Double shell container
The double-shell cryogenic container with ultrafine airgel powder insulation addresses insulation and cost issues in hydrogen storage, enhancing thermal performance and reducing energy consumption.
Patent Information
- Application Number
- JP2020193875
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-20
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-11-20
AI Technical Summary
Current cryogenic chambers for storing and transporting hydrogen have poor insulation properties, requiring high vacuum levels and significant electrical energy for maintenance, and the use of airgel as insulation material is costly and difficult to fill uniformly.
A double-shell cryogenic container using weakly bonded ultrafine airgel powder as insulation, filled between inner and outer cylinders, with a three-dimensional network structure composed of primary particles, and optionally incorporating hollow particles to further reduce thermal conductivity.
The container achieves improved insulation performance, reduces the required vacuum level, lowers energy consumption for cooling, and significantly reduces material costs while ensuring easy filling and maintaining thermal integrity.
Smart Images

Figure 0007587257000003 
Figure 0007587257000004 
Figure 0007587257000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a double-shelled container suitable for use as a tank for storing or transporting liquefied petroleum gas or liquid hydrogen. [Background technology]
[0002] In order to prevent global warming, research into clean energy sources to reduce CO2 emissions is being actively conducted. Hydrogen energy is one of the most promising clean energy sources because it emits zero CO2 during power generation and hydrogen, which is a fuel, can be stored and transported. For long-term storage and long-distance transportation of hydrogen, a liquid with a volume of about 1 / 800 of that of gas at the same weight is selected (see, for example, Non-Patent Document 1). The two most difficult aspects of the application of hydrogen energy are (1) long-distance transportation and (2) long-term storage. Refrigerated containers are widely used to store liquid gases such as LNG (liquefied petroleum gas) and LN2 (liquid nitrogen). However, LH2 (liquid hydrogen) must be stored at a temperature of -253°C or lower, which is considerably lower than the storage temperatures of LNG and LN2. In order to store LH2, a container with excellent long-term refrigeration properties is required, and a lot of electrical energy must be consumed to cool LH2.
[0003] This invention proposes a double-shelled insulated container for storage and transportation of hydrogen (liquid, gas, or both). To achieve ultra-low thermal conductivity, weakly bonded ultrafine aerogel powder is applied as the insulating material. The insulating layer is filled to provide the insulating properties of the double-shelled insulated container. In addition, to ensure the safety of compressed hydrogen storage, the outside of the inner tank is wrapped with glass / carbon fiber.
[0004] <About hydrogen storage> Cryogenic containers are widely used to store LN2 and LNG. On the other hand, because the boiling point of hydrogen at one atmosphere is low at -253°C, cryogenic containers are required to have extremely low thermal conductivity (desired value: 10mW / mK or less). Traditionally, perlite has been chosen as the insulating material. Perlite fills the layer (insulating layer) between the double shells and provides the insulation of the cryogenic container. However, the insulating properties of perlite are not sufficient for storing LH2. To further improve the insulation properties of the cryogenic container, a high degree of vacuum is required in the insulating layer.
[0005] Gas cylinders have been used to store compressed gases. However, storing compressed hydrogen is much more difficult than storing general compressed gases. Hydrogen gas is known to be highly flammable, and will ignite when mixed with normal air, even in small amounts. Due to its chemical properties and the ease with which it reacts with oxygen in the air, it can ignite even when the volume ratio of hydrogen in the air is around 4%, but because hydrogen reacts with oxygen in the air, it can ignite even when the amount of hydrogen in the air is small. Another drawback of compressed hydrogen storage is hydrogen embrittlement (hydrogen-induced cracking). To prevent hydrogen ignition, materials that are less susceptible to hydrogen embrittlement were selected for the gas cylinder material. In addition, the gas cylinder is covered with glass / carbon fiber to further prevent hydrogen-induced ignition.
[0006] <About cryogenic liquid tanks> Patent Document 1 discloses a low-temperature insulated pressure vessel. That is, it has a two-layer structure of an inner layer and a housing, the middle layer is evacuated to form a high vacuum insulation structure, and the inner surface is covered with an insulating material to reduce radiant heat transfer in the middle layer. The insulating material is made of aluminum foil with high reflectivity and flame-retardant glass fiber paper with low thermal conductivity, which are alternately laminated. Patent Document 2 proposes a structure suitable for insulating and keeping cold cryogenic liquid tanks such as vehicle-mounted LNG tanks. That is, the structure has a cryogenic liquid tank including an inner cylinder and an outer cylinder, and includes a composite laminate structure including a radiation prevention material layer as a composite insulation, an aerogel blanket heat shielding layer in contact with the radiation prevention material layer, and a vacuum insulation layer installed on the outside of the aerogel blanket heat shielding layer, in which mirror-finished stainless steel is laid close to one side of the inner cylinder, and an EVA foam material layer in contact with the outer cylinder is provided as an outer clad of the vacuum insulation layer.
[0007] In Patent Document 3, a spherical tank is proposed. In the petroleum and chemical industries, it is customary to store liquids and the like in large tank structures, which are usually installed outdoors and exposed to both heat and cold elements. These storage tanks are usually constructed of steel or other metal tank structures and, since they are installed outdoors, are provided with adequate insulation to keep the product stored in the tank at the desired temperature. In patent document 4, an aircraft cryogenic liquid storage tank is proposed which is capable of providing long-term storage and is characterized by its light weight. Patent Document 5 proposes a silica-based aerogel that has excellent heat insulation properties and flexibility. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] China Patent Application Publication No. 110220107 [Patent Document 2] China Utility Model No. 207112350 Specification [Patent Document 3] US Patent Application Publication No. 20180202607 [Patent Document 4] US Patent Publication No. 20120279971 [Patent Document 5] Patent No. 6288382 [Non-patent literature]
[0009] [Non-Patent Document 1] CO2-free Hydrogen Introduction Concept and Technological Development, Kawasaki Heavy Industries, (2015), slides 17, 25, 28 https: / / www.nedo.go.jp / content / 100765860.pdf Summary of the Invention [Problem to be solved by the invention]
[0010] Toward the realization of a hydrogen energy society, cryogenic tanks with ultra-low thermal conductivity (desired value: 10 mW / mK) are necessary for storing and transporting LH2. However, current cryogenic tanks have poor insulation because the insulating material, perlite, does not exhibit superior insulating properties compared to the latest insulating materials. For this reason, in order to achieve high insulation properties, it is necessary to increase the degree of vacuum in the insulating layer.
