Ferritic stainless steel sheet and its manufacturing method

By employing controlled cold rolling and specific chemical compositions, the method enhances ferritic stainless steel's formability and surface smoothness, addressing the challenges of deep drawing and surface roughness in ferritic stainless steel sheets.

JP7580254B2Active Publication Date: 2024-11-11NIPPON STEEL CORPORATION
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020190026
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-16
Publication Date
2024-11-11
Estimated Expiration
2040-11-16

AI Technical Summary

Technical Problem

Ferritic stainless steel sheets face challenges in achieving both deep drawing formability and resistance to surface roughness after forming, leading to prolonged polishing times and significant dust generation.

Method used

A method involving controlled cold rolling in multiple directions, including an oblique direction, combined with specific chemical compositions and heat treatment, to create a fine-grained ferritic stainless steel structure with enhanced {111} orientation and reduced {411} orientation, improving the r-value and surface smoothness.

Benefits of technology

The method results in a ferritic stainless steel sheet with excellent formability and reduced surface roughness, enabling efficient and low-dust polishing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580254000001
    Figure 0007580254000001
  • Figure 0007580254000002
    Figure 0007580254000002
  • Figure 0007580254000003
    Figure 0007580254000003
Patent Text Reader

Abstract

To provide a ferritic stainless steel sheet which is excellent in moldability and surface characteristics after molding, and a method for manufacturing the same.SOLUTION: A ferritic stainless steel sheet comprises, by mass%, 11.0% or more and 30.0% or less Cr, 0.001% or more and 0.030% or less C, 0.01% or more and 2.00% or less Si, 0.01% or more and 2.00% or less Mn, 0.005% or more and 0.100% or less P, 0.0100% or less S, 2.00% or less Al, 0.030% or less N, further comprises one or two of 0.50% or less Ti and 1.00% or less Nb, and the balance Fe with inevitable impurities, is composed of a ferrite monolayer structure having a crystal grain size number measured according to JIS G 0551 of 9.0 or more, and has a random intensity ratio in a crystal orientation in a surface parallel to a rolled surface at a plate thickness 1 / 2 position of I{111}<112>≥9, I{111}<110>≥6 and I{411}<148>≤1, where I{hkl}<uvw> represents a random intensity ratio of an {hkl}<uvw> orientation.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic stainless steel sheet having excellent formability during forming and polishability after forming, and a method for producing the same. The present invention is particularly suitable for applications requiring polishing to remove surface irregularities of the steel sheet after forming. [Background technology]

[0002] SUS304 (18Cr-8Ni), a representative austenitic stainless steel, is widely used in home appliances, kitchenware, building materials, etc. due to its excellent corrosion resistance, workability, and aesthetics. However, the steel plate is considered expensive because it contains a large amount of Ni, which is expensive and the price fluctuates greatly. On the other hand, ferritic stainless steel does not contain Ni, or contains only a very small amount of Ni, so demand for it as a material with excellent cost performance is increasing.

[0003] When used for forming applications, austenitic stainless steels are easy to work harden and have excellent stretchability. In addition, because it is relatively easy to create a fine-grained structure in austenitic stainless steels, fine-grained steel sheets with a grain size number of about 10 are manufactured. For this reason, surface irregularities (rough skin) after forming are small and are hardly a problem. As mentioned above, austenitic stainless steels have both formability and resistance to surface irregularities after forming.

[0004] On the other hand, when using ferritic stainless steel for forming purposes, the problems are formability and surface irregularities after forming. The stretchability of ferritic stainless steel is low and cannot be changed significantly. However, since deep drawability can be controlled by changing the crystal orientation (texture), ferritic stainless steel is often formed using forming methods that mainly involve deep drawing.

[0005] The r-value (Lankford value) is used as an index of deep drawing characteristics. Generally known methods for improving the r-value of ferritic stainless steel sheets include reducing C and N and adding stabilizing elements such as Ti and Nb, or by growing crystal grains, and ferritic stainless steel sheets with high r-values ​​are manufactured using these methods.

[0006] However, ferritic stainless steel sheets are more likely to have coarse grains than austenitic stainless steel sheets. This is because the recrystallized grain size tends to be large, and the addition of Ti and Nb makes the grains grow more easily. In addition, if grain growth is used to ensure a high r-value, the r-value will decrease if grain growth is not allowed in order to obtain fine-grained steel.

[0007] As described above, it is difficult for a ferritic stainless steel sheet to achieve both deep drawability and resistance to surface roughening after forming.

[0008] When relatively strict formability is required, such as for the housings of home appliances or utensils, high-purity ferritic stainless steels such as SUS430LX are often used. In most cases, the thickness of stainless steel sheets used to ensure strength after forming is 0.6 mm or more, and as mentioned above, the crystal grain size is large, so the surface is rough after forming. For this reason, polishing is usually used to remove the unevenness.

