Multi-layer pipe
The multilayer pipe design with a pigmented second layer facilitates easy identification of updated pipes and maintains ultrapure water quality by using polyolefin resin and a gas barrier layer, addressing the frequent replacement challenge in semiconductor factories.
Patent Information
- Application Number
- JP2024045618
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Conventional ultrapure water pipes used in semiconductor factories need to be replaced frequently due to contamination, making it difficult to distinguish between pre-updated and post-updated pipes, which affects the elution performance and maintenance efficiency.
A multilayer pipe design with a first layer made of polyolefin resin or vinyl chloride resin and a second layer containing a pigment, allowing for a visible color difference between pre-updated and post-updated pipes, and optionally including a gas barrier layer to prevent oxygen ingress.
The multilayer pipe design enables easy identification of updated pipes, maintains elution performance, and ensures high purity of ultrapure water by suppressing metal and organic component elution, suitable for semiconductor manufacturing processes.
Smart Images

Figure 0007594703000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to multi-layer pipes. [Background technology]
[0002] In the manufacture of precision devices such as semiconductor devices or liquid crystal display devices, ultrapure water that has been refined to an extremely high degree of purity is used in wet processes such as cleaning. If metal ions or the like are present in the water at a concentration above a certain level, the metals will be adsorbed onto the wafer surface or the like, adversely affecting the quality of the precision device, and therefore, the amount of impurities in the ultrapure water is strictly controlled.
[0003] Impurities can also get mixed into ultrapure water in the piping that makes up the ultrapure water transport line. Although metals such as stainless steel, which have excellent gas barrier properties, have been used as piping materials, it is considered preferable to use resins in consideration of the effects of metal elution from the piping.
[0004] For example, Patent Document 1 discloses a multi-layer pipe for piping ultrapure water, characterized in that it comprises a first resin layer made of fluororesin and in contact with ultrapure water, and a second resin layer made of gas-impermeable resin and provided on the outer peripheral surface of the first resin layer. It further discloses that a third resin layer is provided on the outer peripheral surface of the second resin layer to protect the second resin layer, and that polyethylene is used for the third resin layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP2010-234576A [Patent Document 2] Patent Publication No. 2021-55764 [Patent Document 3] JP 2023-46656 A Summary of the Invention [Problem to be solved by the invention]
[0006] Pipes used for ultra-pure water in semiconductor factories need to be replaced sooner than regular piping, every 10 to 15 years.
[0007] However, if the pipes were colored with pigments to make it easier to tell the difference between before and after the renewal, it would affect the elution performance, so for conventional PVDF pipes, it was necessary to use uncolored ones. Therefore, even after renewal, the color remained the same, making it difficult to tell the difference between before and after construction.
[0008] An object of the present disclosure is to provide a multi-layer pipe that allows easy distinction between the pipe before and after renewal. [Means for solving the problem]
[0009] In order to achieve the above object, the multi-layer pipe according to the first disclosure is a multi-layer pipe used for transporting a semiconductor cleaning liquid, and includes a first layer and a second layer. The first layer constitutes the innermost layer and is mainly composed of a polyolefin resin or a polyvinyl chloride resin. The second layer is disposed outside the first layer and contains a pigment.
[0010] In this way, by including a pigment in the second layer outside the first layer, it is possible to create a color difference between the tube before and after renewal. This makes it easy to distinguish between the tubes before and after renewal. Also, in semiconductor factories, etc., by making the colors of the tubes that carry room temperature water and high temperature water different, it is easy to distinguish between the tubes that carry liquids of different temperatures.
[0011] The multi-layer pipe according to the second disclosure is the multi-layer pipe according to the first disclosure, wherein the pigment is selected from any one of an organic pigment, an inorganic pigment, and a fluorescent pigment.
[0012] This allows the second layer to be colored to provide a color difference between the pre-renewal and post-renewal tube.
[0013] The multi-layer pipe according to the third disclosure is the multi-layer pipe according to the first disclosure, and has a calcium elution amount of 30 μg / m as measured in accordance with SEMI F-57. 2 is less than.
[0014] This makes it possible to provide a multi-layer pipe that can be used to transport ultrapure water.
[0015] The multi-layer pipe according to the fourth disclosure is the multi-layer pipe according to the first disclosure, in which the color difference between the first layer and the second layer is 0.5 or more.
[0016] By providing a color difference between the first and second layers and coloring the second layer with a pigment, it is possible to distinguish between the pipe before and after renewal, and the first layer can be made a clean layer that does not contain pigment, thereby providing a multi-layer pipe that is suitable for ultrapure water applications.
[0017] The multi-layer pipe according to the fifth disclosure is the multi-layer pipe according to the first disclosure, in which the second layer is an adhesive polyolefin resin.
[0018] In this way, by using the second layer as an adhesive layer, another layer can be provided on the outside of the second layer, and a colored multi-layer pipe can be provided without affecting the other layer provided on the outside of the second layer with the pigment.
[0019] The multi-layer pipe according to the sixth disclosure is the multi-layer pipe according to the first disclosure, wherein the thickness of the second layer is 10 μm or more and 300 μm or less.
[0020] This allows a colored second layer of a predetermined thickness to be provided.
[0021] The multi-layer pipe according to the seventh disclosure is the multi-layer pipe according to the first disclosure, further comprising a gas barrier layer disposed on the outside of the second layer.
[0022] This makes it possible to suppress the intrusion of oxygen from the outside into the first layer.
[0023] The multi-layer pipe according to the eighth disclosure is the multi-layer pipe according to the first disclosure, further comprising a core layer disposed between the first layer and the second layer. The core layer contains a polyolefin resin as a main component.
[0024] This can improve the strength of the multi-layer pipe.
[0025] The multi-layer pipe according to the ninth disclosure is the multi-layer pipe according to the eighth disclosure, wherein the core layer contains a pigment.
[0026] This allows a color difference to be provided between the first layer, the core layer, and the second layer, making it possible to determine whether the thickness of each layer is within a specified range, and facilitating quality control.
[0027] The multi-layer pipe according to the tenth disclosure is the multi-layer pipe according to the first disclosure, in which the polyolefin resin is polyethylene.
[0028] By using polyethylene as the main component of the first layer, the content of low molecular weight components can be reduced, and the elution of organic components into ultrapure water can be suppressed. Effect of the Invention
[0029] According to the present disclosure, it is possible to provide a multi-layer pipe that allows easy distinction between the pipe before and after renewal. [Brief description of the drawings]
[0030] [Figure 1] FIG. 1 is a cross-sectional view showing a multi-layer pipe according to an embodiment of the present disclosure. [Diagram 2] FIG. 11 is a cross-sectional view showing a multi-layer pipe according to another embodiment of the present disclosure. [Diagram 3] FIG. 11 is a cross-sectional view showing a multi-layer pipe according to another embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0032] The multi-layer pipe of this embodiment is used for transporting a semiconductor cleaning liquid and includes a first layer and a second layer. The first layer constitutes the innermost layer and is mainly composed of a polyolefin resin or a polyvinyl chloride resin. The second layer is disposed outside the first layer and contains a pigment.
