Filler for electronic materials and method for producing same, slurry for electronic materials, and resin composition for electronic materials
Patent Information
- Application Number
- JP2023567458
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-16
- Filing Date
- 2021-12-16
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2041-12-16
AI Technical Summary
The increasing demand for electronic materials with higher performance is hindered by the challenge of achieving excellent electrical properties due to high physically adsorbed water content in nanometer-sized fillers, which is not effectively reduced by heating, and existing surface treatments are insufficient to improve electrical characteristics.
A filler for electronic materials with silica particles manufactured using a dry method, having a specific particle size distribution and surface area characteristics, combined with a classification process to remove small particles and surface treatment with silane compounds to reduce water content and enhance electrical properties.
The proposed solution achieves improved electrical characteristics, specifically a lower dielectric loss tangent (Df value), making it suitable for high-frequency applications by controlling particle size distribution and surface treatment, thereby reducing moisture content effectively.
Abstract
Description
Filler for electronic materials and method for producing the same, slurry for electronic materials, and resin composition for electronic materials
[0001] The present invention relates to a filler for electronic materials and a method for producing the same, a slurry for electronic materials, and a resin composition for electronic materials.
[0002] Fillers for electronic materials made of metal oxide particulate materials are used as encapsulants for semiconductor devices, substrate materials, and other electronic materials, and in particular, resin compositions in which fillers for electronic materials are dispersed in resin materials are known (Patent Documents 1 and 2, etc.).
[0003] Incidentally, Patent Document 2 discloses that when a resin composition in which a metal oxide particulate material is dispersed in a resin material is applied to an electronic material, the results of a pressure cooker test are favorable by reducing the amount of physically adsorbed water in the dispersed metal oxide particulate material to 50 ppm or less. Note that, since the surface OH groups (bound water) begin to be removed when silica is heated above 200°C (see, for example, Non-Patent Document 1), the physically adsorbed water of silica is measured by heating it to 200°C.
[0004] The invention disclosed in Patent Document 2 is intended to handle particles with relatively large particle sizes, as specified in claim 1 as 20 to 100 μm. In recent years, the particle size of fillers for electronic materials has been reduced from submicron to nanometer order due to the miniaturization of semiconductor device structures and circuits. Since the amount of physically adsorbed water increases in proportion to the surface area of the particulate material, a smaller particle size also increases the surface area and the amount of physically adsorbed water. For example, in particulate materials with particle sizes ranging from submicron to nanometer order, the moisture content equivalent to the "moisture content of 50 ppm or less" specified in Patent Document 2 is several tens of times greater, exceeding 1,000 ppm. Even when heating was performed with the aim of reducing the moisture content to that level, it was not possible to reduce the moisture content (e.g., bound water) enough to achieve improved electrical properties, and the electrical properties were not satisfactory. In particular, even if the amount of physically adsorbed water was reduced, moisture in the air often quickly recombined thereafter.
[0005] Therefore, Patent Document 3 discloses a filler for electronic materials made of silica particle material in which the water content is reduced by combining a specific surface treatment with other components.
[0006] JP 58-138740 A JP 60-199020 A (Claim 1, 2, etc.) JP 2020-097498 A
[0007] Surface Chemistry and Adhesion Phenomena of Granular Materials, Masatoshi Chikazawa, Takashi Takei, Journal of the Japan Society of Sea Water Science, Vol. 41, No. 4, 1987, pp. 168-180
[0008] However, in recent years, the demand for electronic materials has been insatiable, and there is a strong desire for materials with higher performance than ever before. There is also a demand for even higher performance fillers for electronic materials provided in Patent Document 3.
[0009] In view of the above circumstances, the present inventors have set an object to provide a filler for electronic materials having excellent electrical properties, a method for producing the same, a filler for electronic materials, and a resin composition for electronic materials.
[0010] (1) The filler for electronic materials of the present invention, which solves the above-mentioned problems, contains a silica particle material produced by a dry process and has a D50 of 0.2 μm or more and 7.0 μm or less. Furthermore, the filler for electronic materials of the present invention has a (BET specific surface area) / (theoretical specific surface area calculated from D50) ratio of 0.85 to 1.2 (Requirement 1), and / or a D10 / D50 ratio of 0.55 to 0.75 (Requirement 2).
