How to recover tin

The sulfuric acid oxidation leaching and controlled neutralization process effectively separates tin from copper and lead, enhancing the quality and suitability of recovered tin for smelting, addressing the inefficiencies of previous methods.

JP7589586B2Active Publication Date: 2024-11-26MITSUBISHI MATERIALS CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021028940
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-11-26
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Conventional methods for recovering tin from tin-containing materials face challenges such as the inability to separate lead effectively, high chemical costs, and low quality of recovered tin due to the presence of copper and lead, especially when their concentrations are high.

Method used

A method involving sulfuric acid oxidation leaching with an oxidizing agent to preferentially separate tin from copper and lead, followed by neutralization to form a tin-containing precipitate, using chloride ions to enhance tin transfer and controlling pH between 3.5 and 4.5 for optimal separation.

Benefits of technology

This method achieves high-quality tin recovery with reduced copper and lead content, suitable for direct use in tin smelting processes, improving the economic viability and purity of the recovered tin product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589586000004
    Figure 0007589586000004
  • Figure 0007589586000005
    Figure 0007589586000005
  • Figure 0007589586000001
    Figure 0007589586000001
Patent Text Reader

Abstract

To provide a method for efficiently recovering tin from a tin-containing substance containing copper and lead as well as tin.SOLUTION: A method for recovering tin from a tin-containing substance containing one or both of copper and lead as well as tin includes a sulfuric acid oxidation and leaching step for oxidizing and leaching tin from the tin-containing substance in a sulfuric acid acidic solution and a neutralization step for neutralizing the solution obtained by leaching and forming a tin-containing deposit to recover tin. An acidic solution with a sulfuric acid concentration of 100 g / L or more and 400 g / L or less is preferably used in the sulfuric acid oxidation and leaching step. A chloride ion is preferably added to the acidic solution in the sulfuric acid oxidation and leaching step. The solution is preferably made to a pH of 3.5 or higher and 4.5 or lower in the neutralization step.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for the recovery of tin, in particular Contains copper and lead along with tin The present invention relates to a method for efficiently separating and recovering tin from tin-containing materials. [Background technology]

[0002] Conventionally, a method for recovering tin from tin-containing materials has been known in which the raw material obtained by separating lead from dross generated in the lead smelting process is melted and reduced to obtain a tin-containing material (mainly containing tin and copper), which is oxidized in a NaOH solution to leach tin, and tin is recovered from this tin leachate by electrowinning (Patent Document 1: Patent No. 5188768). However, if the tin-containing material contains lead, lead will be leached together with the tin, and since this lead is a more noble element than tin, it will precipitate preferentially over tin during electrowinning, making it impossible to separate tin and lead. In addition, there is also the problem of high chemical costs due to the use of NaOH for leaching.

[0003] On the other hand, when copper or lead is contained in the tin leaching solution before electrowinning, a method is known in which copper or lead, which is an element more noble than tin, is reduced by adding metallic tin powder to the leaching solution and removed from the solution by substitution precipitation (cementation) (Patent Document 2: JP-A-11-217634). However, when the copper or lead concentration in the raw material is high, the metallic tin used for cementation becomes expensive.

[0004] Unlike the above-mentioned method of recovering tin after leaching by electrowinning, a method is known in which copper smelting dust is leached using hydrochloric acid or nitric acid, and copper and lead are preferentially eluted while tin is concentrated in the leaching residue and recovered (Patent Document 3: JP 2019-151862 A, Patent Document 4: JP 2019-151863 A). This method has the advantage that tin exists as a solid after leaching, so that tin can be easily recovered by solid-liquid separation, but there is a problem in that the tin content of the resulting tin recovery product is low because many elements are not leached together with tin. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5188768 [Patent Document 2] Japanese Patent Application Publication No. 11-217634 [Patent Document 3] JP 2019-151862 A [Patent Document 4] JP 2019-151863 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention solves the above problems in conventional tin recovery methods, and provides a method for efficiently recovering tin from a tin-containing material that contains tin as well as either copper or lead or both. It also provides a tin recovery method that can obtain a tin product with a higher tin content than the above hydrochloric acid leaching or nitric acid leaching. [Means for solving the problem]