[0011] Problems to be solved by the present invention include the following. (1) The characteristics of the insulation materials in conventional cryogenic liquid tanks, such as those shown in Patent Documents 2 and 3, are not suitable for long-term storage of LH2. (2) In conventional cryogenic liquid tanks such as those shown in Patent Documents 2 and 3, the amount of electrical energy used is large in order to maintain a high vacuum level in the cold insulation layer. (3) In conventional cryogenic liquid tanks such as those shown in Patent Documents 2 and 3, the amount of electrical energy used to cool LH2 is large. (4) When aerogel is used as a heat insulating material as shown in Patent Documents 1 to 4, the material cost of the aerogel is high. (5) It is possible to use flexible aerogel panel or blanket materials as insulation materials as shown in Patent Document 5, but this requires attachment to the spherical shell. In addition, since the insulation layer provided on the spherical shell or tank has a narrow gap, it is necessary to fill the insulation material uniformly, which is a very difficult task. [Means for solving the problem]
[0012] The present invention proposes a double-shelled cryogenic vessel for storing hydrogen. It can be used to store hydrogen in liquid, gaseous or coexisting states. In addition, the vessel uses weakly bonded ultrafine aerogel powder, which makes it easy to achieve the desired insulation for LH2 storage.
[0013] [1] The double-shelled container of the present invention is, for example, as shown in Fig. 1, a double-shelled container having an inner cylinder 10, an outer cylinder 20, an aerogel-filled space 30 provided between the inner cylinder 10 and the outer cylinder 20, and a heat insulating material filled in the aerogel-filled space 30, characterized in that the heat insulating material is made of aerogel having a three-dimensional network structure whose skeleton is composed of clusters that are aggregates of primary particles, and contains fine particles having a three-dimensional network structure whose skeleton is composed of the primary particles. The fine particles are preferably weakly bonded ultrafine aerogel powder. Here, primary particles will be explained. In the three-dimensional network structure of conventional aerogel powder particles, the units that constitute the skeleton are called secondary particles (see, for example, paragraph 0035 of Patent Document 5). A primary particle is a smaller unit particle that constitutes a secondary particle when multiple particles gather together. According to the same document, the diameter of a secondary particle is approximately 2 nm to 50 μm, while the diameter of a primary particle is 0.1 nm to 5 μm. However, as common technical knowledge, there is no universally uniform range for the absolute values of the particle diameters of primary particles and secondary particles.
[0014] [2] In the double-shelled container of the present invention, preferably, 50% or more of the total number of the fine particles are dispersed with a mode of particle diameter of 0.1 μm or more and 1.0 μm or less. The particle diameter referred to here is a value observed by a laser diffraction particle size distribution measuring device. In this specification, laser diffraction particle size distribution measurement is abbreviated as PSD (particle size distribution) measurement. In this specification, the particle diameter is described on the premise of PSD measurement. However, in PSD measurement, not only the diameter of the particle itself but also the aggregation of particles is observed as the particle diameter, so that the true particle diameter is likely to be smaller than the measured value. If there is a difference in particle diameter depending on the measurement method, the particle diameter may be appropriately converted and interpreted. [3] In the double-shelled container of the present invention, the insulating material preferably further contains hollow particles. By including hollow particles in the insulating material, the thermal conductivity of the insulating material can be further reduced. [4] In the double-shelled container of the present invention, preferably, the hollow particles have a shell, and the hollow part inside the shell is filled with a gas having a thermal conductivity lower than that of air, thereby further improving the thermal insulation performance of the heat insulating material. [5] In the double-shelled container of the present invention, it is preferable that the space 30 for filling the aerogel between the inner cylinder 10 and the outer cylinder 20 is filled with a gas having a lower thermal conductivity than air. This can further improve the thermal insulation performance of the heat insulating material. [6] In the double-shelled container of the present invention, the aerogel-filling space 30 between the inner cylinder 10 and the outer cylinder 20 is preferably depressurized to a pressure lower than atmospheric pressure, thereby further improving the thermal insulation performance of the heat insulating material.
[0015] [7] In the double-shelled container of the present invention, as shown in Fig. 1, the double-shelled container preferably includes a support mechanism 50 fixed to the outer cylindrical body 20 to support the inner cylindrical body 10, and the support mechanism 50 is preferably configured by folding or winding a member longer than the linear distance between the inner cylindrical body 10 and the outer cylindrical body 20 into a coil shape. This makes it possible to suppress heat conduction through the support mechanism 50 connecting the inner cylindrical body 10 and the outer cylindrical body 20, and improves the thermal insulation performance of the entire double-shelled container. [8] In the double-shelled container of the present invention, preferably, at least three support mechanisms 50 are provided on the bottom side of the outer cylinder 20, and at least one support mechanism 50 is provided on the side side of the outer cylinder 20.
[0016] [9] In the double-shelled container of the present invention, it is preferable that at least one of the inner cylinder 10 and the outer cylinder 20 is further covered with a material containing fiber.
[10] In the double-shelled container of the present invention, the fiber-containing member preferably contains at least one of glass fiber or carbon fiber.
[0017]
[11] In the double-shelled container of the present invention, as shown in FIG. 3, the inner cylinder 10 preferably has a gently sloping surface formed on its upper surface with the apex located approximately at the center.