[0011] By satisfying at least one of the above requirements 1 and 2, electrical properties such as the Df value can be improved. Here, the BET specific surface area is a value measured using nitrogen, and D50 is the 50% mass cumulative diameter, i.e., the median diameter, and means the particle size at 50% mass when the masses of the particles are sequentially accumulated from the smallest particle size. Similarly, D10 is the 10% mass cumulative diameter. (2) The method for producing a filler for electronic materials of the present invention, which solves the above problem, is a method for producing a filler for electronic materials of the above-mentioned (1), and includes a raw silica particle material preparation step of producing a raw silica particle material by a dry method, and a classification step of separating a large particle size fraction from the raw silica particle material.
[0012] The classification process removes small particles. Small particles have a relatively higher water content than large particles, so adjusting the particle size distribution can reduce the water content and improve electrical properties. Also, small particles have a relatively higher silanol group content than large particles, so adjusting the particle size distribution can improve electrical properties.
[0013] The filler for electronic materials of the present invention has the above-mentioned constitution and is excellent in electrical properties such as Df value, etc. In particular, it can be suitably produced by the production method for a filler for electronic materials of the present invention.
[0014] The filler for electronic materials, its manufacturing method, electronic material slurry, and electronic material resin composition of the present invention will be described in detail below based on embodiments. (Filler for electronic materials) The filler for electronic materials of this embodiment can be used as a material for sealing electronic components such as semiconductors, underfill, substrate material, heat transfer material, etc. It is particularly desirable to use it in applications related to electronic components that use high frequencies (e.g., 1 GHz or more). For example, it can be suitably employed to form substrates for electronic devices that handle high frequencies. It is also preferably used as a filler for use in the electronic material slurry and electronic material resin composition described below.
[0015] The filler for electronic materials of this embodiment has a D50 of 0.2 μm or more and 7.0 μm or less. D50 is a value measured using an LA750 500 mode (Horiba, Ltd.). The lower limit of D50 is preferably 0.3 μm, 0.5 μm, or 1.0 μm, and the upper limit is preferably 5.0 μm, 3.5 μm, or 2.5 μm. These lower and upper limits can be combined arbitrarily. The particle size can be measured by a laser scattering method. The silica particle material satisfies at least one of the following requirements 1 and 2, and preferably satisfies both requirements 1 and 2.
[0016] Requirement 1 is that the ratio (BET specific surface area) / (theoretical specific surface area calculated from D50) is 0.85 or more and 1.2 or less. The specific surface area is measured by the BET method using nitrogen. The theoretical specific surface area calculated from D50 is the surface area calculated from the D50 value when the silica particle material is assumed to be spherical, and is specifically calculated using the formula: specific surface area = 6 / (D50 × true specific gravity).
[0017] The ratio (BET specific surface area) / (theoretical specific surface area calculated from D50) may be referred to as the "specific surface area coefficient" as appropriate in the specification. The specific surface area coefficient may have lower limits of 0.90 and 0.95, and upper limits of 1.18, 1.15, and 1.10, and these lower and upper limits can be combined arbitrarily. The closer to 1 the specific surface area coefficient is, the more preferable it is.
[0018] If the specific surface area coefficient is greater than 1, it can be made closer to 1 by removing small particles, and if it is less than 1, it can be made closer to 1 by removing coarse particles.
[0019] The BET specific surface area is not particularly limited, but is preferably 0.3 m 2 / g or more, 10m 2 The lower limit of the specific surface area is preferably 0.7 m / g or less. 2 / g can be exemplified, and the upper limit is 1.5m 2 / g, 4.5m 2 / g, 8m 2 These lower limit values and upper limit values can be combined arbitrarily.
[0020] Requirement 2 is that D10 / D50 is 0.55 or more and 0.75 or less, with the lower limit being 0.60 or 0.65 and the upper limit being 0.70, and the lower and upper limits can be arbitrarily combined. The maximum value of D10 / D50 is 1, and a value approaching 1 can be achieved by removing small particles.
