Hydrocarbon oil hydrotreating catalyst and method for producing the hydrotreating catalyst
A catalyst with a Si, Ti, and Al-based inorganic oxide support enhances metal dispersion and adsorption, addressing the challenge of high desulfurization performance in hydrotreating processes to meet stringent diesel fuel sulfur content regulations.
Patent Information
- Application Number
- JP2020169837
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-10-07
AI Technical Summary
Existing hydrotreating catalysts face challenges in achieving high desulfurization performance due to the limited interaction and dispersion of metal components on alumina-based supports, which are insufficient for meeting stringent sulfur content regulations in diesel fuel.
A catalyst comprising an inorganic oxide support with specific compositions of Si, Ti, and Al, ensuring high dispersion of metal components like molybdenum, tungsten, cobalt, and nickel, with a highly dispersed Ti state and enhanced nitric oxide adsorption, supported on a carrier with specific surface area and pore volume characteristics.
The catalyst achieves high desulfurization performance by maintaining Ti in a highly dispersed state, leading to increased active sites and improved desulfurization activity, effectively meeting stringent sulfur content regulations in diesel fuel.
Smart Images

Figure 0007586683000002 
Figure 0007586683000003 
Figure 0007586683000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a catalyst for hydrotreating a hydrocarbon oil and a method for producing the hydrotreating catalyst. [Background technology]
[0002] Conventionally, catalysts that have been widely used for the purpose of hydrotreating hydrocarbon oils are those in which a metal component selected from Group VIA and Group VIII elements of the periodic table is supported on a support made of a porous inorganic oxide such as alumina, alumina-silica, titania, or alumina-titania.
[0003] Currently, quality regulations on the sulfur content of fuel oil are being strengthened from the perspective of environmental protection. In particular, the sulfur content of diesel fuel is subject to strict regulations of 10 mass ppm or less. For this reason, development of diesel fuel ultra-deep desulfurization catalysts is underway to comply with these regulations.
[0004] For example, Patent Document 1 listed below discloses a catalyst in which a metal component selected from the elements of Groups VIA and VIII of the periodic table is supported on an alumina-silica-titania support. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-72928 A Summary of the Invention [Problem to be solved by the invention]
[0006] Titania has a stronger interaction with metal components such as molybdenum than alumina. Therefore, if titania is highly dispersed in a composite oxide support, the metal components can be supported in a highly dispersed state on the titania as a base point, and the number of active sites can be increased, which is expected to result in high desulfurization performance.
[0007] An object of the present invention is to provide a novel catalyst for hydrotreating hydrocarbon oils and a method for producing the hydrotreating catalyst. [Means for solving the problem]
[0008] One aspect of the present invention relates to a catalyst for hydrotreating a hydrocarbon oil, comprising an inorganic oxide support containing Si, Ti, and Al, and at least one metal component selected from the group consisting of elements of Groups 6, 8, 9, and 10 of the periodic table, wherein the inorganic oxide support has an Al content of 60% by mass or more calculated as Al2O3, a Si content of 1.0 to 10.0% by mass calculated as SiO2, and a Ti content of 12.0 to 30.0% by mass calculated as TiO2, the inorganic oxide support has an absorption edge wavelength of 350 nm or less of an absorption peak derived from Ti as measured by ultraviolet spectroscopy, and an adsorption amount of nitric oxide of 7.5 cc / ml or more as measured by nitric oxide adsorption.
[0009] In one embodiment, the inorganic oxide support may be one in which, in X-ray diffraction analysis, diffraction peaks showing the crystal structure of anatase type titania (101) plane and rutile type titania (110) plane are substantially not detected.
[0010] The hydrotreating catalyst according to one embodiment has a specific surface area (SA) of 150 m 2 / g or more, and the pore volume (PV) may be 0.30 ml / g or more.
[0011] In one embodiment, the metal component may include at least one selected from the group consisting of molybdenum, tungsten, cobalt, and nickel.
[0012] In one embodiment, the content of the metal component may be 1 to 35 mass % calculated as the oxide.
[0013] Another aspect of the present invention is a method for producing the hydrotreating catalyst, comprising the steps of: ,ofthe first aqueous solution, in which the content of the titanium mineral acid salt is 0.15 to 0.70 in terms of a molar ratio relative to the mineral acid, and the mineral acid in the titanium mineral acid salt is the same type of acid as the mineral acid in the titanium mineral acid salt, is mixed with a second aqueous solution containing a basic aluminum salt to obtain a mixed solution having a pH of 6.5 to 9.5, thereby obtaining a carrier precursor precipitated in the mixed solution; washing, shaping, drying and firing the carrier precursor to obtain a carrier; and supporting at least one metal component selected from the group consisting of Group 6 elements, Group 8 elements, Group 9 elements and Group 10 elements of the periodic table on the carrier to obtain the hydrotreatment catalyst.
[0014] In one embodiment, the first aqueous solution may be prepared at 60° C. or below.
[0015] In one embodiment, the first aqueous solution and / or the second aqueous solution may contain silicate ions. Effect of the Invention
[0016] According to the present invention, there are provided a novel catalyst for hydrotreating hydrocarbon oils and a method for producing the hydrotreating catalyst. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a diagram showing X-ray diffraction spectra of inorganic oxide supports in Example 1 and Comparative Example 4. [Diagram 2] FIG. 1 is a diagram showing vectors of diffuse reflection of ultraviolet and visible light of inorganic oxide supports in Example 1 and Comparative Example 4. [Diagram 3] FIG. 2 is a graph showing the amount of nitric oxide adsorbed by hydrotreating catalysts in Example 1 and Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Preferred embodiments of the present invention will now be described in detail.
[0019] <Hydrotreatment catalyst> The hydrotreating catalyst according to this embodiment contains an inorganic oxide support containing Si, Ti, and Al, and at least one metal component selected from the group consisting of Group 6, Group 8, Group 9, and Group 10 elements of the periodic table. In this embodiment, the inorganic oxide support has an Al content of 60 mass% or more in terms of Al2O3, an Si content of 1.0 to 10.0 mass% in terms of SiO2, and an Ti content of 12.0 to 30.0 mass% in terms of TiO2. In this embodiment, the inorganic oxide support has an absorption edge wavelength of 350 nm or less of an absorption peak derived from Ti measured by ultraviolet spectroscopy. In addition, the amount of nitric oxide adsorption measured by nitric oxide adsorption is 7.5 cc / ml or more.
[0020] Titania has a stronger interaction with metal components such as molybdenum than alumina, so if titania is highly dispersed in the composite oxide support, the metal components are supported in a highly dispersed state on the titania as a base point, and the number of active sites increases, so that high desulfurization performance can be expected. The hydrotreatment catalyst according to this embodiment has Ti in a highly dispersed state and adsorbs a large amount of nitrogen monoxide, so that high desulfurization performance can be expected.