[12] In the double-shell container of the present invention, as shown in FIG. 3, the outer cylinder 20 preferably has a bottom surface that is gently inclined with the bottom being located approximately at the center. Effect of the Invention
[0018] The double-shelled container of the present invention has the following advantages. (1) Aerogel powder is used as the insulation material for the cryogenic storage and transportation tank, which significantly improves the insulation performance of the cryogenic tank compared to perlite, which is the insulation material used in conventional cryogenic storage and transportation tanks. (2) The use of aerogel powder improves the cold insulation properties of the cryogenic chamber, reducing the degree of vacuum required in the cold insulation layer and reducing the electricity costs required to maintain a high degree of vacuum in the insulation layer. (3) The use of aerogel powder improves the insulation of the cryogenic chamber, so less energy is needed to cool the LH2. (4) The weakly bonded ultrafine aerogel powder used in the present invention has a very low density, and the volume is 6 to 10 times that of ordinary aerogel for the same weight. Therefore, if the weakly bonded ultrafine aerogel powder used in the present invention is filled in the heat insulating layer, the material cost of the aerogel can be significantly reduced. (5) The weakly bonded ultrafine aerogel powder used in the present invention has very good fluidity. In addition, by providing an inclined shape on the top and bottom of the tank as in the embodiment, it becomes easier for the weakly bonded ultrafine aerogel powder to properly fill the insulating layer. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a cross-sectional structural view of an aerogel insulated tank showing one embodiment of a double-shelled container of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating the temperature distribution in the thickness direction of an aerogel insulated tank showing one embodiment of the double-shelled container of the present invention. [Diagram 3] 1A-1C are schematic diagrams showing the configuration of an aerogel insulated tank, illustrating various embodiments of the double-shelled container of the present invention. [Figure 4] FIG. 1 is an explanatory diagram showing a typical structure of aerogel and aerogel powder produced by pulverizing the aerogel. [Diagram 5] FIG. 1 is an explanatory diagram showing the aerogel of the present invention and ultrafine aerogel powder produced by pulverizing the aerogel. [Figure 6] FIG. 2 is a manufacturing process diagram showing an example of a method for producing the weakly bonded ultrafine aerogel powder used in the present invention. [Figure 7] FIG. 4 is an explanatory diagram showing an example of control of the rotation speed of a crusher in a high-speed crushing process. [Figure 8] FIG. 2 is a distribution diagram showing the particle size distribution after a high speed grinding process. [Figure 9] 1 is an image illustrating the bulk of the aerogel powder used in the double-shelled container of the present invention. [Figure 10] FIG. 2 is a comparative diagram of the densities of the aerogel powders used in the double-shelled container of the present invention. [Figure 11] 1 is a graph showing compression characteristics when vibration is applied to the prototype ultrafine aerogel powder. [Figure 12] FIG. 1 illustrates the thermal conductivity of commercial aerogel powders under different pressures and temperatures. [Figure 13] FIG. 1 is an explanatory diagram of the transportation of liquid hydrogen, which is an application for which the double-shelled container of the present invention is used, showing its use on a ship. [Figure 14] FIG. 1 is an explanatory diagram of liquid hydrogen storage, an application for which the double-shelled container of the present invention is used, showing a spherical tank. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will now be described with reference to the drawings. Fig. 1 is a cross-sectional structural diagram of an aerogel heat-insulating tank showing one embodiment of the double-shelled container of the present invention. In the figure, the aerogel heat-insulating tank has an inner cylinder 10, an outer cylinder 20, an aerogel filling space 30, a support mechanism 50, a sensor 60, and liquid hydrogen 40 contained in the inner cylinder 10. The inner cylinder 10 is also called the inner cylinder, and is preferably made of a metal such as aluminum that is resistant to hydrogen embrittlement, but may also be made of austenitic steel, stainless steel, or plastic reinforced with carbon fiber or gas fiber, which are less brittle at low temperatures and are used as structural materials for low-temperature pressure vessels for LNG, etc. The glass fiber / carbon fiber coating layer 12 covers the surface of the inner cylinder 10 facing the outer cylinder 20, and reinforces the circumferential surface of the inner cylinder 10. The volume of the inner cylinder 10 should be determined to be suitable for transportation and storage, taking into consideration, for example, standards related to pressure vessels and standards under the Fire Service Act. The outer cylinder 20 is also called a housing, and may be made of metals normally used as structural materials, such as stainless steel and carbon steel, or plastics reinforced with carbon fiber or gas fiber. The glass fiber / carbon fiber coating layer 22 coats the surface of the outer cylinder 20 and reinforces the circumferential surface of the outer cylinder 20.
[0021] The aerogel filling space 30 is a spherical shell, ellipsoid shell, or rectangular parallelepiped region located between the inner cylinder 10 and the outer cylinder 20, and acts as a heat insulating layer with low thermal conductivity. The aerogel powder filled in the aerogel filling space 30 will be described later. The bottom of the aerogel filling space 30 is filled with a solid form of baking soda + acid (such as citric acid crystals) that provides a mechanism for slowly releasing CO2. On top of this solid form of baking soda + acid, weakly bonded ultrafine aerogel powder is filled.
[0022] Liquid hydrogen 40 is contained in the inner cylinder 10 and stored or transported. Inside the inner cylinder 10, a mixture of liquid hydrogen 40 and hydrogen gas 41 is formed. The allowable pressure of hydrogen gas may be determined, for example, so as to comply with standards related to pressure vessels; for example, if the internal pressure is less than 0.2 MPa, it is not subject to regulations for pressure vessels under current Japanese standards. However, if the allowable pressure of compressed hydrogen gas is excessively low, it becomes necessary to vent the hydrogen gas during storage or transportation, and the hydrogen gas will be discharged by venting. A liquid hydrogen supply / suction outlet 42 for supplying or suctioning liquid hydrogen is provided on the upper surface of the spherical shell, ellipsoid shell, or rectangular cross-section shell of the outer cylinder 20. A hydrogen gas / liquid hydrogen supply port 43 is provided on the upper surface of the spherical shell, ellipsoid shell, or rectangular cross-section shell of the outer cylinder 20 to supply hydrogen gas or liquid hydrogen. A hydrogen gas suction outlet 44 is provided on the upper surface of the spherical shell, ellipsoid shell, or rectangular cross-section shell of the outer cylinder 20. The aerogel filling ports 45, 46 are provided on the upper surface of the spherical shell, ellipsoid shell, or rectangular cross-section shell of the outer cylinder 20 in order to fill the aerogel powder. The safety valve 48 is provided to prevent the internal pressure of the inner cylinder 10 from increasing abnormally due to liquid hydrogen or hydrogen gas and exceeding the withstand pressure of the inner cylinder 10.
[0023] The support mechanism 50 elastically supports the inner cylinder 10 with the outer cylinder 20, and protects the inner cylinder 10 from vibration and shaking that occurs when the double-shelled container is loaded, for example, on a transport ship or tanker or on a truck. The support mechanism 50 has an outer cylinder side fixed end 52 and an inner cylinder side fixed end 54, and the damper 56 elastically supports between the outer cylinder side fixed end 52 and the inner cylinder side fixed end 54, and is preferably structured to suppress heat conduction between the inner cylinder 10 and the outer cylinder 20 through the support mechanism 50. Therefore, the damper 56 is preferably configured by folding a member longer than the linear distance between the inner cylinder 10 and the outer cylinder 20 or by winding it in a coil shape. The outer cylinder side fixed end 52 and the inner cylinder side fixed end 54 are paired, and here, multiple ones are provided on the bottom side and the top side of the inner cylinder 10. Since the support mechanism 50 is provided in the aerogel filling space 30, it is preferable to use a material with low thermal conductivity so as to have little effect on the thermal conductivity between the inner cylinder 10 and the outer cylinder 20.
