Titanium product surface temperature-sensitive response antibacterial coating and preparation method thereof
By preparing a temperature-sensitive and antibacterial coating on the surface of titanium products, using the piezoelectric effect of co-doped magnesium-zinc barium titanate nanotubes and expandable hydrogels, combined with magnesium and magnesium oxide spraying technology, the insufficient antibacterial ability of titanium products is solved. and the risks of heavy metal ions to human health have achieved efficient and safe antibacterial effects.
Patent Information
- Application Number
- CN202411064099.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
AI Technical Summary
Titanium products themselves lack antibacterial properties, and bacteria may develop resistance after long-term use, and commonly used metal ion antibacterial methods pose potential risks to human health.
Prepare a temperature-sensitive response antibacterial coating on the surface of titanium products, prepare titanium dioxide nanotubes through multiple anodization methods, and form magnesium-zinc co-doped barium titanate nanotubes, and fill it with expandable hydrogel, combined with plasma spraying technology Spray magnesium and magnesium oxide to achieve antibacterial effects using piezoelectric effects and alkaline microenvironment.
Effectively enhance the antibacterial ability of titanium products, avoid the uncontrollable release of heavy metal ions and human health hazards, and improve the service life and antibacterial effect of the coating.
Smart Images

Figure CN118996572A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium product surface coating preparation, and specifically relates to a method for preparing a temperature-sensitive responsive antibacterial coating on the surface of a titanium product, and also relates to the temperature-sensitive responsive antibacterial coating on the surface of the titanium product. Background Art
[0002] Titanium and titanium alloys are widely used in aviation, aerospace, ships, weapons, ocean, petrochemical, biomedicine and other fields due to their high specific strength, low density, non-magnetic, excellent corrosion resistance and biocompatibility. Although titanium and titanium alloys have many advantages, they do not have antibacterial properties themselves. When used as daily tableware or daily necessities, bacteria will accumulate due to lack of cleaning, which is harmful to human health. Therefore, the antibacterial ability of titanium and titanium alloys can be enhanced by surface modification, which is of great significance for expanding the application of titanium products in life. Common methods of providing antibacterial ability to titanium and titanium alloys through surface modification technology usually use surface doping with metal antibacterial ions, such as Ag. + , Cu 2+ Or antibiotics and antibacterial drugs are loaded on the metal surface. However, long-term use may cause bacteria to develop drug resistance. At the same time, the impact of metal ions exceeding a certain dose on the human body is uncontrollable, such as excessive Ag + It will have toxic side effects on the human body. Therefore, giving titanium products a green, non-toxic antibacterial ability through surface modification technology is of great significance to improving the use value of titanium products.
[0003] Chinese patent "A medical titanium material with a surface antibacterial coating, its preparation method and application" (application number: CN202310763810.1, publication number: CN116983474A, publication date: 2023-11-03) discloses a medical titanium material with a surface antibacterial coating, its preparation method and application. The method obtains antibacterial properties by loading titanium dioxide nanotubes, nano zinc and nano copper on the titanium surface, but the release of copper ions in the coating is uncontrollable and has certain risks. Chinese patent "A method for preparing an antibacterial coating on the surface of titanium-based medical devices" (application number: CN201910477669.2, publication number: CN110079849B, publication date: 2019-08-02) discloses a method for preparing an antibacterial coating on the surface of titanium-based medical devices, which obtains antibacterial properties by constructing a titanium dioxide-ruthenium dioxide coating on the surface of the titanium substrate, but ruthenium in this method is a rare earth element and is not suitable for promotion and use. Fang Siyi et al. published a paper titled "Nanosilver / Titanium Oxide Nanotube Composite Antibacterial Coating for Orthopedic Implants", which was selected from the Journal of Materials Science and Engineering, Vol. 38, No. 3, 2020, pp. 363-369. Titanium dioxide nanotubes were prepared on the titanium surface by anodization, followed by surface modification using polydopamine (PDA), and then a composite coating of TiO2 nanotubes loaded with silver nanoparticles was prepared by impregnation and ultraviolet light reduction. However, nanosilver has certain biological toxicity, which is not conducive to its use in daily life. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a temperature-sensitive responsive antibacterial coating on the surface of a titanium product, thereby solving the problem that the existing titanium products have poor antibacterial ability.