[0033] (Double-layer pipes 1, 2, 3) Fig. 1 is a cross-sectional view of a multi-layer pipe 1. Fig. 2 is a cross-sectional view of a multi-layer pipe 2, which is another example of the multi-layer pipe 1. Fig. 3 is a cross-sectional view of a multi-layer pipe 3, which is another example of the multi-layer pipe 1.
[0034] The multi-layer pipe 1 shown in FIG. 1 includes a clean layer 11 and a core material layer 12. The clean layer 11 forms the inner surface 1b of the multi-layer pipe 1. The clean layer 11 contains a polyolefin resin as a main component. The core material layer 12 is disposed on the outside of the clean layer 11. The core material layer 12 contains a polyolefin resin as a main component and a pigment. As will be described in detail later, the core material layer 12 is provided with a color difference from the clean layer 11 by coloring it with a pigment. The outer surface 2c of the multi-layer pipe 2 is formed by the core material layer 12. In the multi-layer pipe 1, the clean layer 11 corresponds to an example of the first layer, and the core material layer 12 corresponds to an example of the second layer.
[0035] The multi-layer pipe 2 shown in FIG. 2 includes a clean layer 11, a core material layer 12, an adhesive layer 13, and a gas barrier layer 14. In the multi-layer pipe 2, the gas barrier layer 14 is disposed on the outside of the core material layer 12 of the multi-layer pipe 1 via the adhesive layer 13. The adhesive layer 13 is disposed on the outer surface of the core material layer 12, and the gas barrier layer 14 is disposed on the outside of the adhesive layer 13. The clean layer 11 constitutes the innermost layer of the multi-layer pipe 2. The clean layer 11 forms the inner surface 2b of the multi-layer pipe 2. The gas barrier layer 14 forms the outer surface 2c of the multi-layer pipe 2. In the multi-layer pipe 2, the clean layer 11 corresponds to an example of the first layer, and the adhesive layer 13 corresponds to an example of the second layer.
[0036] The multi-layer pipe 3 shown in FIG. 3 includes a clean layer 11, an adhesive layer 13, and a gas barrier layer 14. Unlike the multi-layer pipe 2, the multi-layer pipe 3 does not have a core layer 12, and the gas barrier layer 14 is disposed on the outer surface of the clean layer 11 via the adhesive layer 13. The clean layer 11 constitutes the innermost layer of the multi-layer pipe 3. The clean layer 11 forms the inner surface 3b of the multi-layer pipe 3. The gas barrier layer 14 forms the outer surface 3c of the multi-layer pipe 3. In the multi-layer pipe 3, the clean layer 11 corresponds to an example of the first layer, and the adhesive layer 13 corresponds to an example of the second layer.
[0037] Each layer will be described below.
[0038] (Clean layer 11) The clean layer 11 constitutes the innermost layer of the multi-layer pipes 1, 2, and 3. The clean layer 11 forms the inner surfaces 1b, 2b, and 3b of the multi-layer pipes 1, 2, and 3. The clean layer 11 contains a polyolefin resin as a main component. The main component refers to a component with the highest content by mass. The main component refers to a component with a content rate of at least 50%. The lower limit of the content of the polyolefin resin in the clean layer 11 is preferably 50% by mass, more preferably 70% by mass, even more preferably 80% by mass, even more preferably 90% by mass, and even more preferably 95% by mass.
[0039] The polyolefin resin contained as the main component in the clean layer 11 is not particularly limited, and may be a polymer containing a monomer unit derived from an olefin. Examples of the polyolefin resin include polyethylene resin, ethylene-alkenyl carboxylate ester copolymer resin, ethylene-α-olefin copolymer resin, polypropylene resin, polybutene resin, and poly(4-methyl-1-pentene) resin. These polyolefin resins may be used alone or in combination of two or more. Among these polyolefin resins, polyethylene resin and polypropylene resin are preferred from the viewpoint of improving the strength of the semiconductor cleaning liquid pipe. Moreover, among the polyethylene resin and polypropylene resin, polyethylene resin is more preferred from the viewpoint of suppressing the content of low molecular weight components and suppressing the elution of organic components into ultrapure water.
[0040] Examples of polypropylene resins include homopolypropylene, block polypropylene, and random polypropylene. The copolymerization component in block polypropylene and random polypropylene is usually ethylene. Examples of polybutene resins include polybutene-1.
[0041] The polyethylene resin may be copolymerized with an α-olefin as necessary. Examples of the α-olefin to be copolymerized with the polyethylene resin include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-butene-1-hexene, 1-butene-4-methyl-1-pentene, and 1-butene-1-octene.
[0042] The polyethylene resin is polymerized using a catalyst containing one or more transition metal derivatives. From the viewpoint of ensuring long-term durability, in this embodiment, polymerization is performed using a Ziegler catalyst. When polymerizing the polyethylene resin using a Ziegler catalyst, a chlorine-based catalyst is used in an amount appropriately determined by a person skilled in the art to perform multi-stage polymerization, and then a neutralizer for neutralizing the chlorine-based catalyst and preferably an antioxidant are added together. The Ziegler catalyst used in the present invention is well known, and for example, the catalyst systems described in each publication such as JP-A-53-78287, JP-A-54-21483, JP-A-55-71707, and JP-A-58-225105 are used.
[0043] Specifically, there can be mentioned a catalyst system consisting of a solid catalyst component obtained by contacting a tetravalent titanium compound with a co-ground product obtained by co-grinding an aluminum trihalide, an organosilicon compound having a Si-O bond, and a magnesium alcoholate, and an organoaluminum compound.
[0044] The solid catalyst component preferably contains 1 to 15% by weight of titanium atoms.The organosilicon compound preferably has a phenyl group or an aralkyl group, such as diphenyldimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, triphenylethoxysilane, and triphenylmethoxysilane.
[0045] In producing the co-ground product, the ratio of aluminum trihalide and organosilicon compound used per mole of magnesium alcoholate is generally 0.02 to 1.0 mole, preferably 0.05 to 0.20 mole, and the ratio of aluminum atom of aluminum trihalide to silicon atom of organosilicon compound is preferably 0.5 to 2.0 mole ratio.
[0046] To produce the co-ground product, a conventional method may be applied using a grinding machine such as a rotary ball mill, a vibrating ball mill, or a colloid mill that is generally used in the production of this type of solid catalyst component. The average particle size of the obtained co-ground product is usually 50 to 200 μm, and the specific surface area is usually 20 to 200 m. 2 / g.
[0047] The solid catalyst component is obtained by contacting the co-milled product obtained as above with a tetravalent titanium compound in the liquid phase. The organoaluminum compound used in combination with the solid catalyst component is preferably a trialkylaluminum compound, such as triethylaluminum, tri-n-propylaluminum, tri-n-butylaluminum, tri-i-butylaluminum, etc.
[0048] Examples of the neutralizing agent include fatty acid metal salts such as calcium stearate, zinc stearate, and magnesium stearate, and hydrotalcites.
[0049] However, if polyethylene resin is polymerized using magnesium stearate or hydrotalcite as a neutralizing agent, when the resulting resin is molded into a piping material, a large amount of aluminum or magnesium will dissolve into water, which is not preferred for this embodiment.
[0050] In contrast, when the polymerization of polyethylene resin is carried out using calcium stearate as a neutralizing agent, the above-mentioned metal elution of aluminum and magnesium does not occur, and favorable low elution properties can be obtained, so calcium stearate is a preferred neutralizing agent in this embodiment.