[0021] It is known that nitric oxide molecules selectively adsorb to metal component sites in catalysts (e.g., Hyomen Kagaku vol. 30, No. 2, pp. 92-97), and that these metal component sites (e.g., edge sites of molybdenum sulfide in sulfurized catalysts) are reaction sites for desulfurization reactions. Therefore, catalysts that adsorb a large amount of nitric oxide have a large number of edge sites and are considered to have high desulfurization activity.
[0022] (Inorganic oxide carrier) The inorganic oxide support contains Si, Ti, and Al. The Al content in the inorganic oxide support, calculated as Al2O3, is 60 mass% or more based on the total amount of the inorganic oxide support. The Si content in the inorganic oxide support, calculated as SiO2, is 1.0 to 10.0 mass% based on the total amount of the inorganic oxide support. The Ti content in the inorganic oxide support, calculated as TiO2, is 12.0 to 30.0 mass% based on the total amount of the inorganic oxide support.
[0023] The Al content is not particularly limited as long as it is 60% by mass or more, but from the viewpoint of further increasing the surface area and strength of the hydrotreating catalyst, it is preferably 65% by mass or more, and more preferably 70% by mass or more. The Al content may be, for example, 85% by mass or less. Here, if the alumina content is 60% by mass or more, there is little risk of the moldability of the single body, the surface area and strength of the catalyst decreasing. If the alumina content is less than 85% by mass, the Ti content does not become relatively low, and the effect of Ti is easily exerted.
[0024] The Si content is not particularly limited as long as it is 1.0 to 10.0 mass%, but from the viewpoint of further increasing the surface area of the hydrotreating catalyst and the dispersibility of Ti, it is preferably 1.5 mass% or more, and more preferably 2.0 mass% or more. Also, from the viewpoint of uniforming the pore size in the inorganic oxide support, the Si content is preferably 7.0 mass% or less, and more preferably 5.0 mass% or less.
[0025] The Ti content is not particularly limited as long as it is 12.0 to 30.0 mass%, but from the viewpoint of fully exerting the effect of Ti, it is preferably 15.0 mass% or more, and more preferably 18.0 mass% or more. Also, from the viewpoint of effectively suppressing the aggregation of TiO2, the Ti content is preferably 25.0 mass% or less, and more preferably 23.0 mass% or less.
[0026] The inorganic oxide support may further contain other elements in addition to Si, Ti, and Al. Examples of the other elements include P, B, and Zr. When the inorganic oxide support contains other elements, the content of these elements may be, for example, 1% by mass or more and 20% by mass or less in terms of the oxide of each element based on the total amount of the inorganic oxide support.
[0027] In the inorganic oxide support according to this embodiment, it is preferable that diffraction peaks showing the crystal structure of the anatase titania (101) plane and the rutile titania (110) plane measured by X-ray diffraction analysis (hereinafter also referred to as "titania diffraction peaks") are not substantially detected. Here, when titania diffraction peaks are detected, the crystallization of titania proceeds and the specific surface area effective for the reaction decreases. Therefore, even if the amount of titania is increased too much, the desulfurization performance is not achieved to a degree commensurate with its economical efficiency, and the catalyst does not become one of the objects of the present invention, which is to maintain Ti contained in the support in a more highly dispersed state.
[0028] The X-ray diffraction analysis is performed using an X-ray diffractometer (RINT2100 manufactured by Rigaku Corporation), and the measurement sample is measured by pressing the powder onto a non-reflective plate for measurement. The diffraction peak showing the crystal structure of the anatase titania (101) plane is measured at 2θ=25.5°, and the diffraction peak showing the crystal structure of the rutile titania (110) plane is measured at 2θ=27.5°. In this specification, "substantially no titania diffraction peak is detected" means that neither the diffraction peak measured at 2θ=25.5° nor the diffraction peak measured at 2θ=27.5° is detected, and for example, the peak intensity of these diffraction peaks is 0.01 or less, where the peak intensity of the diffraction peak showing the aluminum crystal structure attributed to the γ-alumina (400) plane measured at 2θ=45.9° is taken as 1.
[0029] In the inorganic oxide support, the absorption edge wavelength of the absorption peak derived from Ti measured by ultraviolet spectroscopy is 350 nm or less. If the absorption edge wavelength is 350 nm or less, the dispersibility of Ti in the support can be maintained well. On the other hand, the lower limit of the absorption edge wavelength is not particularly limited, but may be, for example, 325 nm or more from the viewpoint of ensuring a sufficient content of Ti in the support.
[0030] In this specification, the absorption edge wavelength of the absorption peak measured by ultraviolet spectroscopy refers to the wavelength indicating the absorption edge of the ultraviolet-visible light diffuse reflectance spectrum measured by an ultraviolet-visible spectrophotometer, and more specifically, refers to the maximum wavelength at which the spectral intensity value is 0.3 or more when the absorption intensity is subjected to KM conversion using the Kubelka-Munk function (KM function).
[0031] For inorganic oxide supports, the specific surface area (SA) measured by the BET method is, for example, 280 m 2 / g or more, preferably 290m 2 / g or more. The specific surface area (SA) is 280m 2 When the specific surface area (SA) is 450 m / g or more, the metal components described below can be supported in a highly dispersed manner, and the deterioration of the desulfurization performance can be more effectively suppressed. 2 / g or less, preferably 430m 2 / g or less. The specific surface area (SA) is 450m 2 If the content is 0.1 to 1.0 wt % or less, the decrease in the catalyst strength can be more effectively suppressed.
[0032] In the inorganic oxide carrier, the pore volume (PV) measured by the water pore filling method may be, for example, 0.45 ml / g or more, preferably 0.50 ml / g or more. The pore volume (PV) may be, for example, 0.80 ml / g or less, preferably 0.70 ml / g or less. If the pore volume (PV) is 0.80 ml / g or less, the decrease in catalyst strength can be more effectively suppressed.
[0033] (Metal Components) In this embodiment, the metal component supported on the inorganic oxide support is at least one selected from the group consisting of Group 6 elements, Group 8 elements, Group 9 elements, and Group 10 elements of the periodic table. Here, "Group 6 elements", "Group 8 elements", "Group 9 elements", and "Group 10 elements" are names based on the IUPAC-style long periodic table (new periodic table). In addition, based on the short periodic table (old periodic table), "Group 6 elements" are sometimes referred to as "Group VIA elements", and "Group 8 elements", "Group 9 elements", and "Group 10 elements" are sometimes collectively referred to as "Group VIII elements". Examples of the metal components of Group 6 elements include molybdenum (Mo) and tungsten (W), and examples of the metal components of Groups 8 elements, 9 elements, and 10 elements include iron (Fe), cobalt (Co), and nickel (Ni). These metal components may be used alone or in combination of two or more.