[0005] Another object of the present invention is to provide a temperature-sensitive responsive antibacterial coating on the surface of the above-mentioned titanium product.
[0006] The technical solution adopted by the present invention is a method for preparing a temperature-sensitive responsive antibacterial coating on the surface of a titanium product, which is specifically implemented according to the following steps:
[0007] Step 1, preparing a modified barium titanate piezoelectric nanotube coating on a titanium surface;
[0008] Step 2, preparing a temperature-responsive nanotube coating on a titanium surface;
[0009] In step 3, magnesium and magnesium oxide are sprayed on the surface of the titanium sheet in step 2 by plasma spraying technology, so that a temperature-sensitive responsive antibacterial coating can be prepared on the surface of the titanium product.
[0010] The present invention is also characterized in that:
[0011] In step 1, specifically:
[0012] Step 1.1, grinding and smoothing the surface of the titanium sheet and then polishing it by chemical polishing, then preparing titanium dioxide nanotubes on the surface of the titanium sheet by multiple anodizing, and then immersing the titanium sheet in a mixed solution to prepare a magnesium-zinc-coated TiO2 nanotube coating on the titanium surface;
[0013] Step 1.2, placing the titanium sheet prepared in step 1.1 in a reaction kettle, adding a barium hydroxide solution, performing a hydrothermal reaction, and drying, thereby preparing magnesium-zinc co-doped barium titanate nanotubes on the surface of the titanium sheet;
[0014] Step 1.3, placing the titanium sheet obtained in step 1.2 into a dopamine hydrochloride solution for stirring, washing, and nitrogen drying, thereby preparing a modified barium titanate piezoelectric nanotube coating on the titanium surface.
[0015] In step 1.1, during polishing, the polishing liquid is composed of nitric acid, hydrofluoric acid and deionized water in a volume ratio of 1:1 to 10:10 to 50; the multiple anodizing method includes primary anodizing and secondary anodizing, the electrolyte in the primary anodizing is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:1 to 10:100 to 500, the primary anodizing voltage is 50 to 80V, and the primary anodizing time is 0.5 to 3h; the electrolyte in the secondary anodizing is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:5 to 30:100 to 500; the secondary anodizing voltage is 30 to 80V, and the secondary anodizing time is 0.1 to 1h; the mixed solution is composed of magnesium acetate, zinc acetate and deionized water, the magnesium ion concentration is 0.01 to 0.1mol / L, the zinc ion concentration is 0.01 to 0.1mol / L, and the immersion time is 1 to 4h.
[0016] In step 1.2, the concentration of the barium hydroxide solution is 0.1-0.5 mol / L, the hydrothermal temperature is 150-250° C., the hydrothermal time is 1-5 h, the drying temperature is 50-80° C., and the drying time is 1-4 h.
[0017] In step 1.3, the concentration of the dopamine hydrochloride solution is 1 to 10 mg / mL, the stirring temperature is 20 to 80° C., and the stirring time is 10 to 24 h.
[0018] In step 2, specifically:
[0019] Step 2.1, dissolving the hydrogel monomer and the crosslinking agent in deionized water, stirring for 15-20 minutes under N2 flow, and then adding the metal nanomaterial and the initiator and stirring for 1-12 hours to obtain a hydrogel precursor;
[0020] Step 2.2, coating the hydrogel precursor on the surface of the titanium sheet prepared in step 1, and then standing and drying under a vacuum environment to prepare a temperature-responsive nanotube coating on the titanium surface.
[0021] In step 2.1, the hydrogel monomer is any one or more of acrylamide, methacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, ethylene oxide, vinyl methyl ether, hydroxypropyl cellulose, N-vinyl pyrrolidone, and vinyl alcohol; the metal nanomaterial is any one or more of silver nanoparticles, silver nanowires, gold nanoparticles, zinc oxide nanoparticles, and magnesium oxide nanoparticles; the crosslinking agent is any one or more of N-isopropylacrylamide, diethoxyethyl dimethacrylate, acrylamide, and methyl methacrylate; the initiator is any one or more of ammonium persulfate, azobisisobutyronitrile, benzoyl peroxide, diisopropyl peroxide, and diformyl peroxide; the mass ratio of the hydrogel monomer, the crosslinking agent, the initiator, and the metal nanomaterial is 1:0.01-0.1:0.01-0.1:0.1-0.5.