[0007] The present invention provides a tin recovery method that solves the above problems by the following configuration. [1] With Tin Copper and Lead Tin from tin-containing materials, including Separate A method for recovering sulfuric acid from a sulfuric acid solution , in the presence of an oxidizing agent, The tin-containing material leaving copper in Oxidative leaching of tin and precipitates lead a sulfuric acid oxidation leaching step; A leaching solution containing tin and a leaching residue containing copper and lead are subjected to solid-liquid separation; a neutralization step of neutralizing the leaching solution to produce and recover a tin-containing precipitate, Separating and recovering tin from copper and lead A method for recovering tin, comprising the steps of: [2] The method for recovering tin described in the above item [1], wherein an acidic solution having a sulfuric acid concentration of 100 g / L or more and 400 g / L or less is used in the sulfuric acid oxidative leaching step. [3] The method for recovering tin according to the above [1] or [2], wherein chloride ions are added to the acidic solution in the sulfuric acid oxidation leaching step. [4] In the neutralization step, the pH of the liquid is 3.5 or more and 4.5 or less. To 1. A method for recovering tin described in any one of [1] to [3] above.

[0008] [Specific explanation] The present invention will be specifically described below. The method of the present invention is Copper and Lead Tin from tin-containing materials, including Separate A method for recovering sulfuric acid from a sulfuric acid solution , in the presence of an oxidizing agent, The tin-containing material leaving copper in Oxidative leaching of tin and precipitates lead a sulfuric acid oxidation leaching step; A leaching solution containing tin and a leaching residue containing copper and lead are subjected to solid-liquid separation; a neutralization step of neutralizing the leaching solution to produce and recover a tin-containing precipitate, Separating and recovering tin from copper and lead An example of the tin recovery method of the present invention is shown in FIG.

[0009] The tin recovery method of the present invention includes the steps of: Contains copper and lead This is a method for recovering tin from tin-containing materials. Contains copper and lead As the tin-containing material, for example, crushed electronic substrates (crushed substrates), scrap such as solder chips, selected products of various scraps, various intermediate smelting products, and the like can be used.

[0010] [Sulfuric acid oxidation leaching] Tin-containing materials (crushed substrates, etc.) are subjected to oxidative leaching (called sulfuric acid oxidative leaching) in an acidic solution mainly made of sulfuric acid (called sulfuric acidic solution) to leach tin. Most of the tin contained in the crushed substrates is oxidized and leached into the solution in the form of tin sulfate or sulfate complex ions, etc., and the remaining tin is transferred to the leaching residue.

[0011] The sulfuric acid concentration in the sulfuric acid oxidation leaching is preferably 100 g / L or more and 400 g / L or less. If the sulfuric acid concentration is less than 100 g / L, the leaching rate of tin drops significantly. On the other hand, if the sulfuric acid concentration exceeds 400 g / L, the leaching rate of copper increases, which makes it difficult to separate tin and copper, and tin forms a stable sulfate complex ion, making it difficult for tin to precipitate in the neutralization process.

[0012] This sulfuric acid oxidation leaching is preferably carried out by blowing in air or the like as an oxidizing agent. If oxygen gas is used instead of air, the dissolved oxygen concentration increases, and the copper leaching rate increases, so it is preferable to use air or the like.

[0013] Since tin and lead are less noble metals than copper, tin and lead are preferentially oxidized over copper during sulfuric acid oxidation leaching. The oxidized lead reacts with sulfate ions in the solution to form stable lead sulfate, which precipitates. Meanwhile, the tin oxidized and leached remains in the solution, so most of the copper and lead can be separated as leaching residue. As a result, the contamination of the tin-containing precipitate produced in the subsequent neutralization process with copper and lead can be significantly reduced.

