Ferritic Stainless Steel
A ferritic stainless steel with controlled composition and oxidation treatment forms a thin black oxide film enriched with Ti and Cr, addressing polishability and rust issues, enabling effective pattern formation and maintaining a black tone for decorative uses.
Patent Information
- Application Number
- JP2020218548
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-12-28
AI Technical Summary
Existing methods for forming patterns on stainless steel surfaces with black oxide films face challenges such as the time-consuming removal of thick oxide films and the risk of rust initiation from internal oxides, which affect polishability and design integrity.
A ferritic stainless steel material with controlled composition and oxidation treatment conditions to form a thin black oxide film enriched with composite oxides of Ti and Cr, reducing internal oxides and enhancing polishability while maintaining a black tone.
The solution provides a stainless steel material with excellent polishability, allowing for effective pattern formation and maintaining a desired black color tone, suitable for decorative applications.
Smart Images

Figure 0007579140000004 
Figure 0007579140000001 
Figure 0007579140000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel material having excellent polishability and a black oxide film on the surface. [Background technology]
[0002] Stainless steel is not only a material with excellent corrosion resistance, but also has a shiny silver-white surface that makes it suitable for use in interior and exterior building materials, etc. Furthermore, in order to enhance the design of stainless steel, it is often given a color tone, typically black, using methods such as chemical coloring, painting, and oxidation treatment.
[0003] Furthermore, there are also cases where a pattern is imparted to a colored stainless steel by partially polishing or etching the stainless steel base material. Patent Document 1 describes a pattern forming method in which a stainless steel surface that has been colored using a chemical coloring method is mechanically polished to roughen the surface into a predetermined pattern. Patent Document 2 describes a technique for imparting a pattern by mechanically polishing the surface of a Zn-plated steel sheet on which a black oxide film has been formed by an oxidation treatment method.
[0004] Furthermore, Patent Documents 3 and 4 describe black stainless steel materials in which a black oxide film is formed on the surface of the stainless steel by an oxidation treatment method. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 61-213380 [Patent Document 2] JP 2017-218647 A [Patent Document 3] JP 2019-178392 A [Patent Document 4] JP 2018-135591 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when attempting to form a pattern by forming a black oxide film on the surface of stainless steel as a base material and then polishing part of it to expose the silver-white base material, the following problems related to polishability arise. (1) The oxide film formed on the surface of stainless steel by oxidation treatment is mainly composed of hard Cr2O3, so if the oxide film is thick, it takes a long time to remove it by polishing. (2) In addition, an internal oxide layer containing many internal oxides including TiO2 and Al2O3 is formed on the surface of the stainless steel substrate, and if internal oxides are present on the exposed substrate surface, they can easily become the starting point for rusting, which may impair the design. Therefore, when forming a pattern, in addition to the black oxide film, it is necessary to remove the internal oxide layer on the substrate surface, but if there are many internal oxides containing hard TiO2 and Al2O3, it takes time to remove them by polishing.
[0007] In order to make it easier to form a pattern by polishing on the surface of a stainless steel material with a black oxide film formed thereon, that is, to improve the polishability, it is effective to make the oxide film thinner or to reduce the amount of internal oxide precipitation in the surface layer of the stainless steel material base. However, there are problems in that if the thickness of the oxide film is made thin, the black color tone cannot be guaranteed, and if the internal oxide is reduced, the oxide film is more likely to peel off.
[0008] The present invention has been made to solve the above problems, and has an object to provide a ferritic stainless steel material having a black oxide film and excellent polishability. [Means for solving the problem]
[0009] The inventors of the present invention have conducted extensive research to solve the above problems, and have found that by increasing the proportion of Ti and Cr composite oxides in the oxide film, it is possible to ensure a black color tone even when the oxide film is thin, and that by controlling the amount of precipitation of Al2O3 and TiO2, which are particularly hard granular oxides among the internal oxides formed in the surface layer of the base material directly below the oxide film, within a certain range, it is possible to improve polishability while suppressing peeling of the oxide film.The inventors have found that the above object can be achieved by controlling the composition of ferritic stainless steel and the oxidation treatment conditions, and have arrived at the present invention.
[0010] The gist of the present invention, which has been completed based on the above findings, is as follows. (1) A ferritic stainless steel material according to one embodiment of the present invention is a ferritic stainless steel material having a composition, by mass%, of C: 0.100% or less, Si: 1.00% or less, Mn: 0.04 to 1.00%, P: 0.050% or less, S: 0.030% or less, Cr: 16.00 to 25.00%, Ni: 1.00% or less, Cu: 0.60% or less, Mo: 2.00% or less, N: 0.030% or less, Ti: 0.080 to 0.500%, Nb: 0.500% or less, Al: 0.100% or less, with the balance being Fe and impurities, and having a lightness index L * ≦45.0, Chromathetics index -5.0≦a * ≦5.0, -5.0≦b * A black oxide film having a thickness of 0.20 to 1.00 μm and a Ti fraction of 0.20 or more is formed on the surface, and the number of internal oxides having a circle equivalent diameter of 0.04 μm or more existing in an area of 1 μm x 1 μm at a depth of 0.3 μm from the surface of the base material satisfies the above criteria.
