How to recover lithium

JP7587224B1Active Publication Date: 2024-11-20JAPAN METALS & CHEM CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023187858
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-11-01
Publication Date
2024-11-20
Estimated Expiration
2043-11-01

AI Technical Summary

Benefits of technology

【0011】 本発明によれば、リチウム及びアルミニウムを含有する組成物から、リチウムの選択率を高めて浸出して回収できるリチウムの回収方法を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587224000001_ABST
    Figure 0007587224000001_ABST
Patent Text Reader

Abstract

Provided is a method for recovering lithium, which can increase the selectivity of lithium by leaching and recovering it from a composition containing lithium and aluminum. [Solution] The method for recovering lithium includes a step S10 of treating a composition containing lithium and aluminum with an aqueous hydrogen peroxide solution to obtain a leachate in which lithium is dissolved, a step S11 of removing residue from the leachate, a step S12 of neutralizing the leachate after the residue has been removed to precipitate the aluminum contained in the leachate in the form of a poorly soluble substance and removing the aluminum-containing precipitate, and a step S13 of carbonating the leachate after the aluminum-containing precipitate has been removed, and a step S14 of purifying it, thereby recovering lithium from the leachate after the precipitate has been removed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering lithium. [Background technology]

[0002] Lithium-ion secondary batteries are used as storage batteries installed in hybrid and electric vehicles, and the demand for them has been increasing rapidly in recent years. As the demand for lithium-ion secondary batteries increases, the amount of used lithium-ion secondary batteries, defective lithium-ion secondary batteries, and process waste generated in the manufacturing process of lithium-ion secondary batteries also tends to increase. Lithium-ion secondary batteries contain valuable materials such as nickel (Ni) and cobalt (Co), and methods for recovering metal materials containing valuable materials such as nickel and cobalt have been developed to make effective use of resources.

[0003] Lithium-ion secondary batteries contain lithium (Li) in addition to the above-mentioned metallic materials such as nickel and cobalt. Effective use of lithium as a resource is also required, and a method for recovering lithium from lithium-ion secondary batteries is required.

[0004] Patent Document 1 discloses a method for recovering lithium, which comprises melting lithium-ion secondary batteries to be disposed of to obtain slag containing aluminum and lithium in which the mass ratio of aluminum / lithium is adjusted to 6 or less, contacting the slag with dilute sulfuric acid to leach the lithium in the slag, and precipitating and removing unnecessary metals such as aluminum.

[0005] Patent Document 2 discloses a method for recovering lithium, which comprises melting and reducing waste lithium-ion batteries to separate the resulting metal and slag, bringing the separated slag into contact with pure water having a pH of 5 to 7 for a leaching treatment, maintaining the pH of a leached slurry obtained by the leaching treatment at 11 or higher, and subjecting the leached slurry to solid-liquid separation, thereby separating the leached slurry into a leachate containing lithium and a post-leaching slag. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2022 / 085222 [Patent Document 2] JP 2020-029613 A Summary of the Invention [Problem to be solved by the invention]

[0007] The method described in Patent Document 1 has a high lithium leaching rate, but has the problem that the leaching selectivity is low, aluminum also leaches into the liquid, and the lithium recovery rate significantly decreases as the weight ratio of aluminum in the slag increases.

[0008] In the method described in Patent Document 2, it is possible to leach lithium with water, but the leaching rate is low and is not sufficient for recovering lithium in the slag.

[0009] Therefore, an object of the present invention is to provide a method for recovering lithium, which can increase the selectivity of lithium by leaching and recovering lithium from a composition containing lithium and aluminum. [Means for solving the problem]

[0010] The method for recovering lithium according to the present invention includes the steps of treating a composition containing lithium and aluminum with an aqueous hydrogen peroxide solution to obtain a leachate in which lithium is dissolved, removing residue from the leachate, neutralizing the leachate after the residue has been removed to cause the aluminum contained in the leachate to precipitate in the state of a poorly soluble substance and removing the precipitate containing aluminum, and recovering lithium from the leachate after the precipitate has been removed. Effect of the Invention

[0011] According to the present invention, there is provided a method for recovering lithium, which is capable of leaching and recovering lithium with an increased selectivity from a composition containing lithium and aluminum. [Brief description of the drawings]

[0012] [Figure 1] 1 is a flowchart illustrating a lithium recovery method according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] 1. Embodiment Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings.