[0009] Patent Document 1 discloses a method for improving the deep drawability of high-purity ferritic stainless steel while reducing surface roughness, specifically, a method for improving the r-value by grain growth in the final annealing process of a ferritic stainless steel containing Ti and / or Nb. However, the obtained grain size number is 7 or less, which is a coarse grain, and the surface is prone to roughness during processing.

[0010] Patent Document 2 discloses a technology relating to a ferritic stainless steel sheet that contains Ti and / or Nb, has a ferritic single-phase structure with a grain size number exceeding 9.0, and has excellent formability during forming and surface properties after forming, by controlling the random intensity ratio of crystal orientation in a plane parallel to the rolled surface at the 1 / 2 position and the 1 / 10 position of the sheet thickness. This technology is carried out by a manufacturing method with a high cold rolling reduction of 93% or more. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2003-73782 A [Patent Document 2] JP 2019-26913 A [Non-patent literature]

[0012] [Non-Patent Document 1] Hiroshi Inoue; Light Metals, vol42, No6(1992), p358. Summary of the Invention [Problem to be solved by the invention]

[0013] When considering the forming of ferritic stainless steel sheets, there are currently no steel sheets that can be formed into the required strict shapes and that can satisfy the required surface properties after forming. For this reason, in the case of ferritic stainless steel sheets, the polishing process after forming takes a long time and generates a lot of dust during polishing.

[0014] In view of the above, an object of the present invention is to provide a ferritic stainless steel sheet having excellent formability and surface properties after forming, and a method for producing the same. [Means for solving the problem]

[0015] The present inventors have thoroughly investigated the recrystallization process during the final annealing of ferritic stainless steel sheets. As a result, it was found that the {100} <011> It was found that, as the rolled structure having an orientation close to that of the surrounding recrystallized grains is encroached upon and recrystallization is completed, the surrounding recrystallized grains grow, causing the recrystallized grain size to increase.

[0016] Next, the {100} <011> We explored manufacturing conditions to reduce the grain orientation and facilitate recrystallization. As a result, we found that by combining cold rolling in an oblique direction with rolling in a single direction, the {100} <011> It was found that the number of misoriented grains was reduced, recrystallization became easier, and the r-value improved dramatically after recrystallization.

[0017] By performing part of the cold rolling in an oblique direction, it is possible to obtain a recrystallized structure in which the surrounding recrystallized grains remain fine without growing until recrystallization is complete. This makes it possible to produce a metal structure with a high r-value and mainly composed of grains with a {111} orientation, thereby achieving both deep drawability and resistance to surface roughness during processing.

[0018] In addition, by making the surface of the steel sheet fine-grained, it is possible to reduce surface roughness after forming. At the same time, by increasing the concentration of the {111} orientation while decreasing the concentration of other orientations, the r-value, which is an index of deep drawability, can be increased. In particular, the {411} orientation, which tends to accumulate together with the {111} orientation, <148> By reducing the concentration of the particles in the matrix, a high r-value can be obtained, making it possible to perform severe deep drawing.

[0019] In order to obtain the above structure, multiple rolling directions are combined during cold rolling. Ideally, rolling in the 0° direction and the 45° direction from the original rolling direction should be combined at approximately the same rolling reduction ratio to obtain the {100} <011> It is possible to suppress accumulation in orientations other than {111} during cold rolling and to suppress accumulation in orientations other than {111} after annealing.

[0020] The present invention has been made based on the above findings, and the gist of the present invention is as follows.

[0021] (1) In mass%, Cr: 11.0% or more and 30.0% or less, C: 0.001% or more and 0.030% or less, Si: 0.01% or more and 2.00% or less, Mn: 0.01% or more and 2.00% or less, P: 0.005% or more and 0.100% or less, S: 0.010% or less, Al: 2.00% or less, and N: 0.030% or less, and further contains one or two of Ti: 0.50% or less and Nb: 1.00% or less, with the balance being Fe and impurities, the metal structure is a ferrite single layer structure with a grain size number of 9.0 or more measured in accordance with JIS G 0551, and the random intensity ratio of the crystal orientation in a plane parallel to the rolling surface at the 1 / 2 position of the plate thickness is I {111}<112> ≧9, I {111}<110> ≧6, I {411}<148> A ferritic stainless steel sheet characterized in that I≦1. {hkl} <uvw>< / uvw> is {hkl} <uvw>The random intensity ratio of the orientation is shown.

[0022] (2) The ferritic stainless steel sheet according to (1) above, further comprising, in mass %, one or more of the following groups A to C: Group A: Sn: 0.50% or less, Ni: 1.00% or less, Cu: 1.00% or less, Mo: 2.00% or less W: 1.00% or less, Co: 0.50% or less, V: 0.50% or less, Zr: 0.50% or less, and Sb: 0.50% or less One or more of the following Group B: B: 0.0025% or less, Ca: 0.0050% or less, Mg: 0.0050% or less One or more of the following Group C: Y: 0.20% or less, Hf: 0.20% or less, REM: 0.10% or less One or more of the following

[0023] (3) The ferritic stainless steel sheet according to (1) or (2) above, characterized in that the average r-value is 1.5 or more.