[0011] (2) The ferritic stainless steel material described in (1) above may further contain, in the composition of the ferritic stainless steel, one or more elements selected from the group consisting of Zr: 1.00% or less, Co: 1.00% or less, V: 1.00% or less, and W: 1.00% or less, in mass percent.
[0012] (3) The ferritic stainless steel material described in (1) or (2) above may further contain, in mass %, one or more elements selected from the group consisting of REM: 0.100% or less and Ca: 0.100% or less in the composition of the ferritic stainless steel.
[0013] (4) The ferritic stainless steel material according to any one of (1) to (3) above may further contain, in mass %, one or more elements selected from the group consisting of Sn: 0.100% or less and B: 0.0100% or less in the composition of the ferritic stainless steel. Effect of the Invention
[0014] According to the above aspect of the present invention, a ferritic stainless steel material having a black oxide film and excellent polishability can be provided. [Brief description of the drawings]
[0015] [Figure 1] 2 is a cross-sectional view in the plate thickness direction, which diagrammatically shows the vicinity of the surface layer of a stainless steel material. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements to the following embodiments, which are made based on the ordinary knowledge of those skilled in the art, fall within the scope of the present invention, without departing from the spirit of the present invention.
[0017] <1. Ferritic stainless steel material> (1.1 Chemical composition) The base material of the ferritic stainless steel material according to this embodiment (hereinafter, sometimes simply referred to as "stainless steel material") has a composition, in mass%, of C: 0.100% or less, Si: 1.00% or less, Mn: 0.04 to 1.00%, P: 0.050% or less, S: 0.030% or less, Cr: 16.00 to 25.00%, Ni: 1.00% or less, Cu: 0.60% or less, Mo: 2.00% or less, N: 0.030% or less, Ti: 0.080 to 0.500%, Nb: 0.500% or less, Al: 0.100% or less, with the balance being Fe and impurities. That is, the base material of the stainless steel material according to this embodiment has a chemical composition in which the metal structure at room temperature is mainly ferrite phase. The term "impurities" as used herein refers to components that are mixed in during industrial production of the ferritic stainless steel substrate due to various factors in the manufacturing process, such as raw materials such as ores and scraps, and that are acceptable within a range that does not adversely affect the present invention. For example, impurities also include unavoidable impurities.
[0018] In addition, the base material of the stainless steel material according to this embodiment may further contain, by mass%, one or more elements selected from the group consisting of Zr: 1.00% or less, Co: 1.00% or less, V: 1.00% or less, and W: 1.00% or less. Furthermore, the base material of the stainless steel material according to this embodiment may further contain, by mass%, one or more elements selected from the group consisting of REM: 0.100% or less and Ca: 0.100% or less. The base material of the stainless steel material according to this embodiment may further contain, by mass%, one or more elements selected from the group consisting of Sn: 0.100% or less and B: 0.0100% or less. The reasons for limiting the content of each element will be explained below.
[0019] (C: 0.100% by mass or less) C is an element that affects the properties of stainless steel materials, such as intergranular corrosion resistance (sensitization suppression effect) and workability. If the C content is too high, the workability and intergranular corrosion resistance of the stainless steel material will decrease. Therefore, the upper limit of the C content is 0.100 mass%, preferably 0.080 mass%, and more preferably 0.050 mass%. On the other hand, the lower limit of the C content is not particularly limited, but reducing the C content leads to an increase in refining costs. Therefore, the lower limit of the C content is preferably 0.0005 mass%, and preferably 0.001 mass%.
[0020] (Si: 1.00% by mass or less) Silicon is an element that improves the oxidation film peeling resistance and high-temperature oxidation resistance of stainless steel materials. If the Si content is too high, the workability and toughness decrease. Therefore, the upper limit of the Si content is 1.00 mass%, preferably 0.90 mass%, and more preferably 0.80 mass%. On the other hand, the lower limit of the Si content is not particularly limited, but is preferably 0.05 mass%, more preferably 0.10 mass%, and even more preferably 0.15 mass%, from the viewpoint of suppressing deterioration of surface quality due to oxide film peeling during the production of stainless steel materials.