[0024] If at least three support mechanisms 50 are provided on the bottom side of the outer cylindrical body 20, the inner cylindrical body 10 can be supported so that it floats on the outer cylindrical body 20. If at least one support mechanism 50 is provided on the side side of the outer cylindrical body 20, the inner cylindrical body 10 can be protected from acceleration / deceleration and vibration and rocking in a horizontal plane when the double-shelled container is loaded, for example, on a transport ship or tanker or on a truck, but this is not limited to this, and the support mechanism 50 may be provided not only on the front and rear side sides and left and right side sides of the outer cylindrical body 20, but also on the top side of the outer cylindrical body 20. The sensor 60 is provided on the circumferential surface of the inner cylinder 10 on the side of the space 30 for filling with aerogel, and measures the degree of vacuum and the temperature of the space 30 for filling with aerogel.
[0025] 2 is a cross-sectional view illustrating the temperature distribution in the thickness direction of an aerogel heat-insulating tank showing one embodiment of the double-shelled container of the present invention. Inside the inner cylinder 10, liquid hydrogen 40 exists, and the liquid hydrogen 40 is −253° C. or lower. Outside the outer cylinder 20, there is outside air, and the normal temperature of the outside air is, for example, 25° C., but depending on the external environment, it can vary from, for example, about −30° C. in the polar regions to 50° C. during the day in the desert. In the aerogel filling space 30, the temperature distribution between the inner cylinder 10 and the outer cylinder 20 has a gradient from −253° C. to, for example, 25° C.
[0026] FIG. 3 is a schematic diagram of the shape of an aerogel double-shelled insulated tank showing various embodiments of the double-shelled container of the present invention. The cross-sectional shapes of the inner and outer layers are shown for the case where the shape of the double-shelled container is a cylindrical tank having a sphere, an ellipsoid, or a cuboid cross section. The central top of the inner cylinder has a convex or cone-shaped tip, and has an upwardly inclined ceiling surface centered on this tip. This upwardly inclined ceiling surface ensures that the aerogel powder has high fluidity and is sufficiently filled in the insulating layer 30 when filled. The outer cylinder has a convex or cone-shaped downward tip at the center of its bottom surface, and has a bottom surface that slopes downward from the tip. This downward slope ensures that the aerogel powder has high fluidity and is sufficiently filled into the insulating layer 30 when it is filled with the aerogel powder.
[0027] Table 1 provides design guidelines for the geometric shape of double-shell vessels. The thickness of the inner cylinder 10 and the outer cylinder 20 is determined by the volume and material of the double-shelled vessel, as well as the internal pressure of the vessel, and is determined in accordance with, for example, the pressure vessel standards and Fire Service Act regulations of each country for liquid hydrogen. 3 Less than 5,000 m is preferable. 3 Less than 0.1,500 m is more preferable, with the optimal range being 0.1,500 m 3The thickness of the inner cylinder 10 is preferably, for example, 2 mm or more and 1000 mm or less, more preferably 5 mm or more and 300 mm or less, and the optimal range is preferably 10 mm or more and 150 mm or less. The thickness of the outer cylinder 20 is preferably, for example, 2 mm or more and 300 mm or less, more preferably 3 mm or more and 100 mm or less, and the optimal range is preferably 5 mm or more and 50 mm or less. The thickness of the aerogel filling space 30 is preferably, for example, 3 mm or more and 1500 mm or less, more preferably 10 mm or more and 600 mm or less, and the optimal range is preferably 30 mm or more and 300 mm or less. The degree of vacuum of the aerogel filling space 30 is preferably 10 -3 The pressure is preferably from 0.1 Pa to 0.1 MPa, more preferably from 0.13 Pa to 0.1 MPa, and the optimum range is from 133 Pa to 0.1 MPa. [Table 1]
[0028] Next, the cold insulation material used in the double-shelled container of the present invention will be described. The cold insulation material is filled in the space between the inner cylinder 10 and the outer cylinder 20, which is a spherical shell, an ellipsoid shell, or a rectangular parallelepiped cross section, and contains a weakly bonded ultrafine aerogel powder. Here, the weakly bonded ultrafine aerogel powder is a fine particle having a three-dimensional network structure whose skeleton is composed of primary particles, and the raw material is an aerogel having a three-dimensional network structure whose skeleton is composed of clusters that are aggregates of primary particles. This allows a low-cost, high-performance insulation material to be filled in the space between the inner cylinder 10 and the outer cylinder 20, which is a spherical shell, an ellipsoid, or a rectangular parallelepiped cross section. Here, the fine particles preferably have a mode (peak) of dispersion of 1.0 μm or less, and more preferably, 50% or more of the total number of the fine particles have a peak of dispersion of 0.1 μm or more and 1.0 μm or less. This allows the bulk density to be reduced to a fraction of that of conventional aerogel powder, and therefore the amount of aerogel required to fill the space between the inner cylinder and the outer cylinder can be reduced to a fraction of that of conventional aerogel powder.
[0029] It is well known that aerogels with a three-dimensional network structure with fine pores can be produced by subjecting gels produced by the sol-gel method to supercritical drying or the like. A sol produced by hydrolysis and condensation of a metal alkoxide solution is gelled to produce a wet gel, which is then aged and the solvent components are removed by supercritical drying to produce an aerogel. In a metal alkoxide solution, primary particles are dissolved in a solvent, and these primary particles condense with each other through hydrolysis and condensation to form a colloid. This is a gel, and the colloids formed are called secondary particles in contrast to the primary particles before condensation. In the gelled state, it is a wet gel containing solvent components. When the solvent components are removed from the wet gel by supercritical drying or the like, a three-dimensional network structure consisting of secondary particles as units remains. This is the aerogel. Such aerogels are used by mechanically crushing them into powders of approximately tens of μm to several mm.
[0030] The weakly bonded ultrafine aerogel powder used in the present invention is produced by producing an aerogel in which the progress of aging is suppressed more than before, and then pulverizing it at an ultra-high speed. This results in a fine powder that is about 1 / 1000th of the fine powder produced when the conventional aerogel is mechanically pulverized. The weakly bonded ultrafine aerogel powder is preferably one that has a particle size distribution mode (peak) of 1.0 μm or less when observed by PSD measurement, and more preferably produced by pulverizing at an ultra-high speed under aging and pulverization conditions such that 50% or more of the total number of particles are dispersed with a particle size distribution mode of 100 nm to 1.0 μm. The particle size of the weakly bonded ultrafine aerogel powder observed by the inventors by PSD measurement is distributed with a mode of about 300 nm. Details will be described later.