[0021] The filler for electronic materials of this embodiment is a particulate material containing silica particulate material produced by a dry process. The particulate material may be solid, hollow, or a mixture thereof. The particulate material is preferably spherical. For example, the lower limit of the sphericity is preferably 0.9, 0.95, 0.98, or 0.99.
[0022] The content of the silica particle material contained in the filler for electronic materials is not particularly limited, but examples of lower limits of the content include 50%, 60%, 70%, 80%, 90%, 95%, and 100%. Particle materials that can be contained in addition to the silica particle material include inorganic oxides such as alumina, zirconia, and titania, inorganic nitrides such as boron nitride and aluminum nitride, barium titanate, calcium titanate, and strontium titanate, and resin materials such as fluororesins. These may be mixed as separate particle materials from the silica particle material or may be contained in the silica particle material. As the inorganic oxide, composite oxides of these or silica may be used.
[0023] The dry method is a method for forming a silica particle material without contact with water. Specific dry methods include the VMC method, in which powder and granules made of metal silicon are combusted in an oxidizing gas atmosphere and rapidly cooled to prepare a silica particle material, and the fusion method, in which powder and granules made of silica are melted by being introduced into a flame and then rapidly cooled to prepare a silica particle material. Even after this, it is preferable to avoid contact with water. If the material comes into contact with water, it is preferable to reduce the moisture content by heating. The preferred moisture content will be described later.
[0024] The VMC method and the melting method are treated as dry manufacturing methods (dry methods in this specification) because they do not allow the material to come into contact with water after being introduced into a high-temperature atmosphere such as a flame for combustion or after being heated and melted. In both the VMC method and the melting method, the particle size distribution of the prepared silica particle material can be controlled by adjusting the particle size distribution of the powder or granules introduced and the amount introduced. For example, the smaller the particle size of the powder or granules introduced or the smaller the amount introduced, the smaller the particle size of the prepared silica particle material.
[0025] In the VMC method and the melting method, it is preferable to reduce the amount of moisture present in the high-temperature atmosphere into which the raw powder or granular material is introduced. For example, the raw powder or granular material is dispersed in some kind of dispersion medium and transported, and it is desirable to remove the moisture from the dispersion medium. It is also preferable to remove the moisture contained in the oxidizing atmosphere gas in the VMC method and the high-temperature atmosphere in the melting method. Moisture removal can be achieved by general dehumidification methods (such as lowering the temperature to condense and remove the contained moisture, or using a desiccant), or by performing the operation when the moisture content is originally low (using air that changes depending on the season, weather, etc.).
[0026] The filler for electronic materials of this embodiment preferably has a water content generated by heating per unit surface area based on the BET specific surface area in the following range: First, the water content generated when heated from 25°C to 200°C (hereinafter referred to as "water content at 200°C") is 90 ppm / m 2 It is preferably 80 ppm / m or less, and more preferably 80 ppm / m or less. 2 , 60 ppm / m 2 Furthermore, the amount of water generated when heated from 200°C to 550°C (hereinafter referred to as "amount of water generated at 550°C") is preferably 100 ppm / m or less. 2 , 150 ppm / m 2 It is preferable that the concentration is 120 ppm / m or less, and more preferably 120 ppm / m or less. 2 It is preferable that:
[0027] The amount of water generated at 200°C is a value obtained by dividing the part per million of the amount of water generated as the temperature rises from room temperature (25°C) to 200°C by a unit surface area based on the BET specific surface area. The part per million of the amount of water generated at 200°C is calculated by measuring the amount of water generated as the temperature rises from room temperature (25°C) to 200°C by the Karl Fischer method and using the mass of the filler for electronic materials measured as the reference.
[0028] The amount of water generated at 550°C is a value obtained by dividing the part per million of the amount of water generated as the temperature rises from 200°C to 550°C by a unit surface area based on the BET specific surface area. The part per million of the amount of water generated at 550°C is calculated by measuring the amount of water generated as the temperature rises from 200°C to 550°C by the Karl Fischer method and using the mass of the filler for electronic materials measured as the reference.