[0021] (Mn:0.04~1.00% by mass) Mn is a useful element as a deoxidizing element and is also effective in improving high-temperature oxidation resistance such as oxidation film peeling resistance. In addition, Mn is effective in forming a black color tone by forming a complex oxide with Cr. If the Mn content is too high, MnS, which is the starting point of corrosion, is easily generated and the ferrite phase is destabilized. Therefore, the upper limit of the Mn content is 1.00 mass%, preferably 0.95 mass%, and more preferably 0.90 mass%. On the other hand, if the Mn content is too low, the above effects may not be sufficiently obtained. Therefore, the lower limit of the Mn content is 0.04 mass%, and preferably 0.05 mass%.
[0022] (P: 0.050 mass% or less) P is an element that affects the properties of stainless steel materials, such as weldability and workability. If the P content is too high, the above properties may be degraded. Therefore, the upper limit of the P content is 0.050 mass%, preferably 0.045 mass%, and more preferably 0.040 mass%. On the other hand, the lower limit of the P content is not particularly limited, but reducing the P content leads to an increase in refining costs. Therefore, the lower limit of the P content is preferably 0.001 mass%, and more preferably 0.010 mass%.
[0023] (S: 0.030% by mass or less) S is an element that generates MnS, which is a corrosion starting point, and affects the properties of stainless steel materials, such as toughness. If the S content is too high, the above properties may be reduced. Therefore, the upper limit of the S content is 0.030 mass%, preferably 0.025 mass%, and more preferably 0.020 mass%. On the other hand, the lower limit of the S content is not particularly limited, but reducing the S content leads to an increase in refining costs. Therefore, the lower limit of the S content is preferably 0.0001 mass% or more, and more preferably 0.0005 mass% or more.
[0024] (Cr:16.00~25.00% by mass) Cr is an element effective in improving the corrosion resistance and oxidation resistance of stainless steel materials. If the Cr content is too high, the toughness of the stainless steel material decreases, and the growth of the oxide film is inhibited, making it impossible to form an oxide film having a black color tone. Therefore, the upper limit of the Cr content is 25.00 mass%, preferably 24.50 mass%, and more preferably 24.00 mass%. On the other hand, if the Cr content is too low, the above effects may not be sufficiently obtained. Therefore, the lower limit of the Cr content is 16.00 mass%, and preferably 16.50 mass%.
[0025] (Ni: 1.00% by mass or less) Ni is an element effective for improving the corrosion resistance and toughness of stainless steel materials. If the Ni content is too high, the ferrite phase becomes unstable and the manufacturing cost increases. Therefore, the upper limit of the Ni content is 1.00 mass%, preferably 0.90 mass%, and more preferably 0.80 mass%. On the other hand, the lower limit of the Ni content is not particularly limited, but is preferably 0.01 mass%, and more preferably 0.05 mass%, from the viewpoint of obtaining the above-mentioned effects.
[0026] (Cu: 0.60% by mass or less) Cu is an element effective for improving the corrosion resistance of stainless steel materials. If the Cu content is too high, the ferrite phase becomes unstable and the manufacturing cost increases. Therefore, the upper limit of the Cu content is 0.60 mass%, preferably 0.55 mass%, and more preferably 0.50 mass%. On the other hand, the lower limit of the Cu content is not particularly limited, but is preferably 0.001 mass%, and preferably 0.01 mass%.
[0027] (Mo: 2.00% by mass or less) Mo is an element effective for improving the corrosion resistance and oxidation resistance of stainless steel materials. If the Mo content is too high, the workability of the stainless steel material decreases, the manufacturing cost increases, and the oxidation resistance improves, making it difficult to form a black oxide film. Therefore, the upper limit of the Mo content is 2.00 mass%, preferably 1.90 mass%. On the other hand, the lower limit of the Mo content is not particularly limited, but is preferably 0.001 mass%, preferably 0.01 mass%.
[0028] (N: 0.030% by mass or less) N is an element that affects properties such as intergranular corrosion resistance (sensitization suppression effect) and workability. If the N content is too high, the intergranular corrosion resistance and workability of the stainless steel material will decrease. In addition, as described later, Ti is required for the formation of a black oxide film, but if the N content is high, TiN will precipitate, reducing the amount of solid-solubilized Ti in the steel, and the formation of the black oxide film will be inhibited. In addition, the formed nitrides are likely to become the starting point of corrosion, reducing the corrosion resistance, especially the pitting corrosion resistance. Therefore, the upper limit of the N content is 0.030 mass%, preferably 0.028 mass%, and more preferably 0.025 mass%. On the other hand, the lower limit of the N content is not particularly limited, but reducing the N content leads to an increase in refining costs. Therefore, the lower limit of the N content is preferably 0.0005 mass%, and preferably 0.001 mass%.