[0024] (4) The ferritic stainless steel sheet according to any one of (1) to (3) above, which is used for a housing of a home appliance or for an article.

[0025] (5) A method for producing a ferritic stainless steel sheet according to any one of (1) to (3) above, comprising a hot rolling step of hot rolling a steel slab having the composition of (1) or (2) above to obtain a hot rolled steel sheet, a cold rolling step of cold rolling the hot rolled steel sheet to obtain a cold rolled steel sheet, and a heat treatment step of heat treating the cold rolled steel sheet to obtain a heat treated steel sheet, wherein in the cold rolling step, a cold rolling reduction ratio RT is set to 50% or more and 90% or less, and a part of the cold rolling includes cold rolling with a cold rolling reduction ratio RC of 20% or more in an oblique direction at an angle of 20° or more and 70° or less with respect to the direction of the hot rolling.

[0026] (6) The method for producing a ferritic stainless steel sheet according to (5) above, characterized in that part of the cold rolling further includes cold rolling in the same direction as the hot rolling at a cold rolling reduction rate RL of 20% or more.

[0027] (7) The method for producing a ferritic stainless steel sheet according to (6) above, further comprising a hot-rolled sheet annealing step of annealing the hot-rolled steel sheet between the hot rolling step and the cold rolling step. Effect of the Invention

[0028] According to the present invention, a ferritic stainless steel sheet having excellent formability and surface properties after forming can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Each of the requirements of the present invention will be described in detail below. Note that the "%" for the content of each element means "% by mass."

[0030] (I) Chemical composition

[0031] The ferritic stainless steel sheet of the present invention has the following chemical compositions. The reasons for limiting the chemical compositions are explained below.

[0032] Cr: 11.0% or more, 30.0% or less

[0033] Cr is an element that improves corrosion resistance, which is a basic property of stainless steel. If the content is less than 11.0%, sufficient corrosion resistance cannot be obtained, so the lower limit is set to 11.0%. On the other hand, excessive addition promotes the formation of intermetallic compounds equivalent to σ, which promotes cracking during manufacturing and reduced formability, so the upper limit is set to 30.0%. From the viewpoint of stable manufacturing (yield, rolling defects, etc.), 14.0 to 25.0% is preferable. More preferably, it is 16.0 to 20.0%.

[0034] C: 0.001% or more, 0.030% or less

[0035] C is an element that reduces formability (r value), which is important in the present invention, so the less C the better, with the upper limit set at 0.030%. However, an excessive reduction in C content leads to an increase in refining costs, so the lower limit is set at 0.001%. When both refining costs and formability are taken into consideration, a content of 0.002 to 0.018% is preferable.

[0036] Si: 0.01% or more, 2.00% or less

[0037] Silicon is an element that improves oxidation resistance, but excessive addition leads to a decrease in formability, so the upper limit is set to 2.0%. From the viewpoint of formability, a lower content is preferable, but an excessively reduced content leads to an increase in raw material costs, so the lower limit is set to 0.01%. From the viewpoint of manufacturability, the preferred range is 0.05 to 0.30%.

[0038] Mn: 0.01% or more, 2.00% or less

[0039] Like Si, the addition of a large amount of Mn reduces formability, so the upper limit is set at 2.00%. From the standpoint of formability, a lower content is preferable, but an excessive reduction in formability leads to an increase in raw material costs, so the lower limit is set at 0.01%. From the standpoint of manufacturability, the preferred range is 0.05 to 0.30%.

[0040] P: 0.005% or more and 0.100% or less

[0041] Since P is an element that reduces formability (r-value and product elongation), the lower the content, the better, with the upper limit set at 0.100%. However, in order to utilize the r-value-improving effect of phosphide precipitation, the lower limit is set at 0.005%. In addition to the fact that an excessive reduction in P leads to an increase in raw material costs, when both formability and manufacturing costs are taken into consideration, the preferred range is 0.010 to 0.070%, more preferably 0.020 to 0.050%.

[0042] S: 0.010% or less

[0043] S is an unavoidable impurity element that promotes cracking during manufacturing, so the lower the content, the better, with the upper limit set at 0.010%. The lower the S content, the better, and 0.003% or less is preferable. The lower limit is 0. However, since an excessive decrease leads to an increase in refining costs, the lower limit may be set at 0.001%. From the standpoint of manufacturability and cost, the preferred range is 0.001 to 0.002%.

[0044] Al: 2.00% or less

[0045] Al is an element effective in improving corrosion resistance and oxidation resistance. Excessive addition not only leads to a decrease in formability, but also leads to an increase in alloy costs and an impairment of manufacturability, so the upper limit is set to 2.00%. The inclusion of Al is not essential, and the lower limit is 0. In order to obtain the effect of improving corrosion resistance and oxidation resistance, the preferable lower limit of the content is set to 0.01%.