[0051] As the polyethylene resin composition, high density polyethylene (HDPE) is preferred from the viewpoint of obtaining sufficient pressure resistance performance against water pressure during water supply and enabling the pipe wall thickness to be thinned. Among high density polyethylenes (HDPE), HDPE classified as a pressure-resistant class of PE100 or more in ISO9080, ISO1167, and ISO12162 is more preferred from the viewpoint of ensuring the long-term durability of piping materials for ultrapure water. Furthermore, even among HDPE classified as a pressure-resistant class of PE100 or more, HDPE that has high resistance to slow crack growth (slow crack growth resistance) to further improve the safety of the pipe system and has high fluidity to improve the smoothness of the inner surface of the pipe is preferred. Note that slow crack growth refers to a form of damage caused by stress concentration such as scratches on the piping material or the joint between the pipe and the joint.
[0052] As an index of a polyethylene resin composition that satisfies the pressure resistance class of PE100 or more and has good fluidity, specifically, the melt flow rate (MFR) of the polyethylene resin composition at a temperature of 190°C and a load of 21.6 kg is used. 21.6 ) is 6g / 10min or more and 25g / 10min or less, and the melt flow rate (MFR 5 ) and MFR21.6, which is the ratio of FR(MFR 21.6 / MFR 5 ) is 25 to 60, and density is 0.946g / cm 3 More than 0.960g / cm 3 It is preferable that:
[0053] MFR of polyethylene resin composition 21.6 If the MFR is less than 6g / 10min, the fluidity of the resin material is low, the mold transferability is poor, and the smoothness of the inner surface of the pipe is insufficient. 21.6 If the FR exceeds 25g / 10min, it becomes difficult to design a resin that satisfies PE100. Also, if the FR is less than 25, the molecular weight distribution of the polyethylene resin composition becomes narrow, so that the target MFR 21.6 On the other hand, if the FR exceeds 60, the impact resistance of the polyethylene resin composition decreases, and the safety of the piping material may be impaired.3 If the density is less than 0.960 g / cm, the pressure resistance will decrease and it will be difficult to reach PE100. 3 If the temperature exceeds this range, the resistance to slow cracking of the piping material decreases, and the safety of the piping system decreases during long-term use.
[0054] Furthermore, the resin composition for achieving the above-mentioned polyethylene resin composition is preferably composed of multiple components, specifically, a high molecular weight component (A) and a low molecular weight component (B).
[0055] High molecular weight component (A) is MFR 21.6 The content of α-olefins other than ethylene is 0.8 mol% to 2.0 mol%, preferably 0.9 mol% to 1.6 mol%, and the content ratio of the high molecular weight component (A) to the entire resin composition is 35 wt% to 50 wt%, preferably 37 wt% to 43 wt%. On the other hand, the melt flow rate (MFR2.16) of the low molecular weight component (B) at a temperature of 190°C and a load of 2.16 kg is 20 g / 10 min to 500 g / 10 min, preferably 50 g / 10 min to 300 g / 10 min.
[0056] MFR of the high molecular weight component (A) constituting the polyethylene resin composition 21.6 If the MFR is less than 0.05g / 10min, the target MFR 21.6 In order to achieve this, it is necessary to increase the MFR of the low molecular weight component, but in that case, the difference in viscosity between the high molecular weight component and the low molecular weight component when melted increases, reducing their compatibility, resulting in a decrease in various mechanical properties including resistance to slow cracking and roughening of the inner surface of the pipe due to flow instability. 21.6If the content exceeds 1.0 g / 10 min, various mechanical properties are reduced, and among them, the slow crack growth resistance is significantly reduced. If the α-olefin content is less than 0.8 mol%, the slow crack growth resistance is reduced, and if it exceeds 2.0 mol%, the rigidity of the polyethylene resin composition is reduced, making it difficult to design a resin that reaches PE100. If the content ratio of the high molecular weight component (A) is less than 35 wt%, the durability of the pipe is reduced, and if it exceeds 50 wt%, the rigidity of the polyethylene resin composition is reduced, making it difficult to design a resin that reaches PE100.
[0057] When the MFR2.16 of the low molecular weight component (B) constituting the polyethylene resin composition is less than 20 g / 10 min, the flowability of the polyethylene resin composition is low, so that the mold transferability is poor and the smoothness of the inner surface of the pipe is insufficient. On the other hand, when the MFR2.16 exceeds 500 g / 10 min, various mechanical properties, especially impact resistance, are significantly decreased.
[0058] The α-olefin content here includes not only the α-olefins fed to the reactor during polymerization and copolymerized, but also short chain branches (e.g., ethyl branches, methyl branches) produced as by-products. The α-olefin content is measured by 13C-NMR. The α-olefin content can be increased or decreased by increasing or decreasing the amount of α-olefins fed to be copolymerized with ethylene.
[0059] The amount of calcium elution from the clean layer 11 measured in accordance with SEMI F-57 is 30 μg / m 2 The calcium concentration in the clean layer 11 is adjusted so that it is less than 360 ppm. The calcium concentration in the clean layer 11 is 360 ppm or less, preferably 55 ppm or less, and more preferably 50 ppm or less. If the calcium concentration exceeds 60 ppm, the amount of calcium eluted into the ultrapure water becomes excessive, making it impossible to satisfy the required quality of ultrapure water.
[0060] From the viewpoint of further suppressing the amount of calcium eluted into ultrapure water, it is preferable that the calcium concentration in the clean layer 11 is as small as possible. However, from the viewpoint of obtaining good thermal stability and long-term strength of the polyethylene resin composition, the inclusion of a trace amount of calcium is unavoidable.
[0061] That is, when the amount of neutralizing agent added to a polyethylene resin polymerized using a Ziegler catalyst is insufficient, catalyst residue remains active in the resin, and the thermal stability and long-term strength of the polyethylene resin composition may decrease.
[0062] Therefore, in this embodiment, it is essential to add the minimum amount of neutralizing agent necessary to neutralize the catalyst residue. In consideration of the above, the calcium concentration of the clean layer 11 is 10 ppm or more, preferably 13 ppm or more, more preferably 15 ppm or more, and further preferably 20 ppm or more.
[0063] From the viewpoint of ensuring thermal stability, the oxidation induction time (OIT) of the clean layer 11 at 210° C. is preferably 20 minutes or more. If the oxidation induction time at 210° C. is less than 20 minutes, the polyethylene resin may deteriorate when thermally processed, resulting in a decrease in long-term strength and an increase in particles derived from the deterioration, which is not preferable for this embodiment.
[0064] A hot internal pressure creep test is widely used as a method for evaluating the long-term strength of polyethylene resins used as piping materials. From the viewpoint of sufficiently ensuring the long-term strength of piping materials for ultrapure water, it is preferable that the hot internal pressure creep performance of the clean layer 11 molded as a piping material is such that the piping material does not break for 3,000 hours or more when a circumferential stress of 5.0 MPa is applied to the piping material at 80°C.
[0065] The material properties of the polyethylene resin composition are preferably pressure resistance of "PE100" or higher as described in the ISO9080, ISO1167, and ISO12162 standards. Note that "PE100" refers to polyethylene in which the LPL value, which is the minimum guaranteed stress after 50 years at 20°C estimated by extrapolation using multiple correlation averaging after at least 9,000 hours of stress-rupture time curve measurement at three different temperatures with the maximum and minimum temperatures separated by 50°C or more, is 10 MPa or more and 11.19 MPa or less in the classification table specified in ISO12162.