[0029] (Ti: 0.080~0.500% by mass or less) Ti is an element that affects intergranular corrosion resistance (sensitization suppression effect). Furthermore, Ti forms a complex oxide with Cr, imparting a black appearance to the oxide film, and is an element that effectively acts to suppress peeling of the oxide film by forming Ti oxide (TiO2) on the surface of the material. If the Ti content is too high, the workability and surface quality of the stainless steel material will decrease. Therefore, the upper limit of the Ti content is 0.500 mass%, preferably 0.480 mass%, and more preferably 0.450 mass%. Also, if the Ti content is too low, the above-mentioned effects may not be sufficiently obtained. Therefore, the lower limit of the Ti content is 0.080 mass%, preferably 0.090 mass% or more, and more preferably 0.100 mass%.
[0030] (Nb: 0.500% by mass or less) Nb is an element that affects properties such as intergranular corrosion resistance (sensitization suppression effect). On the other hand, if the Nb content is too high, the workability and toughness of the stainless steel material are reduced and the oxidation of Ti is inhibited. Therefore, the upper limit of the Nb content is 0.500 mass%, preferably 0.480 mass%, and more preferably 0.450 mass%.
[0031] (Al: 0.100% by mass or less) Al is an element that effectively prevents the peeling of a black oxide film by forming an Al oxide on the surface of the material. On the other hand, the Al oxide (Al2O3) on the surface of the material is hard and inhibits polishability. Therefore, the upper limit of the Al content is 0.100 mass%, preferably 0.950 mass%, and more preferably 0.900 mass%. On the other hand, the lower limit of the Al content is not particularly limited, but is preferably 0.001 mass%, and preferably 0.010 mass%.
[0032] (Zr: 1.00 mass% or less, Co: 1.00 mass% or less, V: 1.00 mass% or less, W: 1.00 mass% or less) Zr, Co, V and W are elements effective for improving the oxidation resistance of stainless steel materials. If the content of Zr, Co, V and W is too high, the workability and toughness of the stainless steel material will decrease, and the manufacturing cost will increase. Therefore, the upper limit of the content of Zr, Co, V and W is 1.00 mass%, preferably 0.80 mass%, and more preferably 0.50 mass%. On the other hand, the lower limit of the content of Zr, Co, V and W is not particularly limited, but is preferably 0.001 mass%, and more preferably 0.01 mass%.
[0033] (REM: 0.100 mass% or less, Ca: 0.100 mass% or less) REM and Ca are elements effective in improving the oxidation resistance of stainless steel materials. If the content of REM and Ca is too high, it leads to an increase in the manufacturing cost of stainless steel. Therefore, the upper limit of the content of REM and Ca is 0.100 mass%, preferably 0.080 mass%, and more preferably 0.050 mass%. On the other hand, the lower limit of REM and Ca is not particularly limited, but is preferably 0.0001 mass%, more preferably 0.003 mass%. REM is a collective term for 17 elements in total, including Sc, Y, and lanthanoids, and means rare earth metals. Specifically, La, Ce, Nd, etc. can be mentioned, and one of these can be contained alone, or two or more can be contained in combination. When two or more rare earth elements are contained, the above REM content means the total content of these rare earth elements. As a method of addition, for example, a misch metal (MM), which is a mixture of rare earth elements, may be used to contain the REM content in the above range.
[0034] (Sn: 0.100% by mass or less) Sn is an element effective for improving the corrosion resistance of stainless steel materials. If the Sn content is too high, Sn segregates and manufacturability decreases. Therefore, the upper limit of the Sn content is 0.100 mass%, preferably 0.080 mass%, and more preferably 0.050 mass%. On the other hand, the lower limit of the Sn content is not particularly limited, but is preferably 0.001 mass%, and more preferably 0.005 mass%.
[0035] (B: 0.0100% by mass or less) B is an element effective for improving the secondary workability of stainless steel materials. If the B content is too high, the fatigue strength of the stainless steel decreases. Therefore, the upper limit of the B content is 0.0100 mass%, preferably 0.0080 mass%, and more preferably 0.0050 mass%. On the other hand, the lower limit of the B content is not particularly limited, but is preferably 0.0001 mass%, and more preferably 0.0005 mass%.
[0036] (1.2 Composition of ferritic stainless steel) Fig. 1 is a cross-sectional view showing a schematic view of the vicinity of the surface layer in a cross section of the stainless steel material according to this embodiment cut in the plate thickness direction. As shown in Fig. 1, the stainless steel material 10 according to this embodiment has a ferritic stainless steel base material 15 (hereinafter simply referred to as "base material") and an oxide film 11 formed on the surface of the base material 15. Also, an inner oxide layer 12 in which a large number of inner oxides 13 are present is present near the interface between the base material 15 and the oxide film 11 (i.e., the surface layer of the base material 15).