[0046] N: 0.030% or less

[0047] N, like C, is an element that reduces formability (r value), and the upper limit is set to 0.030%. The smaller the N content, the more preferable, and the lower limit is 0. However, since an excessive reduction leads to an increase in refining costs, the lower limit may be set to 0.002%. From the viewpoints of formability and manufacturability, the preferred range is 0.005 to 0.015%.

[0048] Furthermore, one or both of Ti and Nb are contained within the following ranges.

[0049] Ti: 0.50% or less Ti improves the r-value and product elongation through high purification by fixing C and N as precipitates. Although these effects can be obtained even with a small amount of content, in order to obtain the effects effectively, the lower limit is preferably set to 0.03%. On the other hand, excessive addition leads to an increase in alloy cost and a decrease in manufacturability due to an increase in recrystallization temperature, so the upper limit is set to 0.50%. From the viewpoints of formability and manufacturability, the preferred range is 0.05 to 0.40%. Furthermore, the suitable range for actively utilizing the effects of Ti is 0.10 to 0.30%.

[0050] Nb: 1.00% or less Like Ti, Nb also improves the r-value and product elongation through the high purification of steel due to its action as a stabilizing element that fixes C and N. In order to obtain these effects, when added, the lower limit is preferably set to 0.03%. On the other hand, excessive addition leads to an increase in alloy cost and a decrease in manufacturability due to an increase in recrystallization temperature, so the upper limit is set to 1.00%. From the viewpoints of alloy cost and manufacturability, the preferred range is 0.03 to 0.50%. Furthermore, the suitable range for actively utilizing the effects of Nb is 0.04 to 0.30%, and more preferably 0.06 to 0.10%.

[0051] In addition to the above basic composition, the following elements may be selectively added.

[0052] Group A elements: Sn: 0.50% or less, Ni: 1.00% or less, Cu: 1.00% or less, Mo: 2.00% or less W: 1.00% or less, Co: 0.50% or less, V: 0.50% or less, Zr: 0.50% or less, Sb: 0.50% or less

[0053] Sn, Ni, Cu, Mo, W, Co, V, Zr, and Sb are elements effective in improving corrosion resistance and oxidation resistance, and one or more of them are added as necessary. However, excessive addition not only leads to a decrease in formability, but also leads to an increase in alloy cost and an impairment of manufacturability, so the upper limit of Ni, Cu, and W is 1.00%, and the upper limit of Mo is 2.00%. The upper limit of Sn, Co, V, and Zr is 0.50%. The effect of improving corrosion resistance and oxidation resistance can be obtained even with a small amount of content. In particular, in the case of Sn and Sb, it is preferable to contain 0.005% or more to ensure the effect. In the case of Ni, Cu, Mo, W, Co, V, and Zr, the preferable lower limit of the content is 0.05%.

[0054] Group B elements: B: 0.0025% or less, Ca: 0.0050% or less, Mg: 0.0050% or less

[0055] B, Ca, and Mg are elements that improve hot workability and secondary workability, and one or more of them are added as necessary. However, excessive addition leads to impaired manufacturability, so the upper limit of B is 0.0025%, and the upper limits of Ca and Mg are 0.0050%. Although the effect of improving hot workability and secondary workability can be obtained even with a small amount of content, in the case of B, it is preferable to contain 0.0001% or more to ensure the effect. In consideration of manufacturability and hot workability, a more preferable range of B is 0.0003 to 0.0012%, and a preferable range of Ca and Mg is 0.0002 to 0.0010%.

[0056] Group C elements: Y: 0.20% or less, Hf: 0.20% or less, REM: 0.10% or less

[0057] Y, Hf, and REM are elements effective for improving hot workability and cleanliness of steel and improving oxidation resistance, and one or more of them may be added as necessary. When added, the upper limit of Y and Hf is 0.20%, and the upper limit of REM is 0.10%. Although the effect of improving hot workability and cleanliness of steel can be obtained even with a small content, the preferable lower limit is 0.001%. Here, REM is an element belonging to atomic number 57 to 71, such as La, Ce, Pr, Nd, etc.

[0058] In addition to the elements described above, other elements may be contained within a range that does not impair the effects of the present invention. It is preferable to reduce Bi, Pb, Se, H, Ta, etc. as much as possible, but one or more of Bi≦100 ppm, Pb≦100 ppm, Se≦100 ppm, H≦100 ppm, and Ta≦500 ppm may be contained as necessary within a range that does not affect the effects of the present invention.

[0059] (II) Metal structure

[0060] The metal structure will now be described.

[0061] The ferritic stainless steel sheet of the present invention has a metal structure which is a ferritic single layer structure having a grain size number of 9.0 or more as measured in accordance with JIS G 0551.