[0066] The clean layer 11 may or may not contain an antioxidant. Examples of the antioxidant include phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, aromatic amine-based antioxidants, and lactone-based antioxidants.
[0067] Phenolic antioxidants include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-hexane-1,6-diylbis[3-(3,5- di-tert-butyl-4-hydroxyphenyl)propionamide], benzenepropanoic acid, 3,5-bis(1,1-dimethylethyl)-4-hydroxy, C7-C9 side chain alkyl ester, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4,6-triyl)tri-p-cresol, 4,6-bis(dodecylthiomethyl)-o-cresol, 4,6-bis(octyl 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, ... ,3,5-tris[(4-tert-butyl-3-hydroxy-2,6-xylyl)methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-[4,6-bis(octylthio)-1,3,5-triazin-2-ylamino]phenol, and diethyl[{3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl}methyl]phosphonate.
[0068] When using a phenol-based antioxidant, only one type may be used, or two or more types may be used in combination. From the viewpoint of preventing calcium elution, it is preferable that the antioxidant does not have oxygen derived from anything other than the phenol group. For example, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4,6-triyl)tri-p-cresol, 2,6-di-tert-butyl-4-[4,6-bis(octylthio)-1,3,5-triazin-2-ylamino]phenol, 4,4',4''-(1-methylpropanyl-3-ylidene)tris(6-tert-butyl-m-cresol), and 6,6'-di-tert-butyl-4,4'-butylidenebis-m-cresol are mentioned. In addition, when a phenol-based antioxidant having oxygen derived from anything other than the phenol group is used as the antioxidant, the calcium concentration in the polyethylene resin is preferably 50 ppm or less. Examples of functional groups having oxygen derived from groups other than a phenol group include an ester group, a carbonyl group, a carboxy group, an ether group, a nitro group, a nitroso group, an amide group, an azoxy group, and a sulfo group.
[0069] Examples of phosphorus-based antioxidants include tris(2,4-di-tert-butylphenyl)phosphite, tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphen-6-yl]oxy]ethyl]amine, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl ester phosphorous acid, and tetrakis(2,4-di-tert-butylphenyl)(1,1-biphenyl)-4,4'-diylbisphosphonite.
[0070] Examples of the sulfur-based antioxidants include dilauryl thiodipropionate, dimyristyl thiodipropionate, distearyl thiodipropionate, and pentaerythrityl tetrakis(3-lauryl thiopropionate).
[0071] Examples of the aromatic amine-based antioxidant include monoamine compounds such as diphenylamine-based compounds, quinoline-based compounds, and naphthylamine-based compounds, and diamine compounds such as phenylenediamine-based compounds and benzimidazole-based compounds.
[0072] Diphenylamine compounds include p-(p-toluenesulfonylamido)-diphenylamine, 4,4'-(α,α-dimethylbenzyl)diphenylamine, 4,4'-dioctyldiphenylamine derivatives, etc. Quinoline compounds include 2,2,4-trimethyl-1,2-dihydroquinoline polymers, etc.
[0073] Examples of naphthylamine compounds include phenyl-α-naphthylamine and N,N'-di-2-naphthyl-p-phenylenediamine.
[0074] Examples of the phenylenediamine compounds include N-N'-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, a mixture of N-N'-diphenyl-p-phenylenediamines, diaryl-p-phenylenediamine derivatives or mixtures thereof.
[0075] Examples of the benzimidazole compound include 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, the zinc salt of 2-mercaptobenzimidazole, and the zinc salt of 2-mercaptomethylbenzimidazole.
[0076] Examples of lactone-based antioxidants include a reaction product of 3-hydroxy-5,7-di-tert-butyl-furan-2-one and o-xylene, etc. From the viewpoint of suppressing the influence of oxygen and ensuring a preferable strength, the content of the antioxidant in the clean layer 11 is, for example, 0.01% by weight or more, preferably 0.03% by weight or more, and more preferably 0.05% by weight or more, and the upper limit of the content of the antioxidant is, for example, 5% by weight or less, preferably 1% by weight or less, and more preferably 0.5% by weight or less.
[0077] The clean layer 11 may or may not contain a light stabilizer, but it is preferable that it does not contain a light stabilizer from the viewpoint of preventing the elution of total organic carbon (TOC). Examples of light stabilizers include hindered amine light stabilizers (HALS). It is also preferable that the clean layer 11 of the present embodiment does not substantially contain a light stabilizer. Here, "substantially not containing" means that a light stabilizer is not actively added, and that unavoidable mixing as an impurity is permitted. The lower the concentration of the light stabilizer that is inevitably mixed in as an impurity, the better.
[0078] Examples of the hindered amine light stabilizer include an NH type hindered amine compound, an NR type hindered amine compound, and an N-OR type hindered amine compound.
[0079] Examples of NH-type hindered amine compounds include Tinuvin 770DF, Kimassorb 2020FDL, Kimassorb 944FDL (all trade names, manufactured by BASF), Adeka STAB LA-68, Adeka STAB LA-57 (all trade names, manufactured by Adeka Corporation), Cyasorb UV-3346, Cyasorb UV-3853 (all trade names, manufactured by Sun Chemical Company), and the like.
[0080] Examples of the NR-type hindered amine compounds include TINUVIN 622SF, TINUVIN 765, TINUVIN PA144, CHIMASSORB 119, TINUVIN 111 (all trade names, manufactured by BASF), SAVOSTAB UV119 (trade name, manufactured by Sabo Corporation), Adeka STAB LA-63P, and Adeka STAB LA-52 (all trade names, manufactured by Adeka Corporation).
[0081] Examples of the N-OR type hindered amine compound include TINUVIN 123, TINUVIN 5100, TINUVIN NOR371FF, and FLAMESTUB NOR116FF (all trade names, manufactured by BASF).
[0082] The clean layer 11 may or may not contain an ultraviolet absorbing agent (UVA). Examples of the ultraviolet absorbing agent include benzophenone-based ultraviolet absorbing agents, salumarate-based ultraviolet absorbing agents, benzocoat-based ultraviolet absorbing agents, benzotriazole-based ultraviolet absorbing agents, cyanoacrylate-based ultraviolet absorbing agents, and quenchers. For polyethylene or polypropylene, benzophenone-based ultraviolet absorbing agents and benzotriazole-based ultraviolet absorbing agents are particularly preferred.
[0083] Benzophenone-based ultraviolet absorbers include 2-hydroxy-4-methoxy-benzophenone.
[0084] Examples of the benzotriazole-based ultraviolet absorbers include 2-(2-hydroxy-5-methylphenyl)benzotriazole (Sumisorb 200, manufactured by Sumika Chemtex Co., Ltd.), 2-(2-hydroxy-5-t-butyl-5-methylphenyl)-5-chlorobenzotriazole (Tinuvin 326, manufactured by BASF), 2-(2-hydroxy-3,5-di-t-butylphenyl)-5-chlorobenzotriazole (Tinuvin 327, manufactured by BASF), and 2-(2-hydroxy-3,5-di-t-amylphenyl)benzotriazole (Tinuvin 328, manufactured by BASF).