[0029] The filler for electronic materials of this embodiment is preferably surface-treated. The type of surface treatment is not particularly limited, but it is preferably surface-treated with a silane compound having one or more functional groups selected from the group consisting of a vinyl group, a phenyl group, a phenylamino group, an alkyl group having four or more carbon atoms, a methacryl group, and an epoxy group. The amount of silane compound to be treated is omitted here, as it will be explained in the method for producing a filler for electronic materials described below. (Method for producing a filler for electronic materials) The method for producing a filler for electronic materials of this embodiment is a method that can suitably produce the filler for electronic materials of this embodiment described above, and includes a raw silica particle material preparation step, a classification step, and other steps that are adopted as necessary.
[0030] The raw silica particle material preparation process is a process for producing a raw silica particle material by a dry method. Examples of dry methods that can be used include the so-called VMC method, in which a raw particle material containing metallic silicon is introduced into a high-temperature oxidizing atmosphere to oxidize the metallic silicon, causing explosive combustion, and then quenching to form silica, and the so-called fusion method, in which a raw particle material made of silica is introduced into a high-temperature atmosphere above the melting point of silica to melt it, and then quenched to form silica. The raw particle material made of metallic silicon, which is the raw material for the VMC method, and silica, which is the raw material for the fusion method, can also contain materials other than metallic silicon and silica. It is preferable that the obtained raw silica particle material is not exposed to moisture. "Not exposed to moisture" means not contacting liquid water, and further not exposing it to an atmosphere under conditions that would cause condensation.
[0031] The classification process is a process for separating large particle size fractions from raw silica particle material. The classification process can be performed in two ways: by extracting large particle size fractions from the raw silica particle material, or by removing small particle size fractions to leave the large particle size fraction. The classification process can be performed in either a liquid or gas atmosphere. The classification process is repeated until the required particle size distribution is achieved. The speed and accuracy of classification can be improved by applying acceleration such as centrifugal force.
[0032] The classification step is preferably carried out in a moisture-free atmosphere. When the classification step is carried out in a moisture-containing atmosphere, a moisture removal step in which moisture is removed by a heating step is preferably carried out. The lower limit of the heating temperature in the moisture removal step can be 200°C or 550°C, and the upper limit should be a temperature at which the raw silica particle material does not sinter. Whether or not sintering occurs depends on the heating time, and if the raw silica particle material can be separated into primary particles by crushing, it can be determined that sintering has not occurred.
[0033] The term "moisture-free atmosphere" means that, when the classification step is carried out in a liquid, the water content of the liquid is 1000 ppm or less (preferably 500 ppm or less).
[0034] Specific methods that can be used for the classification step include general classification methods such as a method of classifying using a flow such as a swirling flow (air flow classification method), a method of classifying the raw silica particle material as is using a sieve, and a method of classifying based on differences in sedimentation velocity, as well as a method of selectively removing the small particle size fraction by immersing the raw silica particle material in an alkaline solution and dissolving it, taking advantage of the fact that small particles dissolve first.
[0035] It is particularly desirable to use air classification, which has little risk of contact with moisture and little risk of impurities being mixed in due to contact with sieves or the like during classification.
[0036] Alternatively, a step of separating a large particle size fraction by utilizing the difference in sedimentation velocity due to particle size difference after dispersing the raw silica particle material in a dispersion medium can be employed. Specifically, it is preferable to recover the sedimentation layer, which is the large particle size fraction. The dispersion medium employed is not particularly limited, and water or an organic solvent can be used alone or as a mixture. When an organic solvent is employed, it is desirable to use one with a low water content. Examples of the upper limit of the water content in the organic solvent include 1000 ppm and 500 ppm. The reason for selecting an organic solvent is to prevent the raw silica particle material from absorbing water.
[0037] The organic solvent is preferably one that can be easily removed from the silica particle material by drying. Examples of the organic solvent include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, and butanol, and ketones such as acetone, methyl isobutyl ketone, methyl ethyl ketone, and diethyl ketone.
[0038] The concentration of the raw silica particle material dispersed in the dispersion medium is not particularly limited, but examples include 10%, 20%, 30%, 40%, 50%, 60%, and 70% based on the total mass.