[0031] Each weakly bonded ultrafine aerogel powder particle of the present invention has a three-dimensional network structure. Conventional aerogel powder particles also have a three-dimensional network structure, but the weakly bonded ultrafine aerogel powder used in the present invention has a different unit that constitutes its skeleton. That is, as described in paragraph 0035 of Patent Document 5, "aerogel particle 1 is considered to be in the form of a secondary particle composed of a plurality of primary particles," the three-dimensional network structure of conventional aerogel powder particles is composed of secondary particles as units, whereas the ultrafine aerogel powder used in the present invention is characterized in that the unit that constitutes its skeleton is a primary particle.
[0032] FIG. 4 is an explanatory diagram showing the structure of a typical aerogel and the aerogel powder produced by pulverizing the aerogel. (A) shows the structure of a typical aerogel 130 and a cut surface 140 obtained when the aerogel is pulverized. (B) shows secondary particles 120 that form the skeleton of the three-dimensional mesh structure. (C) shows aerogel powder 150 produced by pulverizing aerogel 130 of (A). As shown in FIG. 4(A), in a typical aerogel 130, the colloids contained in the gel before drying become secondary particles 120, and a three-dimensional network structure 130 is formed with the secondary particles 120 as skeleton units. In the aerogel thus created, the skeleton is formed in about 10% of the volume of the three-dimensional network structure, and the remaining 90% is formed by pores. When the size of the pores is smaller than the mean free path of the gas that fills the pores, such as air, almost no heat conduction occurs due to collisions of gas molecules. For this reason, aerogel is used as a thermal insulation material.
[0033] FIG. 4(C) shows a schematic structure of aerogel powder 150 when a general aerogel is crushed. When the general aerogel shown in FIG. 4(A) is crushed, the cut surface 140 by the crusher is not the secondary particles 120 themselves, but the points where the secondary particles are connected. This is thought to be because, as shown in FIG. 4(B), the secondary particles are strongly bonded because the primary particles are densely aggregated, and the bonds between the secondary particles are much weaker. As a result, the aerogel powder 150 when the general aerogel is crushed has a three-dimensional network structure in which the skeleton is formed by the secondary particles 120 (FIG. 4(C)).
[0034] FIG. 5 is an explanatory diagram showing the structure of the aged aerogel 131 of the present invention and the weakly bonded ultrafine aerogel powder 151 produced by pulverizing the aged aerogel 131. (A) shows the three-dimensional mesh structure of the aerogel 131 produced after the aging process in the process of producing the weakly bonded ultrafine aerogel powder 151 used in the present invention. (B) shows the secondary particles 121 that form the skeleton of the three-dimensional mesh structure of the aerogel shown in (A). (C) shows a cut surface 140 when the aerogel 131 shown in (A) is pulverized. (D) shows the weakly bonded ultrafine aerogel powder 151 used in the present invention.
[0035] In the present invention, aerogel is produced by suppressing aging compared to the general process. Therefore, the three-dimensional network structure of the produced aerogel 131 is formed with the secondary particles 121 (FIG. 5(B)) in which the primary particles 111 are more sparsely packed than in the conventional process (FIG. 5(A)). When an aerogel having such a three-dimensional network structure 131 (FIG. 5(A)) is subjected to ultra-high speed pulverization, not only the mutual bonding parts of the secondary particles 121 that constitute the skeleton, but also the secondary particles 121 themselves have cut surfaces 140 by the pulverizer as shown in FIG. 5(C), and it is considered that the secondary particles 121 themselves are pulverized. As a result, the weakly bonded ultrafine particle aerogel powder 151 used in the present invention has a three-dimensional network structure in which the skeleton is formed by the primary particles 111 as shown in FIG. 5(D). In addition, since secondary particle 121 is formed by loosely agglomerating primary particles 111 as shown in Figure 5 (B), the outer edge of actual secondary particle 121 is unclear, but in Figure 5 (C) the part corresponding to the outer edge is shown as a dashed circle to facilitate understanding. [Embodiment 1]
[0036] An example of a method for producing the ultrafine aerogel powder used in the present invention will now be described. FIG. 6 is a production process diagram showing an example of a method for producing the weakly bonded ultrafine aerogel powder used in the present invention.
[0037] Silica aerogel is mainly produced in two steps: forming a wet gel by the sol-gel method and drying the wet gel. The wet gel consists of a nanostructured solid silica network and a liquid solvent, and is produced by hydrolyzing and condensing silica precursor molecules. This silica precursor is produced by mixing TEOS (Tetraethoxysilane) and methanol (mixing step). A total of 6.3 g of oxalic acid (0.01 M) is then added to this mixture, and finally 1.5 g of ammonium hydroxide (NH4OH 0.5 M) is added to produce an alcosol. This alcosol gels when left at room temperature (gelation step). Following gelation, the alcogels were aged in methanol at 60°C for 3, 6, and 12 hours, respectively (aging step). To prevent the methanol from evaporating completely during the aging step, an excess amount of methanol can be added to the gel. The amount of this excess amount of methanol can be determined taking into account the amount of methanol evaporated during the aging step, as well as the aging temperature and aging time.
[0038] To avoid the reverse reaction of the surface modification, the alcogel was immersed in hexane at 60°C for 10 hours, and the hexane-only solvent was replaced with a mixture of hexane and TMCS (Trimethylchlorosilane) to modify the surface (solvent replacement process). Here, the volume ratio of hexane to TMCS was kept constant at 4. In the surface modification process, the alcogel was immersed in a mixture of hexane and TMCS at 60°C for 24 hours (modification process). Before drying the alcogel, the sample was immersed in pure hexane at 60°C for 6 hours to remove excess TMCS (washing process). The final step in creating the aerogel is drying (drying process). The drying process consists of the first to third steps and a cooling step. The first step was kept at 40°C for 4 hours, the second step at 80°C for 2 hours, and the third step at 120°C for 1 hour, and then cooled together with the entire furnace.
[0039] After the drying process, the aerogel sample was subjected to high-speed crushing (crushing process). Using a Wonder Crusher WC-3 manufactured by Osaka Chemical Co., Ltd., a program of about 5 minutes at a high speed of 11200 rpm to 21000 rpm was carried out three times as shown in FIG. 7.