[0034] The content of the metal components may be 1 to 35 mass% in terms of oxides based on the total amount of the hydrotreating catalyst, and is preferably 15 to 30 mass%. In particular, the content of metal components of Group 6 elements is preferably 10 to 30 mass% in terms of oxides based on the total amount of the hydrotreating catalyst, and more preferably 13 to 24 mass%. The total content of Group 8 elements, Group 9 elements, and Group 10 elements is preferably 1 to 10 mass% in terms of oxides, and more preferably 2 to 6 mass%.
[0035] The metal components of the hydrotreating catalyst according to this embodiment are preferably dissolved using an acid, preferably phosphoric acid and / or an organic acid.
[0036] When phosphoric acid is used, the phosphorus content is preferably 1 to 10 mass% and more preferably 2 to 6 mass% calculated as oxide (P2O5) based on the total amount of the hydrotreating catalyst. If the content is 10 mass% or less, there is no risk of the catalytic performance decreasing, and if it is 1 mass% or more, sufficient stability of the metal component solution can be ensured.
[0037] When an organic acid is used, the organic acid is preferably 35 to 75% by mass, more preferably 55 to 65% by mass, based on the metal components of Group 8, Group 9, and Group 10 elements. If the organic acid is 75% by mass or less, the increase in viscosity of the solution containing the metal components (hereinafter also referred to as "supported metal-containing solution") can be suppressed, and if the organic acid is 35% by mass or more, sufficient stability of the supported metal-containing solution can be ensured, and there is no risk of the catalytic performance being reduced. Here, the organic acid is preferably a carboxylic acid compound, and specific examples thereof include citric acid, malic acid, tartaric acid, and gluconic acid.
[0038] The method for supporting or incorporating the metal component, or further phosphorus and / or organic acid on the support is not particularly limited, and known methods such as impregnation methods (e.g., equilibrium adsorption method, pore filling method, incipient wetness method) using a compound containing the metal component, or further a compound containing phosphorus and / or an organic acid, and ion exchange methods can be used. Here, the impregnation method refers to a method in which a support is impregnated with a solution containing the metal component, and then dried and calcined.
[0039] In the impregnation method, it is preferable to simultaneously support the metal components of Group 8, Group 9, and Group 10 elements and the metal component of Group 6 element. If the metals are supported separately, the desulfurization activity may be insufficient.
[0040] (Hydrotreatment catalyst) In hydrotreating catalysts, the specific surface area (SA) measured by the BET method is, for example, 150 m 2 / g or more, preferably 170m 2 / g or more. Specific surface area (SA) is 150m 2 If the specific surface area (SA) is 270 m / g or more, the active sites of the desulfurization reaction can be maintained, and the deterioration of the desulfurization performance can be more effectively suppressed. 2 / g or less, preferably 250m 2 / g or less. The specific surface area (SA) is 270m 2 If the content is 0.1 to 1.0 wt % or less, the decrease in the catalyst strength can be more effectively suppressed.
[0041] In the hydrotreating catalyst, the pore volume (PV) measured by the water pore filling method may be, for example, 0.30 ml / g or more, and preferably 0.35 ml / g or more. The pore volume (PV) may be, for example, 0.60 ml / g or less, and preferably 0.50 ml / g or less. If the pore volume (PV) is 0.60 ml / g or less, the decrease in the catalyst strength can be more effectively suppressed.
[0042] In the hydrotreating catalyst, the amount of nitric oxide adsorbed is 7.5 cc / ml or more as measured by nitric oxide adsorption. As described above, in this embodiment, the hydrotreating catalyst has a large amount of nitric oxide adsorption, so that high desulfurization activity can be expected.
[0043] The amount of nitrogen monoxide adsorption in the hydrotreating catalyst is measured by the following method. Using a fully automatic catalyst gas adsorption amount measuring device (manufactured by Ohkura Riken), a mixed gas of helium gas and nitrogen monoxide gas (nitrogen monoxide concentration 10% by volume) is pulsed into the sulfurized hydrotreating catalyst, and the amount of nitrogen monoxide molecules adsorbed per gram of hydrotreating catalyst is measured. The amount of adsorption is then converted to the compact bulk density (CBD) of the catalyst. More specifically, about 0.02 g of the catalyst crushed to 60 mesh or less is weighed out and filled into a quartz cell, the catalyst is heated to 360°C, and a gas of 5% by volume of hydrogen sulfide / 95% by volume of hydrogen is passed through the catalyst at a flow rate of 0.2 L / min to perform a sulfurization treatment for 1 hour, and then H2 gas is switched to and held at 340°C for 1 hour, and the physically adsorbed hydrogen sulfide is discharged from the system. Then, nitric oxide molecules are adsorbed at 50°C using a mixed gas of helium gas and nitric oxide gas, and the amount of nitric oxide molecules adsorbed is measured.
[0044] The hydrotreating catalyst according to the present embodiment is suitable for use in the hydrotreating (hydrodesulfurizing) of hydrocarbon oils, particularly light oil fractions. That is, hydrodesulfurizing using the hydrotreating catalyst according to the present invention is carried out, for example, by packing the catalyst in a fixed bed reactor and carrying out the hydrodesulfurization under a hydrogen atmosphere under high temperature and high pressure conditions.
[0045] Examples of light oil fractions include straight-run light oil obtained from an atmospheric distillation unit for crude oil, vacuum light oil obtained by treating straight-run heavy oil or residual oil obtained from an atmospheric distillation unit in a vacuum distillation unit, catalytically cracked light oil obtained by catalytically cracking vacuum heavy light oil or desulfurized heavy oil, and hydrocracked light oil obtained by hydrocracking vacuum heavy light oil or desulfurized heavy oil.
[0046] <Method of manufacturing hydrotreating catalyst> The method for producing the hydrotreating catalyst according to the present embodiment will be described. The method for producing the hydrotreating catalyst according to the present embodiment comprises the steps of: ,of The method includes a step of mixing a first aqueous solution containing a titanium mineral salt having a molar ratio of 0.15 to 0.70 relative to the mineral acid, the mineral acid being the same as that in the titanium mineral salt, with a second aqueous solution containing a basic aluminum salt to obtain a mixed solution having a pH of 6.5 to 9.5, and obtaining a carrier precursor precipitated in the mixed solution (hereinafter also referred to as "first step"), a step of washing, shaping, drying and firing the carrier precursor to obtain a carrier (hereinafter also referred to as "second step"), and a step of supporting at least one metal component selected from the group consisting of Group 6 elements, Group 8 elements, Group 9 elements and Group 10 elements on the carrier to obtain a hydrotreating catalyst (hereinafter also referred to as "third step"). Each step will be described below.
[0047] (1st step) The first step is a step of mixing a first aqueous solution containing a titanium mineral salt and a mineral acid with a second aqueous solution containing a basic aluminum salt to obtain a mixed solution having a pH of 6.5 to 9.5, and obtaining a support precursor precipitated in the mixed solution. Here, the first aqueous solution is usually an acidic aqueous solution in which the molar ratio of the titanium mineral salt to the mineral acid is 0.15 to 0.70, and the second aqueous solution is usually a basic aqueous solution.
