Titanium alloy and its manufacturing method
A titanium alloy with a high-crystallinity TiO2 coating on a TiNbSn substrate, anodized and heat-treated, addresses biological activity and antibacterial properties, maintaining a Young's modulus suitable for artificial hip joints.
Patent Information
- Application Number
- JP2021074013
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-22
- Filing Date
- 2021-04-26
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2041-04-26
AI Technical Summary
Existing titanium alloys used in artificial hip joints do not adequately address biological activity and antibacterial properties while maintaining a Young's modulus close to that of bone, and the anodizing method for TiO2 formation is not applicable to biomaterials.
A titanium alloy with a TiO2 coating formed on a TiNbSn alloy substrate, which is anodized in an electrolytic solution containing sodium tartrate and hydrogen peroxide, followed by heat treatment, to achieve a rutile-type TiO2 coating with high crystallinity and antibacterial properties, maintaining a Young's modulus of 30 to 80 GPa.
The titanium alloy exhibits high antibacterial properties, bioactivity, and a Young's modulus close to that of bone, preventing fractures and loosening around the implant due to stress shielding, and is suitable for artificial hip joints.
Smart Images

Figure 0007587832000004 
Figure 0007587832000005 
Figure 0007587832000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a titanium alloy and a method for producing the same. [Background technology]
[0002] In order to prevent fractures and loosening around the implant due to bone atrophy in the proximal femur caused by stress shielding, artificial hip joints are required to have a Young's modulus close to that of bone, to have high adhesion to bone, and to have bioactivity. Titanium alloys are widely used as biomaterials because of their excellent corrosion resistance, biosafety, and strength. The inventors have developed a TiNbSn alloy consisting of a near-β phase with a low Young's modulus of about 40 GPa by controlling the structure and phase through thermomechanical treatment and the crystal orientation, making it possible to suppress stress shielding. When a biomaterial is to be implanted in the body, the biomaterial is first sterilized at a low temperature using an autoclave or the like. However, when TiNbSn alloys are sterilized in an autoclave, the near-β phase transforms into the α phase, which increases the Young's modulus and causes embrittlement due to low-temperature oxidation.
[0003] By the way, TiO, which is in thermal equilibrium with titanium, 2 It is known that when irradiated with light of a wavelength equivalent to the band gap energy, oxygen radicals are generated, resulting in a photocatalytic effect and providing functions such as antibacterial properties and the oxidative decomposition of harmful substances. Conventionally, photocatalytically active TiO 2 Methods for depositing coatings have been proposed. For example, in Patent Document 1, a substrate made of titanium or a titanium alloy is immersed in an electrolyte containing sodium tartrate and hydrogen peroxide, and a voltage of 70 to 140 V is applied to perform anodizing treatment, followed by heat treatment at 400 to 750°C for 1 to 30 minutes, to produce TiO2 that exhibits an anatase-type crystal structure on the surface of the substrate. 2 A method for producing a coated photocatalyst is disclosed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5789058 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the invention described in Patent Document 1 does not take bioactivity into consideration at all. So far, antibacterial TiO 2 The application of coating techniques to biomaterials is not known. An object of the present invention is to provide a titanium alloy having high antibacterial properties and bioactivity while maintaining a Young's modulus close to that of bone, and a method for producing the same. [Means for solving the problem]
[0006] The present invention has the following aspects. [1] The surface of a TiNbSn alloy substrate is coated with TiO 2 A titanium alloy having a coating formed thereon, the titanium alloy having an antibacterial activity value of 2.0 or more as determined by an antibacterial test in accordance with JIS R 1702. [2] The titanium alloy according to [1] above, having a Young's modulus of 30 to 80 GPa. [3] The titanium alloy according to [1] or [2] above, in which hydroxyapatite is produced after immersion in a simulated body fluid at 36.5°C for two weeks. [4] The TiO 2 The coating is a rutile-type TiO with a half-width of the rutile 110 diffraction line of less than 0.4 in X-ray diffraction. 2 The titanium alloy according to any one of [1] to [3] above, containing 60% or more. [5] 400±10nm, 1250mW / cm 2 The titanium alloy according to any one of [1] to [4], wherein the amount of hydroxyl radicals generated when the alloy is irradiated with light for 5 minutes is 1.30 μmol or more. [6] The method for producing a titanium alloy according to any one of [1] to [5] above, comprising immersing the base material in an electrolyte containing sodium tartrate and applying a voltage of 200 V or more to the base material to perform anodizing treatment. [7] The method for producing a titanium alloy according to [6], wherein the electrolyte further contains hydrogen peroxide. [8] The method for producing a titanium alloy according to [6] or [7], further comprising the step of: subjecting the anodizing treatment to a heat treatment at 300 to 450°C for 1 to 5 hours. Effect of the Invention
[0007] According to the present invention, it is possible to provide a titanium alloy having high antibacterial properties and bioactivity while maintaining a Young's modulus close to that of bone, and a method for producing the same. [Brief description of the drawings]
[0008] [Figure 1] 1 shows thin film X-ray diffraction profiles of the titanium alloys obtained in Example 1 and Comparative Examples 1 to 3. [Diagram 2] Photographs of the structure of the titanium alloy obtained in Example 1 (a) and (b) after immersion in simulated body fluid. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The titanium alloy and the manufacturing method thereof according to the present invention will be described below. However, the present invention is not limited to the configuration disclosed in the present embodiment, and various modifications are possible without departing from the spirit of the present invention. In this specification, "Young's modulus close to that of bone" means that the difference from the Young's modulus of bone (Young's modulus of titanium alloy - Young's modulus of bone) is within 50 GPa. The difference from the Young's modulus of bone is preferably within 40 GPa, more preferably within 30 GPa.