[0014] The lithium recovery method of this embodiment is a method for recovering lithium from a composition containing lithium (Li) and aluminum (Al). The composition containing lithium and aluminum is, for example, slag obtained by subjecting a positive electrode of a lithium ion secondary battery to an oxidation-reduction treatment by a thermite reaction and separating it from a metal material. Hereinafter, a method for recovering lithium from slag obtained by subjecting a positive electrode of a lithium ion secondary battery to an oxidation-reduction treatment by a thermite reaction and separating it from a metal material will be described.

[0015] First, a lithium ion secondary battery and slag obtained by subjecting the positive electrode of the lithium ion secondary battery to an oxidation-reduction treatment by a thermite reaction and separating it from the metal material will be described.

[0016] (Lithium-ion secondary battery) The lithium ion secondary battery from which lithium is recovered in the lithium recovery method according to the present embodiment is a used secondary battery that has been used as a storage battery for an automobile such as an electric vehicle or a hybrid vehicle. The lithium ion secondary battery may be an unused battery that has been confirmed to be defective after manufacture. It may also be process waste generated during the manufacturing process.

[0017] The lithium ion secondary battery includes a cell container containing an electrode assembly and an electrolyte, the cell container being made of, for example, an aluminum alloy.

[0018] The electrode assembly includes a positive electrode and a negative electrode wound with a separator interposed therebetween. The electrode assembly is not limited to a wound type, but may be a laminated type in which a positive electrode, a negative electrode, and a separator are laminated.

[0019] The positive electrode has a positive electrode current collector and a positive electrode active material layer. The positive electrode current collector is a foil containing aluminum (hereinafter, also referred to as Al foil). The positive electrode active material layer contains a positive electrode active material, a binder, and a conductive material.

[0020] Any metal composite oxide containing lithium can be used as the positive electrode active material. For example, the positive electrode active material can be selected from lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel cobalt composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, lithium nickel cobalt manganese composite oxide, lithium iron phosphate, etc. In this embodiment, the positive electrode active material is lithium nickel cobalt manganese composite oxide.

[0021] The negative electrode has a negative electrode current collector and a negative electrode active material layer. For example, the negative electrode current collector is a copper (Cu) foil, and the negative electrode active material is graphite.

[0022] The electrolytic solution contains a solvent and a lithium salt (electrolyte).

[0023] As the electrolyte, a substance containing a fluorine compound, such as LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiTFSA (lithium trifluoromethanesulfonylamide), LiTFSI (lithium bis(trifluoromethane)sulfonimide), etc., is used.

[0024] Although the configuration using a separator and an electrolytic solution has been described above, the present invention is not limited thereto, and a configuration using a solid electrolyte instead of the separator and the electrolytic solution may also be used.

[0025] (Slug) The slag from which lithium is recovered in the lithium recovery method of the present embodiment is, for example, slag obtained by removing the positive electrode of the above-mentioned lithium ion secondary battery, subjecting it to an oxidation-reduction treatment by a thermite reaction, and separating it from the metal material. The slag is a composition containing lithium and aluminum.

[0026] (Slag manufacturing method) The slag is produced, for example, by removing a positive electrode from a lithium-ion secondary battery, putting it into a furnace or the like, and reducing and melting it at high temperature. In particular, when the thermite reaction is used, flux and the like are not required, so it is advantageous in obtaining high-purity lithium in recycling. The thermite reaction melts the positive electrode by the reaction heat between the foil and the active material to obtain a molten material, and the molten material is cooled and separated into a metal material containing a metal constituting a metal composite oxide and a slag for recovery. Here, the thermite reaction is an oxidation-reduction reaction in which, when a mixture of a positive electrode current collector made of metal Al and a positive electrode active material made of a metal oxide is reacted, high heat is generated while reducing the metal oxide by metal Al. In addition, in order to promote the thermite reaction, it is preferable to first carry out a heat treatment for the purpose of decomposing and removing the binder and the conductive assistant.

[0027] Regarding the melting of the positive electrode, the positive electrode active material is LiNi x Co y Mn z We will explain the case where O2 is used as an example. In the thermite reaction, the aluminum foil contained in the positive electrode acts as a reducing agent, and the following reaction occurs. LiNi x Co y Mn z O2+Al → 1 / 2Li2O+Ni x Co y Mn z +1 / 2Al2O3

[0028] By cooling the molten cathode, Ni was obtained as a metallic material containing metals that make up the metallic composite oxide. x Co y Mn z and slag containing lithium oxide, aluminum oxide, lithium aluminate, etc. are separated and recovered.

