Method and apparatus for producing granules
The method of irradiating raw material powder with a light beam to form granules addresses the challenges of mass production by achieving uniform size control and high yield, suitable for industrial applications.
Patent Information
- Application Number
- JP2020134057
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-08-06
AI Technical Summary
Existing methods for producing ceramic granules are not suitable for mass production due to complex manufacturing steps, high costs, and difficulty in controlling granule size, particularly for microscopic spheres.
A method involving irradiation of raw material powder with a light beam to bind and form granules, allowing for chemical reactions and size control through energy adjustment, using a simplified apparatus with a moving mechanism to manage the light beam's position.
Enables high-yield, mass production of uniformly sized granules with controlled diameter and maintained crystal structure, suitable for industrial applications like tritium breeder materials in nuclear fusion reactors.
Smart Images

Figure 0007579530000002 
Figure 0007579530000003 
Figure 0007579530000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and apparatus for producing granules. [Background technology]
[0002] Ceramic spheres such as alumina and zirconia are used industrially as heat-resistant parts, wear-resistant parts, bearing parts, and grinding parts (called ball mills). Lithium ceramic spheres such as lithium silicate and lithium zirconate are being developed as CO2 absorbents for thermal power plants, and lithium ceramic microspheres of lithium titanate are used as functional materials for breeding tritium for use in nuclear fusion reactions. Conventionally, methods for producing such spherical particles or granules (hereinafter simply referred to as granules or pebbles) include, for example, the emulsion method, the melting method, and the laser melting method.
[0003] Non-Patent Document 1 discloses a method using an emulsion method in which droplets of a sample slurry are dropped into an organic solvent to produce gel spheres. Non-Patent Document 2 discloses a melting method in which ceramic powder is melted at high temperature in a platinum crucible, and the melt is dropped into the air and cooled to produce spherical granules. Non-Patent Document 3 discloses a method using a laser melting method in which microspheres are produced by layered modeling using a laser. Patent Document 1 discloses a method in which raw material powder is supplied into a laser beam and melted to produce spherical granules. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 125843 / 1983 [Non-patent literature]
[0005] [Non-Patent Document 1] T. Hoshino et al., “Pebble fabrication and tritium release properties of an advanced tritium breeder”, Fusion Engineering and Design, Volumes 109-111, Part B, 1 November 2016, Pages 1114-1118 [Non-Patent Document 2] R. Knitter et al., “Fabrication of modified lithium orthosilicate pebbles by addition of titania”, Journal of Nuclear Materials, Volume 442, Issues 1-3, Supplement 1, November 2013, Pages S433-S436 [Non-Patent Document 3] Q. Zhou et al., “Fabrication of Li2TiO3 pebbles by a selective laser sintering process”, Fusion Engineering and Design, Volume 100, November 2015, Pages 166-170 Summary of the Invention [Problem to be solved by the invention]
[0006] As the industrial use of spherical particles advances, a simplified method suitable for mass production of such particles is required. However, in the method of Non-Patent Document 1, the raw materials are mixed for about 24 hours, the raw material gel balls are dried for about 6 hours or more, and then heat-treated in an electric furnace for several hours. The method of Non-Patent Document 1 involves many manufacturing steps and is not suitable for mass production. It is also not possible to produce tiny balls with a diameter of about 1 mm or less.
[0007] In the method of Non-Patent Document 2, the cost is increased because an expensive large platinum crucible is used. In the method of Non-Patent Document 2, the diameter of the obtained particles is also widely distributed from about 0.25 mm to about 1.25 mm, and it is difficult to control the size of the particles. For this reason, the yield is low and it is not suitable for mass production.
[0008] In the method of Non-Patent Document 3, a single sphere is irradiated with a laser multiple times to perform additive manufacturing, and the additively manufactured unsintered (green) sphere is pressurized by cold isostatic pressing (CIP) and then sintered in an electric furnace for several hours. The method of Non-Patent Document 3 involves many manufacturing steps and is not suitable for mass production. It is also not possible to manufacture tiny spheres with a diameter of approximately 1 mm or less.