[0048] Examples of the titanium mineral salt contained in the first aqueous solution include titanium tetrachloride, titanium trichloride, titanyl sulfate, titanium sulfate, titanium nitrate, etc., and in particular, titanyl sulfate is preferably used because it is inexpensive. Examples of the mineral acid include hydrochloric acid, sulfuric acid, nitric acid, etc., and in particular, sulfuric acid is preferably used because it is economical. From the viewpoint of more effectively adjusting the titania diffraction peak measured by X-ray diffraction analysis of the inorganic oxide support and the absorption edge wavelength of the Ti-derived absorption peak measured by ultraviolet spectroscopy analysis, there is no particular limitation as long as the molar ratio of the titanium mineral salt to the mineral acid is 0.15 to 0.70, but from the viewpoint of obtaining the support precursor at a low cost, it is preferable that it is 0.20 to 0.65. Usually, a method of precipitating an alumina precursor by using a solution containing an acidic aluminum salt in an acidic solution is known, but the inclusion of an acidic aluminum salt is undesirable because it tends to cause aggregation of the titania precursor. Examples of the basic aluminum salt contained in the second aqueous solution include sodium aluminate and potassium aluminate.
[0049] In the first step, the first aqueous solution and / or the second aqueous solution contain silicate ions, but the timing of adding silicate ions (silicic acid compound) to the first aqueous solution and / or the second aqueous solution is not particularly limited. For example, the first aqueous solution may be prepared by adding and mixing a titanium mineral salt, a mineral acid, and a silicate ion substantially simultaneously, or an aqueous solution containing a titanium mineral salt and a mineral acid may be prepared, and silicate ions may be added and mixed immediately before mixing with the second aqueous solution to prepare the first aqueous solution. Similarly, the second aqueous solution may be prepared by adding and mixing a basic aluminum salt and a silicate ion substantially simultaneously, or an aqueous solution containing a basic aluminum salt may be prepared, and silicate ions may be added and mixed immediately before mixing with the first aqueous solution to prepare the second aqueous solution.
[0050] The contents of the titanium mineral salt and mineral acid contained in the first aqueous solution, the basic aluminum salt contained in the second aqueous solution, and the silicate ions contained in the first aqueous solution and / or the second aqueous solution are not particularly limited, and can be appropriately adjusted so that the Al content of the inorganic oxide support obtained in the second step described below is 60 mass% or more calculated as Al2O3, the Si content is 1.0 to 10.0 mass% calculated as SiO2, and the Ti content is 12.0 to 30.0 mass% calculated as TiO2.
[0051] When the first aqueous solution contains silicate ions, the silicate compound used may be, for example, an acidic or neutral silicate compound. An example of an acidic silicate compound is silicic acid, and the SiO2 concentration is preferably 5.0 mass% or less. On the other hand, when the second aqueous solution contains silicate ions, the silicate compound used may be, for example, a basic or neutral silicate compound. An example of a basic silicate compound is sodium silicate, and the SiO2 concentration is preferably 5.0 mass% or less.
[0052] The conditions for preparing the first aqueous solution are not particularly limited, but from the viewpoint of ensuring the stability of the titanium mineral acid salt in the first aqueous solution, for example, the temperature during preparation is preferably 60° C. or lower. Moreover, from the viewpoint of facilitating dissolution of the titanium mineral acid salt, the temperature during preparation of the first aqueous solution may be, for example, room temperature or higher, and is preferably 30° C. or higher.
[0053] In the first step, the mixed solution obtained by mixing the first aqueous solution and the second aqueous solution has a pH of 6.5 to 9.5. By setting the pH of the mixed solution within the above numerical range, the support precursor can be stably precipitated in the mixed solution. The pH of the mixed solution is preferably 6.5 to 8.5, and more preferably 6.5 to 7.5. This makes it easier to remove impurities from the support precursor.
[0054] The method of mixing the first aqueous solution and the second aqueous solution is preferably a method of adding the first aqueous solution to the second aqueous solution and mixing them. As a method of addition, it is preferable to continuously add the first aqueous solution to the second aqueous solution. The time from the start of addition to the completion of addition is not particularly limited, and may be, for example, 5 to 20 minutes, or may be 7 to 15 minutes. In particular, when the first aqueous solution is added to the second aqueous solution and mixed, it is preferable that the time is 13 minutes or less from the viewpoint of sufficiently suppressing the generation of crystals such as bayerite and gibbsite in addition to pseudo-boehmite and more effectively ensuring the specific surface area of the obtained hydrotreating catalyst.
[0055] Other conditions for mixing the first aqueous solution and the second aqueous solution are not particularly limited. For example, the second aqueous solution may be placed in a container equipped with a stirrer, heated and maintained at a temperature of usually 40 to 80° C., preferably 55 to 70° C., and the first aqueous solution heated to a temperature of ±5° C., preferably ±2° C., more preferably ±1° C. of the second aqueous solution may be added to mix the first aqueous solution and the second aqueous solution.
[0056] (2nd process) The second step is a step in which the support precursor obtained in the first step is washed, shaped, dried and calcined to obtain a support (inorganic oxide support).
[0057] The conditions for calcining the support precursor are not particularly limited, but for example, the calcination temperature may be 400 to 700° C., 450 to 600° C., or 500 to 570° C. The calcination time may be, for example, 0.5 to 10 hours, or 2 to 5 hours.
[0058] The carrier precursor to be calcined may be heated and kneaded as desired to form a moldable kneaded product, which may then be molded into a desired shape by extrusion molding or the like, and dried at, for example, 70 to 150°C, preferably 90 to 130°C.
[0059] When calcining the carrier precursor, the carrier precursor may be washed or aged to remove by-product salts, if desired. Examples of the washing liquid for washing the carrier precursor include an aqueous ammonia solution. Examples of the aging method include aging at 80 to 100°C for 5 to 20 hours while stirring using an aging tank equipped with a reflux condenser.
[0060] (3rd step) The third step is a step of supporting at least one metal component selected from the group consisting of Group 6 elements, Group 8 elements, Group 9 elements, and Group 10 elements on the support (inorganic oxide support) obtained in the second step to obtain a hydrotreating catalyst.
[0061] The method for supporting the metal component on the support is not particularly limited, and can be, for example, impregnation, immersion, etc. Examples of raw metal compounds for supporting the metal component on the support include iron nitrate, iron sulfate, nickel nitrate, nickel carbonate, cobalt nitrate, cobalt carbonate, molybdenum trioxide, ammonium molybdate, ammonium paratungstate, ammonium metatungstate, etc.
[0062] When the metal component supported on the carrier contains a metal component of a Group 6 element, it is preferable to dissolve the metal component using an acid. In this case, examples of the acid include phosphoric acid and organic acids. When phosphoric acid is used, the content of phosphoric acid may be 3 to 25 parts by mass, or 10 to 15 parts by mass, calculated as the oxide, per 100 parts by mass of the metal component of the Group 6 element, from the viewpoint of ensuring stable solubility while maintaining catalytic performance.