[0029] (How to recover lithium) As shown in Fig. 1, the lithium recovery method according to the present embodiment includes a hydrogen peroxide dissolution step S10 in which slag, a composition containing lithium and aluminum obtained by subjecting the positive electrode of a lithium ion secondary battery to an oxidation-reduction treatment by a thermite reaction and separating it from the metal material, is treated with an aqueous hydrogen peroxide solution to obtain a leachate in which lithium is dissolved, a residue removal step S11 in which residues in the leachate are removed, an aluminum removal step S12 in which the leachate after the residue removal is neutralized to cause the aluminum contained in the leachate to precipitate in the form of a poorly soluble substance, and the aluminum-containing precipitate is removed, a carbonation step S13 in which the leachate after the aluminum-containing precipitate is removed is carbonated, and a purification step S14 in which the leachate after the precipitate removal is purified is recovered from the leachate. Each step will be described in detail below.

[0030] [Hydrogen peroxide dissolution process] In the hydrogen peroxide dissolution step S10, the slag containing lithium and aluminum obtained by the above-mentioned slag manufacturing method is treated with an aqueous hydrogen peroxide solution to obtain a leachate in which lithium has been dissolved. The dissolution of lithium with hydrogen peroxide is represented, for example, by the following chemical formula: In the formula, the composition containing lithium and aluminum contained in the slag is represented as LiAlO2. 4LiAlO2+2H2O2→4LiOH+2Al2O3+O2↑

[0031] By using an aqueous hydrogen peroxide solution, lithium can be selectively eluted from lithium aluminate and composite oxides containing lithium.

[0032] The above reaction is an exothermic reaction, and the temperature of the leachate increases during the treatment due to the heat of reaction, promoting the dissolution of lithium into the leachate.

[0033] The concentration of the aqueous hydrogen peroxide solution used in the hydrogen peroxide dissolving step S10 is preferably 5% by mass or more and 35% by mass or less, more preferably 10% by mass or more and 20% by mass or less, and specifically 10% by mass.

[0034] The slag used in the hydrogen peroxide dissolving step S10 is an undersize powder obtained by sieving the slag through a 500 μm mesh sieve after pulverization.

[0035] The slurry concentration (g / L), which is the mass (g) of slag relative to the volume (L) of the aqueous hydrogen peroxide solution used in the hydrogen peroxide dissolution step S10, is preferably 10 g / L or more and 100 g / L or less, and more preferably 50 g / L or more and 75 g / L or less.

[0036] The lower limit temperature of the aqueous hydrogen peroxide solution used in the hydrogen peroxide dissolving step S10 is 20°C or more, preferably 40°C or more, more preferably 60°C or more, and the upper limit temperature is 100°C or less. However, from the viewpoint of handling, a temperature of 80°C or more and 95°C or less is preferable. In the hydrogen peroxide dissolving step S10, a leachate is obtained by treating the slag with an aqueous hydrogen peroxide solution. The dissolution of the slag with hydrogen peroxide is an exothermic reaction, and the temperature of the leachate increases due to the reaction heat. The temperature increase due to the reaction heat is, for example, 10°C or more and 15°C or less. This increases the reaction rate of lithium dissolution with hydrogen peroxide. In addition, the cost of heating the leachate to increase the reaction rate can be reduced. In addition, since the reaction rate is increased, the reaction time can be shortened.

[0037] The reaction time for treatment with the aqueous hydrogen peroxide solution in the hydrogen peroxide dissolving step S10 is preferably 6 hours or more and 48 hours or less, and more preferably 16 hours or more and 24 hours or less.

[0038] In the hydrogen peroxide dissolution step S10, it is possible to increase the selectivity of lithium to aluminum from the slag containing lithium and aluminum.

[0039] [Residue removal process] In the residue removal step S11, the residue in the leachate is removed by solid-liquid separation through filtration. The leachate contains residues such as aluminum oxide that did not dissolve in the hydrogen peroxide aqueous solution. By filtering the residues such as aluminum oxide, a leachate in which lithium is dissolved is obtained.