[0009] In the method of Patent Document 1, raw material powder is discharged from a nozzle and allowed to fall freely, and melted while crossing a focused laser beam irradiated in a horizontal direction. In the method of Patent Document 1, if the raw material powder particles are fine, the raw material powder aggregates as it falls freely, and the particle size of the raw material powder before melting tends to increase. This causes variation in the time it takes for the raw material powder to cross the focused laser beam, making it difficult to control the size of the resulting particles. For this reason, the method of Patent Document 1 produces particles of various sizes with diameters of about 1 μm to about 200 μm, resulting in a low yield.
[0010] The present invention aims to provide a simplified method and apparatus for the mass production of granules. [Means for solving the problem]
[0011] In order to achieve the above object, the present invention includes, for example, the following aspects. (Section 1) A method for producing granules of raw material powder, comprising irradiating a light beam onto the raw material powder placed on a support to bond the raw material powder. (Section 2) Item 2. A method for producing granules according to item 1, characterized in that the light beam is irradiated while the position of the raw material powder and the irradiation position of the light beam irradiated onto the raw material powder are moved relatively. (Section 3) 3. A method for producing granules according to claim 1 or 2, characterized in that a mixture of multiple types of raw material powders is irradiated with the light beam to cause a chemical reaction between the multiple types of raw material powders, and granules are produced by binding together compounds produced by the chemical reaction. (Section 4) A method for producing the granules described in any one of items 1 to 3, characterized in that the energy of the light beam is changed to change the size of the granules. (Section 5) 5. A method for producing granules according to any one of claims 1 to 4, characterized in that the raw material powder contains a single or mixed composition of lithium compounds Li2O, Li2TiO3, Li4SiO4 and Li2ZrO3. (Section 6) A support on which the raw material powder is placed; a light source that irradiates light rays for binding the raw material powder; An apparatus for producing granules of the raw material powder, comprising: (Section 7) Item 7. The apparatus for producing granules according to item 6, further comprising a moving mechanism for relatively moving the position of the raw material powder and the irradiation position of the light beam irradiated onto the raw material powder. (Section 8) The support has a plurality of types of mixed raw material powders placed thereon, Item 8. The apparatus for producing granules according to item 6 or 7, characterized in that the light source irradiates the light beam for producing granules by chemically reacting the plurality of types of raw material powders and binding together compounds produced by the chemical reaction. Effect of the Invention
[0012] According to the present invention, a simplified method and apparatus for producing granules in large quantities can be provided. [Brief description of the drawings]
[0013] [Figure 1] 1 is a diagram showing a schematic configuration of a granule manufacturing apparatus according to an embodiment of the present invention; [Diagram 2] 1 is a flowchart showing the steps of a granule manufacturing method according to an embodiment of the present invention. [Diagram 3] 1 is a schematic diagram for explaining, in a plan view, the movement of the irradiation position of a light beam in a granule manufacturing method according to one embodiment of the present invention. FIG. [Figure 4] 1 is a photograph showing the appearance of granules produced by a granule production method according to one embodiment of the present invention. [Diagram 5] 1 is an electron microscope photograph of granules produced by a granule production method according to one embodiment of the present invention. [Figure 6] 4 is a graph showing the distribution of diameters of particles produced by a method for producing particles according to an embodiment of the present invention. [Figure 7] 2 is a graph showing the results of X-ray diffraction measurement of granular powder produced by a granular production method according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. In the following description and drawings, the same reference numerals denote the same or similar components, and therefore, redundant description of the same or similar components will be omitted. [Device configuration]
[0015] FIG. 1 is a diagram showing a schematic configuration of a granule manufacturing apparatus according to one embodiment of the present invention.
[0016] A granule manufacturing apparatus 10 according to one embodiment of the present invention includes a support 1 on which raw material powder 9 is placed, and a light source 2 that irradiates a light beam 3 for binding the raw material powder 9. In this embodiment, the support 1 and raw material powder 9 are placed in the atmosphere under normal pressure (atmospheric pressure). In other embodiments, the support 1 and raw material powder 9 may be placed in an atmosphere under reduced pressure below atmospheric pressure or under pressurized pressure higher than atmospheric pressure. The atmosphere surrounding the raw material powder 9 is not limited to the atmosphere, and may be various gas atmospheres.