[0022] In step 2.2, the standing temperature is 35 to 50° C., the standing time is 1 to 12 hours, and the drying time is 1 to 10 hours.
[0023] In step 3, the parameters of plasma spraying are: spraying distance is 10-20 mm, powder feeding voltage is 10-20 V, powder feeding current is 500-1000 A, spray gun moving speed is 5-10 mm / s, hydrogen rate is 5-10 L / h, argon rate is 1500-2500 L / h, nitrogen rate is 2000-3000 L / h, nitrogen pressure is 10-15 MPa; the mass ratio of magnesium to magnesium oxide is 1:1-5.
[0024] Another technical solution adopted by the present invention is a temperature-sensitive responsive antibacterial coating on the surface of a titanium product prepared by the above method.
[0025] The beneficial effects of the present invention are: by forming a temperature-responsive piezoelectric nanotube coating on the titanium surface, the piezoelectric effect and the change of the surface microenvironment are used for antibacterial; under the stimulation of the external environment, the thermosensitive swellable hydrogel will expand, and then squeeze the inner wall of the nanotube, and the squeezed nanotube will generate current under the action of the piezoelectric effect, and the coating surface will be charged as the current reaches the coating surface, so that the coating has the ability to affect the adhesion of bacteria, and at the same time, the magnesium ions in the coating will form an alkaline microenvironment on the coating surface and form a synergistic antibacterial effect with the generated piezoelectric effect, and the magnesium oxide particles on the surface not only avoid the leakage of the hydrogel and improve the antibacterial ability, but also can enhance the service life of the coating. The thermosensitive responsive antibacterial coating on the surface of titanium products prepared by the present invention can solve the problems of poor antibacterial ability of titanium products and uncontrollable harm of antibacterial heavy metal ions to human health. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a photo of the colony distribution after pure titanium and Escherichia coli were co-cultured;
[0027] Figure 2 This is a photo of the colony distribution after co-culture with Escherichia coli in Example 1;
[0028] Figure 3 It is a schematic diagram of the cross-sectional structure of the thermosensitive responsive antibacterial coating on the surface of a titanium product prepared in the method of the present invention.
[0029] In the figure, 1. titanium matrix, 2. titanium dioxide nanotubes, 3. magnesium-zinc co-doped barium titanate nanotubes, 4. swellable hydrogel, 5. magnesium oxide nanoparticles, 6. magnesium nanoparticles. DETAILED DESCRIPTION
[0030] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] The method for preparing a temperature-sensitive responsive antibacterial coating on the surface of a titanium product of the present invention comprises the following steps: obtaining titanium dioxide nanotubes by multiple anodic oxidations on the surface of a titanium metal, converting the titanium dioxide nanotubes into magnesium-zinc-doped barium titanate nanotubes with piezoelectric properties by a hydrothermal method, and then modifying them with dopamine to obtain a modified barium titanate piezoelectric nanotube coating, and then filling the prepared temperature-sensitive swellable hydrogel precursor into the nanotubes after modification of the magnesium-zinc-doped barium titanate nanotubes in a vacuum environment to achieve an intelligent response of the piezoelectric effect, and finally spraying magnesium and magnesium oxide on the titanium surface by a plasma spraying method to provide a basis for the generation of an alkaline microenvironment, thereby finally obtaining a temperature-sensitive responsive antibacterial coating on the surface of a titanium product;
[0032] Follow the steps below to implement it:
[0033] Step 1, preparing a modified barium titanate piezoelectric nanotube coating on a titanium surface; specifically:
[0034] Step 1.1, grinding and smoothing the surface of the titanium sheet and then polishing it by chemical polishing, then preparing titanium dioxide nanotubes on the surface of the titanium sheet by multiple anodizing, and then immersing the titanium sheet in a mixed solution to prepare a magnesium-zinc-coated TiO2 nanotube coating on the titanium surface;
[0035] During polishing, the polishing liquid is a mixture of nitric acid, hydrofluoric acid and deionized water in a volume ratio of 1:1 to 10:10 to 50;
[0036] The multiple anodization method includes primary anodization and secondary anodization. In the primary anodization, the electrolyte is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:1 to 10:100 to 500. The primary anodization voltage is 50 to 80 V and the primary anodization time is 0.5 to 3 h.