[0085] The density of the polyethylene resin composition of the clean layer 11 is preferably 0.946 g / cm from the viewpoint of obtaining good rigidity of the polyethylene resin composition. 3 More preferably, 0.947 g / cm 3 More preferably, 0.948 g / cm 3 The density is preferably 0.960 g / cm from the viewpoint of obtaining good long-term durability and flexibility of the polyethylene resin composition. 3 Less than or equal to 0.957 g / cm 3 More preferably, 0.953 g / cm 3 The density is a value established in accordance with JIS K6922-2:1997.
[0086] The melt flow rate (MFR) of the polyethylene resin composition of the clean layer 11 at a temperature of 190° C. and a load of 21.6 kg 21.6 In order to obtain good processability of the polyethylene resin composition, the MFR 21.6 The MFR is preferably 8 g / 10 min or more, more preferably 12 g / 10 min or more, and even more preferably 15 g / min or more. 21.6 The MFR is preferably 22 g / 10 min or less, and more preferably 20 g / 10 min or less. 21.6 is a value established in accordance with JISK6922-2:1997.
[0087] The smoothness of the inner surface of the clean layer 11 (arithmetic mean roughness Ra) is not particularly limited, and may be, for example, 0.50 μm or less. From the viewpoint of obtaining good low elution properties of the pipe, the smoothness of the inner surface of the clean layer 11 is preferably 0.40 μm or less, more preferably 0.35 μm or less.
[0088] The ratio of the thickness of the clean layer 11 to the total thickness of the clean layer 11 and the core layer 12 is preferably 0.011 or more and 0.500 or less.
[0089] The thickness t1 of the clean layer 11 is preferably 0.3 mm or more and 4 mm or less.
[0090] (Core layer 12) The core layer 12 is disposed on the outside of the clean layer 11. In this embodiment, the core layer 12 is used in the multi-layer pipe 1 and the multi-layer pipe 2. The core layer 12 contains a polyolefin resin as a main component. The polyolefin resin used in the core layer 12 is not particularly limited, and can be appropriately selected from the polyolefin resins listed above as the polyolefin resins used in the clean layer 11. Among the above-mentioned polyolefin resins, high density polyethylene (HDPE) is preferred from the viewpoint of suppressing the elution of low molecular weight components and / or from the viewpoint of durability when pipes are cleaned with chemicals. The polyolefin resin used in the core layer 12 may be the same or different from the polyolefin resin used in the clean layer 11, but when the two layers are laminated in contact with each other, it is more preferred that the polyolefin resins are the same from the viewpoint of improving the adhesion between the two layers and expressing a preferred strength.
[0091] The core layer 12 contains a pigment. As the pigment, any of conventionally known organic pigments, inorganic pigments, and extender pigments can be used, and there is no particular limitation. Examples of organic pigments include phthalocyanine-based, azo-based, condensed azo-based, anthraquinone-based, perinone-perylene-based, indigo-thioindigo-based, isoindolinone-based, azomethine azo-based, dioxazine-based, quinacridone-based, aniline black-based, and triphenylmethane-based pigments. Examples of inorganic pigments include carbon black-based, titanium oxide-based, iron oxide-based, iron hydroxide-based, chromium oxide-based, spinel-type calcined pigments, lead chromate-based, vermilion chromate-based, Prussian blue-based, aluminum powder, and bronze powder. Examples of extender pigments include calcium carbonate-based, barium sulfate-based, silicon oxide-based, and aluminum hydroxide-based pigments. The pigments are used alone or in combination so that the core layer 12 has a predetermined color.
[0092] The color of the core layer 12 is set so that the color difference ΔE between the clean layer 11 and the core layer 12 is 0.5 or more. The color difference ΔE is preferably 1.0, and more preferably 2.0 or more. For example, since the clean layer does not contain a pigment, it can be set to the natural color of polyethylene (milky white), and the core layer 12 can be set to blue. The core layer 12 may also be set to a yellowish color.
[0093] The pigment content in the core layer 12 is not particularly limited as long as the above color difference can be achieved, but is preferably 0.05 wt% or more and 1.00 wt% or less. If the content is less than 0.05 wt%, it may be difficult to distinguish the pipes before and after renewal based on their colors, and it may also be difficult to distinguish between the clean layer 11 and the core layer 12.
[0094] The amount of calcium elution from the material (polyolefin resin composition) of the core layer 12, measured in accordance with EMIF-57, is preferably 30 μg / m from the viewpoint of ensuring the strength of the semiconductor cleaning liquid piping in a 60° C. operating environment. 2 More preferably, 50 μg / m 2 More preferably, 70 μg / m 2 More preferably, 80 μg / m 2 More than 90 μg / m 2 More preferably, 95 μg / m 2 The above can be mentioned.
[0095] The multi-layer pipes 1 and 2 of the present invention have an excellent effect of suppressing the elution of calcium and organic components, and therefore can effectively suppress the elution of calcium even if the material of the core layer 12 contains a large amount of calcium. From this point of view, a suitable example of the amount of calcium elution is 80 μg / m 2 More than 90μg / m 2 or more than 95 μg / m 2 The upper limit of the amount of calcium elution is not particularly limited, but from the viewpoint of suppressing calcium elution, it is preferably 120 μg / m 2 Below, 110μg / m 2or less than 100μg / m 2 Examples of the calcium concentration include the following. The calcium concentration in the material (polyolefin resin composition) of the core layer 12 is not particularly limited as long as it satisfies the above calcium elution amount, but from the viewpoint of ensuring the strength of the semiconductor cleaning liquid pipe in a 60° C. use environment, for example, 20 ppm or more, preferably 30 ppm or more, more preferably 40 ppm or more, even more preferably 50 ppm or more, and even more preferably 60 ppm or more. The upper limit of the calcium concentration range is, from the viewpoint of suppressing a lack of strength caused by the contained calcium itself becoming the starting point of destruction, and from the viewpoint of suppressing the elution of calcium and organic components, for example, 200 ppm or less, preferably 150 ppm or less, more preferably 130 ppm or less, and even more preferably 100 ppm or less.
[0096] The amount of organic components (TOC) eluted from the material (polyolefin resin composition) of the core layer 12 as measured in accordance with EMIF-57 is, for example, 30,000 μg / m 2 The multi-layer pipes 2 and 3 of the present invention are excellent in the effect of suppressing the elution of calcium and organic components, so that even if the material of the core layer 12 contains a large amount of organic components, the elution of the organic components can be effectively suppressed. From this point of view, a suitable example of the amount of eluted organic components is 31,000 μg / m 2 or more, preferably 31500 μg / m 2 The upper limit of the amount of eluted organic components is not particularly limited, but from the viewpoint of suppressing elution of organic components, it is preferably, for example, 35,000 μg / m 2 Less than or equal to 34000 μg / m 2 Less than or equal to 33,000 μg / m 2 More preferably, 32000 μg / m 2 The following are included:
[0097] The core layer 12 preferably contains an antioxidant. Examples of the antioxidant include phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, aromatic amine-based antioxidants, and lactone-based antioxidants. From the viewpoint of suppressing the influence of oxygen and ensuring a preferable strength, the content of the antioxidant in the core layer 12 is, for example, 0.01% by weight or more, preferably 0.1% by weight or more, and the upper limit of the content of the antioxidant is, for example, 5% by weight or less, preferably 1% by weight or less, and more preferably 0.5% by weight or less.