[0017] In this embodiment, the raw material powder 9 is lithium titanate (Li2TiO3), and the granule manufacturing apparatus 10 manufactures lithium ceramic granules. In another embodiment, the raw material powder 9 may include a single or mixed composition of lithium compounds, such as lithium oxide (Li2O), lithium titanate (Li2TiO3), lithium silicate (Li4SiO4), and lithium zirconate (Li2ZrO3). In another embodiment, the raw material powder 9 may be a plurality of types of raw material substances that react when irradiated with the light beam 3.
[0018] In this embodiment, the support 1 is a generally plate-shaped stage having a depression in the approximate center in a plan view, and the raw material powder 9 is placed generally flat on the support 1. In other embodiments, the support 1 may be integrated with a moving mechanism 6 described later, for example, like a belt conveyor.
[0019] In this embodiment, the light source 2 is a laser light source. In this embodiment, the laser light, i.e., the light beam 3, is irradiated to the raw material powder 9 in a pulsed manner. For the light source 2, various light sources that output the light beam 3 of various wavelengths can be used. For example, for the light source 2, a known Nd:YAG (Yttrium Aluminum Garnet) laser that irradiates infrared light having a wavelength of 1.06 μm in a pulsed or continuous manner can be used. In another embodiment, for the light source 2, a CO2 laser can be used. In this embodiment, the output of the light source 2 is about 30 J per pulse. For example, the pulse width (irradiation time of the pulse) of the light beam 3 is about 3 milliseconds, which can reduce bumping and scattering of the raw material powder 9.
[0020] In this embodiment, the light beam 3 emitted from the light source 2 is irradiated onto the raw material powder 9 through the optical system 4. The illustrated optical system 4 includes a mirror 41 and a condenser lens 42, and condenses the light beam 3 onto the raw material powder 9 placed on the support 1. In other embodiments, the optical system 4 can be omitted, and the light beam 3 emitted from the light source 2 can be directly irradiated onto the raw material powder 9.
[0021] The controller 5 controls the operation of the light source 2. In this embodiment, the controller 5 controls the operation of the light source 2 via a control line 51, and controls the operation of the moving mechanism 6 (described later) via a control line 52. Illustratively, the controller 5 can be a computer equipped with a CPU and a memory, and various interfaces such as GP-IB (IEEE488) and USB can be used for connecting the control lines 51 and 52. The connection between the controller 5 and the light source 2 and the moving mechanism 6 may be a wired connection using the control lines 51 and 52 as shown in the figure, or in other embodiments, may be a wireless connection such as Wi-Fi (registered trademark) or Bluetooth (registered trademark).
[0022] In this embodiment, a moving mechanism 6 is provided below the support 1. The illustrated moving mechanism 6 can change its position in each of two orthogonal axis directions (X-axis and Y-axis shown in the figure). By driving the moving mechanism 6, the irradiation position 31 of the light beam 3 can be moved on the support 1, and the irradiation position 31 of the light beam 3 on the raw material powder 9 can be moved. In other embodiments, the position of the raw material powder 9 side may be fixed, and the light source 2 and optical system 4 side may be moved to move the irradiation position 31 of the light beam 3 on the raw material powder 9. [Manufacturing method]
[0023] Fig. 2 is a flow chart showing the procedure of a granule manufacturing method according to one embodiment of the present invention. The following procedure of the granule manufacturing method described with reference to Fig. 2 may be performed by an operator (user) using the granule manufacturing apparatus 10, or may be performed autonomously by the granule manufacturing apparatus 10.
[0024] In step S1, the raw material powder 9 placed on the support 1 is irradiated with a light beam 3 to bind the raw material powder 9. When the raw material powder 9 is irradiated with the light beam 3, a molten or sintered body of the raw material powder 9 floats slightly above the layer of the raw material powder 9 placed on the support 1, and roughly spherical grains of the raw material powder 9 are produced. As will be explained below, the binding of the raw material powder 9 includes the concepts of both melting the raw material powder 9 and sintering the raw material powder 9.
