Pavement surface reinforcement method using MMA based coating with improved surface friction resistance and wear resistance

The MMA-based repair material with elastic beads and friction improvers addresses adhesion and durability issues, enhancing tensile strength and crack-following ability, while maintaining rapid curing and slip resistance for road pavement repairs.

KR103042789B1Active Publication Date: 2026-11-06NETFORM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020250103123
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-07-29
Publication Date
2026-11-06
Estimated Expiration
2045-07-29

AI Technical Summary

Technical Problem

Existing MMA-based road repair materials face issues with weak interfacial adhesion, insufficient durability, and vulnerability to cracking, along with limitations in impact resistance and crack propagation, especially when exposed to UV rays.

Method used

A composition comprising MMA resin, elastic beads, friction improvers, and silica sand is used to enhance tensile strength, crack-following ability, and surface friction resistance, while maintaining rapid curing characteristics and durability, with optional additives for non-slip, color, and antibacterial properties.

Benefits of technology

The repair material exhibits high elasticity, tensile strength, and crack-following properties, suppressing crack propagation and ensuring adhesion, with fast curing times and improved slip resistance, suitable for concrete and asphalt pavements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025086087516-PAT00001
    Figure 112025086087516-PAT00001
  • Figure 112025086087516-PAT00002
    Figure 112025086087516-PAT00002
  • Figure 112026087827879-PAT00004
    Figure 112026087827879-PAT00004
Patent Text Reader

Abstract

The present invention relates to a pavement surface reinforcement method using an MMA-based coating, wherein the method utilizes a high-performance MMA repair material in construction that is applied to concrete and / or asphalt road pavements where cracks and surface wear have occurred, and which has excellent surface friction resistance and wear resistance, while simultaneously ensuring high elasticity, tensile strength, crack-following ability, and slip resistance performance of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a repair material for forming a high-performance MMA-based coating that is applied to the repair of concrete and / or asphalt road pavements where cracks and surface wear have occurred, and to a construction method using the same, which is configured to increase the elasticity and tensile strength of the coating and simultaneously secure crack-following performance and slip resistance performance. Background Technology

[0003] As the summer climate gradually resembles a subtropical climate, localized heavy rainfall and torrential downpours are recurring, and the frequency of heavy snowfall is increasing during the winter. To overcome this, de-icing agents containing salt are frequently sprayed on roads. Due to these climate changes, the occurrence of spalling and potholes on Korea's paved roads is gradually increasing, and road repairs are becoming more frequent to address these issues. Spalling refers to the phenomenon where the surface gradually peels off due to the application of load to areas with surface cracks or inclusions, while a pothole is a hole shaped like a jar.

[0004] Road pavements can be broadly classified into asphalt and concrete pavements. Among these, potholes in asphalt pavements are on the rise due to fatigue caused by heavy rainfall, heavy snowfall, increased heavy cargo, and high-speed vehicle driving. These potholes occur when water penetrates the pavement layer, weakening the adhesion of the asphalt. In the case of concrete pavements, unlike asphalt pavements, spalling mostly occurs at the joints, and the concrete surface also deteriorates due to saltwater, causing the surface to peel off. Furthermore, in the case of bridge pavements, potholes and damage to expansion joints primarily occur due to pavement deterioration. In particular, unlike roads, water and saltwater penetrate the pavement layer in bridge pavements, deteriorating the concrete bridge deck structure and subsequently accelerating pavement deterioration, thereby threatening the safety of the bridge.

[0005] Meanwhile, repair coatings using methyl methacrylate (MMA) resin, which have recently been attracting increasing attention, have excellent acid, alkali, and salt water resistance. They also have the advantage of allowing repair work to be carried out even in winter, as they can be applied at -30°C, unlike ultra-fast curing concrete road repair materials or road repair materials using polyurethane resins. Furthermore, unlike ultra-fast curing concrete road repair materials, they can cure within one hour and develop mechanical strength, making them useful as emergency repair materials. However, general road repair materials using MMA resin have the disadvantage of weak interfacial adhesion with the concrete surface and have limitations due to insufficient durability. To solve these problems with MMA resin road repair materials, unsaturated polyester, epoxy acrylate, and urethane acrylate are sometimes added; however, this presents a problem in that yellowing occurs upon exposure to ultraviolet rays, accelerating aging.