[0039] When classification is performed using a liquid, a step of removing the liquid used (liquid removal step) is included. Even air classification methods can have a drying step similar to the liquid removal step. When an organic solvent is used as the liquid, an organic solvent removal step is included as a liquid removal step. The removal step is a step of removing the liquid from the large particle size fraction after classification. There are no particular restrictions on the specific method of removing the liquid, but it is preferable to adopt a drying step in which the liquid is removed by evaporation.
[0040] The drying step can be carried out by heating, blowing in a dry gas, reducing the pressure, or a combination of these operations. Since the drying step may cause particles to aggregate, a crushing step can be carried out after the drying step. When a drying step is used as the moisture removal step described above, it may be carried out simultaneously with the moisture removal step.
[0041] Other processes may include a surface treatment process. The surface treatment is not particularly limited, but is preferably performed with a silane compound having one or more functional groups selected from the group consisting of a vinyl group, a phenyl group, a phenylamino group, an alkyl group having four or more carbon atoms, a methacryl group, and an epoxy group. The surface treatment may be performed on the dried silica particle material after the drying process, or on the silica particle material in a dispersed state in an organic solvent during the classification process.
[0042] The surface treatment can be carried out in two or more stages. For example, after the above-mentioned surface treatment, the surface treatment with organosilazane can be performed to reduce the number of OH groups present on the surface. Since the OH groups present on the surface are also related to bound water, the amount of bound water can be reduced by reacting organosilazane with the OH groups on the surface. Here, the organosilazane to be reacted is not particularly limited, but hexamethyldisilazane is an example. The amount of organosilazane used for surface treatment is preferably an amount that can react with all of the OH groups present on the surface, or an excess amount.
[0043] Surface treatment with a silane compound is carried out by directly contacting the silane compound with the silica particle material, or by contacting the surface of the silica particle material with a surface treatment agent containing a silane compound (e.g., a solution in which a silane compound is dissolved in a solvent).
[0044] The amount of silane compound to be used for the treatment can be 200%, 150%, 120%, 100%, 80%, 50%, etc., where 100% is the amount capable of reacting with all of the OH groups present on the surface of the filler for electronic materials before surface treatment. These lower and upper limits can be combined arbitrarily. (Slurry for Electronic Materials) The slurry for electronic materials of this embodiment is a composition in which the filler for electronic materials of this embodiment described above is dispersed in a dispersion medium. The slurry for electronic materials of this embodiment can be used for semiconductor substrate materials, etc., and is particularly preferably used for high-frequency substrate materials. The dispersion medium is substantially free of moisture, and the moisture content is preferably 1000 ppm or less, and more preferably 500 ppm or less.
[0045] The mixing ratio of the filler for electronic materials to the dispersion medium in the electronic material slurry is not particularly limited, but it is preferable that the content of the filler for electronic materials be as high as possible. Note that, since the viscosity tends to increase as the amount of filler for electronic materials mixed increases, the filler for electronic materials can be mixed until the viscosity reaches the maximum allowable level, taking into consideration handleability. For example, the (filler for electronic materials):(dispersion medium) can be mixed at a mass ratio of about 20:80 to 80:20.
[0046] The dispersion medium is not particularly limited, but examples thereof include organic solvents such as silicone oil, methyl ethyl ketone, alcohol, and hexane, and resin precursors such as epoxy resin precursors, polyester precursors, and silicone resin precursors.
[0047] The filler for electronic materials is preferably surface-treated. The surface treatment preferably introduces a functional group that can improve the affinity between the dispersion medium used and the mating member with which the filler for electronic materials will come into contact when finally used. (Resin Composition for Electronic Materials) The resin composition for electronic materials of this embodiment is a cured product comprising the above-described filler for electronic materials and a resin material that disperses the filler for electronic materials. The resin material preferably has a moisture content of 1000 ppm or less, more preferably 500 ppm or less.
[0048] As an electronic material, it is preferably applied to high frequency applications such as high frequency substrates, etc. Since the filler for electronic materials of this embodiment has a low Df value, it is possible to reduce loss even when used in applications where high frequency waves are passed.
[0049] The mixing ratio of the filler for electronic materials to the resin material in the resin composition for electronic materials is not particularly limited, but the content of the filler for electronic materials is preferably as high as possible. For example, the filler for electronic materials:resin material can be mixed at a mass ratio of about 10:90 to 90:10.