[0025] For example, if the light beam 3 has a sufficient heat quantity and the heat quantity of the light beam 3 raises the temperature of the raw material powder 9 to a temperature equal to or higher than the melting point, the raw material powder 9 will melt when the light beam 3 is irradiated onto the raw material powder 9. When irradiated with the light beam 3, the molten material of the raw material powder 9 floats slightly above the layer of the raw material powder 9 placed on the support 1. While floating, the molten material is formed into a roughly spherical shape by the surface tension of the liquid phase, and then, while it is falling slightly free, it is naturally cooled in the air or a specific gas atmosphere, becoming roughly spherical granules.
[0026] If the amount of heat possessed by the light beam 3 is insufficient and the temperature rise of the raw material powder 9 is below the melting point, the raw material powder 9 will be sintered when the light beam 3 is irradiated onto the raw material powder 9. Similar to a molten body, a sintered body of the raw material powder 9 will float slightly above the layer of raw material powder 9 placed on the support 1 when irradiated with the light beam 3. The sintered body is formed into a roughly spherical shape while floating, and then, while it is falling slightly freely, it is naturally cooled in the air or a specific gas atmosphere, becoming roughly spherical granules.
[0027] In another embodiment, a granule can be produced by irradiating a light beam 3 onto a mixed raw material powder 9, chemically reacting the raw material powder 9 with the raw material powder 9, and bonding the compound produced by the chemical reaction. An example of such a raw material powder 9 is lithium carbonate (Li2CO3) and titanium oxide (TiO2). That is, in another embodiment, a raw material powder 9 in which lithium carbonate powder and titanium oxide powder are mixed is irradiated with the light beam 3, chemically reacting the raw material powder 9 with the raw material powder 9, and bonding the lithium titanate (Li2TiO3) produced by the chemical reaction.
[0028] In this embodiment and other embodiments, the size of the bound particles can be changed by changing the energy of the irradiated light beam 3. In addition, the density of the produced particles 90 can be changed by changing the energy of the irradiated light beam 3. For example, in the other embodiment described above, lithium titanate (Li2TiO3) and carbon dioxide gas (CO2) are generated by the chemical reaction represented by Li2CO3+ TiO2→ Li2TiO3+ CO2, which changes the density of the produced particles 90.
[0029] In step S2, if the production of granules is to be completed (Yes in step S2), the series of steps is completed. If the production is not to be completed (No in step S2), the process continues to step S3.
[0030] The decision as to whether or not to end the production of granules may be made by an operator (user) of the granule production apparatus 10, or may be made autonomously by the controller 5. When the operator makes the decision to end, the operator operates the controller 5 to stop the operation of the light source 2 and the moving mechanism 6. When the controller 5 makes the decision to end, the decision to end is made, for example, by pre-recording in the memory of the controller 5 the value of the number of times the process of step S1 is executed, and the controller 5 makes the decision to end based on this pre-recorded value. The controller 5 stops the operation of the light source 2 and the moving mechanism 6 based on the decision result.
[0031] In step S3, the irradiation position of the light beam 3 on the raw material powder 9 is moved. This causes a relative movement between the position of the raw material powder 9 and the irradiation position of the light beam 3 irradiated onto the raw material powder 9. Fig. 3 is a schematic diagram for explaining, in a plan view, the movement of the irradiation position of the light beam in a granule manufacturing method according to one embodiment of the present invention.
[0032] In this embodiment, the moving mechanism 6 is driven to move the irradiation position 31 of the light beam 3 on the raw material powder 9 in the directions of the X-axis and Y-axis shown in the figure. When the raw material powder 9 is irradiated with the light beam 3 in a pulsed manner in step S1, the irradiation position 31 of the light beam 3 moves by one arrow shown in the figure, for example, each time the light beam 3 is irradiated once in a pulsed manner. In the embodiment shown in the figure, the irradiation position 31 of the light beam 3 moves in a zigzag manner so as to form successive S's.
[0033] In another embodiment, the irradiation position 31 of the light beam 3 may be moved in one direction. Alternatively, the moving mechanism 6 may be configured using a turntable, for example, to move the irradiation position 31 of the light beam 3 on the raw material powder 9 in a circular manner in the circumferential direction.