[0040] [Aluminum removal process] In the aluminum removal step S12, the leachate after removing the residue is neutralized to cause the aluminum contained in the leachate to precipitate in the form of a poorly soluble substance, and the aluminum-containing precipitate is removed. The precipitate is removed by solid-liquid separation, for example, by filtration such as suction filtration. The formation of the aluminum-containing precipitate by neutralization is represented, for example, by the following chemical formula: Al(OH) 4- +H + →Al(OH)3↓+H2O

[0041] Examples of acids used to neutralize the leachate in the aluminum removal step S12 include hydrochloric acid, sulfuric acid, and nitric acid.

[0042] In the aluminum removal step S12, the pH of the leachate after neutralization is preferably 6.0 or more and 9.0 or less, and more preferably 7.0 or more and 8.0 or less.

[0043] In the aluminum removal step S12, the aluminum component becomes poorly soluble precipitates such as aluminum hydroxide. The poorly soluble precipitates such as aluminum hydroxide are washed with ion-exchanged water as necessary. In the hydrogen peroxide dissolution step S10, if the leachate contains a large amount of aluminum, gel-like aluminum hydroxide is generated during neutralization, and lithium dissolved in the leachate is absorbed into this gel-like aluminum hydroxide. In the hydrogen peroxide dissolution step S10 of this embodiment, the selectivity of lithium is increased relative to aluminum, so that the aluminum content in the leachate is reduced, and the decrease in the lithium yield due to the incorporation of lithium components into the gel can be suppressed. Here, the lithium yield is the ratio (mass%) of the mass of lithium in the leachate after aluminum removal to the mass of lithium in the raw slag.

[0044] Next, the following carbonation step S13 and purification step S14 are carried out, and a step of recovering lithium from the leachate after removing the precipitate is carried out.

[0045] [Carbonation process] In the carbonation step S13, the leachate from which the aluminum-containing precipitate has been removed is carbonated to produce lithium carbonate from the lithium component. The carbonation is performed, for example, by contacting the leachate from which the aluminum-containing precipitate has been removed with a carbonate or carbon dioxide gas.

[0046] [Refining process] In order to increase the purity of the recovered lithium carbonate, the obtained lithium carbonate is purified by a carbonation treatment as necessary (purification step S14).

[0047] As described above, lithium can be recovered from the lithium- and aluminum-containing slag obtained by subjecting the positive electrode of a lithium-ion secondary battery to an oxidation-reduction treatment by a thermite reaction and separating it from the metal material.

[0048] 2. Actions and Effects According to the lithium recovery method of the present embodiment, in the hydrogen peroxide dissolving step S10, the slag containing lithium and aluminum is treated with an aqueous hydrogen peroxide solution, whereby the selectivity of lithium relative to aluminum can be increased and dissolved.

[0049] By increasing the selectivity of lithium over aluminum and dissolving it in the hydrogen peroxide dissolution step S10, the aluminum content in the leachate can be reduced, thereby suppressing a decrease in the lithium yield due to the incorporation of lithium components into gel-like aluminum hydroxide when the aluminum components are converted into a poorly soluble precipitate in the aluminum removal step S12. In addition, compared to the case where sulfuric acid is used to dissolve lithium, the amount of neutralizing agent, the precipitate during neutralization, and gypsum generated during removal of excess sulfuric acid can be reduced.

[0050] When the slag is treated with the hydrogen peroxide solution in the hydrogen peroxide dissolution step S10, heat is generated and the temperature of the leachate rises. This increases the reaction rate of dissolving lithium with hydrogen peroxide. In addition, the cost of heating the leachate to increase the reaction rate can be reduced. In addition, since the reaction rate is increased, the reaction time can be shortened.

[0051] 3. Working Example The following describes experiments carried out to confirm the effects of the present invention.

[0052] Example 1 A positive electrode was prepared as process waste generated during the manufacturing process of a lithium ion secondary battery.

[0053] <Positive electrode> Al foil 30% by mass Active material (LiNi 1 / 6 Co 2 / 3 Mn 1 / 6 O2) 61~62% by mass Binder (PVDF) 2-3% by mass Conductive material 5~6% by mass

[0054] The positive electrode was heated and melted by thermite reaction to obtain a molten material. The molten material was cooled and separated into a metal material containing the metals (Ni, Co, Mn) constituting the metal composite oxide of the positive electrode active material, and a slag containing lithium and aluminum.