[0050] The resin material is not particularly limited, but examples include common resin materials such as thermosetting resins (which may be mixed either before or after curing), thermoplastic resins, and the like, for example, epoxy resins, melamine resins, acrylic resins, polycarbonate resins, polyesters, silicone resins, liquid crystal polymers (LCPs), polyimides, cyclic olefin polymers (COPs), and polyphenylene oxides (PPOs). The resin material may be used alone, or multiple types of resin materials may be mixed (e.g., alloyed) and used. The resin material preferably has a moisture content of 1000 ppm or less, and more preferably 500 ppm or less.
[0051] The filler for electronic materials is preferably surface-treated, and the surface treatment preferably involves introducing a functional group that can improve affinity with the resin material used.
[0052] The method may further include a heating step as another step. The heating step is a step of removing moisture contained in the filler for electronic materials by heating. Even when the raw silica particle material is produced by a dry method, moisture present in the atmosphere may adhere to the surface of the raw silica particle material, so the moisture content is reduced by heating.
[0053] For example, by heating to about 550°C, or even above 550°C, the amount of water generated at 550°C or 200°C can be effectively reduced. The heating step is performed at a temperature that does not cause the silica particle material to melt or sinter. The heating step may be performed at any time during the production process, but it is particularly preferable to perform the heating simultaneously with the preparation of the silica particle material in the raw silica particle material preparation step.
[0054] Specific heating methods include heating using an electric furnace or a gas furnace. Specific heating devices include a rotary kiln, a fluidized bed furnace, and a calcination furnace. The heating atmosphere is not particularly limited, but examples of the heating atmosphere include nitrogen, argon, and dry air.
[0055] The filler for electronic materials and the method for producing the same of the present invention will be described in detail below with reference to examples.
[0056] (Sample Preparation) Test Examples 1 and 10 (D10: 1.7 μm, D50: 2.5 μm) Silica produced by the VMC method was used as the raw silica particle material (raw silica particle material preparation step). The raw silica particle material had a D50 of 1.9 μm and a D10 of 1.0 μm. This raw silica particle material was classified into a large particle size fraction by air classification (classification step). The silica particle material contained in the obtained large particle size fraction was reacted with vinyltrimethoxysilane as a silane compound (first surface treatment step). Hexamethyldisilazane was reacted to prepare a test sample for this test example (second surface treatment step). The specific surface area of this silica particle material was 1.1 m 2 The test sample of Test Example 10 was one that was not subjected to the surface treatment step.
[0057] Test Examples 2 and 3 (D10: 1.7 μm, D50: 2.5 μm) A filler for electronic materials was produced in the same manner as in Test Example 1, except that phenyltrimethoxysilane was used instead of vinyltrimethoxysilane, and this was used as a test sample for Test Example 2. A filler for electronic materials was produced in the same manner as in Test Example 1, except that N-phenyl-3-aminopropyltrimethoxysilane was used instead of vinyltrimethoxysilane, and this was used as a test sample for Test Example 2.
[0058] Test Examples 4, 5, and 12 (D10: 0.4 μm, D50: 0.7 μm) Fillers for electronic materials were produced in the same manner as Test Examples 1 and 2, except that raw silica particle material produced by the VMC method and having a D50 of 0.5 μm and a D10 of 0.3 μm was used, and these were used as test samples for Test Example 4 (vinyltrimethoxysilane) and Test Example 5 (phenyltrimethoxysilane), respectively. The amount of the treatment agent used for the surface treatment was the same amount per unit surface area. The test sample for Test Example 12 was one that was not subjected to the surface treatment process.
[0059] Test Examples 6, 7, and 11 (D10: 1.4 μm, D50: 2.3 μm) Fillers for electronic materials were produced in the same manner as Test Examples 1 and 2, except that raw silica particle material produced by the VMC method and having a D50 of 2.0 μm and a D10 of 1.1 μm was used, and these were used as test samples for Test Example 6 (vinyltrimethoxysilane) and Test Example 7 (phenyltrimethoxysilane), respectively. The amount of the treatment agent used for the surface treatment was the same amount per unit surface area. The test sample for Test Example 11 was one that was not subjected to the surface treatment step.