[0034] After performing the process of step S3, the series of steps are subsequently repeated from step S1, thereby making it possible to continuously produce a plurality of granules of the raw material powder 9. Table 1 shows various conditions exemplified in the granule production method according to this embodiment and the performance of the granules produced. [Table 1]
[0035] Fig. 4 is a photograph showing the appearance of granules produced by the granule production method according to one embodiment of the present invention, Fig. 5 is an electron microscope photograph of granules produced by the granule production method according to one embodiment of the present invention, and Fig. 6 is a graph showing the diameter distribution of granules produced by the granule production method according to one embodiment of the present invention.
[0036] As shown in Figs. 4 to 6, the size of the granules 90 of the raw powder 9 produced is, for example, about 0.4 mm to about 1 mm in diameter. The size of the granules 90 can be controlled by changing the output of the light source 2 or by changing the pulse width of the light beam 3, that is, by changing the energy of the light beam 3. As shown in the electron microscope photograph of Fig. 5, the granules 90 are generally spherical with high sphericity, and the surfaces of the granules 90 are generally smooth. As shown in the graph of Fig. 6, the diameters of the granules 90 produced by the granule production method according to this embodiment are distributed within a range of ±120 µm with a center of about 780 µm for about 63.2% of the total number, and the standard deviation of the diameters of the granules 90 is less than about 120 µm. The slope of the graph, whose vertical axis is expressed in common logarithm, rises sharply from about 700 µm to about 800 µm in diameter, and it can be seen that the median value of the diameter distribution is within this range.
[0037] In the conventional method of Patent Document 1, dispersion and aggregation of the raw powder occurs when the raw powder falls, making it difficult to control the size of the resulting granules. Such dispersion and aggregation of the raw powder when the raw powder falls is believed to be due to the type of raw powder, the particle size of the raw powder, and the particle size distribution of the powder. Also, in the conventional method of Patent Document 1, as shown in Figure 3, the average diameter of the resulting granules increases when the laser output is increased, but the non-uniformity of the size is not improved.
[0038] In contrast, according to the granule manufacturing method of this embodiment, the raw material powder 9 is placed on the support 1. The raw material powder 9 floats from the layer of the raw material powder 9 due to the irradiation of the light beam 3 for only a short time, and the raw material powder 90 falls freely for only a short time. Therefore, the size of the resulting granules 90 can be controlled by controlling the output of the light source 2 or the pulse width of the light beam 3. In the granule manufacturing method of this embodiment, the raw material powder 9 is placed on the support 1, and unlike the conventional method of Patent Document 1, the raw material powder 9 does not fall before the raw material powder 9 is irradiated with the light beam 3, and the raw material powder does not disperse or aggregate before the raw material powder 9 is irradiated with the light beam 3. As shown in the graph of FIG. 6, the size nonuniformity of the resulting granules is improved compared to the conventional method of Patent Document 1.
[0039] 7 is a graph showing the results of X-ray diffraction measurement of granular powder produced by a granular production method according to one embodiment of the present invention. In the graph, the measurement data for the powder of granules 90 produced from raw material powder 9 is shown by a solid line, and the measurement data for raw material powder 9 itself, which is used for comparison, is shown by a dashed line. The vertical axis of the graph shows the diffraction intensity of X-rays, and the horizontal axis of the graph shows the diffraction angle of X-rays.
[0040] By irradiating the raw material powder 9 with the light beam 3, the raw material powder 9 melts, and there is concern that the melting may cause the granules 90 to become amorphous. However, when the measurement data shown by the solid line is compared with the measurement data shown by the dashed line, the diffraction peak positions are roughly the same. This shows that the granules 90 manufactured from the raw material powder 9 by the granule manufacturing method according to this embodiment maintain the crystal structure of the original raw material powder 9 (specifically, β-Li2TiO3: monoclinic type) and are not amorphous. [effect]
[0041] As described above, the granule manufacturing method and granule manufacturing apparatus of the present invention can provide a simplified method and apparatus for mass-producing granules.
[0042] According to the granule manufacturing method of the present invention, granules 90 can be manufactured through a single process of irradiating raw material powder 9 with light beam 3, and therefore the granule manufacturing process can be significantly simplified. The size of the manufactured granules 90 varies little, and the yield is high. For this reason, the granule manufacturing method of the present invention is suitable for mass production of granules.
[0043] Furthermore, the crystal structure of the produced granules 90 maintains the crystal structure of the original raw material powder 9. For this reason, the effect of the granule production method of the present invention on the crystal structure of the granules is extremely slight or negligible.