[0010] [Titanium alloy] The titanium alloy of this embodiment (hereinafter also referred to as the "present titanium alloy") is a TiNbSn alloy substrate having a TiO 2 A coating is formed.
[0011] <Base material> The substrate is made of a TiNbSn alloy. When titanium or titanium alloys are anodized, TiO 2 In particular, when a substrate made of a TiNbSn alloy is anodized by applying high voltage under a constant current, the rutile-type TiO 2 High proportion of TiO 2 The reason for this is believed to be as follows. The TiNbSn alloy has a higher electrical resistance than titanium, and has a higher potential than titanium during anodizing at a constant current. As a result, the TiNbSn alloy surface becomes insulated with TiO 2 As the film is formed, self-heating occurs, causing discharge, and the temperature of the substrate surface rises, forming rutile-type TiO, which is stable at high temperatures. 2 In addition, the diffusion is promoted, so the rutile type TiO 2 The crystallization of the compound proceeds.
[0012] The substrate is substantially free of components other than the TiNbSn alloy. Here, "substantially free" means that it includes the presence of impurities to an extent that does not impair the effects of the present invention. The content of impurities is preferably less than 0.04 mass% based on the total mass of the substrate. The shape of the substrate is not particularly limited, and the TiNbSn alloy may be processed into a desired shape suited to the use of the titanium alloy of this embodiment.
[0013] The TiNbSn alloy is a titanium alloy containing titanium, niobium, and tin. The TiNbSn alloy has a composition in which the proportion of niobium is 16 to 35 mass%, the proportion of tin is 3 to 13 mass%, and the remainder is titanium and impurities (however, the proportion of impurities is less than 0.04 mass%).
[0014] <TiO 2 Coating> TiO 2 The coating is a TiO film formed on the surface of the substrate. 2 It is. TiO 2 When the coating is irradiated with light of a wavelength equivalent to the band gap energy, it generates excited species, which react with oxygen and moisture in the air to generate highly oxidizing hydroxyl radicals (OH radicals). OH radicals can oxidize and decompose substrates such as bacteria, rendering them harmless, and therefore can exhibit antibacterial properties equivalent to those achieved through sterilization.
[0015] The more OH radicals are generated when irradiated with light of a wavelength equivalent to the band gap energy (OH radical amount), the higher the antibacterial properties tend to be. The amount of OH radicals is calculated by the formula: TiO 2 The crystallinity of TiO due to the electrolyte used in anodizing the substrate will be described in detail later. 2 It depends on the band structure modification brought about by doping into TiO. 2 The higher the crystallinity, the greater the amount of OH radicals due to the reduction in lattice defects that serve as recombination sites for excited species. TiO 2 The crystallinity of TiO 2 The diffusion of titanium and oxygen, which are the constituent elements of TiO, is promoted. 2 When heat-treated, it turns into rutile-type TiO, which is highly crystalline and thermodynamically stable. 2 The proportion of increases. From this perspective, TiO 2 The coating is a highly crystalline rutile-type TiO 2 It is preferable that the material contains TiO 2 The coating is a rutile-type TiO with a half-width of the rutile 110 diffraction line of less than 0.4 in X-ray diffraction. 2 It is preferable that the TiO 2 content is 60% or more, more preferably 70% or more, even more preferably 80% or more, particularly preferably 85% or more, even more preferably 90% or more, and most preferably 95% or more. In addition, the rutile-type TiO 2 content is less than 0.4 in the half-width of the rutile 110 diffraction line in X-ray diffraction. 2 Contains 60% or more of TiO 2 The coating is particularly "rutile type TiO 2 Also called "coating." TiO 2The coating is rutile type TiO 2 The content of 60% or more of TiO 2 This means that the diffusion of the constituent elements of TiO is promoted and the crystallinity is high. 2 When the coating is irradiated, the amount of OH radicals generated increases, which tends to enhance the antibacterial properties. 2 is anatase type TiO 2 Compared to , the band gap energy is lower by about 0.2 V, so light closer to the visible light region than the ultraviolet region can be used, and visible light activity is also increased.