[0006] In addition, while existing coating repair materials using MMA resin have excellent basic performance such as curing speed, adhesion, and weather resistance, they are not sufficient for controlling the propagation of microcracks or for resisting repetitive vibration and impact loads. Furthermore, a silica sand-based composition alone is insufficient to alleviate stress concentration occurring within the coating, and there are limitations such as cracks gradually spreading within the coating and defects like peeling or detachment. In particular, it is difficult to ensure the ductility of the coating, so the coating cannot keep up with the shrinkage and expansion of the concrete, resulting in a problem of vulnerability to cracking.

[0007] Accordingly, there is a need to develop new MMA-based road repair materials that secure physical properties such as anti-slip properties while compensating for the low impact resistance and durability of existing road repair materials using MMA resins. Prior art literature

[0009] Republic of Korea Patent Registration No. 10-1901294 (Publication Date: September 28, 2018) Republic of Korea Patent Registration No. 10-1091774 (Publication Date: December 12, 2011) Republic of Korea Patent Registration No. 10-0966791 (Publication Date: June 29, 2010) Republic of Korea Patent Registration No. 10-1739365 (Publication Date: May 24, 2017) The problem to be solved

[0010] The present invention aims to provide an MMA-based repair material having an optimal composition that improves surface friction resistance, strengthens tensile strength and crack-following ability of the coating film by additionally mixing special beads and friction improvers with silica sand in MMA resin, and provides a structural buffering effect to the entire coating film, while maintaining the unique rapid curing characteristics of MMA-based repair materials and ensuring durability as well as bonding strength between repair material components and bonding strength to the construction surface, and a surface repair and reinforcement method for concrete and / or asphalt road pavements using the same. means of solving the problem

[0012] The present invention, for achieving the above objective, is a pavement surface reinforcement method using an MMA-based coating, comprising: a first step of preparing the surface by removing deteriorated parts and foreign substances from the pavement surface of a road to be repaired; a second step of forming a base layer by applying a primer after performing a protective work on the surface of the prepared area; and a third step of forming a coating by applying a repair material to the surface of the base layer and then leveling it. By performing a process that repairs and reinforces the pavement surface of a road to be repaired. Effects of the invention

[0014] The MMA-based repair material of the present invention is a repair material applied to the surface of concrete and / or asphalt road pavements where cracks and surface wear have occurred. By enhancing the internal stress distribution function of the coating film, it suppresses crack propagation and maintains appropriate elasticity even under repeated loads and shrinkage / expansion of structures. It also enables anti-slip properties without the need for additional aggregate application and reduces defect factors by ensuring adhesion between the substrate and the base material through a uniform thickness after penetration into the substrate. In other words, the repair material using the composition of the present invention is a repair material with high elasticity and tensile strength of the coating film, excellent crack-following properties, and excellent surface friction and wear resistance. Furthermore, due to its fast curing time, the process time is short, and the site can be opened within approximately one hour after application. Additionally, functions such as non-slip, color, design, and antibacterial properties can be selectively incorporated, allowing for the implementation and management of functions that meet the requirements of the site. Specific details for implementing the invention

[0016] The present invention will be described in more detail below.

[0017] The present invention relates to a method for repairing the surface of concrete and / or asphalt structures and a coating composition applied thereto, comprising a process including: a first step of preparing the surface by removing deteriorated parts of the structure to be repaired and removing foreign substances; a second step of forming a base layer by applying a primer after performing a curing operation on the surface of the prepared area; a third step of forming a coating by applying a repair material mixed with an MMA-based coating composition to the surface of the base layer and then leveling it; and a fourth step of forming a non-slip pattern before the coating is gelled.

[0018] The structures subject to repair in Stage 1 include concrete and / or asphalt structures such as road pavements and bridge pavements.

[0019] In addition, the surface preparation of the first step refers to removing foreign substances from the surface of the repair work area. For example, after removing the deteriorated area, the surface of the repair work area is cleaned by removing dust and contaminants through high-pressure washing, vacuum suction, etc.

[0021] The second stage of curing work includes all general curing work, such as masking. Additionally, the primer applied to the formation of the above undercoat layer may be any general primer used in the industry without limitation, and preferably, using a primer containing a methyl methacrylate (MMA)-based compound is advantageous in terms of bonding strength with the coating film formed by the repair material of the third stage.