[0040] It should be noted that it is practically difficult to completely distinguish between gelation and aging, and that the aggregation of fine particles proceeds simultaneously with gelation, leading to a reaction similar to that of aging. In this example, the temperature of the alcosol is raised from room temperature to 60°C to promote aging, but in applications where fine particles are preferred, the temperature of the alcosol may be kept at room temperature, and the aging process may be a short process of about 1 second to 1 minute, in which case it may not be clearly distinguishable from the gelation process.
[0041] FIG. 8 is a distribution diagram showing the particle size distribution after the high-speed grinding process. For each sample with an aging time of 3 hours, 6 hours, and 12 hours, the particle size is plotted on the horizontal axis in a logarithmic scale, and the frequency (left vertical axis) and cumulative value (right vertical axis) of the relative particle amount are shown. For comparison, data on conventional (commercially available) aerogel powder is also shown. Here, the particle size was observed by PSD measurement. More specifically, FIG. 8 shows the results of measurement using a laser diffraction particle size distribution measuring device SALD-2300 manufactured by Shimadzu Corporation. Note that in PSD measurement, not only the diameter of the particle itself but also the aggregation of particles is observed as the particle diameter, so it is necessary to note that the measured value is biased in the positive direction (there are many errors in which a value larger than the true value is measured). However, as described below, sufficient information has been obtained to explain the characteristics of the ultrafine aerogel powder used in the present invention.
[0042] In the conventional aerogel powder, the relative particle amount has only one peak with the average particle size of about 300 μm. In contrast, in the ultrafine aerogel powder of the present invention, the frequency of the relative particle amount after the high-speed grinding process for the samples aged for 3, 6, and 12 hours has a bimodal peak. In the sample aged for 3 hours, the first peak has an average of 0.32 μm with a standard deviation of 0.10, and the second peak has an average of 21.14 μm with a standard deviation of 0.14. In the sample aged for 6 hours, the first peak has an average of 0.66 μm with a standard deviation of 0.15, and the second peak has an average of 31.89 μm with a standard deviation of 0.40. In the sample aged for 12 hours, the first peak has an average of 0.96 μm with a standard deviation of 0.13, and the second peak has an average of 38.52 μm with a standard deviation of 0.21.
[0043] The fact that the peaks are divided into two peaks strongly suggests that there is an essential difference between the particles that make up each peak. If there is no essential change and the diameter of the particles produced changes depending on the aging conditions, it is difficult to imagine that two peaks would appear, even if the position of the peak changes accordingly. Therefore, it is natural to think that the particles that make up the second peak, which has a large particle size, have a three-dimensional network structure with secondary particles as the skeleton unit as in the past, while the particles that make up the first peak, which has a small particle size, have a three-dimensional network structure with primary particles as the skeleton unit. In other words, this result supports the explanation above with reference to Figures 4 and 5.
[0044] It is also found that by changing the aging conditions, the properties of the particles generated after high-speed grinding, i.e., whether the secondary particles or primary particles are the structural units of the skeleton, can be significantly changed, i.e., controlled. The mode of the dispersion of the larger particle size is 10 μm or more, and the mode of the dispersion of the smaller particle size is 1 μm or less. In the samples aged for 6 and 12 hours and then high-speed grinding, the cumulative value of the relative particle amount exceeds 50% on the side of the larger particle size peak. The cumulative value of the relative particle amount exceeds 50% on the side of the second peak when the particle size is about 20 μm in the sample aged for 6 hours and then high-speed grinding, and when the particle size is about 40 μm in the sample aged for 12 hours and then high-speed grinding. On the other hand, in the sample that was aged for 3 hours and then crushed at high speed, the cumulative value of the relative particle amount exceeds 50% at the peak (first peak) with a particle diameter of about 0.3 μm. From another perspective, in the samples that were aged for 6 and 12 hours and then crushed at high speed, 60% to 70% of the particles have a diameter of 10 μm or more, and the particles are mainly composed of secondary particles as skeleton units based on their size, whereas in the weakly bonded ultrafine particle aerogel powder of this embodiment that was aged for 3 hours, about 80% of the particles have a diameter in the range of 0.1 μm to 1.0 μm, that is, the particles are mainly composed of primary particles as skeleton units based on their size.
[0045] As for the aging conditions, in addition to shortening the time as described above, it is also effective to lower the temperature as compared to the conventional conditions. That is, the aging conditions for producing the ultrafine particle aerogel powder used in the present invention are preferably 15°C to 70°C, more preferably 20°C to 70°C, and even more preferably 25°C to 60°C, and the aging time is preferably 0 to 24 hours, more preferably 0 to 12 hours, and even more preferably 3 to 12 hours. As for the grinding parameters, the rotation speed of the grinder is preferably 10,000 to 28,000 rpm, more preferably 10,000 to 25,000 rpm, and even more preferably 11,000 to 22,000 rpm, and the grinding time is preferably 1 to 120 minutes, more preferably 3 to 60 minutes, and even more preferably 5 to 45 minutes.
[0046] FIG. 9 is an image for explaining the bulk of the aerogel powder used in the double-shelled container of the present invention, showing the case where 5 g of aerogel powder is placed in a beaker with a capacity of 200 cc or 500 cc. From the left, the images show an aerogel powder obtained by crushing a commercially available aerogel, and samples of ultrafine aerogel powder aged for 12 hours, 6 hours, and 3 hours. The samples of ultrafine aerogel powder are the same as those described in FIG. 8. When the aging time is short, at 3 hours, the bulk of the weakly bonded ultrafine aerogel powder increases to more than 10 times that of the commercially available aerogel powder.
[0047] FIG. 10 is a comparative diagram of the densities of the aerogel powders used in the double-shelled container of the present invention. The bulk density of the experimentally produced weakly bonded ultrafine aerogel powder was 0.018 g / cm 3 This is in line with the bulk density of commercially available aerogel powder, which is 0.06 g / cm. 3 ~0.20g / cm 3 The thermal conductivity is 1 / 3 to 1 / 11 of that of commercially available aerogel powder. On the other hand, the thermal conductivity is measured to be 23 mW / mK, which is the same level as that of commercially available aerogel powder.