[0016] <Antibacterial> The titanium alloy of this embodiment has high antibacterial properties, specifically, an antibacterial activity value of 2.0 or more, and preferably an antibacterial activity value of 2.5 or more. The antibacterial activity value of this titanium alloy was determined by antibacterial testing in accordance with JIS R 1702.
[0017] <Young's modulus> The Young's modulus of the titanium alloy of this embodiment is preferably 30 to 80 GPa, more preferably 30 to 60 GPa, further preferably 30 to 50 GPa, and particularly preferably 30 to 40 GPa. Generally, the Young's modulus of bone is about 10 to 30 GPa, so if the Young's modulus of the titanium alloy is within the above range, it will be close to the Young's modulus of bone, and when used as an artificial hip joint implant material, it can prevent fracture or loosening around the implant due to bone atrophy in the proximal femur caused by stress shielding. The Young's modulus of this titanium alloy is a value determined by a resonance method in accordance with JIS Z 2280 at room temperature (for example, 20° C.).
[0018] <Bioactivity> The TiNbSn alloy that constitutes the base material is a material for artificial hip joint implants. The bioactivity evaluation, which is a requirement for implant materials, is determined by whether hydroxyapatite, which is the main component of bone, precipitates on the alloy surface after immersing the titanium alloy in simulated body fluid (SBF) at 36.5 °C for 2 weeks. If precipitation occurs, it indicates bioactivity. As the simulated body fluid, for example, Hanks’ Balanced Salt Solution (HBSS) is used. The hydroxyapatite formed on the surface of this titanium alloy can be confirmed by phase analysis using thin film X-ray diffraction, tissue observation using SEM (scanning electron microscope) and EPMA (field emission type electron beam microanalyzer), composition analysis using EDX (energy dispersive X-ray analyzer) and WDX (wavelength dispersive X-ray analyzer), and surface analysis using XPS (X-ray photoelectron spectrometer), etc. For example, when hydroxyapatite is confirmed from the tissue observation and composition analysis of the surface of the titanium alloy after immersion in simulated body fluid, it can be judged to have bioactivity.
[0019] <Amount of OH radicals> The titanium alloy of this embodiment has a TiO 2 coating formed on the surface of the base material, and generates oxygen radicals by irradiating the TiO 2 coating with light having a wavelength corresponding to the band gap energy, and the main radical among them is the OH radical. Specifically, when irradiating the TiO 2 coating with light of 400 ± 10 nm and 1250 mW / cm 2 for 5 minutes, the amount of OH radicals generated is preferably 1.30 μmol or more, more preferably 1.50 μmol or more, and still more preferably 1.60 μmol or more. The amount of OH radicals is measured by the spin trapping method using electron spin resonance (ESR). For the measurement, a disk-shaped titanium alloy with a diameter of 10 mm is used.
[0020] <Manufacturing method> The TiO 2The titanium alloy coating formed on the surface of the substrate made of TiNbSn alloy can be obtained by anodizing the substrate made of TiNbSn alloy using an electrolyte containing sodium tartrate, using the substrate made of TiNbSn alloy as an anode electrode, and applying a voltage of 200 V or more between the anode and the counter electrode. If necessary, a heat treatment may be performed after the anodizing treatment.
[0021] (anodizing) The TiNbSn alloy substrate is anodized to form a TiO 2 As mentioned above, the substrate is a TiNbSn alloy, but the electrical conductivity of this alloy is 1 / 3 to 1 / 2 that of pure titanium, so by performing anodizing treatment at a constant current, the insulating TiO 2 As the film is formed, the temperature of the substrate surface increases due to self-heating, and TiO 2 As a result, the crystallization of rutile TiO, which is in thermodynamic equilibrium, is promoted. 2 is more likely to be generated.
[0022] The electrolyte used in the anodizing treatment is an aqueous solution containing sodium tartrate. By anodizing the substrate using such an electrolyte, a TiO film is obtained that generates oxygen radicals such as OH radicals when irradiated with light of a wavelength corresponding to the band gap energy. 2 A coating (anodic oxide film) can be formed on the surface of the substrate. The electrolyte preferably further contains hydrogen peroxide. When the electrolyte further contains hydrogen peroxide, the antibacterial activity value is further increased. In particular, when the voltage between the electrodes during anodization is 200V or more and less than 350V, it is preferable to use sodium tartrate and hydrogen peroxide in combination.