[0023] The 3-stage MMA-based repair material consists of the following composition.

[0024] The above MMA-based repair material includes a main component, elastic beads, a friction enhancer, and a curing agent.

[0025] The amount of the composition in the above repair material includes 2 to 5 parts by weight of the elastic beads, 2 to 7 parts by weight of the friction improver, and 1 to 5 parts by weight of the curing agent per 100 parts by weight of the main component, and more preferably, may include 4 to 5 parts by weight of the elastic beads, 4 to 7 parts by weight of the friction improver, and 2 to 4 parts by weight of the curing agent per 100 parts by weight of the main component. At this time, if the elastic bead content is less than 2 parts by weight, the anti-slip effect of the repair material film may be insufficient, and if used in excess of 5 parts by weight, the impact resistance of the film may decrease due to excessive use, which may lead to reduced durability. In addition, if the friction improver is less than 2 to 7 parts by weight, the increased anti-slip effect due to the improvement of surface friction resistance of the film caused by its use may be insufficient, and if used in excess of 7 parts by weight, the mechanical properties of the film may be significantly degraded; therefore, it is appropriate to use it within the above range. In addition, if the amount of hardener used is less than 1 part by weight, the curing time of the repair material becomes too long and physical properties such as the tensile strength of the film and the bonding strength to the construction surface may be poor, and if more than 5 parts by weight is used, the curing time of the repair material becomes too fast, resulting in poor workability and an uneven formation of the film surface, so it is appropriate to use it within the above range.

[0027] Next, the subject comprises methyl methacrylate (MMA) resin, acrylic copolymer resin, silica sand, a dispersant, and a diluent, preferably comprising 20 to 32 weight% of MMA resin, 15 to 30 weight% of acrylic copolymer resin, 10 to 15 weight% of silica sand, 4 to 8 weight% of dispersant, and the remaining amount of diluent among 100 weight%, more preferably comprising 27 to 32 weight% of MMA resin, 16 to 25 weight% of acrylic copolymer resin, 10 to 13 weight% of silica sand, 5 to 8 weight% of dispersant, and the remaining amount of diluent among 100 weight%. At this time, if the MMA resin content is less than 20 weight%, there may be a problem with insufficient acid resistance, alkali resistance, salt water resistance, etc., of the coating film formed by the repair material, which is a mixture of the above composition; if used in excess of 30 weight%, there may be a problem with reduced physical properties such as durability of the coating film due to a relative lack of content of other components. Furthermore, if the acrylic copolymer resin in the composition is less than 15 weight%, the effects such as improved impact resistance, durability, and water resistance of the coating film resulting from its use may be insufficient, and using it in excess of 30 weight% is an excessive use and may instead lead to a problem of reduced tensile strength of the coating film. In addition, if the silica sand content in the composition is less than 10 weight%, the durability of the coating film may be insufficient, and using it in excess of 15 weight% may be uneconomical. In addition, if the amount of dispersant used in the composition is less than 4 weight%, the dispersion of silica sand, elastic beads, and / or friction improvers within the coating film may not be uniform, and if used in excess of 8 weight%, the acid resistance, alkali resistance, and / or salt water resistance of the coating film may decrease due to excessive use, so it is appropriate to use it within the above range.

[0029] Among the main components, the aforementioned acrylic copolymer resin, together with the MMA resin, plays a role in improving the durability of the coating film by imparting elasticity and enhancing water resistance.

[0030] And, the acrylic copolymer resin comprises a copolymer obtained by copolymerizing a mixture comprising a hydroxylpropyl acrylate monomer, an aromatic vinyl monomer represented by the following chemical formula 1, 2-hydroxyethyl methacrylate, methacrylic acid, a chain transfer agent, a polymerization initiator, and a solvent, preferably comprising a copolymer obtained by copolymerizing a mixture comprising 43 to 50 wt% of hydroxylpropyl acrylate monomer, 3 to 8 wt% of the aromatic vinyl monomer, 2 to 6 wt% of 2-hydroxyethyl methacrylate, 0.5 to 4.0 wt% of methacrylic acid, 4 to 8 wt% of a chain transfer agent, 0.01 to 0.5 wt% of a polymerization initiator, and the remaining amount of solvent out of a total of 100 wt%, more preferably comprising 47 to 50 wt% of hydroxylpropyl acrylate monomer, the aromatic It may include a copolymer obtained by copolymerizing a mixture comprising 4 to 6 wt% of a vinyl monomer, 3 to 5 wt% of 2-hydroxyethyl methacrylate, 1.0 to 2.5 wt% of methacrylic acid, 5 to 8 wt% of a chain transfer agent, 0.01 to 0.5 wt% of a polymerization initiator, and the remaining amount of solvent out of a total of 100 wt%.