[0098] The thickness t2 of the core layer 12 is preferably 1.7 mm or more and 12 mm or less.
[0099] 1, when the core material layer 12 forms the outer peripheral surface 1c, the color of the core material layer 12 can be seen from the outside of the multi-layer pipe 1. This makes it possible to distinguish between the pipe before and after renewal by changing the color of the core material layer 12 before and after renewal.
[0100] Furthermore, by providing a color difference between the clean layer 11 and the core layer 12, the thickness of each can be easily measured, making it easier to control the quality.
[0101] (adhesive layer 13) As shown in Fig. 2, the adhesive layer 13 is disposed on the outside of the core layer 12. The adhesive layer 13 adheres the gas barrier layer 14 to the outside of the core layer 12. From the viewpoint of achieving a desired strength, the material of the adhesive layer 13 is preferably a homogeneous polyolefin resin. For example, maleic anhydride-modified adhesive polyethylene can be used.
[0102] The adhesive layer 13 contains an adhesive polyolefin as a main component and further contains a pigment. For example, modified polyolefin can be used as the adhesive polyolefin. By adding a pigment to the adhesive layer 13, the adhesive layer 13 can be colored. The pigment can be selected from organic pigments, inorganic pigments, fluorescent pigments, and combinations thereof. Although the pigment is not particularly limited, examples of preferred compounds as inorganic pigments include titanium oxide, iron oxide, silica, calcium carbonate, carbon black, and mica. Examples of preferred compounds as organic pigments include azo, insoluble azo, which is a phthalocyanine, and copper phthalocyanine blue. Examples of preferred compounds as fluorescent pigments include sulfides of barium, strontium, and zinc. When mica is used as the pigment, it is preferable to mix mica powder, which is a powder of mica, with the adhesive polyethylene, and the average particle size of the mica powder is preferably 300 μm or less, and more preferably 100 μm or less. The adhesive layer 13 may be colored metallic blue by including in the pigment, for example, mica or iron oxide.
[0103] The thickness t3 of the adhesive layer 13 is preferably 10 μm or more and 300 μm or less.
[0104] The pigment concentration in the adhesive layer 13 is, for example, preferably 0.30 wt% to 3.0 wt%, more preferably 0.8 wt% to 2.5 wt%, and even more preferably 1.0 wt% to 2.0 wt%. If the pigment concentration is less than 0.3 wt%, it may be difficult to distinguish the color difference between the tubes, and if it is more than 3.0 wt%, the adhesive performance may decrease.
[0105] The color difference between the adhesive layer 13 and the clean layer 11 in the multi-layer pipe 3 as shown in Fig. 3 is preferably 0.5 or more. In the case of the multi-layer pipe 2 in Fig. 2 in which the core layer 12 is disposed between the clean layer 11 and the adhesive layer 13, the color difference ΔE between the adhesive layer 13 and the core layer 12 is preferably 0.5 or more.
[0106] For example, in the case of a four-layered multi-layer pipe 3 as shown in Fig. 2, the clean layer 11 may be darker in color than the core layer 12 and adhesive layer 13. From the viewpoint of preventing the elution of impurities, the clean layer 11 does not contain pigment and is milky white. The color difference ΔE between the clean layer 11 and the core layer 12 is preferably 0.5 or more, more preferably 1.0 or more. The color difference ΔE between the core layer 12 and the adhesive layer 13 is preferably 0.5 or more.
[0107] (Gas barrier layer 14) The provision of the gas barrier layer 14 effectively prevents gas from dissolving in ultrapure water. The gas barrier layer 14 also prevents oxygen from penetrating from the outer surfaces 2c, 3c of the multi-layer pipes 2, 3 into the innermost clean layer 11 or the core layer 12, improving the long-term strength of the multi-layer pipes 2, 3. The provision of the gas barrier layer 14 is also preferable in that it effectively prevents gas from dissolving in ultrapure water.
[0108] Examples of materials for the gas barrier layer include polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer (EVOH), polyvinylidene chloride resin (PVDC), and polyacrylonitrile (PAN), and preferably polyvinyl alcohol (PVA) and ethylene-vinyl alcohol copolymer (EVOH).
[0109] The thickness t4 of the gas barrier layer 14 is not particularly limited as long as it is a thickness that can ensure the gas barrier properties of at least the polyethylene resin, but is preferably, for example, 50 μm or more and 300 μm or less.
[0110] The gas barrier layer 14 is transparent, and the color of the adhesive layer 13 can be seen from the outside of the multi-layer pipes 2 and 3. This makes it possible to distinguish the pipes before and after renewal by changing the color of the adhesive layer 13 between the pipes before and after renewal.
[0111] Furthermore, since the clean layer 11, the core layer 12, the adhesive layer 13, and the gas barrier layer 14 have different colors from their adjacent layers, the thickness of each layer can be easily measured, facilitating quality control.
[0112] (Ultra-pure water piping material applications) The multi-layer pipe of the embodiment of the present invention can be used for transporting ultrapure water. Specifically, the multi-layer pipe of the embodiment of the present invention can be used as piping in an ultrapure water production apparatus, piping for transporting ultrapure water from an ultrapure water production apparatus to a use point, and piping for returning ultrapure water from a use point. Note that ultrapure water in the present invention is defined as having a resistivity of 10 MΩ·cm or more at 25°C, more strictly, a resistivity of 15 MΩ·cm or more at 25°C, and even more strictly, a resistivity of 18 MΩ·cm or more at 25°C.
[0113] The multi-layer pipe according to the embodiment of the present invention is preferably used as a water pipe for nuclear power generation, which requires particularly strict water quality for ultrapure water, or as a transport pipe for ultrapure water used in wet processing steps such as washing in the manufacturing process of pharmaceuticals, semiconductor elements or liquid crystals, and more preferably in the manufacturing process of semiconductor elements. The semiconductor elements are preferably those having a higher integration degree, and more preferably, those used in the manufacturing process of semiconductor elements with a minimum line width of 65 nm or less. For example, SEMI F75 is a standard for the quality of ultrapure water used in semiconductor manufacturing.
[0114] In addition, since the multi-layer pipe according to the embodiment of the present invention has a polyolefin resin layer, it is easy to work with. For example, fusion work such as butt fusion joining and EF (electrical fusion) joining can be easily performed at a relatively low temperature.
[0115] (Manufacturing of multi-layered pipes) The multi-layer pipe of the embodiment of the present invention can be manufactured by preparing a polyolefin resin that is the main component of the clean layer 11 that forms the inner surface 2b of the piping material, a polyolefin resin that is the main component of the core layer 12, and, if necessary, preparing coating resins that form the outer adhesive layer 13 and the gas barrier layer 64, and co-extrusion molding so that each layer has a predetermined thickness. Since the multi-layer pipe of the embodiment of the present invention is made of polyolefin resin, it can be manufactured inexpensively.
[0116] (Other embodiments) Although one embodiment of the present disclosure has been described above, the present disclosure is not limited to the above embodiment, and various modifications are possible without departing from the gist of the invention.