[0037] (Oxide film) The substrate side 15 of the oxide film 11 in the stainless steel material 10 according to this embodiment is a Cr oxide region 111 mainly containing Cr2O3, and the surface side of the oxide film 11 is a Ti-enriched region 112 containing a high proportion of composite oxides of Cr and Ti. The presence of the Ti-enriched region 112 on the surface side of the oxide film 11 imparts a black color tone.
[0038] (Oxide film color tone) The stainless steel material 10 according to the present embodiment has a lightness index L * , Chromanetics Index a * , b * The numerical value indicating the color tone according to this embodiment is obtained by performing color tone measurement according to JIS Z 8722:2009 at any five points, averaging the average value, and calculating the CIELAB (L) value according to JIS Z 8781-4:2013. * a * b * The lightness index L * , Chromanetics Index a * , b * The oxide film of the stainless steel plate according to the present invention has a surface of L * ≦45.0, -5.0≦a * ≦5.0, -5.0≦b * It has a range of ≦5.0.
[0039] (Oxide film thickness) From the viewpoint of ease of polishing, the oxide film 11 of the stainless steel material 10 according to this embodiment has an upper limit of the thickness of 1.00 μm or less, preferably 0.95 μm or less, and more preferably 0.90 μm or less. On the other hand, if the thickness of the oxide film 11 is too thin, the black color tone cannot be ensured, so the lower limit of the thickness of the oxide film 11 is 0.20 μm, preferably 0.25 μm, and more preferably 0.30 μm. The thickness of the oxide film 11 according to this embodiment is a numerical value corresponding to the depth from the surface to the point where O (oxygen) is half the maximum value in a profile obtained using glow discharge optical emission spectroscopy (GDS).
[0040] (Ti fraction of oxide film) The stainless steel material 10 according to this embodiment ensures polishability by reducing the thickness of the oxide film 11. However, reducing the thickness of the oxide film 11 results in a lighter black color tone. Therefore, in order to ensure the black color tone, the proportion of the composite oxide of Ti and Cr in the oxide film 11 is increased. That is, the Ti fraction in the oxide film (Ti fraction=Ti concentration / (Fe concentration+Cr concentration+Mn concentration+Ti concentration)) is in the range of 0.20 or more, preferably 0.25 or more, and more preferably 0.30 or more. Here, the Ti fraction in the oxide film 11 is obtained by analysis using glow discharge optical emission spectroscopy (GDS).
[0041] The Ti fraction in the oxide film according to this embodiment is a ratio calculated by measuring the concentration profile of each element by glow discharge optical emission spectrometry (GD-OES) in accordance with JIS K 0144:2018 and dividing the "Ti concentration" at the point where the O (oxygen) peak intensity is maximum by the "Fe concentration + Cr concentration + Mn concentration + Ti concentration."
[0042] The point where the O (oxygen) peak intensity is at its maximum value is on the surface side of the oxide film 11. If the Ti fraction in the oxide film is within this range, the proportion of composite oxides of Ti and Cr is high on the surface side of the oxide film 11, that is, a Ti-enriched region 112 is formed. Therefore, even if the thickness of the oxide film 11 is thin, the L* ≦45.0, -5.0≦a * ≦5.0, -5.0≦b * Therefore, it is possible to obtain a stainless steel material 10 having excellent polishability and a desired black tone.
[0043] (internal oxide layer) The stainless steel material 10 according to this embodiment has an inner oxide layer 12 on the substrate side (substrate surface layer) near the interface between the oxide film 11 and substrate 15. The inner oxide layer 12 is a region of the substrate surface layer where a large number of inner oxides 13 such as TiO2 and Al2O3 are present, and its thickness is about 0.4 μm to 1.0 μm. The inner oxide 13 may be, for example, a Ti oxide (TiO2), an Al oxide (Al2O3), a Mn oxide (MnO2), or a Si oxide (SiO2).
[0044] (Number of internal oxides) The stainless steel material 10 according to the present embodiment has good film adhesion and excellent polishability because the number of inner oxides 13 in the inner oxide layer 12 of the substrate surface layer is within a predetermined range. Since the inner oxides contain hard TiO2 and Al2O3, if the number of inner oxides 13 is too large, the surface layer of the substrate 15 becomes hard, making mechanical polishing with a grinder or the like difficult. Conversely, if the number of inner oxides 13 is too small, the oxide film 11 becomes easily peeled off, resulting in a problem of low film adhesion. Therefore, the number of inner oxides 13 with a circle equivalent diameter of 0.04 μm or more present in an area of 1 μm × 1 μm at a depth of 0.3 μm from the substrate surface is 5 to 30, preferably 6 to 28, and more preferably 7 to 25.