[0060] Test Examples 8 and 13 (D10: 2.7 μm, D50: 4.8 μm) A filler for electronic materials was produced in the same manner as in Test Example 1, except that a raw silica particle material produced by a melting method and having a D50 of 4.4 μm and a D10 of 1.5 μm was used, and this was used as the test sample of Test Example 8. The amount of the treatment agent used for the surface treatment was the same amount per unit surface area. The sample that was not subjected to the surface treatment step was used as the test sample of Test Example 13.
[0061] Test Examples 9 and 14 (D10: 3.8 μm, D50: 7.0 μm) A filler for electronic materials was produced in the same manner as in Test Example 1, except that a raw silica particle material produced by a melting method and having a D50 of 6.8 μm and a D10 of 2.4 μm was used, and this was used as the test sample of Test Example 9. The amount of the treatment agent used for the surface treatment was the same amount per unit surface area. The test sample of Test Example 14 was one that was not subjected to the surface treatment step.
[0062] Test Example 15 (D10: 1.3 μm, D50: 2.2 μm) A filler for electronic materials was produced in the same manner as in Test Example 1, except that a raw silica particle material produced by the VMC method and having a D50 of 1.9 μm and a D10 of 1.0 μm was used, that classification was performed using water, and that no surface treatment was performed, and this was used as the test sample of Test Example 15. By dispersing in water and then classifying, the water content increased.
[0063] Test Examples 16-20: Raw silica particle material produced by the VMC method and having D50 and D10 values shown in Table 4 was used as the test sample for each test example. D50 and D10 values were determined by varying the amount of metallic silicon added (atmospheric concentration) and the particle size of the metallic silicon. For Test Example 20, the sample was surface-treated with 3-methacryloxypropylmethyldimethoxysilane.
[0064] Test Example 21 (Preparation of Raw Silica Particle Material by Wet Method) A raw silica particle material was synthesized by hydrolyzing tetraethyl orthosilicate in the presence of an alkali catalyst, and used as a test sample in this test example. The obtained raw silica particle material had a D10 of 0.2 μm and a D50 of 0.4 μm.
[0065] Test Example 22 (Surface Treatment Step in the Presence of Moisture) A vinyltrimethoxysilane aqueous solution was added to the test sample of Test Example 12, and the surface treatment step was carried out by reacting, to obtain a test sample of this test example.
[0066] Test Examples 23 and 24 (D10: 1.7 μm, D50: 2.6 μm) Silica produced by the VMC method was used as a raw silica particle material (raw silica particle material preparation step). The raw silica particle material had a D50 of 1.9 μm and a D10 of 1.0 μm. This raw silica particle material was dispersed in an organic solvent to prepare a raw slurry. The raw slurry was allowed to stand for a certain period of time to allow a large particle size fraction to settle (classification step). The resulting large particle size fraction was dried to remove the organic solvent, thereby obtaining a silica particle material (organic solvent removal step). This silica particle material was reacted with vinyltrimethoxysilane as a silane compound (first surface treatment step). Hexamethyldisilazane was then reacted to obtain a test sample for Test Example 23 (second surface treatment step). The specific surface area of this silica particle material was 1.1 m 2 The test sample of Test Example 24 was one that was not subjected to the surface treatment step.
[0067] (Test) For the test samples of each test example, D10 and D50 were measured using an LA-750 manufactured by Horiba, Ltd., the specific surface area was measured by the BET method using nitrogen gas, and the amount of water generated at 200°C and 550°C was measured by the Karl Fischer method and converted to per unit surface area, and each is shown in the table.
[0068] The value of D10 / D50 was calculated from the measured D10 and D50, and SSA / ssa was calculated from the measured specific surface area (actual value: SSA) and the specific surface area (calculated value: ssa) calculated from D50, and these values are shown in the table.
[0069] Furthermore, the dielectric loss tangent (Df) at 1 GHz was measured for each sample in each test example. The dielectric loss tangent was measured in accordance with JIS C 2138. Specifically, the relative permittivity and dielectric loss tangent at 1 GHz were measured using a network analyzer (Keysight Corporation, E5071C) and a cavity resonator perturbation method. This measurement was performed in accordance with ASTM D2520 (JIS C2565).