[0063] In the third step, after the metal components are supported on the support by the above-mentioned method, the support may be calcined as desired to prepare a hydrotreating catalyst. The calcination conditions are not particularly limited, and for example, the calcination temperature may be 400 to 700° C., 450 to 600° C., or 500 to 570° C. The calcination time may be, for example, 0.5 to 5 hours, or 1 to 3 hours.
[0064] Although the hydrotreating catalyst and the method for producing the same according to the present invention have been described above, the present invention is not limited to the above-mentioned embodiments.
[0065] For example, in the production of a hydrotreating catalyst, the hydrotreating catalyst obtained in the above-mentioned third step can be presulfided in a reactor to produce a presulfided hydrotreating catalyst. More specifically, the hydrotreating catalyst may be contacted with a mixed oil of a petroleum distillate (hydrocarbon oil) containing sulfur compounds and a sulfiding agent (dimethyl sulfide, dimethyl disulfide, carbon disulfide, etc.) at 200 to 400°C (preferably 240 to 340°C) under a hydrogen atmosphere of normal pressure or higher hydrogen partial pressure (e.g., 2 to 15 MPa) to perform presulfidation to obtain a presulfided hydrotreating catalyst, or the hydrotreating catalyst may be simply contacted with hydrogen sulfide under the same conditions as above to obtain a presulfided hydrotreating catalyst.
[0066] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments. EXAMPLES
[0067] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0068] Example 1 <Preparation of Support Precursor> A 100-L tank equipped with a steam jacket was charged with 10.5 kg of a 22% by mass aqueous sodium aluminate solution (manufactured by JGC Catalysts and Chemicals Co., Ltd.) calculated as Al2O3, and diluted with 51 kg of ion-exchanged water. Then, 1.80 kg of a 5% by mass aqueous sodium silicate solution (manufactured by AGC Si-Tech Co., Ltd.; SiO2 concentration 24% by mass) calculated as SiO2 was added with stirring, and the mixture was heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt.
[0069] Solution A was prepared by dissolving 1.82 kg of 33 mass% titanyl sulfate (manufactured by Teika Corporation) converted to TiO2 in 10 kg of ion-exchanged water, and then mixed with 7.62 kg of 25 mass% sulfuric acid (solution B) and heated to 50°C to prepare a first aqueous solution containing titanium mineral acid salt and sulfuric acid.
[0070] The molar ratio of the titanium mineral salt to the mineral acid was 0.39. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant rate over 10 minutes using a roller pump until the pH reached 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) a was precipitated was obtained. The time from mixing of solution A and solution B to the completion of the addition of the first aqueous solution to the second aqueous solution (addition completion time) was 30 minutes.
[0071] <Preparation of inorganic oxide support> The resulting mixture was stirred at 60°C for 1 hour, dehydrated using a flat filter, and further washed with 150L of 0.3% by mass ammonia aqueous solution. The washed cake-like carrier precursor a was diluted with ion-exchanged water to 10% by mass in terms of Al2O3, and then the pH was adjusted to 10.5 with 15% by mass ammonia aqueous solution. The resulting diluted solution was transferred to an aging tank equipped with a reflux condenser, and aged at an aging temperature of 95°C for 10 hours while stirring. The mixture after aging was dehydrated, and concentrated and kneaded to a predetermined water content while kneading with a twin-arm kneader equipped with a steam jacket. The kneaded product obtained was molded into a cylindrical shape with a diameter of 1.6 mm using an extrusion molding machine, and dried at 110°C. The dried molded product was fired in an electric furnace at a temperature of 550°C for 3 hours to obtain an inorganic oxide carrier a containing Si, Ti, and Al.
[0072] Inorganic oxide support a contained 77% by mass of Al in terms of Al2O3, 3% by mass of Si in terms of SiO2, and 20% by mass of Ti in terms of TiO2, all based on the total amount of the support. The properties of inorganic oxide support a (pore volume (PV) and specific surface area (SA)) were measured according to the methods shown below.
[0073] In addition, the inorganic oxide support a was subjected to X-ray diffraction analysis according to the method described above. The analysis results are shown in Figure 1. From the analysis results, a peak at 2θ=25.5° assigned to the anatase-type titania (101) plane and a peak at 2θ=27.5° assigned to the rutile-type titania (110) plane were not detected.
[0074] Furthermore, the ultraviolet-visible light diffuse reflectance spectrum of inorganic oxide support a was analyzed according to the method described below. The analysis results are shown in Figure 2. The absorption edge wavelength of inorganic oxide support a was calculated from the analysis results to be 337 nm.
[0075] <Preparation of Hydrotreating Catalyst> Next, 267 g of molybdenum trioxide (Climax Corp.; MoO3 concentration 99% by mass) and 54 g of cobalt carbonate (Tanaka Chemical Laboratory Co., Ltd.; CoO concentration 61% by mass) were suspended in 500 ml of ion-exchanged water, and the suspension was heated at 95°C for 5 hours using an appropriate reflux device so as not to reduce the volume of the liquid, and then 54 g of phosphoric acid (Kanto Chemical Co., Ltd.; P2O5 concentration 62% by mass) was added and dissolved to prepare an impregnation solution. The obtained impregnation solution was sprayed onto 1000 g of the inorganic oxide support a to impregnate it, and then the support was dried at 250°C and calcined in an electric furnace at a calcination temperature of 550°C for 1 hour to obtain a hydrotreating catalyst A1.
[0076] The metal components in the hydrotreating catalyst A1 were 20 mass % MoO3, 2.5 mass % CoO, and 2.5 mass % P2O5, all based on the total mass of the catalyst.
[0077] The amount of nitric oxide adsorbed by the hydrotreating catalyst A1 was measured according to the method described above. The results are shown in Figure 3. The amount of nitric oxide adsorbed by the hydrotreating catalyst A was 8.2 cc / ml.
[0078] Furthermore, the properties (pore volume (PV) and specific surface area (SA)) of the hydrotreating catalyst A1 were measured according to the methods described below. Table 1 shows the properties.
[0079] Example 2 11.2 kg of a 22% by mass sodium aluminate aqueous solution in terms of Al2O3 was added, diluted with 52 kg of ion-exchanged water, and 1.80 kg of a 5% by mass sodium silicate solution in terms of SiO2 was added while stirring and heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt. 1.36 kg of a 33% by mass titanyl sulfate in terms of TiO2 was dissolved in 8 kg of ion-exchanged water, mixed with 9.28 kg of 25% by mass sulfuric acid, and heated to 50°C to prepare a first aqueous solution containing titanium mineral salt and sulfuric acid. The molar ratio of titanium mineral salt to mineral acid was 0.24. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant speed using a roller pump over 10 minutes until the pH became 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) b was precipitated was obtained.