[0014] In sulfuric acid oxidation leaching, the addition of chloride ions to the sulfuric acid solution promotes the leaching of tin, and can increase the tin transfer rate to the tin recovered material. Specifically, for example, as shown in Examples (No. A2 to A5), when 50 g of crushed substrate (raw material) containing 2.5 mass % tin is leached using 1 L of sulfuric acid with a concentration of 100 g / L, the addition of 1 g to 10 g of NaCl (about 1 to 10 times the amount of tin in the raw material) as a chloride ion additive can increase the tin transfer rate to the tin recovered material by 45% to 83% compared to when NaCl is not added. As the chloride ion additive, salts such as NaCl and KCl, aqueous solutions of these salts, hydrochloric acid, etc. can be used.

[0015] [Separation of post-leaching solution and leaching residue] The leachate after the sulfuric acid oxidation leaching is separated from the leach residue into solid and liquid. The leachate mainly contains tin, and the leach residue contains most of the copper and lead.

[0016] [Neutralization: Formation of tin-containing precipitate] The separated post-leaching solution is neutralized by adding an alkaline solution, and a precipitate containing mainly tin (called a tin-containing precipitate) is generated. The post-leaching solution containing tin is strongly acidic, and when an alkaline solution such as a NaOH solution is added to it to neutralize the solution to a pH of 3.5 or more to 4.5 or less, a tin-containing precipitate is generated. As shown in FIG. 2, the tin concentration in the solution decreases with an increase in pH, and when neutralized to a pH of more than 3.5, almost all of the tin can be precipitated. On the other hand, if a part of copper has been leached in the sulfuric acid oxidation leaching process, when neutralized to a pH of more than 4.5, the copper in the solution precipitates and is mixed into the tin-containing precipitate. Therefore, it is preferable to control the pH in the neutralization process to 3.5 or more to 4.5 or less. The generated tin-containing precipitate is recovered by solid-liquid separation to obtain a recovered tin product. Effect of the Invention

[0017] According to the tin recovery method of the present invention, Contains copper and lead By carrying out sulfuric acid oxidation leaching on a tin-containing material, tin can be preferentially leached, and most of the copper and lead can be transferred to the leaching residue. As a result, a leaching solution having a high tin concentration and low copper and lead concentrations can be obtained, and a tin recovered product with a high tin content can be obtained by neutralizing the resulting leaching solution. According to the tin recovery method of the present invention, a tin recovered product with a higher tin content can be obtained than the tin-containing leaching residue obtained by hydrochloric acid leaching or nitric acid leaching.

[0018] The tin recovered by the method of the present invention can be used as a raw material for the tin smelting process. In addition, since the copper concentration of the tin recovered is significantly lower than that of the conventional methods and it contains almost no lead, it can be economically processed into tin metal by processing it in a general tin smelting process. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a process diagram showing an example of a tin recovery method of the present invention. [Diagram 2] Graph showing the relationship between tin concentration and pH of the leaching solution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Examples of the present invention will be described below. The percentages of concentrations are by mass. [Example] 2 kg of waste electronic circuit boards were crushed with a biaxial crusher, then classified with a sieve with 3.35 mm openings, and the crushed circuit boards that fell under the sieve were collected. 50 g of the crushed circuit boards were immersed in 1 L of an acidic solution with a sulfuric acid concentration of 50 to 500 g / L maintained at 60 °C, and stirred for 6 hours while blowing air at a rate of 0.5 L / min to perform sulfuric acid oxidation leaching. For some samples, 1 g to 10 g of NaCl was added to the sulfuric acid solution to perform sulfuric acid oxidation leaching. Then, solid-liquid separation was performed using a suction filtration device, and a post-leaching liquid and leaching residue were obtained. A 48% NaOH solution was added to the obtained post-leaching liquid to neutralize it to pH 3.0 to pH 5.0. After the neutralization process, solid-liquid separation was performed using a suction filtration device, and a post-neutralization liquid and tin recovered material were obtained. The obtained tin recovered material was dried in a dryer at 105 °C for 12 hours. The tin, copper, and lead contents in the crushed substrates used as raw materials are shown in Table 1. The treatment conditions for sulfuric acid oxidation leaching, the pH during neutralization, and the concentrations and transfer rates of tin, copper, and lead in the tin recovered material are shown in Table 2. Table 3 also shows the transfer rates of tin, copper, and lead in the leaching residue and neutralized solution for each Example and Comparative Example. These concentrations were measured by ICP-AES. The transfer rates were calculated using the following formula [3]. Transfer rate (%) = [amount of metal in recovered material] / [amount of metal in raw material] × 100 [3]