[0045] The number of the inner oxides 13 according to this embodiment can be obtained by the following measurement method. The substrate side of a cross-sectional sample taken from the stainless steel material 10 was observed at a magnification of 40,000 times using a TEM (scanning transmission electron microscope). 2The number of granular regions with a circular equivalent diameter of 0.04 μm or more that existed when observing one field of view was counted visually, and this operation was performed for three fields of view, and the arithmetic average was taken as the number of internal oxides 13. The circular equivalent diameter means the diameter of a circle when the area of each observed granular region is converted into a circle having the same area.
[0046] In this measurement, the granular oxides TiO2, Al2O3, and MnO2 are counted. TiO2, Al2O3, and MnO2 are not distinguished from each other, but since MnO2, even if it exists, is in a much smaller amount than TiO2 and Al2O3, the number of internal oxides obtained as a result of this measurement can be considered to be substantially equal to the total of Al2O3 and TiO2, which are hard granular oxides that affect polishability. Moreover, most of the granular oxides observed by visual observation under the above measurement conditions can be considered to have a circle equivalent diameter of 0.04 μm or more. The number of inner oxides according to this embodiment corresponds to the value obtained by the above-mentioned measurement method.
[0047] (Application of stainless steel materials) The stainless steel material 10 according to the present embodiment has a desired black color tone and excellent polishability because the chemical composition of the base material 15, the color tone, thickness, Ti fraction, and the number of the internal oxides 13 are within a predetermined range. For example, by using the stainless steel material 10 according to the present embodiment and removing a part of the black oxide film 11 by polishing to expose the shiny silver-white base material 15, a pattern can be formed, and a steel material with excellent designability can be provided. Therefore, the stainless steel material 10 is suitable for use as a design member, and is applied to various members that require designability, such as building materials (especially interior members such as decorative panels) and piping, although not limited thereto.
[0048] <2. Manufacturing method of ferritic stainless steel material> The stainless steel material 10 according to the present embodiment described above can be manufactured, for example, by the method described below. A preferred manufacturing method for the stainless steel material 10 according to this embodiment includes an oxidation treatment step of heating a ferritic stainless steel material (base material 15) having the above-mentioned chemical composition in an oxidizing atmosphere at a heating temperature of 1000°C or more and 1100°C or less, for a heating time of 60 seconds or more and 300 seconds or less, with an average heating rate of 18°C / second or more from 500°C to 800°C, to form an oxide film 11. The manufacturing conditions are described below.
[0049] (Preparation of stainless steel materials) First, prior to the above-mentioned oxidation treatment step, a ferritic stainless steel material is prepared. The material may have the above-mentioned chemical composition, and may be manufactured by a known method. For example, a ferritic stainless steel slab having the above-mentioned chemical composition is hot-rolled, and the resulting hot-rolled coil is annealed and pickled, and then cold-rolled at a cold rolling rate of 50% or more to produce a cold-rolled sheet. Next, the surface of the resulting cold-rolled sheet is finish-polished with a polishing belt of #180 or more to obtain a base material 15. By using the base material 15 with the surface polished in this manner, the appearance unevenness of the black oxide film 11 formed on the base surface in the subsequent process is suppressed.
[0050] (Oxidation treatment process) This step is a step of forming a black oxide film 11 by heat treatment on the surface of the base material 15. The base material 15 is subjected to an oxidation treatment (annealing) in which the base material 15 is heated in an oxidizing atmosphere at a temperature of 1000° C. to 1100° C. for a time of 60 to 300 seconds with an average heating rate of 18° C. / sec or more from 500° C. to 800° C., thereby forming a black oxide film 11 having a thickness of 0.30 to 1.00 μm on the surface of the base material 15.
[0051] If the heating temperature during the oxidation treatment is too high or the heating time is too long, the oxide film 11 becomes too thick and the number of internal oxides 13 in the surface layer of the substrate increases, so that excellent polishability cannot be obtained. Therefore, the heating temperature is 1100°C or less. Also, the heating time is 300 seconds or less. On the other hand, if the heating temperature during the oxidation treatment is too low, the Ti fraction in the oxide film 11 becomes low and the desired black color tone cannot be obtained. Therefore, the heating temperature is 1000°C or more. Also, if the heating time is too short, the oxide film does not develop sufficiently and the desired thickness cannot be obtained. Therefore, the heating time is 60 seconds or more. The preferred heating temperature is 1050 to 1080°C, and the preferred heating time is 120 to 180 seconds.
[0052] Moreover, by increasing the heating rate, a composite oxide of Ti and Cr is preferentially formed on the surface side of the oxide film 11. This causes Ti to be concentrated in the oxide film 11, and the formation of TiO2 in the surface layer of the base material is suppressed. As a result, the Ti fraction of the oxide film 11 is 0.20 or more, and a thin oxide film 11 having a desired black color tone is obtained. In addition, the number of internal oxides 13 having a circle equivalent diameter of 0.04 μm or more in the surface layer of the base material is 5 to 30, and the polishing property is excellent. On the other hand, if the heating rate is slow, the Ti fraction of the oxide film 11 is low, and the thin oxide film 11 does not obtain the desired black color tone. In addition, since a large amount of TiO2 is present in the surface layer of the base material, excellent polishing property cannot be obtained. Therefore, the average heating rate at 500°C to 800°C is 18°C / sec or more. In addition, the upper limit of the heating rate is not particularly limited, but the practical upper limit that can be implemented is 50°C / sec.