[0080] Support b was obtained from support precursor b in the same manner as in Example 1. Support b contained 82 mass % of Al calculated as Al2O3, 3 mass % of Si calculated as SiO2, and 15 mass % of Ti calculated as TiO2, all based on the total mass of the support.
[0081] X-ray diffraction analysis was carried out in the same manner as in Example 1 (not shown), but the diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were not detected.
[0082] Furthermore, the absorption edge wavelength of the inorganic oxide support b was calculated in the same manner as in Example 1 and was found to be 329 nm.
[0083] Catalyst B was prepared from carrier b in the same manner as in Example 1. Catalyst B contained 20 mass % of MoO3, 2.5 mass % of CoO, and 2.5 mass % of P2O5.
[0084] The amount of nitric oxide adsorbed was measured in the same manner as in Example 1. The amount of nitric oxide adsorbed by the hydrotreating catalyst B was 8.0 cc / ml.
[0085] Example 3 9.84 kg of sodium aluminate aqueous solution of 22% by mass in terms of Al2O3 was added, diluted with 51 kg of ion-exchanged water, and 1.80 kg of sodium silicate solution of 5% by mass in terms of SiO2 was added while stirring and heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt. 2.27 kg of titanyl sulfate of 33% by mass in terms of TiO2 was dissolved in 13 kg of ion-exchanged water, mixed with 6.00 kg of sulfuric acid of 25% by mass, and heated to 50°C to prepare a first aqueous solution containing titanium mineral salt and sulfuric acid. The molar ratio of titanium mineral salt to mineral acid was 0.61. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant speed using a roller pump over 10 minutes until the pH became 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) c was precipitated was obtained.
[0086] Support c was obtained from support precursor c in the same manner as in Example 1. Support c contained 72 mass % of Al calculated as Al2O3, 3 mass % of Si calculated as SiO2, and 25 mass % of Ti calculated as TiO2, all based on the total mass of the support.
[0087] X-ray diffraction analysis was carried out in the same manner as in Example 1 (not shown), but the diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were not detected.
[0088] The absorption edge wavelength of the inorganic oxide support c was calculated in the same manner as in Example 1 and was found to be 346 nm.
[0089] Catalyst C was prepared from carrier c in the same manner as in Example 1. Catalyst C contained 20 mass % of MoO3, 2.5 mass % of CoO, and 2.5 mass % of P2O5.
[0090] The amount of nitric oxide adsorption was measured in the same manner as in Example 1. The amount of nitric oxide adsorption of the hydrotreating catalyst C was 8.3 cc / ml.
[0091] Example 4 9.95 kg of sodium aluminate aqueous solution of 22% by mass in terms of Al2O3 was added, diluted with 50 kg of ion-exchanged water, and 4.20 kg of sodium silicate solution of 5% by mass in terms of SiO2 was added while stirring and heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt. 1.82 kg of titanyl sulfate of 33% by mass in terms of TiO2 was dissolved in 10 kg of ion-exchanged water, mixed with 7.04 kg of sulfuric acid of 25% by mass, and heated to 50°C to prepare a first aqueous solution containing titanium mineral salt and sulfuric acid. The molar ratio of titanium mineral salt to mineral acid was 0.42. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant speed using a roller pump over 10 minutes until the pH became 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) d was precipitated was obtained.
[0092] Carrier d was obtained from carrier precursor d in the same manner as in Example 1. Carrier d contained 73 mass% Al in terms of Al2O3, 7 mass% Si in terms of SiO2, and 20 mass% Ti in terms of TiO2, all based on the total amount of the carrier.
[0093] X-ray diffraction analysis was carried out in the same manner as in Example 1 (not shown), but the diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were not detected.
[0094] The absorption edge wavelength of the inorganic oxide support d was calculated in the same manner as in Example 1 and was found to be 340 nm.
[0095] Catalyst D was prepared from carrier d in the same manner as in Example 1. Catalyst D contained 20 mass % of MoO3, 2.5 mass % of CoO, and 2.5 mass % of P2O5.
[0096] The amount of nitric oxide adsorbed was measured in the same manner as in Example 1. The amount of nitric oxide adsorbed by the hydrotreating catalyst D was 7.9 cc / ml.
[0097] Example 5 Catalyst A2 was obtained in the same manner as in Catalyst A1, except that the carrier a was used, and 272 g of molybdenum trioxide, 55 g of cobalt carbonate, 37 g of nickel carbonate (manufactured by Seido Chemical Industry Co., Ltd.; NiO concentration 55 mass%), and 55 g of phosphoric acid were used.
[0098] Catalyst A2 contained 20 mass % MoO3, 2.5 mass % CoO, 1.5 mass % NiO, and 2.5 mass % P2O5.
[0099] The amount of nitric oxide adsorbed was measured in the same manner as in Example 1. The amount of nitric oxide adsorbed by the hydrotreating catalyst A2 was 8.5 cc / ml.
[0100] Comparative Example 1 8.16 kg of sodium aluminate aqueous solution of 22% by mass in terms of Al2O3 was added, diluted with 41 kg of ion-exchanged water, and 1.80 kg of sodium silicate solution of 5% by mass in terms of SiO2 was added while stirring and heated to 60 ° C. to prepare a second aqueous solution containing a basic aluminum salt. A solution obtained by diluting 7.38 kg of an aluminum sulfate aqueous solution of 7% by mass in terms of Al2O3 (manufactured by JGC Catalysts and Chemicals Co., Ltd.) with 13 kg of ion-exchanged water and a solution obtained by dissolving 1.82 kg of titanyl sulfate of 33% by mass in terms of TiO2 in 10 kg of ion-exchanged water were mixed and heated to 50 ° C. to prepare a first aqueous solution containing a titanium mineral salt and an acidic aluminum salt. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant speed over 10 minutes using a roller pump until the pH became 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) e was precipitated was obtained.
[0101] Support e was obtained from support precursor e in the same manner as in Example 1. Support e contained 77 mass % of Al calculated as Al2O3, 3 mass % of Si calculated as SiO2, and 20 mass % of Ti calculated as TiO2, all based on the total mass of the support.
[0102] X-ray diffraction analysis was carried out in the same manner as in Example 1 (not shown), but the diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were not detected.
[0103] The absorption edge wavelength of the inorganic oxide support e was calculated in the same manner as in Example 1 and was found to be 348 nm.
[0104] Catalyst E was prepared from carrier e in the same manner as in Example 1. Catalyst E contained 20 mass % of MoO3, 2.5 mass % of CoO, and 2.5 mass % of P2O5.
[0105] The amount of nitric oxide adsorbed was measured in the same manner as in Example 1. The amount of nitric oxide adsorbed by the hydrotreating catalyst E was 7.1 cc / ml.