[0055] An experiment was conducted to obtain a leachate by dissolving lithium from the slag obtained as described above. The slag was pulverized with a rod mill, and the powder that passed through a 500 μm mesh was used. For Experiment No. 1 to 5, a hydrogen peroxide dissolution process was performed by a dissolution method using an aqueous hydrogen peroxide solution, and a residue removal process was also performed to obtain a leachate. The concentration of the aqueous hydrogen peroxide solution in the dissolution using hydrogen peroxide was 10%, and the slurry concentration was 50 to 75 g / L. The reaction was carried out under atmospheric pressure, and the slag and the aqueous hydrogen peroxide solution were stirred using a stirrer such as a magnetic stirrer. Thereafter, the leaching rates of lithium, aluminum, and magnesium in the leachate were examined as described below.

[0056] In the experiment No. 6, lithium was dissolved by a dissolution method using water, and the residue was removed to obtain a leachate. The slurry concentration was 50g / L when dissolving using pure water with a pH of 7. The leaching rates of lithium, aluminum, and magnesium in the leachate were investigated. Except for the above, the same procedures were followed as in the experiments No. 1 to 5.

[0057] For Experiment Nos. 7 to 9, lithium was dissolved by a dissolution method using sulfuric acid, and the residue was removed to obtain a leachate. The sulfuric acid concentration in the dissolution using sulfuric acid was 10%, and the slurry concentration was 50 g / L. The leaching rates of lithium, aluminum, and magnesium in the leachate were investigated. Except for the above, the same procedures were followed as for Experiment Nos. 1 to 5.

[0058] Table 1 shows the dissolution method, temperature, reaction time, and slurry concentration for Experiment No. 1 to 9. Experiment No. 1 to 5 correspond to the examples, and Experiment No. 6 to 8 correspond to the comparative examples. The temperatures shown in Table 1 are the temperatures of the aqueous hydrogen peroxide solution, water, and sulfuric acid before the start of the reaction.

[0059] [Table 1]

[0060] The leaching rates of lithium (Li), aluminum (Al), and magnesium (Mg) were examined for the leaching solutions obtained in the above Experiments No. 1 to 9, and the results are shown in Table 1. The leaching rate is the ratio (mass%) of the mass of the leaching solution before neutralization to the mass of each element in the raw slag. The mass of each element in the slag was calculated from the results of elemental analysis of the slag (content of each element per unit mass of slag) and the mass of the slag used in the experiment. The elemental analysis of the slag was performed using an ICP optical emission spectrometer (manufactured by Hitachi High-Tech Science Corporation, product name "SPS3520UV-DD"). The mass of each element in the leaching solution was calculated from the results of ICP mass analysis and the amount of solution. The ICP mass analysis of the leaching solution was performed using an ICP mass spectrometer (manufactured by Thermo Fisher Scientific, product name "ELEMENT XR").

[0061] In the treatment with the aqueous hydrogen peroxide solution of Experiment Nos. 1 to 5, the leaching rate of aluminum in the leachate was low regardless of the treatment time, treatment temperature, or slurry concentration, and it was confirmed that the leaching rate of lithium relative to the leaching rate of aluminum could be increased, and dissolution could be performed with increased selectivity for lithium relative to aluminum. In the treatment with the aqueous hydrogen peroxide solution of Experiment Nos. 1 to 5, the leaching rate of lithium could be increased with a longer treatment time, a higher treatment temperature, and a higher slurry concentration.

[0062] In the sulfuric acid treatment of Experiment No. 7 to 9, the leaching rate of lithium in the leachate is high, but the leaching rate of aluminum is also high. When the leachate is neutralized to remove aluminum, the aluminum component becomes a poorly soluble gelled precipitate (Al(OH)3). When the leachate leaching rate is high, a large amount of gelled precipitate is generated, which increases the load of filtration separation and gel washing, and also generates co-precipitates such as LiAlO2, which reduces the yield of lithium after removing aluminum. In addition, leaching of magnesium was confirmed in the leachate obtained by treatment with sulfuric acid. Magnesium is derived from the furnace material when the positive electrode is melted. When neutralizing the leachate obtained by treatment with sulfuric acid to remove aluminum, a large amount of neutralizing agent is required, and there is a disadvantage that a large amount of precipitate is generated by neutralization, and a large amount of gypsum is generated to remove sulfate ions in the liquid. For these reasons, the lower the aluminum concentration in the leachate, the better.