[0053] The above steps produce a stainless steel material 10 having excellent polishability and a black oxide film 11 on the surface according to this embodiment. Furthermore, since the stainless steel material 10 according to this embodiment has excellent polishability, for example, by using this stainless steel material 10, it is possible to produce a steel material having excellent designability, in which part of the black oxide film is removed by polishing to expose the shiny silver-white base material and form a pattern. Therefore, it is suitable for use as a design component, and is applied to various components that require designability, such as building materials (especially interior components such as decorative panels) and piping. EXAMPLES
[0054] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these.
[0055] A ferritic stainless steel having the chemical composition shown in Table 1 was hot-rolled to produce a hot-rolled sheet having a thickness of 3.0 mm. The hot-rolled sheet was annealed at 1050°C for 3 minutes, and then the oxide scale on the surface was removed by dry honing. The sheet was then cold-rolled to a thickness of 1.0 mm, and finished annealed at 1000°C for 1 minute. The sheet was then hand-polished using dry polishing papers of No. 120 and No. 240 in sequence to remove the oxide scale on the steel sheet surface. The chemical composition in Table 1 is shown in mass%, with the balance being Fe and impurities. In addition, REM in the table means rare earth elements, and here, misch metal (MM) containing La, Ce, and Nd was used. In addition, the underline indicates that it is outside the scope of the present invention.
[0056] [Table 1]
[0057] Then, in order to form a black oxide film on the surface of the above obtained stainless steel sheet, oxidation treatment was performed in an air atmosphere at a temperature rise rate (°C / sec), heating temperature (°C), and heating time (min) of 500 to 800°C as shown in Table 2. After that, a test piece having a width of 50 mm and a length of 100 mm was cut out from the center in the sheet width direction excluding the ends of the steel sheet. Similarly, a test piece for a cross-sectional sample having a width of 15 mm and a length of 15 mm was cut out from the center in the sheet width direction excluding the ends of the steel sheet after the oxidation treatment.
[0058] [Table 2]
[0059] The measurement method is described below.
[0060] (Method of measuring color tone) Using the above test piece, measure the color tone in five places on the oxide film on the surface using a spectrophotometer with a measurement diameter of 3 mm in accordance with JIS Z8722:2009, and calculate the average value according to CIELAB(L) in accordance with JIS Z 8781-4:2013. * a * b * The lightness index L * , Chromanetics Index a * , b * As shown in.
[0061] The conditions for measuring the color tone are as follows. Equipment: Konica Minolta Spectrophotometer CM-700d Light source: Pulsed xenon lamp Photodetector: Dual 36-element silicon photodiode array Target mask: Φ3mm Measurement: 10° field of view Auxiliary Illuminant: D65 daylight, color temperature 6504K Specular reflection processing mode: SCI
[0062] (Oxide film thickness and Ti content) Using the above test pieces, the exposed part of the substrate was analyzed by GDS (glow discharge optical emission spectroscopy), and the structure of the oxide film was analyzed by glow discharge optical emission spectroscopy (GD-OES) in accordance with JIS K0144:2018. In the GDS analysis (GD-OES), the depth from the surface to the point where the O (oxygen) peak intensity was half of the maximum value was taken as the thickness of the oxide film. In addition, the Ti concentration at the point where the O (oxygen) peak intensity was maximum / (Fe concentration + Cr concentration + Mn concentration + Ti concentration) was taken as the Ti fraction of the oxide film.
[0063] The measurement conditions for GDS are as follows. Equipment: Rigaku Corporation GDA750 Analysis diameter (anode diameter): Φ4mm Voltage: 650V Ar pressure: 2.8hPa
[0064] (Number of internal oxides) Cross-sectional samples were prepared from the above test pieces for cross-sectional samples by FIB (focused ion beam) processing, and the number of internal oxides was measured by observing the substrate side of the cross-sectional samples with a TEM (field emission transmission electron microscope: TalosF200X, accelerating voltage 200V, manufactured by Japan FEI Inc.). The observation position was 0.3 μm deep from the substrate surface (oxide film / substrate interface), and the observation range was 1 μm in area. 2 The magnification was 40,000 times, and the number of granular regions with a circular equivalent diameter of 0.04 μm or more was counted. The number of granular regions measured at three locations was averaged to obtain the number of internal oxides (number).