[0031] [Chemical Formula 1]

[0032]

[0033] R of Chemical Formula 1 1 is a hydrogen atom or a C1-C3 alkyl group, preferably a hydrogen atom. And, R of Chemical Formula 1 2 is a C1-C3 alkylene group, preferably a propylene group. In addition, R of Formula 1 3 and R 4 Each is independently a hydrogen atom or a straight-chain C1-C5 alkyl group, preferably a hydrogen atom or a methyl group.

[0034] The chain transfer agent used in the manufacture of acrylic copolymer resin may include one or more selected from CPDA (4-cyano-4-(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid), DDMAT (S-Dodecyl-S'-(α,α'-dimethyl-α"-aceticacid)trithiocarbonate) and CPDB (2-cyano-2-propyl benzodithioate).

[0035] The polymerization initiator used in the manufacture of acrylic copolymer resins is C1~C 10 It may include one or more selected from alkyllithium, sodium alkoxide, potassium alkoxide, and lithium sulfonate, and preferably may include C2 to C5 alkyllithium or lithium sulfonate.

[0036] The solvent used in the manufacture of the acrylic copolymer resin may include one or more selected from n-pentane, n-hexane, n-heptane, isooctane, cyclohexane, toluene, benzene, and xylene, and preferably may include one or more selected from n-hexane, n-heptane, and cyclohexane.

[0038] Among the main components, the above-mentioned dispersant comprises a mixture of sodium polyacrylate-2-sodium carboxymethylcellulose sodium and ethylene glycol, and preferably may comprise a mixture of 20 to 40 weight% sodium polyacrylate-2-sodium carboxymethylcellulose sodium and 60 to 80 weight% ethylene glycol.

[0040] Among the main components, the above silica sand may be applied as general aggregate used for road paving, road paving repair materials, etc., and the type thereof is not specifically limited.

[0041] Among the main components, the above diluent serves to mix the MMA resin, acrylic copolymer resin, dispersant, and silica sand and maintain the appropriate viscosity of the main component, and may include one or more selected from ethyl acetate, butyl acetate, tetrahydrofuran, normal hexane, methanol, ethanol, methylcyclohexanone, methylcyclohexanol, methylbutyl ketone, methyl ethyl ketone, methyl isobutyl ketone, 1-butanol, 2-butanol, cyclohexanone, cyclohexanol, acetone, ethylene glycol monobutyl ether, ethylene glycol monoethyl ether acetate, isopentyl alcohol, and isopropyl alcohol, and preferably, a mixture of normal hexane, butyl acetate, and ethylene glycol monoethyl ether acetate in a weight ratio of 1:0.1 to 0.3:0.1 to 0.2 may be used.

[0043] Next, among MMA-based repair materials, elastic beads enhance the anti-slip effect by imparting frictional resistance performance to the coating film, act as a structural buffer layer for the entire coating film, and enhance impact resistance. They are sheath-core type beads with a particle size of 10 to 100 μm, preferably 20 to 70 μm, and are spherical or elliptical.

[0044] The above-mentioned sheath-core type bead is composed of a sheath portion having an elastomer coating layer formed on all or part of the surface of a core portion composed of glass beads surface-modified with SiH4.

[0045] The above elastomer coating layer comprises a copolyester ether elastomer, and the copolyester ether elastomer may comprise poly(cyclohexylene dipropylene cyclohexane dicarboxylate).

[0047] Next, among the MMA-based repair materials, the friction improver plays a role in improving surface friction resistance and increasing wear resistance of the surface of the coating film formed by the repair material together with elastic beads, and is composed of elliptical or circular elastomer particles with a particle size of 0.5 to 2 mm. In addition, the friction improver is manufactured by feeding a mixture of mixed elastomers; polyethylene wax; and binder resin into an extruder, and then melting, extruding, and cutting.