[0062] Since the larger the grain size number, the less likely the surface roughness after processing after molding is to occur, the grain size number is set to 9.0 or more. In order to further suppress the surface roughness, the grain size number is preferably 9.5 or more, and more preferably 10.0 or more.

[0063] The measurement method of the grain size number is the line segment method of JIS G 0551 (2013). Grain size number: 9 corresponds to an average line segment length of 14.1 μm per crystal grain crossing the grain, and grain size number: 10 corresponds to an average line segment length of 10.0 μm per crystal grain crossing the grain. The grain size measurement is performed using an optical microscope structure photograph of the cross section of the test piece, with the number of crossed grains per sample being 500 or more. The etching solution is preferably aqua regia or inverse aqua regia, but other solutions can be used as long as the grain boundaries can be identified. Also, depending on the orientation relationship of adjacent grains, the grain boundaries may not be clearly visible, so it is preferable to etch darkly. Also, twin grain boundaries are not measured when measuring the grain boundaries.

[0064] A ferritic single-phase metal structure means that it does not contain austenite or martensite. If these phases are included, it is relatively easy to make the grain size fine, and the austenite phase exhibits high formability due to the TRIP effect. However, the raw material cost increases, and the yield is likely to decrease due to edge cracks during manufacturing.

[0065] Whether the structure is a ferrite single phase or not can be checked by EBSD (Electron Backscatter Diffraction) measurement. In the present invention, in addition to judging the austenite phase by EBSD measurement of the cross section, the region with an IQ value lower than 3000 when an EBSD pattern is taken under the conditions of an acceleration voltage of 15 kV and a focal length of 19 mm is regarded as a martensite phase, and if the area ratio of austenite and martensite is 1 / 100 or less of the total, it is judged to be a ferrite single phase.

[0066] (III) Collective structure

[0067] The texture will now be described.

[0068] In the ferritic stainless steel sheet of the present invention, the workability can be improved by controlling the random intensity ratio of the crystal orientation in the plane parallel to the rolled surface at the 1 / 2 position of the sheet thickness within the following range.

[0069] I {111}<112> ≧9 I {111}<110> ≧6 I {411}<148> <= 1

[0070] {111} <112> The {111} orientation is known to be generated as a recrystallization orientation in high purity steel and to be an orientation that improves formability. It is required to increase it when performing forming processes such as deep drawing. Since this is the orientation that is most likely to have a strong random strength ratio when a sufficient cold rolling rate is ensured, the random strength ratio is set to 15 or more. <112> Since a higher random strength ratio is more advantageous for formability, it is preferably 18 or more, and more preferably 20 or more.

[0071] {111} <110> The direction is also <112> Like the {111} orientation, it is a recrystallization orientation in high purity steel and improves formability. <110> The direction is {111} <112> Compared to the direction, this is a direction in which the concentration is less likely to increase. <112> The random intensity ratio is high, and the {111} <110> When the degree of integration of {111} is low, the anisotropy of the r-value becomes large, and when forming is performed by deep drawing, the height of the edge becomes large, leading to a decrease in yield. <110> It is also desirable that the orientation is highly concentrated, i.e. {111} <110> The random intensity ratio is set to 10 or more, preferably 12 or more, and more preferably 14 or more.

[0072] {411} <148> Since the orientation is not favorable for formability, the random intensity ratio is set to 1 or less, preferably 0.7 or less, and more preferably 0.5 or less. <148> is easily generated as a recrystallization orientation, and until now it has not been possible to sufficiently reduce its concentration, making it impossible to obtain high formability.

[0073] In the present invention, the {111} <112> and {111} <110> It also increases the concentration of orientation, <148> The feature of this method is that it establishes ideal crystal orientation control that reduces the degree of orientation concentration, and simultaneously satisfies these random intensity ratios.

[0074] Also, <148> By suppressing the accumulation in the {111} orientation, it is possible to increase the degree of accumulation in the {111} orientation, which is advantageous for improving formability.

[0075] The random intensity ratio of the crystal orientation is measured by the following method.

[0076] X-ray diffraction is performed at 1 / 2t of the sheet thickness t on a plane parallel to the rolled surface of the steel sheet. The 1 / 2t position often shows the average texture of the steel material and can be an index of formability. Using the obtained data, a 3D orientation analysis is performed using the Bunge method described in Non-Patent Document 1. The random intensity ratio in the relevant orientation is read from the crystal orientation distribution diagram.

[0077] (IV) r value

[0078] We will explain the r value.

[0079] The ferritic stainless steel sheet of the present invention preferably has an average r-value (Lankford value) of 1.5 or more. By making the average r-value 1.5 or more, the formability of the ferritic stainless steel sheet is improved, and severe processing can be performed, while the load during forming can be reduced, and wear of the mold can be suppressed. The average r-value is more preferably 1.7 or more.