[0044] The granule manufacturing method and apparatus of the present invention are particularly suitable for producing lithium titanate microspheres to be used as tritium breeding materials in nuclear fusion reactors.
[0045] In the granule manufacturing method of the present invention, lithium titanate microspheres with high sphericity can be manufactured by using lithium titanate as the raw material powder 9. The lithium titanate microspheres are used as tritium breeding materials in nuclear fusion reactors, and improving the sphericity of the lithium titanate microspheres increases the mechanical strength of the tritium breeding material, making it possible to prevent the breeding material from being destroyed by thermal stress during the operation of the nuclear fusion reactor.
[0046] Furthermore, when the sphericity of the lithium titanate microspheres is improved, the size matching with the neutron multiplier material (e.g., beryllium microspheres) filled together with the lithium titanate in the blanket surrounding the plasma in the nuclear fusion reactor is improved, and the filling rate of the tritium breeding material and the neutron multiplier material in the blanket is improved. Illustratively, the diameter ratio of the beryllium microspheres and the lithium titanate microspheres filled in the blanket is about 5:1 to about 10:1. [Other formats]
[0047] Although the present invention has been described above with reference to specific embodiments, the present invention is not limited to the above-described embodiments.
[0048] The raw material powder 9 is not limited to lithium ceramics, and various ceramics such as alumina (AL2O3) and zirconia (ZrO2) can be used for the raw material powder 9 as long as the raw material powder 9 can be bound. In addition, the raw material powder 9 is not limited to ceramics, and various metals and organic substances can be used for the raw material powder 9 as long as the raw material powder 9 can be bound.
[0049] The light beam 3 may be capable of binding the raw material powder 9, and the light beam 3 irradiated to the raw material powder 9 does not need to be pulsed, and the light beam 3 may be irradiated continuously. In this case, for example, the raw material powder 9 may be bound by scanning the light beam 3 while being continuously irradiated with the light beam 3. [Explanation of symbols]
[0050] 1 Support 2 light source 3 rays 4 Optical system 5. Controller 6 Moving mechanism 9 Raw material powder 10 Granule manufacturing equipment 31 Irradiation position 41 Mirror 42 Condenser Lens 51,52 Control line 90 grains
Claims
1. A method for producing granules of raw material powder, comprising irradiating a YAG laser beam onto a raw material powder containing one or more of Li2O, Li2TiO3, Li4SiO4, Li2ZrO3, and Li2CO3, which is placed on a support, to bond the raw material powder.
2. 2. A method for producing granules according to claim 1, characterized in that the light beam is irradiated while the position of the raw material powder and the irradiation position of the light beam irradiated onto the raw material powder are moved relatively.
3. 3. A method for producing granules as described in claim 1 or 2, characterized in that the light beam is irradiated to a mixture of multiple types of raw material powders, causing a chemical reaction between the multiple types of raw material powders, and producing granules in which compounds produced by the chemical reaction are bound together.
4. A method for producing granules according to any one of claims 1 to 3, characterized in that the energy of the light beam is varied to vary the size of the granules.
5. A support for placing a raw material powder containing one or more of Li2O, Li2TiO3, Li4SiO4, Li2ZrO3, and Li2CO3 as a single substance or a mixture thereof; a light source that irradiates a YAG laser beam to bind the raw material powder; An apparatus for producing granules of the raw material powder, comprising:
6. 6. The apparatus for producing granules according to claim 5, further comprising a moving mechanism for relatively moving a position of the raw material powder and an irradiation position of the light beam irradiated onto the raw material powder.
7. The support has a plurality of types of mixed raw material powders placed thereon, The apparatus for manufacturing granules described in claim 5 or 6, characterized in that the light source irradiates the light beam for chemically reacting the plurality of types of raw material powders and manufacturing granules in which compounds produced by the chemical reaction are bound together.
Citation Information
Patent Citations
Preparation method of transparent camouflage material
CN110372384A
Production of spherical particle
JP1987125843A
Production of inorganic compound by combustion synthesis reaction
JP2000262889A
Method for making powdery fine particle into granule by baking
JP2001137685A
metal oxide particles
JP2002529352A