[0070]
[0071]
[0072]
[0073] As is clear from the table, Test Examples 1 to 14 satisfied Requirement 1: specific surface area coefficient (SSA / ssa) and Requirement 2: D10 / D50, and were found to have smaller Df values than Test Examples 16 to 22, which did not satisfy Requirements 1 and 2. Note that Test Example 15 satisfied Requirements 1 and 2, but the amount of water generated at 200°C and 550°C was large, which is thought to be why Test Examples 1 to 14 had smaller Df values than Test Example 15 and were superior.
[0074] Among Test Examples 1 to 14, Test Examples 1 to 8, which were surface-treated with a silane compound, were found to have smaller Df than the corresponding Test Example 10 (corresponding to Test Examples 1 to 3), Test Example 11 (corresponding to Test Examples 6 and 7), Test Example 12 (corresponding to Test Examples 4 and 5), and Test Example 13 (corresponding to Test Example 8), which had the same D10 and D50 values. Therefore, it was found that Df was reduced by performing surface treatment.
[0075] Furthermore, when comparing silane compounds having a vinyl group with those having a phenyl group, it was found that both were superior because their Df values were the same. Furthermore, Test Examples 2 and 3, which were treated with silane compounds having a vinyl group or a phenyl group, had smaller Df values than Test Example 3, which was treated with a silane compound having a phenylamino group, so it was found that silane compounds having a vinyl group or a phenyl group were superior to those having a phenylamino group.
[0076] In Test Examples 23 and 24, classification was carried out by utilizing the difference in sedimentation velocity in the liquid, and it was found that, like the Test Examples employing the air classification method, requirements 1 and 2 were satisfied, and that small Df was obtained.
Claims
1. D50 is 0.2 μm or more and 7.0 μm or less, (BET specific surface area) / (theoretical specific surface area calculated from D50) is 0.85 or more and 1.2 or less, and D10 / D50 is 0.55 or more and 0.75 or less, Unit surface area based on BET specific surface area (1 m 2 When heated from 25°C to 200°C, the amount of moisture generated is 90 ppm or less per unit. Unit surface area based on BET specific surface area (1 m 2 When heated from 200°C to 550°C per 100g, the amount of moisture generated is 150ppm or less. A filler for electronic materials comprising silica particle material produced by a dry method.
2. D50 is 0.2 μm or more and 2.5 μm or less, D10 / D50 is 0.62 or more and 0.75 or less, The BET specific surface area is 4.5 m 2 / g or less. A filler for electronic materials comprising silica particle material produced by a dry method.
3. Unit surface area based on BET specific surface area (1 m 2 The amount of moisture generated when heated from 25°C to 200°C per unit is 90 ppm or less, Unit surface area based on BET specific surface area (1 m 2 When heated from 200°C to 550°C per 100g of the mixture, the amount of moisture generated is 150 ppm or less. The filler for electronic materials according to claim 2 .
4. The filler for electronic materials according to any one of claims 1 to 3, wherein the electronic material is a high-frequency substrate.
5. 5. The filler for electronic materials according to claim 1, which is surface-treated with a silane compound having one or more functional groups selected from the group consisting of a vinyl group and a phenyl group.
6. A filler for electronic materials according to any one of claims 1 to 5, a dispersion medium for dispersing the filler for electronic materials; The electronic material slurry has the following properties:
7. A filler for electronic materials according to any one of claims 1 to 5, a resin material in which the filler for electronic materials is dispersed; The resin composition for electronic materials comprises:
8. A method for producing a filler for electronic materials according to any one of claims 1 to 5, comprising the steps of: A raw silica particle material preparation step of producing a raw silica particle material by a dry method; a classification step of separating a large particle size fraction from the raw silica particle material; having The classification step includes: The method for producing a filler for electronic materials comprises a step of centrifugal classification of the raw silica particle material in a state where the raw silica particle material is dispersed in a gas, or a sedimentation classification step of dispersing the raw silica particle material in a dispersion medium and then separating the raw silica particle material based on the difference in sedimentation velocity.
9. The method for producing a filler for electronic materials according to claim 8 , further comprising a drying step after the classification step.