[0037] The electrolyte in the secondary anodization is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:5-30:100-500; the secondary anodization voltage is 30-80V, and the secondary anodization time is 0.1-1h;
[0038] The mixed solution is composed of magnesium acetate, zinc acetate and deionized water, the magnesium ion concentration is 0.01-0.1 mol / L, the zinc ion concentration is 0.01-0.1 mol / L, and the immersion time is 1-4 hours;
[0039] Step 1.2, placing the titanium sheet prepared in step 1.1 in a reaction kettle, adding a barium hydroxide solution, performing a hydrothermal reaction, and drying, thereby preparing magnesium-zinc co-doped barium titanate nanotubes on the surface of the titanium sheet;
[0040] The concentration of the barium hydroxide solution is 0.1-0.5 mol / L, the hydrothermal temperature is 150-250° C., the hydrothermal time is 1-5 h, the drying temperature is 50-80° C., and the drying time is 1-4 h.
[0041] Step 1.3, placing the titanium sheet obtained in step 1.2 into a dopamine hydrochloride solution for stirring, washing, and nitrogen drying to prepare a modified barium titanate piezoelectric nanotube coating on the titanium surface;
[0042] The concentration of the dopamine hydrochloride solution is 1-10 mg / mL, the stirring temperature is 20-80° C., and the stirring time is 10-24 h.
[0043] Step 2, preparing a temperature-responsive nanotube coating on the titanium surface; specifically:
[0044] Step 2.1, dissolving the hydrogel monomer and the crosslinking agent in deionized water, stirring for 15-20 minutes under N2 flow, and then adding the metal nanomaterial and the initiator and stirring for 1-12 hours to obtain a hydrogel precursor;
[0045] The hydrogel monomer is any one or more of acrylamide, methacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, ethylene oxide, vinyl methyl ether, hydroxypropyl cellulose, N-vinyl pyrrolidone, and vinyl alcohol; the metal nanomaterial is any one or more of silver nanoparticles, silver nanowires, gold nanoparticles, zinc oxide nanoparticles, and magnesium oxide nanoparticles; the crosslinking agent is any one or more of N-isopropylacrylamide, diethoxyethyl dimethacrylate, acrylamide, and methyl methacrylate; the initiator is any one or more of ammonium persulfate, azobisisobutyronitrile, benzoyl peroxide, diisopropylbenzene peroxide, and diformyl peroxide;
[0046] The mass ratio of hydrogel monomer, crosslinking agent, initiator and metal nanomaterial is 1: 0.01-0.1: 0.01-0.1: 0.1-0.5;
[0047] Step 2.2, coating the hydrogel precursor on the surface of the titanium sheet prepared in step 1, and then standing and drying under a vacuum environment to prepare a temperature-responsive nanotube coating on the titanium surface;
[0048] The standing temperature is 35-50°C, the standing time is 1h-12h, and the drying time is 1-10h.
[0049] Step 3, encapsulating the nanotubes;
[0050] By using plasma spraying technology, magnesium and magnesium oxide are sprayed on the surface of the titanium sheet in step 2, so that a temperature-sensitive responsive antibacterial coating can be prepared on the surface of the titanium product;
[0051] The parameters of plasma spraying are: spraying distance is 10-20mm, powder feeding voltage is 10-20v, powder feeding current is 500-1000A, spray gun moving speed is 5-10mm / s, hydrogen rate is 5-10L / h, argon rate is 1500-2500L / h, nitrogen rate is 2000-3000L / h, nitrogen pressure is 10-15Mpa;
[0052] The mass ratio of magnesium to magnesium oxide is 1:1 to 5;
[0053] The method for preparing the thermosensitive responsive antibacterial coating on the surface of titanium products of the present invention comprises the following steps: preparing magnesium-zinc co-doped barium titanate piezoelectric nanotubes, and filling the nanotubes with thermosensitive swellable hydrogels. When the hydrogels swell, they squeeze the nanotube walls, and the piezoelectric effect generates electric current which is transmitted to the surface, thereby affecting the adhesion and proliferation of bacteria, and playing a synergistic antibacterial role with the alkaline microenvironment generated by magnesium ions.