[0048] The above mixed elastomer may contain styrene-ethylene-propylene-styrene and epichlorohydrin rubber in a weight ratio of 1:0.2 to 0.3. In addition, the content of the mixed elastomer in the mixture may be 40 to 65 weight%, preferably 55 to 65 weight%.

[0049] The above polyethylene wax acts as a lubricant and can be used in an amount of 2 to 5 weight percent, preferably 2 to 4 weight percent, within the mixture.

[0050] And, the binder resin is a resin prepared by reacting a mixture of 40 to 50 wt% of a urethane acrylate oligomer having a weight-average molecular weight of 2000 to 5000, 30 to 40 wt% of n-octyl (meth)acrylate, and the remainder of 100 wt% of diethylene glycol-2-ethylhexyl ether. And, the content of the binder resin is the remainder excluding the mixed elastomer and polyethylene wax from 100 wt%.

[0051] The compression head of the above extruder is equipped with a die capable of controlling the size of the elastomer particles.

[0053] Next, the curing agent in the MMA-based coating composition is a curing accelerating component that serves to initiate the curing of the main component, and comprises benzoyl peroxide powder and a mixed solvent, preferably comprising 10 to 20 weight% of benzoyl peroxide powder and the remaining amount of the mixed solvent from 100 weight%, and more preferably comprising 12 to 18 weight% of benzoyl peroxide powder and the remaining amount of the mixed solvent from 100 weight%.

[0054] In addition, among the curing agent components, the above-mentioned mixed solvent may be used by mixing abietic acid and polyindene in a weight ratio of 1:1 to 2.

[0056] The MMA-based coating composition of the present invention described above may further include one or more additives selected from heat insulation agents, antioxidants, heat stabilizers, leveling agents, hiding power enhancers, pigments, waterproofing enhancers, adhesion enhancers, defoaming agents, antifreeze agents, fillers, and UV stabilizers, within a range that does not degrade the physical properties of the coating formed from the repair material.

[0057] Among the additives, the above defoamer is a water-based silicone defoamer that removes air bubbles within the repair material during application, thereby improving the appearance of the coating film upon drying. If the defoamer is not used, air bubbles may form in the coating film, and conversely, if an excessive amount is used, the appearance of the coating film may become poor, such as with the appearance of craters. A preferred example of the above defoamer is a modified silicone-based defoamer, and more specifically, SanNopco’s Nopco NXZ, Nopco 8034, LNopco NDW, SNDef 154, etc., may be used.

[0058] Among the additives, the above-mentioned heat-insulating agent serves to impart a heat-insulating effect to the coating film, and any paint heat-insulating component used in the industry can be used without limitation; preferably, heat-insulating pigments such as alumina powder or titanium oxide powder can be used.

[0059] In addition, among the additives, if it is desired to additionally impart color to the repair coating film, various organic pigments and / or inorganic pigments may be optionally used. As a preferred example, white pigments such as titanium dioxide, zinc white, zinc sulfide, or lithopone, and yellow pigments such as yellow iron oxide, nickel titanium yellow, chromium titanium yellow, cadmium sulfide, zinc cadmium sulfide, chromium yellow, etc. may be used.

[0060] Among the additives, the leveling agent increases smoothness so that the surface of the coating film is formed homogeneously and uniformly. Leveling agents used in the industry can be used without limitation, and preferably, water-based leveling agents are used.

[0061] Among the additives, the above-mentioned antifreeze may use glycols such as ethylene glycol and propylene glycol.

[0062] In addition, among the additives, the filler plays a role in improving mechanical properties such as the wear resistance of the coating film, and extender pigments such as talc, silica sand, mica, and kaolin can be used.

[0063] Furthermore, among the additives, the aforementioned UV stabilizer prevents the discoloration of the coating film caused by contact with ultraviolet rays and air during or after drying. Since the UV stabilizer is the most effective at controlling long-term discoloration and yellowing, it enables the attainment of good physical properties in terms of weather resistance of the coating film against ultraviolet rays and air. Additionally, UV stabilizers are classified according to their functional roles into UV absorbers, UV blockers, etc., and may include one or more of benzotriazol-based UV blockers, benzophenone-based UV blockers, triazine-based UV blockers, organonickel-based UV blockers, and UV absorbers, but are not limited thereto.