[0080] The average r-value is measured by the plastic strain ratio test method of JIS Z 2254 (2008), and can be calculated by the following formula (1) in accordance with JIS Z 2254 (2008).

[0081] Average r value = (r0 + 2r 45 +r 90 ) / 4 · · Equation (1)

[0082] In the formula (1), r0 is the r value in the rolling direction, r 90 is the r value in the direction perpendicular to the rolling direction, r 45 indicates the r-value in the 45 degree rolling direction.

[0083] Next, a method for producing the ferritic stainless steel sheet of the present invention will be described.

[0084] (I) Hot rolling process

[0085] The stainless steel slab having the above-mentioned components is heated and then hot-rolled, consisting of rough rolling and finish rolling, to obtain a hot-rolled steel sheet. If the slab heating temperature is too high, Ti carbosulfide (Ti4C2S2) dissolves during heating, increasing the amount of solute carbon, and reprecipitation during the hot rolling process delays recrystallization. These phenomena inhibit the development of recrystallization texture in the product sheet and deteriorate workability. In addition, the crystal grains are significantly enlarged, and coarse elongated grains are formed in the hot rolling process, deteriorating the workability of the product sheet. In addition, excessive temperature reduction causes surface defects and leads to deterioration of corrosion resistance due to rusting from the defects. For this reason, the slab heating temperature is preferably 1100 to 1250°C. Furthermore, in consideration of the decrease in productivity due to rolling roll seizure, the slab heating temperature is preferably 1130 to 1230°C.

[0086] (II) Hot-rolled sheet annealing process

[0087] Following the hot rolling, hot-rolled sheet annealing may be performed for the purpose of recrystallization, but is not essential.

[0088] By performing hot-rolled sheet annealing, it is possible to reduce surface defects that occur during forming, called ridging, of the product. Hot-rolled sheet annealing is preferably performed in the range of T to T + 50°C, where T is the recrystallization temperature. If the temperature is too low, poor recrystallization occurs and the effect of reducing ridging cannot be sufficiently obtained, and if the temperature is too high, the crystal grains become enlarged, and the random strength ratio of a specified crystal orientation cannot be improved after cold-rolled annealing, resulting in deterioration of the workability of the product sheet. However, since it is possible to reduce ridging more than in the conventional method by performing cold rolling as described below, hot-rolled sheet annealing may be omitted.

[0089] After hot-rolled sheet annealing (if hot-rolled sheet annealing is omitted), surface scale is formed after hot rolling, and if problems such as surface defects occur in subsequent processes, a descaling treatment such as pickling may be performed as necessary.

[0090] (III) Cold rolling process

[0091] Cold rolling rate RT:50~90%

[0092] Following descaling, which is carried out as necessary, cold rolling is carried out. If the cold rolling rate RT is too low, the metal structure becomes coarse and the random strength ratio of the {111} orientation decreases, so the lower limit of the cold rolling rate RT is 50%. It is preferably 55% or more, and more preferably 60% or more. Moreover, if the cold rolling rate RT is too high, it actually decreases the formability, so the upper limit is 90%. It is preferably 87% or less, and more preferably 85% or less.

[0093] Diagonal rolling angle: 20~70° Total cold rolling ratio RC: 20% or more

[0094] The cold rolling of the present invention is characterized in that it is not cold rolling in only the hot rolling direction, but is rolling in an oblique direction under the above conditions. <112> and {111} <110> The random intensity ratio of the orientation is improved. <148> The random intensity ratio of the orientation is reduced, and at the same time, the grain size can be reduced.

[0095] By combining cold rolling in the diagonal direction, {111} <112> and {111} <110> The random intensity ratio of the orientation is improved. <148> The reason why the random intensity ratio of the orientation can be decreased while the grain size can be reduced is considered to be as follows.

[0096] During cold rolling, {001} <110> or {112} <110> , {111} <110> It is known that the grains accumulate in the cold rolling preferred orientations such as {001} <110> It is known that the orientation of the cold rolling is the rate-determining factor for the completion of recrystallization because the cold rolling strain is less likely to accumulate in the {001} direction. <110> Direction, for example {100} <001> The orientation of the cold rolling can be changed to one that is easy to accumulate strain and easy to recrystallize, and a fine grain structure can be obtained to hasten the completion of recrystallization. <001> The rolling orientation of the {411} <148> It is known that it easily recrystallizes in orientations that are unfavorable to formability, such as {411} <148> It is believed that the ratio of grains with {111} orientation, which is advantageous for formability, increases due to the decrease in orientation.