[0054] Figure 3 This is a schematic diagram of the cross-sectional structure of a thermosensitive responsive antibacterial coating on the surface of a titanium product prepared in the method of the present invention. From the figure, it can be seen that titanium dioxide nanotubes 2 are evenly distributed on the surface of a titanium substrate 1, and magnesium zinc-doped barium titanate nanotubes 3 are in situ formed inside the nanotubes by a hydrothermal reaction. After the thermosensitive expandable hydrogel is filled in the tube, plasma spraying is used to make the magnesium nanoparticles 6 and magnesium oxide nanoparticles 5 seal the tube mouth of the nanotube, thereby avoiding the ectopic location of the expandable hydrogel 4 and enhancing the surface properties of the coating.
[0055] Example 1
[0056] After the surface of the titanium sheet is smoothed by sandpaper, it is polished in a polishing solution composed of hydrofluoric acid, nitric acid and deionized water in a volume ratio of 2:1:10, and the polished titanium sheet is anodized multiple times; the electrolyte for the first anodization is composed of ammonium fluoride, water and ethylene glycol in a ratio of 1:5:100, the anodization voltage is 50V, and the oxidation time is 1h; the electrolyte for the second anodization is composed of ammonium fluoride, water and ethylene glycol in a ratio of 1:10:100, the anodization voltage is 40V, and the oxidation time is 0.3h; the anodized titanium sheet is immersed in a mixed solution, the mixed solution is composed of magnesium acetate, zinc acetate and deionized water, the magnesium ion concentration is 0.02mol / L, the zinc ion concentration is 0.02mol / L, and the immersion time is 2h. The soaked titanium sheet was placed in a reactor, and a barium hydroxide solution was added to perform a hydrothermal reaction, wherein the barium ion concentration was 0.1 mol / L, the hydrothermal temperature was 180°C, and the hydrothermal time was 1.5 h. After the hydrothermal reaction, the reaction was dried at 50°C for 3 h. The dried titanium sheet was placed in a 2 mg / mL dopamine hydrochloride solution, stirred at 30°C for 12 h, and the titanium sheet was taken out, cleaned, and dried to obtain a modified barium titanate piezoelectric nanotube coating. N, N-dimethylacrylamide and acrylamide were dissolved in deionized water, and then stirred for 15 min under N2 conditions, and magnesium oxide nanoparticles and ammonium persulfate were added and stirred for 12 h to obtain a thermosensitive hydrogel precursor. The mass ratio of N, N-dimethylacrylamide, acrylamide, ammonium persulfate and magnesium oxide nanoparticles was 1: 0.02: 0.03: 0.2. The prepared hydrogel precursor was added dropwise onto the titanium surface on which the nanotube coating had been prepared, and allowed to stand for 6 h in a vacuum environment at 40°C, and dried for 3 h. The prepared titanium metal was plasma sprayed, and the spraying parameters were: spraying distance 10mm, powder feeding voltage 12v, powder feeding current 600A, spray gun moving speed 5mm / s, hydrogen rate 5L / h, argon rate 1700L / h, nitrogen rate 2200L / h, nitrogen pressure 10Mpa; the mass ratio of magnesium to magnesium oxide was 1:1; and finally a temperature-sensitive responsive antibacterial coating was obtained on the surface of the titanium metal.