[0065] In the third step of the construction method of the present invention, since the repair material prepared as a film composition is a fast-curing repair material, the film composition is rapidly mixed in a certain ratio to prepare the repair material. Then, after applying the repair material appropriately to the upper surface of the undercoat layer, a film is formed by leveling it to a minimum thickness of 1 mm or more.

[0067] Next, in order to further impart non-slip properties to the coating film, the fourth step of the construction method of the present invention may form a non-slip pattern before the coating film gels. As a preferred example of forming a non-slip pattern, a non-slip pattern may be formed on the surface of the coating film using a roller. At this time, a small amount of silica sand may be evenly sprinkled on the surface of the coating film before the coating film gels and before the non-slip pattern is formed, and then the non-slip pattern may be formed.

[0069] After performing Step 4, if there is any protective work done before performing Step 2, remove it before the coating is completely cured, and once the coating is fully cured, inspect the surface of the construction and the surface of the structure.

[0071] The present invention will be explained in more detail below through examples, but the following examples are not intended to limit the scope of the invention and should be interpreted as being for the purpose of aiding understanding of the invention.

[0072] [Example]

[0073] Example 1: Preparation of MMA-based coating composition and repair material

[0074] (1) Subject manufacturing

[0075] A main component was prepared by mixing 29.5 wt% MMA resin, 23.3 wt% acrylic copolymer resin, 17.9 wt% silica sand, 3.9 wt% dispersant, and the remaining amount of diluent out of 100 wt%.

[0076] At this time, the acrylic copolymer resin is a copolymer produced by copolymerizing a mixture of 48.6 wt% hydroxylpropyl acrylate monomer, 4.7 wt% aromatic vinyl monomer represented by chemical formula 1-1, 3.8 wt% 2-hydroxyethyl methacrylate, 1.7 wt% methacrylic acid, 6.2 wt% CPDB (2-cyano-2-propyl benzodithioate) as a chain transfer agent, 0.22 wt% lithium sulfonate as a polymerization initiator, and the remaining amount of solvent (n-hexane) out of the total 100 wt%.

[0077] [Chemical Formula 1-1]

[0078]

[0079] R of chemical formula 1-1 1 is a hydrogen atom, and R 2 is a propylene group, and R 3 and R 4 Each is a methyl group.

[0080] And, the above dispersant used a mixture of 28.2% by weight of sodium polyacrylate-2-sodium carboxymethylcellulose sodium and the remaining amount of ethylene glycol out of 100% by weight.

[0081] In addition, the above diluent used was a mixture of normal hexane, butyl acetate, and ethylene glycol monoethyl ether acetate in a weight ratio of 1:0.15:0.11.

[0082] (2) Preparation of curing agent

[0083] A curing agent was prepared by mixing 13.5 wt% of benzoyl peroxide powder and the remaining amount of a mixed solvent from 100 wt%.

[0084] At this time, the above-mentioned mixed solvent used was a mixture of abietic acid and polyindene in a weight ratio of 1:1.4.

[0085] (3) Manufacturing of repair materials

[0086] A repair material was prepared by stirring 4.2 parts by weight of elastic beads, 5.5 parts by weight of friction improver, and 4.1 parts by weight of the curing agent with respect to 100 parts by weight of the above-mentioned subject.

[0087] The above elastic beads are spherical sheath-core type beads with a particle size in the range of 40 to 70 μm, and were used in which poly(cyclohexylene dipropylene cyclohexane dicarboxylate) was coated on the surface of a glass bead (core part) surface-modified with SiH4 using a spray method, and then heat-treated to form a coating layer (sheath part).

[0088] The friction improver is an elastomer particle with a particle size of approximately 1.4 to 1.6 mm, manufactured by mixing 57.4 wt% of a mixed elastomer comprising styrene-ethylene-propylene-styrene and epichlorohydrin rubber in a weight ratio of 1:0.23, 2.6 wt% of polyethylene wax, and the remainder of 100 wt% of a binder resin, feeding the mixture into an extruder equipped with a die in the extrusion head, followed by melting, extrusion, and cutting. The binder resin is a resin prepared by reacting a mixed resin comprising 44.5 wt% of a urethane acrylate oligomer with a weight-average molecular weight of 3800 to 4000, 31.6 wt% of n-octyl (meth)acrylate, and the remainder of 100 wt% of diethylene glycol-2-ethylhexyl ether.