[0097] The cold rolling direction is diagonal rolling at an angle of 20 to 70° to the direction of the hot rolling in the previous process, with a cold rolling reduction rate of 20% or more. If the diagonal rolling angle is less than 20°, the {411} <148> The effect of lowering the random strength ratio of {111} orientation, the effect of improving the random strength ratio of {111} orientation, and the effect of refining grains are not obtained, and improvement of formability and suppression of roughness of the processed surface cannot be realized, so the lower limit of the diagonal rolling angle is 20°. Similarly, at 70° or more, improvement of formability and grain refinement cannot be achieved, so 70° is the upper limit. Similarly, when the cold rolling rate RC in the diagonal direction is less than 20%, improvement of formability and grain refinement cannot be achieved, so the lower limit of the cold rolling rate RC is set to 20%.

[0098] Total cold rolling ratio in the hot rolling direction RL: 20% or more

[0099] The effect of the oblique rolling in the present invention is obtained by combining rolling in multiple directions, not simply by rolling obliquely. Therefore, in the case of a steel sheet that has been subjected to hot-rolled sheet annealing, in addition to cold rolling in the oblique direction at a cold rolling reduction rate RC, cold rolling in the hot rolling direction at a cold rolling reduction rate RL of 20% or more is performed.

[0100] However, when annealing of the hot-rolled sheet is omitted, the cold rolling in the hot rolling direction may be omitted since the desired effect can be obtained by combining the hot rolling direction and cold rolling in an oblique direction.

[0101] (IV) Heat treatment process (finish annealing process)

[0102] The cold-rolled steel sheet obtained by the above-mentioned cold rolling is subjected to a heat treatment for the purpose of recrystallization to obtain a heat-treated steel sheet. The heat treatment temperature is preferably in the range of T to T + 30°C, where T is the recrystallization temperature. If the temperature is too low, a non-recrystallized structure will be formed, deteriorating formability, and if the temperature is too high, grain growth will cause significant roughness of the processed surface. EXAMPLES

[0103] Next, an embodiment of the present invention will be described.

[0104] The stainless steels shown in Tables 1 and 2 were melted, hot rolled to the thicknesses shown in Tables 3 and 4, cold rolled to a thickness of 1.0 mm, and then cold-rolled to produce product sheets. Some of the hot-rolled sheets were annealed at 980°C for 2 minutes, followed by cold rolling and cold-rolled annealing. The process conditions were changed as shown in Table 2.

[0105] [Table 1]

[0106] [Table 2]

[0107] [Table 3]

[0108] [Table 4]

[0109] The manufactured stainless steel sheets were subjected to the following evaluations.

[0110] <Grain size number>

[0111] The grain size number was determined by the line method of JIS G 0551 (2013). A value of 9.0 or more, which indicates mild surface roughness after molding, was considered to pass.

[0112] <Random intensity ratio>

[0113] The random strength ratio was determined by performing X-ray diffraction at a position 1 / 2t of the sheet thickness t on a plane parallel to the rolled surface of the steel sheet, and using the obtained data, a three-dimensional orientation analysis was performed using the Bunge method described in Non-Patent Document 1. The I{111} orientation, which enables deep drawing with a drawing ratio of 2.4 or more, was determined. <112> ≧9, I{111} <110> ≧6, I{411} <148> A score of ≦1 was considered a pass.

[0114] <Average r value>

[0115] The average r-value was measured according to the plastic strain ratio test method of JIS Z 2254 (2008) and calculated using formula (1) in accordance with JIS Z 2254 (2008).

[0116] Average r value = (r0 + 2r 45 +r 90 ) / 4 · · Equation (1)

[0117] A drawing ratio of 1.50 or more, which is considered a guideline for deep drawing forming of 2.4 or more, was considered to be acceptable, and anything less than 1.50 was considered to be unacceptable.

[0118] <Moldability> A test piece with a diameter of 120 mm was cut out from the product plate, and a cup forming test was carried out with a drawing ratio of 2.4, which allows a cylinder with a height greater than the diameter to be formed in one process.The conditions for this test were punch diameter of 50 mm, punch shoulder R of 5R, clearance of 1.2 mm on one side, and lubrication between the steel plate and punch was performed by applying rust-preventive oil Z3 and then attaching a PTFE (polytetrafluoroethylene) sheet.

[0119] The formability of the samples that were able to complete the cup forming test with a drawing ratio of 2.4 was evaluated as "good", while the formability of the samples that broke during forming was evaluated as "poor".

[0120] <Skin roughness after molding>

[0121] For samples that could be formed with a drawing ratio of 2.4, the surface roughness after cup formation was evaluated using the arithmetic mean roughness Ra.

[0122] The surface roughness was measured according to JIS B 0601 using a contact type surface roughness measuring device over a length of 5 mm parallel to the height direction at a position 15 mm to 20 mm above the bottom of the cup on the inside of the vertical wall of the cup, and the arithmetic mean roughness Ra was calculated.

[0123] If the surface roughness after molding is mild and the removal of unevenness by rough polishing with a grit of about 80 is not necessary, the surface roughness after molding is deemed to pass if its arithmetic mean roughness Ra ≦ 1.2, and if Ra > 1.2, the removal of unevenness by rough polishing is essential, the surface roughness after molding is deemed to fail.