[0106] Comparative Example 2 8.44 kg of sodium aluminate aqueous solution of 22% by mass in terms of Al2O3 was added, diluted with 49 kg of ion-exchanged water, and 1.80 kg of sodium silicate solution of 5% by mass in terms of SiO2 was added while stirring and heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt. 3.18 kg of titanyl sulfate of 33% by mass in terms of TiO2 was dissolved in 18 kg of ion-exchanged water, mixed with 2.69 kg of sulfuric acid of 25% by mass, and heated to 50°C to prepare a first aqueous solution containing titanium mineral salt and sulfuric acid. The molar ratio of titanium mineral salt to mineral acid was 1.92. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant speed using a roller pump over 10 minutes until the pH became 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) f was precipitated was obtained.
[0107] Support f was obtained from support precursor f in the same manner as in Example 1. Support f contained 62 mass% Al in terms of Al2O3, 3 mass% Si in terms of SiO2, and 35 mass% Ti in terms of TiO2, all based on the total mass of the support.
[0108] As a result of carrying out X-ray diffraction analysis in the same manner as in Example 1 (not shown), diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were detected.
[0109] The absorption edge wavelength of the inorganic oxide support f was calculated in the same manner as in Example 1 and was found to be 367 nm.
[0110] Catalyst F was prepared from carrier f in the same manner as in Example 1. Catalyst F contained 20 mass % of MoO3, 2.5 mass % of CoO, and 2.5 mass % of P2O5.
[0111] The amount of nitric oxide adsorption was measured in the same manner as in Example 1. The amount of nitric oxide adsorption of the hydrotreating catalyst F was 7.2 cc / ml.
[0112] Comparative Example 3 12.5 kg of sodium aluminate aqueous solution of 22% by mass in terms of Al2O3 was added, diluted with 53 kg of ion-exchanged water, and 1.80 kg of sodium silicate solution of 5% by mass in terms of SiO2 was added while stirring and heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt. 0.45 kg of titanyl sulfate of 33% by mass in terms of TiO2 was dissolved in 2.5 kg of ion-exchanged water, mixed with 12.6 kg of sulfuric acid of 25% by mass, and heated to 50°C to prepare a first aqueous solution containing titanium mineral salt and sulfuric acid. The molar ratio of titanium mineral salt to mineral acid was 0.06. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant speed using a roller pump over 10 minutes until the pH became 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) g was precipitated was obtained.
[0113] Support g was obtained from support precursor g in the same manner as in Example 1. Support g contained 92 mass % of Al calculated as Al2O3, 3 mass % of Si calculated as SiO2, and 5 mass % of Ti calculated as TiO2, all based on the total amount of the support.
[0114] X-ray diffraction analysis was carried out in the same manner as in Example 1 (not shown), but the diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were not detected.
[0115] The absorption edge wavelength of the inorganic oxide support g was calculated in the same manner as in Example 1 and was found to be 320 nm.
[0116] Catalyst G was prepared from carrier g in the same manner as in Example 1. Catalyst G contained 20 mass % of MoO3, 2.5 mass % of CoO, and 2.5 mass % of P2O5.
[0117] The amount of nitric oxide adsorbed was measured in the same manner as in Example 1. The amount of nitric oxide adsorbed by the hydrotreating catalyst G was 6.8 cc / ml.
[0118] Comparative Example 4 7.00 kg of a 22 mass% sodium aluminate aqueous solution calculated as Al2O3 was added and diluted with 16.5 kg of ion-exchanged water, after which 1.80 kg of a 5 mass% sodium silicate solution calculated as SiO2 was added with stirring and heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt.
[0119] A solution of 1.82 kg of titanyl sulfate (33 mass% in terms of TiO2) dissolved in 10 kg of ion-exchanged water was heated to 50°C, and a solution of 1.55 kg of 48 mass% sodium hydroxide solution diluted with 13 kg of ion-exchanged water was added at a constant rate over 90 minutes until the pH reached 7.2, preparing a titania precursor (gel).
[0120] A solution obtained by diluting 11.0 kg of an aqueous aluminum sulfate solution having a concentration of 7 mass % in terms of Al2O3 with 19 kg of ion-exchanged water was added to the second aqueous solution at a constant speed over a period of 10 minutes using a roller pump until the pH reached 7.2 to prepare an alumina precursor, and then 27 kg of the titania precursor was mixed therein to obtain a carrier precursor h.
[0121] Support h was obtained from support precursor h in the same manner as in Example 1. Support h contained 77 mass % of Al calculated as Al2O3, 3 mass % of Si calculated as SiO2, and 20 mass % of Ti calculated as TiO2, all based on the total mass of the support.
[0122] X-ray diffraction analysis was carried out in the same manner as in Example 1 (FIG. 1), and diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were detected.
[0123] The absorption edge wavelength of the inorganic oxide support h was calculated in the same manner as in Example 1 and was found to be 370 nm.
[0124] Catalyst H was prepared from carrier h in the same manner as in Example 1. Catalyst I contained 20 mass % MoO3, 2.5 mass % CoO, and 2.5 mass % P2O5.
[0125] The amount of nitric oxide adsorbed was measured in the same manner as in Example 1. The results are shown in Figure 3. The amount of nitric oxide adsorbed by the hydrotreating catalyst H was 6.5 cc / ml.
[0126] Comparative Example 5 8.85 kg of sodium aluminate aqueous solution of 22% by mass in terms of Al2O3 was added, diluted with 47 kg of ion-exchanged water, and 9.00 kg of sodium silicate solution of 5% by mass in terms of SiO2 was added while stirring and heated to 60°C to prepare a second aqueous solution containing a basic aluminum salt. 1.82 kg of titanyl sulfate of 33% by mass in terms of TiO2 was dissolved in 10 kg of ion-exchanged water, mixed with 5.86 kg of sulfuric acid of 25% by mass, and heated to 50°C to prepare a first aqueous solution containing titanium mineral salt and sulfuric acid. The molar ratio of titanium mineral salt to mineral acid was 0.50. Next, the first aqueous solution was added to the tank containing the second aqueous solution at a constant speed using a roller pump over 10 minutes until the pH became 7.2, and a mixed solution (slurry) in which the carrier precursor (hydrate) i was precipitated was obtained.
[0127] Support i was obtained from support precursor i in the same manner as in Example 1. Support i contained 65 mass % Al in terms of Al2O3, 15 mass % Si in terms of SiO2, and 20 mass % Ti in terms of TiO2, all based on the total mass of the support.
[0128] X-ray diffraction analysis was carried out in the same manner as in Example 1 (not shown), but the diffraction peaks indicating the crystal structures of anatase type titania and rutile type titania were not detected.
[0129] The absorption edge wavelength of the inorganic oxide support i was calculated in the same manner as in Example 1 and was found to be 355 nm.
[0130] Catalyst I was prepared from support i in the same manner as in Example 1. Catalyst I contained 20 mass % of MoO3, 2.5 mass % of CoO, and 2.5 mass % of P2O5.