[0023] The molar concentration of sodium tartrate in the electrolyte is preferably 0.01 to 0.5 mol / L, more preferably 0.02 to 0.1 mol / L, and even more preferably 0.03 to 0.07 mol / L. When the molar concentration of sodium tartrate is equal to or higher than the lower limit, TiO 2When the molar concentration of sodium tartrate is equal to or less than the upper limit, an increase in solution resistance can be suppressed. The molar concentration of hydrogen peroxide in the electrolyte is preferably 0.1 to 2 mol / L, more preferably 0.2 to 1 mol / L, and even more preferably 0.3 to 0.7 mol / L. When the molar concentration of hydrogen peroxide is equal to or higher than the lower limit, TiO 2 When the molar concentration of hydrogen peroxide is equal to or less than the upper limit, the promotion of oxygen generation can be suppressed.
[0024] The voltage between the electrodes during anodizing is 200 V or more. If the voltage is 200 V or more, the TiNbSn alloy will turn into an insulating TiO 2 As the film is formed, self-heating occurs, causing the temperature of the substrate surface to rise, resulting in TiO 2 The crystallization of rutile TiO is promoted. 2 As a result, TiO 2 When the coating is irradiated with light of a specific wavelength, the amount of OH radicals generated increases. With constant current control, the higher the voltage, the higher the self-heating temperature becomes, and the TiO 2 The crystallization of rutile TiO is promoted. 2 The proportion of tends to increase. In a constant current controlled anodization reaction, the voltage increases over time, and when it reaches the set voltage, it switches to constant voltage control, the current decreases, and the oxidation reaction does not proceed. In other words, the higher the set voltage, the better, specifically 300V or more is preferable, and 400V or more is more preferable. There is no particular limit on the upper voltage value, but it is about 500V in consideration of the safety of the experiment.
[0025] The anodizing time depends on the set potential under constant current control. For example, under conditions where the set potential is sufficiently high so that a current drop does not occur within the anodizing time, the anodizing time is preferably 0.016 to 2 hours, more preferably 0.016 to 1 hour, even more preferably 0.05 to 1 hour, particularly preferably 0.08 to 1 hour, and most preferably 0.08 to 0.5 hours.
[0026] The current density during the anodization treatment is not particularly limited, but may be, for example, 10 mA / cm 2 More than 20mA / cm is preferable. 2 More preferably, 30 mA / cm or more. 2 More preferably, 50 mA / cm 2 The above is particularly preferred.
[0027] Anodizing is usually carried out at room temperature (e.g., 20°C). However, in order to prevent an increase in the temperature of the electrolytic bath due to self-heating of the electrodes, the electrolytic solution is generally cooled during the anodizing process. For example, it is preferable to carry out the process while maintaining the temperature of the electrolytic solution at 5 to 15°C. The anodizing treatment may be performed by applying a direct current, an AC / DC superimposed current, or a pulse wave. It is also possible to perform the treatment by applying a single-phase half wave, a three-phase half wave, or a six-phase half wave using a thyristor-type DC power supply. This anodization process produces highly crystalline TiO 2 Even if the substrate has a complex shape, the antibacterial TiO 2 A coating can be formed on the surface of the substrate. In particular, by controlling the voltage and current density, the TiO 2 The thickness of the coating can be controlled.
[0028] A typical embodiment of the anodizing process is as follows. First, a substrate made of a TiNbSn alloy that has been formed into a desired shape and, if necessary, subjected to pretreatment such as polishing and cleaning is connected to the anode, and a pure titanium plate is connected to the cathode. A set current density (e.g., 50 mA / cm) is applied to each electrode in a cell filled with an electrolyte containing sodium tartrate and hydrogen peroxide. 2 ) and a potential (e.g. 300 V) to perform anodizing. As a result, TiO 2 At this time, the set voltage, current density, and anodization time are increased to form a rutile-type TiO 2 It is preferable to increase the crystallinity and the ratio of
[0029] The anodized substrate is washed with a washing liquid. Alcohol is used as the cleaning liquid.
[0030] (Heat treatment) The heat treatment is a process carried out after the anodizing treatment. If heat treatment is performed after anodization, TiO 2 The crystallization of the above is further promoted. The lower the set voltage during constant current controlled anodizing, the shorter the time it takes to reach the set potential and switch to constant voltage control, resulting in a shorter time for self-heating to occur. Therefore, it is preferable to perform a heat treatment after anodizing. As mentioned above, TiO 2 The crystallinity of TiO 2 The TiO 2 When this is heat-treated at high temperatures, it turns out to be rutile-type TiO, which is highly crystalline and stable at high temperatures. 2 However, the higher the set voltage during anodizing and the lower the electrical conductivity of the substrate, the more effective it becomes to obtain rutile-type TiO without heat treatment. 2 In the manufacturing method of this embodiment, the set voltage during the anodizing treatment is 200 V or more, so that TiO 2 The crystallization of rutile TiO is promoted. 2 Therefore, depending on the electrical conductivity of the base material, it is not always necessary to carry out a heat treatment.