[0063] On the other hand, in the treatment with the aqueous hydrogen peroxide solution in Experiments No. 1 to 5, the aluminum leaching rate was low, so the formation of a gelled precipitate was suppressed and the uptake of lithium by the gelled precipitate was suppressed. As a result, the lithium content in the leachate did not decrease during the aluminum removal treatment, and almost the entire amount of lithium in the leachate could be recovered.

[0064] Regarding the treatment with water in Experiment No. 6, a comparison with Experiment No. 2 (Example) and Experiment No. 6 (Comparative Example), which were conducted at the same temperature, reaction time, and slurry concentration, confirmed that the lithium leaching rate in the treatment with an aqueous hydrogen peroxide solution was higher than that in the treatment with water.

[0065] In addition, a comparison of Experiment No. 3 (Example) and Experiment No. 6 (Comparative Example), in which the lithium leaching rates were almost the same, confirmed that the reaction time in the treatment with an aqueous hydrogen peroxide solution could be shortened compared to the treatment with water.

[0066] As described above, in the method of recovering lithium by treating slag obtained from a lithium-ion secondary battery with an aqueous hydrogen peroxide solution, the aluminum leaching rate was lower and the lithium selectivity was higher than in the treatment using sulfuric acid, and the lithium leaching rate was higher than in the treatment using water, which resulted in a higher lithium recovery yield.

[0067] Example 2 From the slag obtained in the same manner as in Example 1, lithium was dissolved by a dissolution method using sulfuric acid in the same manner as in Experiment No. 9 above to obtain a leachate, and then an experiment was conducted to remove aluminum by neutralization to investigate the effect of lithium uptake by the gelled precipitate. The leachate after removing the residue was neutralized with an aqueous NaOH solution (concentration 7.4 mass%). The gelled precipitate generated by neutralization was subjected to solid-liquid separation by centrifugation, and after washing with a gel washing solution, the gel was separated from the washing solution using a centrifuge in the same manner.

[0068] The lithium content in the leachate after neutralization was about 50% by mass of the lithium content in the leachate before neutralization. When washing was performed using 1.4 times the amount of water relative to the water content of the gelled precipitate, the lithium content in the solution after aluminum removal was 60% by mass of the amount before aluminum removal (before neutralization), when washing was performed using 4.2 times the amount of water, the lithium content in the solution after aluminum removal was 75% by mass of the amount before aluminum removal, and when washing was performed using 7.6 times the amount of water, the lithium content in the solution after aluminum removal was 80% by mass of the amount before aluminum removal. That is, when lithium is dissolved by the dissolution method using sulfuric acid in the comparative example to obtain a leachate, the lithium content in the solution decreases in the aluminum removal step due to the incorporation of lithium by the gelled precipitate. It was confirmed that the lithium content in the solution after aluminum removal was only 60% to 80% by mass of the amount before aluminum removal, even when washing was performed using a large amount of water and solid-liquid separation was performed by centrifugation.

[0069] Meanwhile, a leachate was obtained by dissolving using hydrogen peroxide in the same manner as in Experiment No. 4 above, and then neutralized with an aqueous sulfuric acid solution (concentration 10% by mass). Solid-liquid separation to separate the leachate from the aluminum-containing precipitate generated during neutralization was performed by suction filtration, and the separated aluminum-containing precipitate was subjected to through-washing with ion-exchanged water. The lithium content in the solution after aluminum removal was 94% by mass of that before aluminum removal (before neutralization). It was confirmed that the lithium content in the leachate did not decrease during the aluminum removal process, and almost the entire amount of lithium in the leachate could be recovered.

[0070] From the above, it was confirmed that when lithium is dissolved to obtain a leachate by the dissolution method using sulfuric acid in the comparative example, the lithium content in the solution is greatly reduced in the aluminum removal process due to the incorporation of lithium by the gelled precipitate (Al(OH)3). Therefore, in order to obtain a high lithium yield, it is preferable that the amount of aluminum in the leachate is as small as possible, and it is effective to obtain a leachate by the dissolution method using an aqueous hydrogen peroxide solution.