[0048] Figure 11 is a graph showing the compression characteristics when vibration is applied to the experimentally produced weakly bonded ultrafine aerogel powder. The experimentally produced ultrafine aerogel powder was placed in a container with a fixed base area, and vibration was applied to measure the change in height of the aerogel powder over time, and the graph shows a comparison with commercially available aerogel powder. The horizontal axis shows the vibration time in arbitrary units. The conventional aerogel powder reached a constant value at 82% of its initial height, whereas the experimentally produced weakly bonded ultrafine aerogel powder reached a constant value at 69%. Using this characteristic, the saturation point at which the bulk density is compressed due to changes over time is estimated to be 0.018 g / cm for the experimentally produced weakly bonded ultrafine aerogel powder mentioned above. 3 can be reduced by up to 0.026g / cm 3 On the other hand, according to the same theory, the bulk density of commercially available aerogel powder is 0.12 g / cm 3 is a maximum of 0.13g / cm 3Although the difference is slightly smaller, there is still a ratio of 1:5. The weakly bonded ultrafine aerogel powder used in the present invention has a bulk density that is a fraction of that of conventional aerogel powders, and requires a fraction of the amount to fill the same space.
[0049] Figure 12 illustrates the thermal conductivity of commercial aerogels under different pressures and temperatures, taken from the references shown in the figure. The thermal conductivity of commercially available aerogel decreases with decreasing pressure, being approximately 20 mW / mK at normal pressure of 760 Torr (0.1 MPa), approximately 14 mW / mK at 10 Torr (1333 Pa), and approximately 4 mW / mK at 1 Torr (133 Pa). The thermal conductivity of commercially available aerogel decreases with decreasing temperature, being approximately 23 mW / mK at room temperature (25°C) and approximately 9 mW / mK at liquid nitrogen temperature (-196°C).
[0050] Table 2 explains the composition range of the weakly bonded ultrafine aerogel powder used in the double-shelled container of the present invention. The particle size of the weakly bonded ultrafine aerogel powder used in the double-shelled container of the present invention is preferably 0.1 to 400 μm, more preferably 0.1 to 50 μm, and even more preferably 0.1 to 1 μm. The density is 0.003 to 0.15 [g / cm 3 ] is preferable, and more preferably 0.01 to 0.08 [g / cm 3 ], and more preferably 0.015 to 0.03 [g / cm 3 ]. [Table 2]
[0051] As described above, in the present invention, if the weakly bonded ultrafine aerogel powder is used as a heat insulating material to fill the space between the inner and outer cylinders of a double-shelled container, which is spherical, ellipsoidal, or rectangular in cross section, the bulk density is a fraction of that of conventional aerogel powder, so the cost of the heat insulating material required for filling can be significantly reduced. In addition, since the ultrafine aerogel powder is hydrophobic, there is almost no deterioration over time due to reaction with moisture remaining in the spherical, ellipsoidal, or rectangular in cross section space, so the maintenance cost of periodically replacing the heat insulating material can be significantly reduced. Furthermore, since the ultrafine aerogel powder is very fine, it can be filled to every corner even if there is a narrowed part in the spherical, ellipsoidal, or rectangular in cross section space between the inner and outer cylinders, which greatly contributes to improving the thermal insulation performance of the double-shelled container. [Embodiment 2]
[0052] In the double-shelled container of the first embodiment, hollow particles may be added to the weakly bonded ultrafine aerogel powder filled as a heat insulating material in the space between the inner cylinder 10 and the outer cylinder 20 that is spherical, ellipsoidal, or rectangular in cross section. This can reduce the thermal conductivity of the heat insulating material.
[0053] By using aerogel as a thermal insulation material, the size of the pores in the aerogel is smaller than the mean free path of air, so that heat conduction through the gas due to collisions of gas molecules or convection is suppressed, and thermal insulation performance close to that when the pores are a vacuum is expected. However, in reality, the performance does not reach that of a vacuum. As a result of the inventor's investigation into the cause, it was found that fine interconnected pores remain in the insulation material filled with aerogel powder, and the above-mentioned heat conduction occurs through these interconnected pores. Therefore, the inventors created a technology to reduce the thermal conductivity by adding hollow particles to the aerogel to hybridize it (patent application filed as Patent Application 2020-120921). The added hollow particles block the fine interconnected pores as described above, suppressing the slight heat conduction through the gas, and therefore the thermal conductivity can be reduced.
[0054] In addition, since the spherical shells constituting the hollow particles are highly airtight, the thermal conductivity of the insulating material can be further reduced by sealing a gas with a lower thermal conductivity than air inside the spherical shells. The hollow particles to be added are not particularly limited, but may be nano-hollow particles, micro-hollow particles, or both. The nano-hollow particles are preferably prepared to have an outer diameter of 30 nm to 360 nm and a shell thickness of 7.5 nm to 65 nm. The outer diameter corresponds to a range of about 1 / 2 to about 5 times the mean free path of air at room temperature and normal pressure. In this way, the hollow size of the nano-hollow particles is prepared to be on the same order as the mean free path of air, so when added to aerogel, it contributes greatly to the heat insulating effect. The micro-hollow particles are preferably prepared to have an outer diameter of 1 μm to 23 μm and a shell thickness of 0.35 μm to 3 μm. The outer diameter is larger than 15 times the mean free path of air at room temperature and normal pressure, and in addition to contributing to the heat insulating effect, it has the effect of increasing the structural strength of the mesh. The fine interconnected pores described above remain in the aerogel, but the added hollow particles block these pores and suppress heat conduction through gas, such as convection, which occurs through the interconnected pores, thereby improving the insulating effect.
[0055] Hollow nanoparticles can be produced, for example, by the soft template method. That is, the surface of a polymer electrolyte is modified with ammonia in ethanol and then coated with silica (SiO2) to produce particles consisting of a core and a spherical shell. The medium trapped in the core is removed by washing or baking the particles, and hollow particles are produced. For example, the double emulsion method is suitable for producing hollow microparticles. From a dispersed multiphase system consisting of an immiscible liquid such as an oil phase containing a surfactant and an aqueous phase consisting of a precursor and a surfactant, an emulsion containing droplets with the oil phase as the continuous phase and the aqueous phase as the center is produced by emulsification, and by adding aqueous phase to this, it is changed to an emulsion containing droplets with the gel as the center in the aqueous phase continuous phase. By washing / filtering or baking this, hollow microparticles are produced.
[0056] In the method for producing the ultrafine aerogel powder used in the present invention, the hollow particles may be added to a mixture of TEOS and methanol prepared as a silica precursor (mixing step) before the gelation step in the manufacturing process diagram shown in Figure 6. After the addition, the mixture may be sufficiently stirred by ultrasonic vibration to uniformly disperse the added hollow particles. The amount of hollow particles added is adjusted to the entire hybridized aerogel so as to have the following composition, for example.