[0031] The temperature of the heat treatment is preferably 300 to 450° C., more preferably 350 to 400° C. When the temperature of the heat treatment is equal to or higher than the lower limit, TiO 2 When the temperature of the heat treatment is equal to or lower than the upper limit, an increase in Young's modulus can be suppressed. The heat treatment time is preferably 1 to 5 hours, more preferably 2 to 5 hours. The heat treatment may be carried out in air.
[0032] <Action and effect> The titanium alloy of the present embodiment described above has TiO 2Since a coating is formed, OH radicals are generated by irradiating the material with light of a wavelength equivalent to the band gap energy, and antibacterial activity of 2.0 or more is achieved. This has the same effect as sterilization, and can prevent an increase in the Young's modulus of TiNbSn alloy caused by autoclave sterilization. Moreover, the coating formed on the substrate surface is made of TiO, which has excellent biocompatibility. 2 Therefore, it has bioactivity.
[0033] <Application> The titanium alloy of this embodiment is suitable for use in the body, and since it can maintain a Young's modulus close to that of bone, it is particularly suitable as a biomaterial for artificial hip joints and the like. EXAMPLES
[0034] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following description. The raw materials used in this example are as follows:
[0035] [Example 1] <Production of titanium alloys> A disk-shaped substrate made of a TiNbSn alloy (33% by mass of niobium, 4% by mass of tin, and the remainder being titanium and impurities (however, the impurities were less than 0.04% by mass)) with a diameter of 10 mm and a thickness of 1 mm was immersed in an electrolyte containing sodium tartrate and hydrogen peroxide. The molar concentration of sodium tartrate in the electrolyte was 0.05 mol / L, and the molar concentration of hydrogen peroxide was 0.7 mol / L. Voltage 220V, current density 50mA / cm 2 The anodization treatment was carried out for 0.5 hours under the condition of an electrolyte temperature of 10°C, and TiO was formed on the surface of the substrate. 2 A coating was formed. After the anodizing treatment, the plate was washed with ethanol and dried at room temperature to obtain a titanium alloy. The dried titanium alloy was heat treated in air at 450°C for 5 hours. The titanium alloy after heat treatment was treated as follows: TiO 2The crystal structure of the coating was analyzed by thin film X-ray diffraction. In addition, the antibacterial activity value, Young's modulus, methylene blue decomposition rate (MB decomposition rate), amount of OH radicals, and amount of hydrogen peroxide were measured for the titanium alloy after the heat treatment as follows. Furthermore, the bioactivity of the titanium alloy before heat treatment was evaluated as follows.
[0036] <Measurement and Evaluation> (Thin film X-ray diffraction) TiO formed on the surface of the substrate 2 The crystal structure of the coating was analyzed using a thin-film X-ray diffractometer (Panalytical Corp., Cu target) in the range of 2θ = 24 to 28.5°. The thin-film X-ray diffraction profile is shown in Figure 1. The half-widths of the diffraction lines (anatase 101) near 2θ = 25° and the diffraction lines (rutile 110) near 2θ = 27° were calculated from the profiles. 2 The ratio (fraction) of was calculated from the following formula (1). The results are shown in Table 1. f rutile = {0.679×I rutile / (I rutile +I anatase )}+0.312×{I rutile / (I rutile +I anatase )} 2 (1) In formula (1), “I rutile " is the integrated intensity of the rutile 110 diffraction line, "I anatase " is the integrated intensity of the anatase 101 diffraction line, and "f rutile " is rutile type TiO 2 is a fraction of.