[0071] The neutralizing agent (sulfuric acid aqueous solution) used when neutralizing leachate obtained by dissolution using hydrogen peroxide is less expensive than the neutralizing agent (NaOH aqueous solution or Ca(OH)2 aqueous solution) used when neutralizing leachate obtained by dissolution using sulfuric acid. In addition, the amount of precipitate generated when neutralizing leachate obtained by dissolution using hydrogen peroxide is significantly less than when neutralizing leachate obtained by dissolution using sulfuric acid. In addition, a large amount of gypsum is generated when neutralizing leachate obtained by dissolution using sulfuric acid, but no gypsum is generated when neutralizing leachate obtained by dissolution using hydrogen peroxide.

[0072] In addition, when the leachate is obtained by the dissolution method using hydrogen peroxide, the absolute value of the lithium leaching rate is smaller than that when the leachate is obtained by the dissolution method using sulfuric acid, but the lithium components that are not leached into the leachate remain in the slag residue. Therefore, the hydrogen peroxide dissolution step can be further performed using the slag residue obtained in the residue removal step, and the lithium recovery yield can be increased by repeating the lithium recovery step multiple times. In the case of treatment with an aqueous hydrogen peroxide solution, almost the entire amount of lithium in the leachate can be recovered, so the final yield approaches 100% by repeating the lithium recovery step multiple times.

[0073] 4. Variations The present invention is not limited to the above-described embodiment, and can be modified as appropriate within the scope of the present invention.

[0074] The lithium recovery method of the present invention is a technique that can be widely applied when recovering lithium from a composition containing lithium and aluminum. In the above embodiment, the lithium and aluminum-containing composition is slag obtained by reducing the positive electrode of a lithium ion secondary battery by a thermite reaction and separating it from the metal material, but the present invention is not limited thereto. For example, the lithium and aluminum-containing composition may be slag obtained by melting and separating the metal material from black mass obtained by roasting, crushing, and sorting a lithium ion battery. The melting may be performed in an air atmosphere or a reducing atmosphere using a reducing agent. In addition, the lithium recovery method of the present invention can be applied to any composition containing lithium and aluminum. In the above embodiment, lithium aluminate is exemplified as an example of the object from which lithium is recovered, but the object may be an object in which lithium and aluminum are individually mixed.

[0075] The lithium ion secondary batteries to be recovered may be unused batteries as well as used batteries. Also, process waste generated in the manufacturing process of lithium ion secondary batteries may be the subject of lithium recovery. Although the subject of lithium recovery in this specification is a lithium ion secondary battery, it may be a lithium primary battery or an ore containing lithium and aluminum. [Explanation of symbols]

[0076] S10 Hydrogen peroxide dissolution process S11 Residue removal process S12 Aluminum removal process S13 Carbonation process S14 Purification process

Claims

1. A step of treating a composition containing lithium and aluminum with an aqueous hydrogen peroxide solution to obtain a leachate in which lithium is dissolved; removing residues from the leachate; a step of neutralizing the leachate from which the residue has been removed to cause aluminum contained in the leachate to precipitate in the form of a poorly soluble substance, and removing the aluminum-containing precipitate; recovering lithium from the leachate after removing the precipitate; (However, the hydrogen peroxide aqueous solution does not contain sulfuric acid, nitric acid or hydrochloric acid.)

2. In the step of recovering lithium from the leachate after the precipitate has been removed, the leachate after the precipitate has been removed is carbonated, and the lithium component contained in the leachate is recovered as lithium carbonate. The method for recovering lithium according to claim 1.

3. The concentration of the aqueous hydrogen peroxide solution is 5% by mass or more and 35% by mass or less. The method for recovering lithium according to claim 1 or 2.

4. The composition containing lithium and aluminum is a slag obtained by melting a lithium ion secondary battery and separating the metal material. The method for recovering lithium according to claim 1 or 2.

5. The composition containing lithium and aluminum is a slag obtained by subjecting a positive electrode of a lithium ion secondary battery to a reduction treatment by a thermite reaction and separating the metal material. The method for recovering lithium according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for processing lithium ion battery, and metal material for nickel metal hydride battery or metal material for hydrogen storage

    JP2018190610A

  • Lithium recovery method

    JP2020029613A

  • Process, apparatus, and system for recovering materials from batteries

    JP2020522617A

  • A process for recovering cobalt, lithium, and other metals from spent lithium-based batteries and other feeds

    JP2020522622A

  • Method for separating cobalt and nickel

    JP2022042982A