
[0069] Next, the cold-rolled steel sheet was subjected to finish annealing under the conditions of an annealing temperature of 1200°C and an annealing time of 5 hours. The temperature rise time from 300°C to 700°C was 100 hours, and the average temperature rise rate from 700°C to 1200°C was 20°C / hr. After the finish annealing, unreacted annealing separator was removed with a brush. Next, the cold-rolled steel sheet was subjected to flattening annealing in a non-oxidizing atmosphere of 98 vol% nitrogen and the remainder hydrogen under the conditions of an annealing temperature of 820°C and an annealing time of 30 seconds, to obtain a grain-oriented electrical steel sheet as the final product.
[0070] Then, in the same manner as in Example 1, samples with a length of 300 mm and a width (in the sheet width direction) of 100 mm were taken from the center of the coil (center of the sheet width) and the coil edge, respectively, and the magnetic aging of the obtained grain-oriented electrical steel sheet was evaluated. The results are shown in Table 2. The evaluation criteria were the same as in Example 1. In addition, the W of the samples taken from the center of the coil (center of the sheet width) and the coil edge before stress relief annealing was 17 / 50 All of the B8 values for the samples taken from the coil center (widthwise center) and coil edge before stress relief annealing were within the range of 1.865 to 1.875 T.
[0071] [Table 2]
[0072] As shown in Table 2, all of the inventive examples had excellent uniformity in magnetic properties in the sheet width direction. In addition, in all of the inventive examples, the carbon content of the base steel at the coil edge was suppressed to less than 40 ppm by mass. Furthermore, all of the inventive examples had a good coating appearance. On the other hand, in the comparative example, sufficient uniformity of the magnetic properties in the sheet width direction was not obtained.
Claims
[Claim 1] A method for producing a grain-oriented electrical steel sheet, comprising the steps of: A step of preparing a cold-rolled steel sheet having a composition of C: 0.0100 mass% or more and Si: 1.0 mass% or more; A step of subjecting the cold-rolled steel sheet to decarburization annealing; An annealing separator mainly composed of MgO is applied to the surface of the cold-rolled steel sheet (excluding annealing separators containing one or more halogen compounds selected from F, Cl and Br in total amounts of F, Cl and Br in the ranges of 0.03 to 0.30 mass % and 0.5 to 5.5 mass %, and annealing separators in which the total amount of F and Cl is 200 ppm by mass are excluded). and drying the annealing separator; A step of storing the cold-rolled steel sheet after winding the cold-rolled steel sheet into a coil; A step of subjecting the cold rolled steel sheet to finish annealing; a storage time of the cold-rolled steel sheet: T (hr); and a carbon dioxide concentration in a storage environment of the cold-rolled steel sheet: A (ppm by mass), which satisfy the relationship of the following formula (1). A×IGLOSS≦-1500×Ln(T)+9000...(1) Here, the ignition loss (IGLOSS) (mass %) of the annealing separator after drying is measured at an ignition temperature of 500° C.±10° C. and a soaking time of 30 minutes.
Citation Information
Patent Citations
Production of grain-oriented silicon steel sheet reduced in deterioration in iron loss accompanying stress relief annealing
JP1990093021A
Production of grain oriented electromagnetic steel sheet excellent in surface characteristic and magnetic characteristic
JP1998158744A
Production of ultrahigh magnetic flux density grain oriented silicon steel sheet
JP1999229036A
Grain-oriented electromagnetic steel sheet in coiled form and manufacturing method therefor
JP2007169755A
Method for producing grain oriented silicon steel sheet coil
JP2007177298A