[0037] (Measurement of antibacterial activity value) The antibacterial activity value was measured by an antibacterial test in accordance with JIS R 1702. Specifically, the test was performed as follows. In Example 1, the antibacterial test was performed on three different titanium alloys produced under the same conditions. Escherichia coli (NBRC3972) purchased from the National Institute of Technology and Evaluation was cultured on nutrient agar medium at 37°C for 24 hours and then frozen and stored. For the experiment, a new nutrient agar medium was used to culture the frozen Escherichia coli at 37°C for 20 hours and used. The cultured E. coli was placed in a 1 / 500 concentration normal bouillon medium, with the number of bacteria at 1 x 10 7 The concentration was adjusted to 1 / mL, and this was used as the test bacteria solution. The titanium alloy was placed in a petri dish, and the TiO 2 Apply 20 μL (2 × 10 5 The bacteria solution was then inoculated with sterilized OHP film and the bacterial solution was then attached to the petri dish. To prevent drying, a 1.1 mm thick glass plate was placed on top of the dish. The amount of ultraviolet light at 365 ± 25 nm transmitted through the OHP film and the glass plate was 0.25 mW / cm. 2 The mixture was then irradiated with ultraviolet light at 25°C for 21 hours. After UV irradiation, the titanium alloy and OHP film were placed in a tube containing 10 mL of SCDLP medium, and the test bacteria liquid was washed away. The collected SCDLP medium (10 mL) was diluted with physiological saline. The SCDLP medium and 50 μL of the resulting dilution were spread onto nutrient agar medium and cultured at 37°C for 16 hours, after which the number of colonies formed was counted to calculate the viable cell count (A). Separately, an antibacterial test was conducted in the same manner except that soda glass was used instead of the titanium alloy, and the viable cell count (B) was calculated. The antibacterial activity value of the titanium alloy was calculated using the following formula (2). The results are shown in Table 2. Antibacterial activity value = log10 (number of viable bacteria (B) / number of viable bacteria (A)) (2) In addition, when no viable bacteria were found in the titanium alloy, the calculation was performed by substituting "10" for the number of viable bacteria (A) in formula (2).
[0038] (Young's modulus measurement) The Young's modulus of the titanium alloy was measured at room temperature (20°C) by the resonance method in accordance with JIS Z 2280. The Young's modulus was measured for five different titanium alloys produced under the same conditions, and the average value was calculated. The results are shown in Table 2.
[0039] (Measurement of MB decomposition rate) The MB decomposition rate was measured in accordance with JIS R 1703-2. Specifically, the measurement was performed as follows. The titanium alloy was immersed in a quartz cell filled with a 25 mg / L methylene blue solution and exposed to light at 365 ± 25 nm and 1500 mW / cm for 3 hours. 2 The solution was periodically sampled from the quartz glass and its absorbance at 664 nm was measured using a spectrophotometer. The MB decomposition rate was calculated from the change in absorbance. The MB decomposition rates were measured for three different titanium alloys produced under the same conditions, and the average values were calculated. The results are shown in Table 2.
[0040] (OH radical amount measurement) 5,5-Dimethyl-1-pyrroline N-oxide (DMPO) was used as an OH scavenger. DMPO was dissolved in pure water to a concentration of 0.3 mol / L to prepare an aqueous DMPO solution. A titanium alloy was placed in a 24-well plate, 500 μL of DMPO aqueous solution was dropped, and the intensity was measured at 400 ± 10 nm and 1250 mW / cm 2 The wells were irradiated with ultraviolet light at room temperature (20°C) for 5 minutes. Then, 200 μL of the test solution was taken from the wells into a flat aqueous solution cell, and the amount of OH radicals was measured based on the ESR spin trapping method. The ESR measurement was performed using an electron spin resonance device (manufactured by JEOL Ltd., "JES-FA-100") and X-band (9.4 GHz) microwaves. The amount of OH radicals was measured for three different titanium alloys produced under the same conditions, and the average value was calculated. The results are shown in Table 2.
[0041] (Measurement of hydrogen peroxide amount) Mixture A was prepared by mixing 24 mL of pure water, 6 mL of 0.1 mol / L sulfuric acid, and 11.8 mg of ammonium iron (II) sulfate hexahydrate. Separately, mixed solution B was prepared by mixing 30 mL of pure water, 9.1 mg of xylenol orange tetrasodium, and 2186.0 mg of D-sorbitol. The titanium alloy was placed in a 24-well plate, 500 μL of pure water was dropped, and the 400 ± 10 nm, 1250 mW / cm 2 The film was exposed to ultraviolet light at room temperature (20° C.) for 5 minutes. 200 μL of mixed solution A and 200 μL of mixed solution B were mixed to prepare a xylenol orange mixed solution. Next, 400 μL of the test solution was collected from the well into a test tube, and the amount of hydrogen peroxide was measured by colorimetry. Specifically, 400 μL of the xylenol orange mixture was added to the test tube containing the test solution, and the mixture was stirred. After that, the mixture was left to stand at room temperature (20° C.) for 45 minutes to complete the reaction, and the absorbance at a wavelength of 560 nm was measured using a spectrophotometer (manufactured by Biochrom, "GeneQuant1300"). Furthermore, the amount of hydrogen peroxide was measured by colorimetry using a commercially available hydrogen peroxide reagent (special grade), and a calibration curve was created. Through the above experiments, the amount of hydrogen peroxide was calculated from the absorbance using a hydrogen peroxide calibration curve. The amount of hydrogen peroxide was measured for three different titanium alloys produced under the same conditions, and the average value was calculated. The results are shown in Table 2.