[0124] The evaluation results are shown in Table 5.

[0125] [Table 5]

[0126] According to the present invention, the random strength ratio can be controlled by appropriately selecting the cold rolling direction and the cold rolling rate, and a ferritic stainless steel sheet having excellent formability and abrasion resistance after forming can be obtained. As shown in Table 5, in the invention example, it was possible to complete forming without fracture at a drawing ratio of 2.4, and the surface roughness after processing was suppressed with Ra≦1.2 μm.

[0127] In the comparative examples c1, c4, c5, and c9 shown in Table 5, the grain size, random strength ratio, and average r-value are within the claimed range, but c1 has an excessive Cr content, c4 has an excessive Si content, c5 has an excessive Mn content, and c9 has an excessive Al content, which increases the strength and reduces the ductility, causing fracture during forming and making it impossible to complete the forming process. In addition, in the case of c14, the average r-value was high and cup forming was possible, but the grain size number was large, and the processing surface roughness after forming was significant. [Industrial Applicability]

[0128] According to the present invention, by performing only a part of the rolling in an oblique direction, it is possible to obtain properties far superior to those of the conventional manufacturing method of stainless steel sheets, and therefore the present invention has great industrial applicability. In addition, the product form is not important, and it can be a cut sheet or a coil. In particular, the present invention is suitable for applications requiring relatively strict formability, such as the housings of home appliances or utensils.< / uvw>

Claims

1. In mass percent, Cr: 11.0% or more, 30.0% or less, C: 0.001% or more, 0.030% or less, Si: 0.01% or more, 2.00% or less, Mn: 0.01% or more, 2.00% or less, P: 0.005% or more, 0.100% or less, S: 0.010% or less, Al: 0.05% or more and 2.00% or less, and N: 0.030% or less, Including, moreover, Ti: 0.50% or less, and Nb: 1.00% or less The balance is Fe and impurities. The metal structure is a ferrite single layer structure having a grain size number of 9.0 or more as measured in accordance with JIS G 0551, The random intensity ratio of the crystal orientation in a plane parallel to the rolling surface at the sheet thickness 1 / 2 position is I {111}<112> ≧9、 I {111}<110> ≧6、 I {411}<148> ≦1 A ferritic stainless steel sheet comprising: Here, I {hkl} <uvw>< / uvw> indicates the random intensity ratio in the {hkl}<uvw> directions.

2. The ferritic stainless steel sheet according to claim 1, further comprising, in mass %, one or more of the following groups A to C: Group A: Sn: 0.50% or less, Ni: 1.00% or less, Cu: 1.00% or less, Mo: 2.00% or less, W: 1.00% or less, Co: 0.50% or less, V: 0.50% or less, Zr: 0.50% or less, and Sb: 0.50% or less One or more of the following Group B: B: 0.0025% or less, Ca: 0.0050% or less, Mg: 0.0050% or less One or more of the following Group C: Y: 0.20% or less, Hf: 0.20% or less, REM: 0.10% or less One or more of the following

3. 3. The ferritic stainless steel sheet according to claim 1, wherein the average r-value is 1.5 or more.

4. The ferritic stainless steel sheet according to any one of claims 1 to 3, which is used for a housing of a home appliance or for an article.

5. A method for producing the ferritic stainless steel sheet according to any one of claims 1 to 3, comprising the steps of: A hot rolling process in which a steel slab having the composition according to claim 1 or 2 is hot rolled to obtain a hot rolled steel sheet; A cold rolling process of cold rolling the hot-rolled steel sheet to obtain a cold-rolled steel sheet; a heat treatment step of heat treating the cold-rolled steel sheet to obtain a heat-treated steel sheet; Equipped with In the cold rolling step, the cold rolling rate RT is set to 50% or more and 90% or less, and a part of the cold rolling includes cold rolling at an angle of 20° or more and 70° or less to the hot rolling direction at a cold rolling rate RC of 20% or more. A method for producing a ferritic stainless steel sheet comprising the steps of:

6. A part of the cold rolling further includes cold rolling at a cold rolling rate RL of 20% or more in the same direction as the hot rolling. The method for producing a ferritic stainless steel sheet according to claim 5 .

7. The method for producing a ferritic stainless steel sheet according to claim 6, further comprising a hot-rolled sheet annealing step of annealing the hot-rolled steel sheet between the hot rolling step and the cold rolling step.

Citation Information

Patent Citations

  • Manufacture of ferritic stainless steel sheet excellent in ridging property

    JP1998015601A

  • Ferritic stainless steel sheet excellent in ridging resistance and formability and its production method

    JP2001316775A

  • Ferritic stainless steel sheet superior in deep drawability

    JP2003073782A

  • Ferritic stainless steel sheet with excellent workability, and its manufacturing method

    JP2006193771A

  • Ferritic stainless steel sheet for exhaust component excellent in processability, steel tube and manufacturing method therefor