[0057] Example 2
[0058] After the surface of the titanium sheet is smoothed by sandpaper, it is polished in a polishing solution composed of hydrofluoric acid, nitric acid and deionized water in a volume ratio of 4:1:20, and the polished titanium sheet is anodized multiple times; the electrolyte for the first anodization is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:5:200, the anodization voltage is 60V, and the oxidation time is 1h; the electrolyte for the second anodization is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:20:200, the anodization voltage is 50V, and the oxidation time is 0.5h; the anodized titanium sheet is immersed in a mixed solution, the mixed solution is composed of magnesium acetate, zinc acetate and deionized water, the magnesium ion concentration is 0.04mol / L, the zinc ion concentration is 0.03mol / L, and the immersion time is 3h. The soaked titanium sheet was placed in a reactor, and a barium hydroxide solution was added to perform a hydrothermal reaction, wherein the barium ion concentration was 0.2 mol / L, the hydrothermal temperature was 200°C, and the hydrothermal time was 2h. After the hydrothermal reaction, the titanium sheet was dried at 70°C and the drying time was 2h. The dried titanium sheet was placed in a 4mg / mL dopamine hydrochloride solution, stirred at 60°C for 15h, and the titanium sheet was taken out, cleaned, and dried to obtain a modified barium titanate piezoelectric nanotube coating. N,N-dimethylacrylamide and acrylamide were dissolved in deionized water, and then stirred for 20min under N2 conditions, and then magnesium oxide nanoparticles and ammonium persulfate were added and stirred for 12h to obtain a thermosensitive hydrogel precursor. The mass ratio of N,N-dimethylacrylamide, acrylamide, ammonium persulfate and magnesium oxide nanoparticles was 1:0.04:0.05:0.3. The prepared hydrogel precursor was added dropwise onto the titanium surface on which the nanotube coating had been prepared, and allowed to stand for 10h in a vacuum environment at 35°C, and then dried for 5h. The prepared titanium metal was plasma sprayed, and the spraying parameters were: spraying distance 12mm, powder feeding voltage 10v, powder feeding current 700A, spray gun moving speed 6mm / s, hydrogen rate 6L / h, argon rate 1800L / h, nitrogen rate 2500L / h, nitrogen pressure 12Mpa; the mass ratio of magnesium to magnesium oxide was 1:2; and finally a temperature-sensitive responsive antibacterial coating was obtained on the surface of the titanium metal.
[0059] Example 3
[0060] After the surface of the titanium sheet is smoothed by sandpaper, it is polished in a polishing solution composed of hydrofluoric acid, nitric acid and deionized water in a volume ratio of 5:1:30, and the polished titanium sheet is anodized multiple times; the electrolyte for the first anodization is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:5:300, the anodization voltage is 70V, and the oxidation time is 2h; the electrolyte for the second anodization is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:30:400, the anodization voltage is 60V, and the oxidation time is 1h; the anodized titanium sheet is immersed in a mixed solution, the mixed solution is composed of magnesium acetate, zinc acetate and deionized water, the magnesium ion concentration is 0.06mol / L, the zinc ion concentration is 0.06mol / L, and the immersion time is 1h. The soaked titanium sheet was placed in a reactor, and a barium hydroxide solution was added to perform a hydrothermal reaction, wherein the barium ion concentration was 0.3 mol / L, the hydrothermal temperature was 220°C, and the hydrothermal time was 4 h. After the hydrothermal reaction, the reaction was dried at 60°C for 4 h. The dried titanium sheet was placed in a 6 mg / mL dopamine hydrochloride solution, stirred at 40°C for 16 h, and the titanium sheet was taken out, cleaned, and dried to obtain a modified barium titanate piezoelectric nanotube coating. N, N-dimethylacrylamide and acrylamide were dissolved in deionized water, and then stirred for 15 min under N2 conditions, and then magnesium oxide nanoparticles and ammonium persulfate were added and stirred for 12 h to obtain a thermosensitive hydrogel precursor. The mass ratio of N, N-dimethylacrylamide, acrylamide, ammonium persulfate and magnesium oxide nanoparticles was 1: 0.05: 0.06: 0.4. The prepared hydrogel precursor was added dropwise onto the titanium surface on which the nanotube coating had been prepared, and allowed to stand for 10 h in a vacuum environment at 40°C, and then dried for 8 h. The prepared titanium metal was plasma sprayed, and the spraying parameters were: spraying distance 15mm, powder feeding voltage 15v, powder feeding current 600A, spray gun moving speed 7mm / s, hydrogen rate 8L / h, argon rate 2000L / h, nitrogen rate 2500L / h, nitrogen pressure 13Mpa; the mass ratio of magnesium to magnesium oxide was 1:3; and finally a temperature-sensitive responsive antibacterial coating was obtained on the surface of the titanium metal.