[0057] The content of the hollow nanoparticles is preferably 0.01% to 30% by weight, more preferably 0.10% to 15% by weight, and most preferably 1.00% to 10% by weight. Similarly, the content of the hollow microparticles is preferably 0.01% to 30% by weight, more preferably 0.10% to 15% by weight, and most preferably 1.00% to 10% by weight.
[0058] As described above, in a double-shelled container, by adding hollow particles to the weakly bonded ultrafine aerogel powder that is filled as an insulating material in the spherical, ellipsoidal, or rectangular space between the inner and outer cylindrical bodies 10 and 20, the thermal conductivity of the insulating material can be reduced.
[0059] Next, the equipment for transporting and storing liquid hydrogen in which the heat insulating material of the present invention is used will be described. Fig. 13 is an explanatory diagram of liquid hydrogen transport, which is an application in which the double-shelled container of the present invention is used, showing its use on a ship. The double-shelled container of the present invention is suitable for use as a container on a ship. Fig. 14 is an explanatory diagram of liquid hydrogen storage, which is an application for which the double-shelled container of the present invention is used, showing a spherical tank. The double-shelled container of the present invention is suitable for use as a container for storing liquid hydrogen. [Industrial Applicability]
[0060] The double-shelled container of the present invention can store hydrogen in a liquid state, a gaseous state, or a mixture of these states. Also, since the double-shelled container of the present invention uses weakly bonded ultrafine aerogel powder, a lower degree of vacuum is preferred to achieve the desired insulation for LH2 storage. [Explanation of symbols]
[0061] 10 Inner cylinder 12 Glass fiber / carbon fiber coating layer 20 Outer cylinder (housing) 22 Glass fiber / carbon fiber coating layer 30 Space for filling with aerogel (vacuum insulation layer) 40 Liquid Hydrogen 41 Hydrogen Gas 42 Liquid hydrogen supply / suction outlet 43 Hydrogen gas / liquid hydrogen supply port 44 Hydrogen gas outlet 45, 46 Aerogel filling port 47 Gas outlet for aerogel filling space 48 Safety valve 50 Support mechanism 52 External cylinder side fixed end 54 Inner cylinder side fixed end 56 Damper 60 Sensors 111 Primary particles 120 Secondary particles 121 Secondary particles formed by sparsely packing primary particles 130 Three-dimensional network structure formed by a skeleton of secondary particles 131 Three-dimensional network structure formed by a skeleton of secondary particles in which primary particles are sparsely packed 140 Cut surface by crusher 150 General Aerogel Powder 151 Weakly bonded ultrafine airgel powder
Claims
1. A double-shelled container having an inner cylinder, an outer cylinder, an aerogel-filling space provided between the inner cylinder and the outer cylinder, and a heat insulating material filled in the aerogel-filling space, The heat insulating material is made of an aerogel having a three-dimensional mesh structure with a skeleton formed of clusters that are aggregates of primary particles, and includes first fine particles having a three-dimensional mesh structure with a skeleton formed of the primary particles, and second fine particles having a three-dimensional mesh structure with a skeleton formed of secondary particles formed by an aggregation of a plurality of the primary particles, A double-shelled container, wherein 50% or more of the total number of the first fine particles are dispersed with a particle diameter having a mode of 0.1 μm to 1.0 μm.
2. 2. The double-shelled container of claim 1, wherein the insulating material further comprises hollow particles.
3. The aerogel has fine interconnecting pores remaining, 3. The double-shelled container according to claim 2, wherein the hollow particles block the communicating holes.
4. The hollow particles are nano-hollow particles, micro-hollow particles, or both, The hollow nanoparticles are prepared so that their outer diameter is in the range of 30 nm to 360 nm and their shell thickness is in the range of 7.5 nm to 65 nm; 4. The double-shelled container according to claim 2 or 3, wherein the hollow microparticles are prepared to have an outer diameter in the range of 1 μm to 23 μm and a shell thickness in the range of 0.35 μm to 3 μm.
5. The hollow particles are nano-hollow particles, micro-hollow particles, or both, The hollow nanoparticles have an outer diameter that is in the range of 1 / 2 to 5 times the mean free path of air at room temperature and pressure, 4. The double-shelled container according to claim 2 or 3, wherein the outer diameter of the hollow microparticles is adjusted to be greater than 15 times the mean free path of air at room temperature and pressure.
6. In the case where the hollow nanoparticles are contained, the composition ratio thereof is 0.01% by weight or more and 30% by weight or less, In the case where the hollow microparticles are contained, the composition ratio thereof is 0.01% by weight or more and 30% by weight or less, 6. The double-shelled container according to claim 4, wherein the remainder is made of said aerogel.
7. The double-shelled container according to any one of claims 2 to 6, characterized in that the insulating material is a hollow particle further having a shell, and a gas having a thermal conductivity lower than that of air is sealed in the hollow part inside the shell.
8. 8. The double-shelled container according to claim 1, wherein the space for filling the aerogel provided between the inner cylinder and the outer cylinder is filled with a gas having a thermal conductivity lower than that of air.
9. The double-shelled container according to any one of claims 1 to 8, characterized in that the space for filling the aerogel provided between the inner cylinder and the outer cylinder is depressurized to a pressure lower than atmospheric pressure.
10. The double-shelled container includes a support mechanism fixed to the outer cylindrical body and supporting the inner cylindrical body, 10. The double-shelled container according to claim 1, wherein the support mechanism is configured by folding or winding a member that is longer than the linear distance between the inner cylindrical body and the outer cylindrical body into a coil shape.
11. At least three of the support mechanisms are provided on the bottom surface side of the outer cylinder body, 11. The double-shell container according to claim 10, wherein at least one of the nozzles is provided on a side surface of the outer cylinder.
12. 12. The double-shelled container according to claim 1, wherein at least one of the inner and outer cylindrical bodies is further covered with a material containing fibers.
13. 13. The double-shelled container according to claim 12, wherein the fiber-containing member contains at least one of glass fiber and carbon fiber.
14. 14. The double-shelled container according to claim 1, wherein the inner cylinder has an upper surface formed with a gently sloping surface having an apex approximately at the center.
15. 15. The double-shelled container according to claim 1, wherein the outer cylinder has a bottom surface formed with a gentle inclination with the bottom being located approximately at the center.
Citation Information
Patent Citations
Preparation method of cryogenic insulation container
CN110220107A
Low -temperature liquid storage tank with compound heat insulation layer
CN207112350U
Storage*delivery system for rocket thrust agent
JP1979147517A
Electrostriction effect element
JP1987088382A
JP1992078394U