[0021] As shown in Tables 2 and 3, in the range of sulfuric acid concentrations of 100 to 400 g / L, about 45 to 62% of the tin in the crushed substrate was leached, and almost all of the leached tin was transferred to the tin recovery material (No. A1, A5 to A9). In addition, the tin recovery rate increased from about 42% to about 83% by adding chloride ions, confirming the effect of adding chloride ions (No. A2 to A4). On the other hand, at a sulfuric acid concentration of 50 g / L, only about 5% of the tin was leached (No. B1), and at a sulfuric acid concentration of 500 g / L, the leached tin stably formed sulfate complex ions, so that not all of the tin precipitated even when neutralized to pH 4, and about 20% of the total tin was transferred to the neutralized solution. Furthermore, the high sulfuric acid concentration increased the copper leaching rate, and the copper transfer rate to the neutralized solution and the tin recovery material increased (No. B2). Copper has a negative effect on the tin smelting process, so tin recovered material that contains a lot of copper is not suitable as a raw material for tin smelting. In addition, when the solution was only neutralized to pH 3.0, the entire amount of tin did not precipitate regardless of the sulfuric acid concentration during leaching, and about 4.1% of the tin transferred to the neutralized solution (No. B3). On the other hand, when the solution was neutralized to pH 5.0, most of the leached copper precipitated, and the quality of the tin recovered material decreased (No. B4).

[0022] [Table 1]

[0023] [Table 2]

[0024] [Table 3]

Claims

1. This method for separating and recovering tin from a tin-containing material which contains copper and lead together with tin comprises a sulfuric acid oxidative leaching step in which, in a sulfuric acid acidic solution and in the presence of an oxidizing agent, tin is oxidatively leached from the tin-containing material, leaving copper behind, and lead is precipitated, and a neutralization step in which a post-leaching solution containing tin and a leaching residue containing copper and lead are separated into solid and liquid, and this post-leaching solution is neutralized to produce and recover a tin-containing precipitate, characterized in that the tin recovery method separates and recovers the tin from the copper and lead.

2. 2. The method for recovering tin according to claim 1, wherein an acidic solution having a sulfuric acid concentration of 100 g / L or more and 400 g / L or less is used in the sulfuric acid oxidative leaching step.

3. 3. The method for recovering tin according to claim 1 or 2, wherein chloride ions are added to the acidic solution in the sulfuric acid oxidative leaching step.

4. The method for recovering tin according to any one of claims 1 to 3, wherein in the neutralization step, the pH of the liquid is adjusted to 3.5 or more and 4.5 or less.

Citation Information

Patent Citations

  • Meryasukikaiyoamijihikidashisochi

    JP1976088768A

  • Method for recovering tin

    JP1987250133A

  • Treatment of decopperized dross

    JP1993098367A

  • Recovery of metallic tin from tin-containing waste

    JP1999217634A

  • TREATMENT METHOD FOR SUBSTANCE CONTAINING Sn, Pb AND Cu

    JP2005264252A