[0042] (Evaluation of bioactivity) The titanium alloy was subjected to hot water treatment by immersing it in hot water at 80°C for 12 hours. The titanium alloy after the hot water treatment was immersed in 25 mL of Gibco Hanks' balanced salt solution as a simulated body fluid at 36.5°C for one week. Thereafter, the titanium alloy was removed from the Hanks' balanced salt solution, washed with distilled water, and dried in a dry incubator for 24 hours. The dried titanium alloy was immersed in 25 mL of Hanks' balanced salt solution at 36.5°C for one week. During this time, the Hanks' balanced salt solution was replaced with fresh one at intermediate intervals. Thereafter, the titanium alloy was removed from the Hanks' balanced salt solution, washed with distilled water, and dried in a dry incubator for 24 hours. The titanium alloy after drying was examined for the presence or absence of hydroxyapatite formation by structural observation using FE-EPMA (manufactured by JEOL Ltd.) and WDX analysis, and was evaluated according to the following evaluation criteria. The results are shown in Table 2. Photographs of the structure are shown in Figures 2(a) and (b). ○: Hydroxyapatite was confirmed. ×: Hydroxyapatite not observed.
[0043] [Example 2] A titanium alloy was produced in the same manner as in Example 1, except that the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1. The results are shown in Table 2.
[0044] [Example 3] A titanium alloy was produced in the same manner as in Example 1, except that an electrolyte having a molar concentration of sodium tartrate of 0.05 mol / L and a molar concentration of hydrogen peroxide of 0 mol / L was used, and the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1. The results are shown in Table 2.
[0045] [Comparative Example 1] A titanium alloy was produced in the same manner as in Example 1, except that the heat treatment was not carried out after the anodizing treatment. The obtained titanium alloy was subjected to the same procedure as in Example 1 to obtain TiO 2 The crystal structure of the coating was analyzed by thin-film X-ray diffraction, and the results are shown in Figure 1 and Table 1. The obtained titanium alloy was evaluated for its bioactivity by measuring its antibacterial activity value, Young's modulus, MB decomposition rate, amount of OH radicals, and amount of hydrogen peroxide in the same manner as in Example 1. The results are shown in Table 2. In Comparative Example 1, antibacterial tests were performed on two different titanium alloys prepared under the same conditions.
[0046] [Comparative Example 2] A titanium alloy was produced in the same manner as in Example 1, except that an electrolyte solution having a molar concentration of sodium tartrate of 0.05 mol / L and a molar concentration of hydrogen peroxide of 0 mol / L was used. The obtained titanium alloy was subjected to the same procedure as in Example 1 to obtain TiO 2 The crystal structure of the coating was analyzed by thin-film X-ray diffraction, and the results are shown in Figure 1 and Table 1. The obtained titanium alloy was also evaluated for its bioactivity by measuring the antibacterial activity value, Young's modulus, MB decomposition rate, OH radical amount, and hydrogen peroxide amount in the same manner as in Example 1. These results are shown in Table 2.
[0047] [Comparative Example 3] A titanium alloy was produced in the same manner as in Example 1, except that an electrolyte having a molar concentration of sodium tartrate of 0.05 mol / L and a molar concentration of hydrogen peroxide of 0 mol / L was used and no heat treatment was performed after the anodization treatment. The obtained titanium alloy was subjected to the same procedure as in Example 1 to obtain TiO 2 The crystal structure of the coating was analyzed by thin-film X-ray diffraction, and the results are shown in Figure 1 and Table 1. Furthermore, the Young's modulus, MB decomposition rate, amount of OH radicals, and amount of hydrogen peroxide of the obtained titanium alloy were measured to evaluate the bioactivity in the same manner as in Example 1. These results are shown in Table 2.
[0048] [Comparative Example 4] For a substrate made of a disk-shaped TiNbSn alloy (33% by mass of niobium, 4% by mass of tin, and the remainder being titanium and impurities (with the impurities being less than 0.04% by mass)) with a diameter of 10 mm and a thickness of 1 mm, the Young's modulus and MB decomposition rate were measured and the bioactivity was evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0049] [Table 1]
[0050] [Table 2]
[0051] As is clear from Figure 1 and Table 1, when the TiNbSn alloy is anodized, rutile-type TiO 2 High proportion of TiO 2 A coating was formed on the surface of the substrate. Rutile TiO 2 The proportion of increased by heat treatment after anodizing. Furthermore, as is clear from FIG. 2 and Table 2, hydroxyapatite was formed when the titanium alloy manufactured using the substrate made of TiNbSn alloy was immersed in the simulated body fluid for two weeks, but no hydroxyapatite was formed when the titanium alloy was not anodized. As is clear from Table 2, the titanium alloy obtained in Example 1 had a Young's modulus close to that of bone. In addition, the antibacterial activity value, MB decomposition rate, OH radical amount, and hydrogen peroxide amount were higher than those of the titanium alloys obtained in Comparative Examples 1 to 3, and the antibacterial properties were also excellent. The titanium alloys obtained in Examples 2 and 3 also had high antibacterial activity values and excellent antibacterial properties.