[0117] (A) In the above embodiment, the clean layer 11 contains a polyolefin resin as a main component, but it is not limited to polyolefin resin, and the clean layer 11 may contain a vinyl chloride resin as a main component. Also, the core layer 12 contains a polyolefin resin as a main component, but it is not limited to polyolefin resin, and the core layer 12 may contain a vinyl chloride resin as a main component.
[0118] (B) In the above embodiment, the clean layer 11 contains a polyolefin resin as a main component, but is not limited to polyolefin resin and may be PVDF. In this case, a layer containing a pigment may be provided to color the outside of the clean layer 11. The main component of the pigment layer may be selected from PVDF, polyolefin resin, vinyl chloride resin, etc.
[0119] (C) In the above embodiment, the core layer 12 contains a pigment. In the above embodiment, the core layer 12 is colored with a pigment to provide a color difference between the clean layer 11, but the pigment is not limited to the pigment, and it is sufficient if a color difference can be provided between the clean layer 11 and the core layer 12. For example, the core layer 12 may contain a dye or a colorant and be colored with the dye or colorant. Also, in the above embodiment, the core layer 12 is colored, but the clean layer 11 may be colored with a pigment, a dye, a colorant, or the like.
[0120] (D) In the above embodiment, the adhesive layer 13 contains a pigment. In the above embodiment, the adhesive layer 13 is colored with a pigment to provide a color difference between the adhesive layer 13 and the clean layer 11 or the core layer 12, but the color is not limited to a pigment and may be any color that can provide a color difference between the adhesive layer 13 and the clean layer 11 or the core layer 12. For example, the adhesive layer 13 may contain a dye or colorant and be colored by the dye or colorant.
[0121] (E) In the above embodiment, the adhesive layer 13 contains a pigment, but this is not limited to the adhesive layer 13, and the gas barrier layer 14 may contain a pigment. However, if the gas barrier layer 14 contains a pigment, there is a risk that the efficiency of the gas barrier performance may decrease, so it is preferable not to contain a pigment in the gas barrier layer 14 but to contain a pigment in the adhesive layer 13.
[0122] (F) In the multi-layer pipe 3 in the above embodiment, the core layer 12 and the adhesive layer 13 contain pigments. However, from the viewpoint of distinguishing the color from the outside of the multi-layer pipe 3, only one of them may contain pigments.
[0123] (G) In the above embodiment shown in FIG. 3, the multi-layer pipe 3 is a four-layer pipe including a clean layer 11, a core layer 12, an adhesive layer 13, and a gas barrier layer 14, but it is not limited to four layers and may be five or more layers.
[0124] (Example) Next, the multi-layer pipe of this embodiment will be described in detail using examples.
[0125] In this example, it was confirmed whether or not it was possible to distinguish it from an existing pipe made of one layer of PVDF. The results are shown in Table 1. The existing one layer PVDF pipe is milky white.
[0126] Example 1 In this Example 1, the configuration of the multi-layer pipe 1 shown in FIG. 1 was used. The clean layer 11 of the multi-layer pipe 1 of Example 1 contains clean polyethylene as a main component. HDPE1 was used as the clean layer 11. Novatec HB534N (manufactured by Japan Polyethylene Co., Ltd.) was used as the HDPE1. Novatec HB534N is a completely additive-free high-density polyethylene that does not contain any antioxidants. The core layer 12 contains polyethylene as a main component and is HDPE2. Novatec HE222W (manufactured by Japan Polyethylene Co., Ltd.) was used as the HDPE2. Novatec HE222W is a PE100-grade high-density polyethylene that contains an antioxidant. As a pigment, it contains a pigment (Toyo Color) containing ferrocyanide (III) and mica that is colored metallic blue.
[0127] The color difference ΔE between the clean layer 11 and the core layer 12 was 10. In addition, since the existing PVDF pipe and the multi-layer pipe of Example 1 could be visually distinguished from the outside, they are indicated as "◯" in Table 1. The color difference of the press plate of the material forming the clean layer 11 and the color difference of the material forming the core layer 12 were measured, and the color difference ΔE between the clean layer 11 and the core layer was measured. A colorimetric color difference meter (ZE-2000, Nippon Denshoku Co., Ltd.) was used to measure ΔE.
[0128] Example 2 In this Example 2, a multi-layer pipe 1 having the configuration shown in Fig. 1 was used. The clean layer 11 of the multi-layer pipe 1 of Example 2 contains clean polyethylene as a main component. The core layer 12 contains polyethylene as a main component and fluorescently colored umbelliferone as a pigment.
[0129] The color difference ΔE between the clean layer 11 and the core layer 12 was measured in the same manner as in Example 1 and was found to be 8, meaning that the existing PVDF pipe and the multi-layer pipe of Example 2 could be visually distinguished from each other from the outside.
[0130] Example 3 In this Example 3, the multi-layer pipe 3 shown in Fig. 3 was used. The clean layer 11 of the multi-layer pipe 3 of Example 3 contains clean polyethylene as a main component. The adhesive layer 13 contains Admer NF528 (manufactured by Mitsui Chemicals, Inc.), which is a modified polyethylene as a main component, and contains a pigment (Toyo Color) containing ferrocyanide (III) and mica that is colored metallic blue as a pigment. The material of the gas barrier layer 14 is ethylene vinyl alcohol copolymer (EVOH).
[0131] The color difference ΔE between the clean layer 11 and the adhesive layer 13 was 10, and the existing PVDF pipe and the multi-layer pipe of Example 3 could be visually distinguished from each other. The color difference ΔE between the clean layer 11 and the adhesive layer 13 was measured by measuring the color difference of the press plate of the material forming the clean layer 11 and the color difference of the press plate formed by laminating the clean layer 11, the adhesive layer 13, and the gas barrier layer 14. The color of the adhesive layer 13 was measured from the outside of the gas barrier layer.
[0132] Example 4 In this Example 4, the multi-layer pipe 3 shown in Fig. 3 was used. The clean layer 11 of the multi-layer pipe 3 in Example 4 contains clean polyethylene as a main component. The adhesive layer 13 contains Admer NF528 (manufactured by Mitsui Chemicals, Inc.) as a main component and fluorescently colored umbelliferone as a pigment. The material of the gas barrier layer 14 is ethylene vinyl alcohol copolymer (EVOH).
[0133] The color difference ΔE between the clean layer 11 and the adhesive layer 13 was measured in the same manner as in Example 3 and was found to be 8, meaning that the existing PVDF pipe and the multi-layer pipe of Example 4 could be visually distinguished from each other from the outside.
[0134] Example 5 In this Example 5, the configuration of the multi-layer pipe 2 shown in FIG. 2 was used. The clean layer 11 of the multi-layer pipe 2 of Example 5 contains clean polyethylene as a main component. The core layer 12 of the multi-layer pipe 2 of Example 5 contains polyethylene as a main component and contains a light blue pigment, which is a cyan pigment colored light blue, as a pigment. The adhesive layer 13 contains Admer NF528 (manufactured by Mitsui Chemicals, Inc.) as a main component, and uses a pigment (Toyo Color) containing ferrocyanide (III) and mica colored metallic blue as a pigment. The material of the gas barrier layer 14 is ethylene vinyl alcohol copolymer (EVOH).