[0065] The FIB processing was performed using a system manufactured by Hitachi High-Technologies Corporation (now Hitachi High-Tech Corporation). A focused ion beam processing device (FB-2000A) was used, with an acceleration voltage of 30 kV and an ion source of Ga. In order to protect the top surface of the sample, a tungsten film was coated on it, and then a cross-sectional sample was extracted by FIB μ sampling.
[0066] The measurement results of the evaluation items are explained below. (abrasive) The test pieces that had been subjected to the above color tone evaluation were subjected to a grinding evaluation using a hand grinder. The test pieces were ground by pressing a hand grinder equipped with a #40 flap wheel at a rotation speed of 7000 rpm with a load of 500 g for 60 seconds. The color tone of the ground part was measured, and the obtained lightness index L * L * If the value satisfies ≧70, the abrasiveness is excellent (○), L * When the abrasiveness was less than 70, the abrasiveness was evaluated as insufficient (×). The evaluation results are shown in Table 3. The underlined values indicate values outside the range of the present invention.
[0067] [Table 3]
[0068] As shown in Table 3, the stainless steel sheets of Examples 1 to 6 within the scope of the present invention met the color standard because the chemical composition of the base material, the thickness of the oxide film, and the Ti fraction of the oxide film met the requirements. In addition, the thickness of the oxide film and the number of internal oxides met the standards, so they showed good polishability.
[0069] In contrast, the stainless steel sheets of Comparative Examples 1 to 8 were inferior to the Examples in either color tone or polishability. In Comparative Examples 1 and 2, the oxidation treatment was performed at a high temperature or for a long time, so that a thick oxide film was formed and a large amount of internal oxide was formed, resulting in insufficient polishability. In Comparative Examples 3 and 4, the oxidation treatment was performed at a low temperature or the temperature rise rate was slow, so that the Ti fraction of the oxide film was low and the lightness index L * did not meet the color standard. In Comparative Examples 5 and 6, the Ti and Al contents of the substrate were high, respectively, and thus a large amount of internal oxides (hard TiO2 and Al2O3) was formed, resulting in insufficient polishability. In Comparative Example 7, the Cr content of the substrate was low, resulting in the formation of a thick oxide film mainly composed of Fe, which did not meet the color standard of the oxide film and therefore insufficient polishability. In Comparative Example 8, since Ti was not added to the substrate, a composite oxide of Ti and Cr was not formed, and therefore the color standard of the oxide film was not met.
[0070] As can be seen from the above results, the present invention can provide a black ferritic stainless steel material that is excellent in polishability and designability. [Explanation of symbols]
[0071] 10 Stainless steel 11 Oxide film 111 Cr oxide region 112 Ti enriched region 12 Inner oxide layer 13. Internal oxide 15 Base
Claims
1. A ferritic stainless steel having a composition, in mass%, of C: 0.100% or less, Si: 1.00% or less, Mn: 0.04 to 1.00%, P: 0.050% or less, S: 0.030% or less, Cr: 16.00 to 25.00%, Ni: 1.00% or less, Cu: 0.60% or less, Mo: 2.00% or less, N: 0.030% or less, Ti: 0.080 to 0.500%, Nb: 0.500% or less, Al: 0.100% or less, with the balance being Fe and impurities, is used as a base material, and a lightness index L * ≦45.0, Chromathetics index -5.0≦a * ≦5.0, −5.0≦b * ≦5.0, a black oxide film having a thickness of 0.20 to 1.00 μm and a Ti fraction of 0.20 or more is formed on the surface, the number of internal oxides having a circle equivalent diameter of 0.04 μm or more existing within an area of 1 μm × 1 μm at a depth of 0.3 μm from the surface of the base material is 5 to 30; Here, the Ti fraction in the oxide film is expressed as Ti fraction = Ti concentration / (Fe concentration + Cr concentration + Mn concentration + Ti concentration).
2. The ferritic stainless steel material according to claim 1, further comprising, in mass%, one or more selected from the group consisting of Zr: 1.00% or less, Co: 1.00% or less, V: 1.0% or less, and W: 1.00% or less.
3. The ferritic stainless steel material according to claim 1 or 2, further comprising, in mass%, one or more selected from the group consisting of REM: 0.100% or less and Ca: 0.100% or less.
4. The ferritic stainless steel material according to any one of claims 1 to 3, wherein the ferritic stainless steel further comprises one or more selected from the group consisting of Sn: 0.100% or less and B: 0.0100% or less by mass.
Citation Information
Patent Citations
Formation of pattern on surface of metallic plate
JP1986213380A
Black stainless steel plate and its production
JP1999061376A
MOLTEN Zn-BASED PLATED STEEL SHEET HAVING LINEAR PATTERN
JP2017218647A
Black ferritic stainless steel sheet