[0052] [Example 4] A titanium alloy was produced in the same manner as in Example 1, except that the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1. The results are shown in Table 3. In Example 4, the antibacterial test was carried out on two different titanium alloys produced under the same conditions.
[0053] [Example 5] A titanium alloy was produced in the same manner as in Example 1, except that the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1, except that methicillin-resistant Staphylococcus aureus (MRSA) was cultured instead of Escherichia coli (E. coli). The results are shown in Table 3. In Example 5, antibacterial tests were performed on two different titanium alloys produced under the same conditions.
[0054] [Example 6] A titanium alloy was produced in the same manner as in Example 1, except that the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1, except that Staphylococcus aureus (S. aureus) was cultured instead of Escherichia coli. The results are shown in Table 3. In Example 6, the antibacterial activity test was performed on two different titanium alloys produced under the same conditions.
[0055] [Example 7] A titanium alloy was produced in the same manner as in Example 1, except that an electrolyte having a molar concentration of sodium tartrate of 0.05 mol / L and a molar concentration of hydrogen peroxide of 0 mol / L was used, and the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1. The results are shown in Table 3. In Example 7, the antibacterial test was carried out on two different titanium alloys produced under the same conditions.
[0056] [Example 8] A titanium alloy was produced in the same manner as in Example 1, except that an electrolyte having a molar concentration of sodium tartrate of 0.05 mol / L and a molar concentration of hydrogen peroxide of 0 mol / L was used, and the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1, except that methicillin-resistant Staphylococcus aureus was cultured instead of Escherichia coli. The results are shown in Table 3. In Example 8, the antibacterial activity test was performed on two different titanium alloys produced under the same conditions.
[0057] [Example 9] A titanium alloy was produced in the same manner as in Example 1, except that an electrolyte having a molar concentration of sodium tartrate of 0.05 mol / L and a molar concentration of hydrogen peroxide of 0 mol / L was used, and the voltage during anodizing treatment was changed to 380 V. The antibacterial activity value of the obtained titanium alloy was measured in the same manner as in Example 1, except that Staphylococcus aureus was cultured instead of Escherichia coli. The results are shown in Table 3. In Example 9, the antibacterial activity test was performed on two different titanium alloys produced under the same conditions.
[0058] [Table 3]
[0059] As is clear from Table 3, the titanium alloys obtained in Examples 4 to 9 had high antibacterial activity values and excellent antibacterial properties even when different types of bacteria were used. In particular, it was shown that the titanium alloys of the present invention have high antibacterial properties even against methicillin-resistant Staphylococcus aureus, which is a resistant bacterium. [Industrial Applicability]
[0060] The titanium alloy of the present invention maintains a Young's modulus close to that of bone, while having high antibacterial properties and bioactivity, making it suitable as a biomaterial.
Claims
1. The surface of the substrate made of TiNbSn alloy is coated with TiO 2 A titanium alloy having a coating formed thereon, The antibacterial activity value determined by the antibacterial test in accordance with JIS R 1702 is 2.0 or more, A titanium alloy, wherein the TiO 2 coating contains 60% or more of rutile-type TiO 2 having a half-width of less than 0.4 in rutile 110 diffraction line in X-ray diffraction.
2. 2. The titanium alloy of claim 1, having a Young's modulus of 30 to 80 GPa.
3. The titanium alloy according to claim 1 or 2, which generates hydroxyapatite after immersion in a simulated body fluid at 36.5°C for two weeks.
4. 400±10nm, 1250mW / cm 2 The titanium alloy according to any one of claims 1 to 3, wherein the amount of hydroxyl radicals generated when irradiated with light for 5 minutes is 1.30 μmol or more.
5. A method for producing a titanium alloy according to any one of claims 1 to 4, A method for producing a titanium alloy, comprising immersing the substrate in an electrolyte containing sodium tartrate and applying a voltage of 200 V or more to the substrate to perform anodizing treatment.
6. The method for producing a titanium alloy according to claim 5, wherein the electrolyte further comprises hydrogen peroxide.
7. The method for producing a titanium alloy according to claim 5 or 6, wherein the anodizing treatment is followed by a heat treatment at 300 to 450°C for 1 to 5 hours.
Citation Information
Patent Citations
Mounting of baseboard
JP1982089058A
Visible light-responsive photocatalyst body and method for producing same
WO2015022960A1