[0135] The color difference ΔE between the clean layer 11 and the adhesive layer 13 was 10 as a result of measurement in the same manner as in Example 3, and the existing PVDF pipe and the multi-layer pipe of Example 5 could be visually distinguished from the outside. The color difference ΔE between the core layer 12 and the adhesive layer 13 was 7. The color difference ΔE between the core layer 13 and the adhesive layer 13 was measured by measuring the color difference of the press plate of the material forming the core layer 13 and the color difference of the press plate formed by laminating the clean layer 11, the adhesive layer 13, and the gas barrier layer 14. The color difference ΔE between the clean layer 11 and the core layer 12 was 1.6 as a result of measurement in the same manner as in Example 1.
[0136] Example 6 In this Example 6, the configuration of the multi-layer pipe 2 shown in Figure 2 was used. The clean layer 11 of the multi-layer pipe 2 of Example 5 contains clean polyethylene as a main component. The core layer 12 of the multi-layer pipe 2 of Example 5 contains polyethylene as a main component and does not contain a pigment. The adhesive layer 13 contains Admer NF528 (manufactured by Mitsui Chemicals, Inc.) as a main component, and contains tin sphene (CaO·SnO2·SiO2) colored cherry metallic and mica as pigments. The material of the gas barrier layer 14 is ethylene vinyl alcohol copolymer (EVOH).
[0137] The color difference ΔE between the clean layer 11 and the adhesive layer 13 was 6.2 as a result of measurement in the same manner as in Example 3, and the existing PVDF pipe and the multi-layer pipe of Example 6 could be visually distinguished from the outside. The color difference ΔE between the core layer 12 and the adhesive layer 13 was 6 as a result of measurement in the same manner as in Example 5. The color difference ΔE between the clean layer 11 and the core layer 12 was 1.6 as a result of measurement in the same manner as in Example 1.
[0138] Example 7 In this Example 7, the multi-layer pipe 2 shown in Fig. 2 was used. The clean layer 11 of the multi-layer pipe 2 of Example 7 contains clean polyethylene as a main component. The core layer 12 of the multi-layer pipe 2 of Example 7 contains polyethylene as a main component and does not contain a pigment. The adhesive layer 13 contains Admer NF528 (manufactured by Mitsui Chemicals, Inc.) as a main component and contains a cyan pigment that is colored blue as a pigment. The material of the gas barrier layer 14 is ethylene vinyl alcohol copolymer (EVOH).
[0139] The color difference ΔE between the clean layer 11 and the adhesive layer 13 was 9.8 as a result of measurement in the same manner as in Example 3, and the existing PVDF pipe and the multi-layer pipe of Example 7 could be visually distinguished from the outside. The color difference ΔE between the core layer 12 and the adhesive layer 13 was 7.5 as a result of measurement in the same manner as in Example 5. The color difference ΔE between the clean layer 11 and the core layer 12 was 1.6 as a result of measurement in the same manner as in Example 1.
[0140] Comparative Example 1 In Comparative Example 1, a multi-layer pipe having the configuration shown in Fig. 1 was used. The clean layer of the multi-layer pipe of Comparative Example 1 contains clean polyethylene as a main component. The core layer of the multi-layer pipe of Comparative Example 1 contains polyethylene as a main component and does not contain a pigment.
[0141] As a result of carrying out measurements similar to those in Example 1, no color difference was observed between the clean layer and the core layer, and the existing PVDF pipe and the multi-layer pipe of Comparative Example 1 could not be distinguished from the outside.
[0142] Comparative Example 2 In Comparative Example 2, a multi-layer pipe having the configuration shown in Fig. 1 was used. The clean layer of the multi-layer pipe of Comparative Example 2 contains clean polyethylene as a main component. The core layer of the multi-layer pipe of Comparative Example 2 contains polyethylene as a main component and does not contain a pigment. The adhesive layer of Comparative Example 2 contains Admer NF528 (manufactured by Mitsui Chemicals, Inc.) as a main component and does not contain a pigment. The material of the gas barrier layer is ethylene vinyl alcohol copolymer (EVOH).
[0143] As a result of carrying out the same measurement as in Example 3, the color difference ΔE between the clean layer and the gas barrier layer was 0.4 due to the light reflection occurring in the gas barrier layer, but the existing PVDF pipe and the multi-layer pipe of Comparative Example 2 could not be distinguished from the outside. As a result of carrying out the same measurement as in Example 1, no color difference occurred between the clean layer and the core layer. Furthermore, as a result of carrying out the same measurement as in Example 5, the color difference ΔE between the core layer and the adhesive layer was 0.4 due to the light reflection occurring in the gas barrier layer as described above.
[0144] (Table 1) TIFF0007594703000002.tif55170
[0145] As described above, by using multi-layer pipes with a colored core layer or adhesive layer that can be seen from the outside, pipes of different colors can be arranged, and pipes can be distinguished before and after renewal. For example, by using a metallic blue multi-layer pipe as shown in Example 3 before renewal and a fluorescent multi-layer pipe as shown in Example 4 after renewal, it is easy to distinguish whether the pipe has been renewed.
[0146] In addition, since the existing PVDF pipe does not contain pigments to prevent the elution of impurities, it has the same natural color (milky white) as the clean layer of the multi-layer pipe of the present disclosure. Therefore, in the multi-layer pipe of the present disclosure, by coloring the core layer or adhesive layer so as to have a color difference from the clean layer, it can be distinguished from the existing PVDF pipe. [Explanation of symbols]
[0147] 1: Multi-layer pipe 2: Multi-layer pipe 3: Multi-layer pipe 11: Clean layer 12: Core layer 13: Adhesive layer 14: Gas barrier layer
Claims
1. A multi-layer pipe used for transporting a semiconductor cleaning solution, a first layer constituting the innermost layer and containing a polyolefin resin or a polyvinyl chloride resin as a main component; a second layer disposed outside the first layer and including a pigment; a core layer disposed between the first layer and the second layer, The core layer contains a polyolefin resin as a main component, The core layer contains a pigment, The content of the pigment in the core layer is 0.05 wt % or more and 1.00 wt % or less, The content of the pigment in the second layer is 0.30 wt % or more and 3.0 wt % or less. Multi-layer pipe.
2. The pigment is selected from one or more of an organic pigment, an inorganic pigment, or a fluorescent pigment. The multi-layer pipe according to claim 1.
3. Calcium elution measured according to SEMI F-57 is 30 μg / m 2 is less than The multi-layer pipe according to claim 1.
4. A color difference between the first layer and the second layer is 0.5 or more. The multi-layer pipe according to claim 1.
5. The second layer is an adhesive polyolefin resin. The multi-layer pipe according to claim 1.
6. The thickness of the second layer is 10 μm or more and 300 μm or less. The multi-layer pipe according to claim 1.
7. Further comprising a gas barrier layer disposed on the outer side of the second layer. The multi-layer pipe according to claim 1.
8. The polyolefin resin is polyethylene. The multi-layer pipe according to claim 1.
9. The first layer does not contain a pigment. The multi-layer pipe according to any one of claims 1 to 8.
Citation Information
Patent Citations
Pipe material for ultrapure water
JP2022159129A
Fiber-reinforced composite pipe and cold / warm water piping system
WO2016133167A1
Multilayer tube
JP2010234576A
Multilayered pipe
JP2021055764A
Electric fusion joint
JP2023046656A