[0131] The amount of nitric oxide adsorbed was measured in the same manner as in Example 1. The amount of nitric oxide adsorbed by the hydrotreating catalyst I was 6.6 cc / ml.
[0132] [Evaluation of inorganic oxide support properties] <Measurement of UV-visible light diffuse reflectance spectrum of inorganic oxide support and calculation of absorption edge> Using a UV-visible light spectrophotometer (V-660 manufactured by JASCO Corporation) equipped with an integrating sphere unit ISV-772 for diffuse reflectance measurement, the UV-visible light diffuse reflectance spectrum was measured as follows.
[0133] After filling 200 mg of inorganic oxide support sample into a cell holder for diffuse reflection samples, the absorbance was measured at room temperature. Specifically, in photometry mode, the band width was 5.0 nm, the measurement range was 500-200 nm, the data acquisition interval was 0.1 nm, the scanning speed was 100 nm / min, the light source switching wavelength was 340 nm, and background correction was performed in the wave number range of 500-200 nm. Note that the background measurement was performed under the above conditions using a reference white plate.
[0134] The method for calculating the absorption edge from the diffuse reflectance spectrum obtained above was to perform KM transformation using the Kubelka-Munk function (KM function), and the maximum wavelength at which the spectral intensity value was 0.3 or more was calculated as the absorption edge wavelength.
[0135] <Measurement of pore volume (PV) of inorganic oxide support> The pore volume (PV) was measured and calculated by the water pore filling method.
[0136] <Measurement of specific surface area (SA) of inorganic oxide support> The specific surface area (SA) was measured and calculated by the BET method using nitrogen adsorption using a BERSORP-mini (Microtrack-Bell Corporation).
[0137] <Measurement of pore volume (PV) of hydrotreating catalyst> The pore volume (PV) was measured and calculated by the water pore filling method.
[0138] <Measurement of specific surface area (SA) of hydrotreating catalyst> The specific surface area (SA) was measured and calculated by the BET method using nitrogen adsorption using a BERSORP-mini (Microtrack-Bell Corporation).
[0139] (Catalyst properties and test evaluation results) Table 1 shows the results of confirming the amount of titania and silica in the carrier, the presence or absence of anatase / rutile titania crystals, and the effect of the acid solution when preparing the carrier precursor. When aluminum sulfate is contained in the acid solution of the carrier precursor as in Comparative Example 1, alumina derived from aluminum sulfate is further precipitated on the surface of the alumina-silica-titania precursor precipitated when mixed with the basic second aqueous solution, and the effect of the titania contained is not effectively exhibited, so that the dispersibility of titania is insufficient and the amount of nitric oxide adsorption is low. When titania crystals are confirmed in the carrier as in Comparative Examples 2 and 4 and the UV absorption edge wavelength is significantly greater than 350 nm, the specific surface area (SA) is reduced and the amount of nitric oxide adsorption is low. When the amount of titania in the carrier is less than 12% by mass as in Comparative Example 3, the effect of titania as an active ingredient is not exhibited and the amount of nitric oxide adsorption is low. When the amount of silica in the carrier exceeds 10% by mass as in Comparative Example 5, the reactivity of the sodium silicate solution is high and excessive aggregation of the carrier precursor (hydrate) occurs, so that the dispersibility of titania is insufficient and the amount of nitric oxide adsorption is low.
[0140] All of the Examples in which no titania crystals were observed and in which the carrier components and UV absorption edge wavelengths satisfied the required ranges showed high amounts of nitric oxide adsorption.
[0141] From the above results, it was found that the catalyst of the present invention can maintain Ti, which is an active component for desulfurization performance, in a more highly dispersed state, and can support the metal components more dispersedly on the support.
[0142] [Table 1] [Industrial Applicability]
[0143] INDUSTRIAL APPLICABILITY The hydrotreating catalyst of the present invention is capable of hydrodesulfurizing hydrocarbon oils to a high degree and is therefore extremely useful industrially.
Claims
1. A catalyst for hydrotreating a hydrocarbon oil, comprising an inorganic oxide support containing Si, Ti, and Al, and at least one metal component selected from the group consisting of molybdenum, tungsten, cobalt, and nickel, The content of Al in the inorganic oxide support is Al 2 O 3 The Si content is 60 mass% or more in terms of SiO 2 The Ti content is 1.0 to 10.0 mass% in terms of TiO 2 This is calculated as 12.0 to 30.0 mass%. The inorganic oxide support has an absorption edge wavelength of an absorption peak derived from Ti, as measured by ultraviolet spectroscopy, of 350 nm or less; A catalyst for hydrotreating a hydrocarbon oil, which has an adsorption amount of nitric oxide of 7.5 cc / ml or more as measured by nitric oxide adsorption.
2. 2. The hydrotreating catalyst according to claim 1, wherein in an X-ray diffraction analysis of the inorganic oxide support, substantially no diffraction peaks showing a crystal structure of an anatase type titania (101) plane and a rutile type titania (110) plane are detected.
3. Specific surface area (SA) is 150m 2 3. The hydrotreating catalyst according to claim 1, wherein the pore volume (PV) is 0.30 ml / g or more and the pore volume (PV) is 0.5 ml / g or more.
4. The hydrotreating catalyst according to any one of claims 1 to 3, wherein the content of the metal component is 1 to 35 mass % calculated as an oxide.
5. A method for producing the hydrotreating catalyst according to any one of claims 1 to 4, comprising the steps of: a step of mixing a first aqueous solution containing a mineral acid and a titanium mineral acid salt, the content of the titanium mineral acid salt being 0.15 to 0.70 in terms of a molar ratio relative to the mineral acid, the mineral acid being the same as the mineral acid in the titanium mineral acid salt, with a second aqueous solution containing a basic aluminum salt to obtain a mixed solution having a pH of 6.5 to 9.5, and obtaining a carrier precursor precipitated in the mixed solution; washing, shaping, drying and calcining the carrier precursor to obtain a carrier; and a step of supporting at least one metal component selected from the group consisting of molybdenum, tungsten, cobalt and nickel on the support to obtain the hydrotreating catalyst; A method comprising:
6. 6. The method of claim 5, wherein the first aqueous solution is prepared at 60° C. or below.
7. The method according to claim 5 or 6, wherein the first aqueous solution and / or the second aqueous solution comprises silicate ions.
Citation Information
Patent Citations
Method of producing catalyst for hydrogenating / purifying diesel oil, and method of hydrogenating / purifying diesel oil
JP2010221158A
Hydrodesulfurization catalyst for hydrocarbon oil and method for manufacturing the same
JP2011072928A
Method of hydrorefining hydrocarbon oil
JP2011074235A
Hydrodesulfurization catalyst for hydrocarbon oil
JP2015188790A
Hydrotreating catalyst for hydrocarbon oil, production method of the same, and hydrotreating method
JP2016203074A