[0061] Example 4
[0062] After the surface of the titanium sheet was smoothed by sandpaper, it was polished in a polishing solution composed of hydrofluoric acid, nitric acid and deionized water in a volume ratio of 8:1:40, and the polished titanium sheet was anodized multiple times; the electrolyte for the first anodization consisted of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:10:400, the anodization voltage was 75V, and the oxidation time was 3h; the electrolyte for the second anodization consisted of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:20:400, the anodization voltage was 70V, and the oxidation time was 1h; the anodized titanium sheet was immersed in a mixed solution, the mixed solution consisted of magnesium acetate, zinc acetate and deionized water, the magnesium ion concentration was 0.08mol / L, the zinc ion concentration was 0.1mol / L, and the immersion time was 4h. The soaked titanium sheet was placed in a reactor, and a barium hydroxide solution was added to perform a hydrothermal reaction, wherein the barium ion concentration was 0.5 mol / L, the hydrothermal temperature was 200°C, the hydrothermal time was 5 h, and the hydrothermal reaction was performed after the hydrothermal reaction, the drying temperature was 80°C, and the drying time was 1 h. The dried titanium sheet was placed in a 10 mg / mL dopamine hydrochloride solution, stirred at 80°C for 20 h, and the titanium sheet was taken out, cleaned, and dried to obtain a modified barium titanate piezoelectric nanotube coating. N, N-dimethylacrylamide and acrylamide were dissolved in deionized water, and then stirred for 30 min under N2 conditions, and then magnesium oxide nanoparticles and ammonium persulfate were added and stirred for 12 h to obtain a thermosensitive hydrogel precursor, and the mass ratio of N, N-dimethylacrylamide, acrylamide, ammonium persulfate, and magnesium oxide nanoparticles was 1:0.08:0.1:0.4. The prepared hydrogel precursor was added dropwise onto the titanium surface on which the nanotube coating had been prepared, and allowed to stand for 8 h in a vacuum environment at 50°C, and then dried for 10 h. The prepared titanium metal was plasma sprayed, and the spraying parameters were: spraying distance 18mm, powder feeding voltage 18v, powder feeding current 800A, spray gun moving speed 6mm / s, hydrogen rate 10L / h, argon rate 2200L / h, nitrogen rate 2700L / h, nitrogen pressure 14Mpa; the mass ratio of magnesium to magnesium oxide was 1:5, and finally a temperature-sensitive responsive antibacterial coating was obtained on the surface of the titanium metal.
[0063] Table 1 shows the pH value, Mg content and the concentration of the antibacterial coating and pure titanium in each embodiment after immersion in liquid for 24 hours. 2+ It can be seen from the table that after the biological antibacterial coatings prepared in Examples 1 to 4 were immersed in the liquid for 24 hours, an alkaline microenvironment was formed around the titanium surface. The strength of the alkalinity was related to the Mg content in the coating. 2+ With the increase of magnesium content, Mg 2 +As the concentration increases, the pH value of the solution also tends to increase. The antibacterial experimental results of co-culture with E. coli at different temperatures show that each embodiment can have a certain antibacterial property against E. coli at a lower temperature, while at a higher temperature, the thermosensitive swellable hydrogel in the nanotubes expands due to the change in temperature and squeezes the inner wall of the nanotubes. The nanotubes generate current due to their own piezoelectric properties, which enhances the antibacterial property of the coating. Figure 1 and Figure 2 It can also be seen from the comparison that the temperature-sensitive responsive antibacterial coating prepared on the titanium surface has better antibacterial ability than pure titanium. In addition, each embodiment has good antibacterial performance at low and high temperatures, which provides a channel for the widespread use of titanium products in daily life.
[0064] Table 1 Performance comparison of antibacterial coatings in various embodiments and pure titanium
[0065]
Claims
1. Preparation method of thermosensitive antibacterial coating on the surface of titanium products, It is characterized in that Follow the steps below to implement it: Step 1, preparing a modified barium titanate piezoelectric nanotube coating on a titanium surface; Step 2, preparing a temperature-responsive nanotube coating on a titanium surface; In step 3, magnesium and magnesium oxide are sprayed on the surface of the titanium sheet in step 2 by plasma spraying technology, so that a temperature-sensitive responsive antibacterial coating can be prepared on the surface of the titanium product.
2. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 1, It is characterized in that In the step 1, specifically: Step 1.1, the surface of the titanium sheet is polished by chemical polishing, and then titanium dioxide nanotubes are prepared on the surface of the titanium sheet by multiple anodizing methods, and then the titanium sheet is immersed in a mixed solution to prepare magnesium-zinc-coated TiO on the titanium surface. 2 Nanotube coating; Step 1.2, placing the titanium sheet prepared in step 1.1 in a reaction kettle, adding a barium hydroxide solution, performing a hydrothermal reaction, and drying, thereby preparing magnesium-zinc co-doped barium titanate nanotubes on the surface of the titanium sheet; Step 1.3, placing the titanium sheet obtained in step 1.2 into a dopamine hydrochloride solution for stirring, washing, and nitrogen drying, thereby preparing a modified barium titanate piezoelectric nanotube coating on the titanium surface.
3. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 2, It is characterized in that In the step 1.1, during polishing, the polishing liquid is a mixture of nitric acid, hydrofluoric acid and deionized water in a volume ratio of 1:1 to 10:10 to 50; the multiple anodizing method includes primary anodizing and secondary anodizing, the electrolyte in the primary anodizing is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:1 to 10:100 to 500, the primary anodizing voltage is 50 to 80V, and the primary anodizing time is 0.5 to 3h; the electrolyte in the secondary anodizing is composed of ammonium fluoride, water and ethylene glycol in a volume ratio of 1:5 to 30:100 to 500; the secondary anodizing voltage is 30 to 80V, and the secondary anodizing time is 0.1 to 1h; the mixed solution is composed of magnesium acetate, zinc acetate and deionized water, the magnesium ion concentration is 0.01 to 0.1 mol / L, the zinc ion concentration is 0.01 to 0.1 mol / L, and the immersion time is 1 to 4h.
4. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 2, It is characterized in that In the step 1.2, the concentration of the barium hydroxide solution is 0.1-0.5 mol / L, the hydrothermal temperature is 150-250° C., the hydrothermal time is 1-5 h, the drying temperature is 50-80° C., and the drying time is 1-4 h.
5. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 2, It is characterized in that In the step 1.3, the concentration of the dopamine hydrochloride solution is 1 to 10 mg / mL, the stirring temperature is 20 to 80° C., and the stirring time is 10 to 24 h.
6. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 1, It is characterized in that In the step 2, specifically: Step 2.1: Dissolve the hydrogel monomer and crosslinker in deionized water and then pass N 2 The mixture is stirred for 15-20 minutes under the conditions of , and then the metal nanomaterial and the initiator are added and stirred for 1-12 hours to obtain a hydrogel precursor; Step 2.2, coating the hydrogel precursor on the surface of the titanium sheet prepared in step 1, and then standing and drying under a vacuum environment to prepare a temperature-responsive nanotube coating on the titanium surface.
7. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 6, It is characterized in that In the step 2.1, the hydrogel monomer is any one or more of acrylamide, methacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, ethylene oxide, vinyl methyl ether, hydroxypropyl cellulose, N-vinyl pyrrolidone, and vinyl alcohol; the metal nanomaterial is any one or more of silver nanoparticles, silver nanowires, gold nanoparticles, zinc oxide nanoparticles, and magnesium oxide nanoparticles; the crosslinking agent is any one or more of N-isopropylacrylamide, diethoxyethyl dimethacrylate, acrylamide, and methyl methacrylate; the initiator is any one or more of ammonium persulfate, azobisisobutyronitrile, benzoyl peroxide, dicumyl peroxide, and diformyl peroxide; and the mass ratio of the hydrogel monomer, the crosslinking agent, the initiator, and the metal nanomaterial is 1:0.01-0.1:0.01-0.1:0.1-0.
5.
8. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 6, It is characterized in that In the step 2.2, the standing temperature is 35 to 50° C., the standing time is 1 to 12 hours, and the drying time is 1 to 10 hours.
9. The method for preparing the temperature-sensitive antibacterial coating on the surface of a titanium product according to claim 1, It is characterized in that In the step 3, the parameters of plasma spraying are: spraying distance is 10-20 mm, powder feeding voltage is 10-20 V, powder feeding current is 500-1000 A, spray gun moving speed is 5-10 mm / s, hydrogen rate is 5-10 L / h, argon rate is 1500-2500 L / h, nitrogen rate is 2000-3000 L / h, nitrogen pressure is 10-15 MPa; the mass ratio of magnesium to magnesium oxide is 1:1-5.
10. Thermosensitive responsive antibacterial coating on the surface of titanium product prepared by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Stabilized preparation method of high-purity low-impurity sodium hypochlorite
CN122147353A