[0090] Examples 2 to 4 and Comparative Examples 1 to 2

[0091] Examples 2 to 4 and Comparative Examples 1 to 2 were carried out, respectively, by preparing a repair material using the same composition as in Example 1 above, but with the composition having the content as shown in Table 1 below.

[0092] In the case of Example 4, a mixture of 29.5 wt% MMA resin, 23.3 wt% acrylic copolymer resin, 17.9 wt% silica sand, 3.9 wt% dispersant, and the remaining amount of diluent out of 100 wt% was used as the main component.

[0094] Comparative Example 3

[0095] A main component was prepared by mixing 52.7 wt% MMA resin, 18.2 wt% silica sand, 4.0 wt% dispersant, and the remaining amount of diluent out of 100 wt%, without using an acrylic copolymer resin in the main component.

[0096] division Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 subject 100 100 100 100 100 100 100 elastic beads 4.2 5.0 3.2 6.0 - 6.0 4.2 Friction enhancer 5.5 6.8 3.3 0 - 8.0 5.5 hardener 4.1 4.1 4.1 3.5 4.1 4.1 4.1

[0098] Experimental Example 1: Measurement of Physical Properties

[0099] The tensile strength, elongation, adhesion strength, and slip resistance (BPN) of the repair materials prepared in the above examples and comparative examples were measured, and the results are shown in Table 2 below.

[0100] A concrete specimen measuring 1m in width and 1m in length was prepared by applying a repair material to a thickness of 3mm and curing it to form a film, and the following physical properties were measured.

[0101] The adhesion strength of the asphalt was measured on an asphalt specimen prepared by applying a repair material to a thickness of 3 mm on an asphalt specimen measuring 1 m in width and 1 m in length, and then curing it to form a film.

[0102] (1) Measurement of tensile strength, elongation, and maximum elastic modulus

[0103] Tensile strength, elongation, and maximum elastic modulus were measured using test specimens prepared in a separate mold according to ASTM D 638 (Standard Test Method for Tensile Properties of Plastics). If the tensile strength is 14 to 35 MPa and the elongation is 30 to 70%, the properties are suitable for use as a repair material for road pavements.

[0104] (2) Adhesion strength (adhesion strength)

[0105] The adhesion strength of the repair material film to concrete and asphalt substrates was measured according to ASTM D4541, and if the adhesion strength to a concrete substrate is 1.7 MPa or higher, it is suitable for use as a road pavement repair material, and if the adhesion strength to an asphalt substrate is 1.0 MPa or higher, it is suitable for use as a road pavement repair material.

[0106] (3) Measurement of wear rate and slip resistance (BPN)

[0107] The wear rate (%) and slip resistance (BPN) were measured according to the Road Association standards, and if the wear rate was 1.0% or less and the slip resistance was 55 BPN or more, it was evaluated as acceptable as a road repair material.

[0108] (4) Measurement of freeze-thaw resistance

[0109] A freeze-thaw resistance test was conducted according to the method specified in KS F 2456, and the durability index was indicated. Freeze-thaw refers to the freezing and thawing of moisture absorbed by concrete; if freeze-thaw cycles are repeated, fine cracks occur in the concrete structure, leading to a decrease in durability.

[0110] division Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength (Mpa) 27.9 28.8 27.7 28.2 28.6 21.4 20.4 Growth rate (%) 6.7 7.2 6.2 6.9 7.3 5.0 5.8 Maximum elastic modulus (Mpa) 76.9 75.3 73.5 77.8 69.7 73.3 67.5 Concrete bond strength 1.7pa or higher 3.7 3.6 3.9 3.8 4.0 1.9 3.6 Asphalt adhesion strength 1.0 MPa or higher 2.2 2.1 2.4 2.3 2.6 1.4 2.0 Wear rate (%) 1.0% or less 0.1 0.1 0.1 0.2 0.8 0.1 1.4 Slip resistance (BPN) 55 BPN or higher 91 95 89 87 53 97 86 Durability Index 100 102 99 99 89 105 79

[0111] Looking at the physical property measurement results in Table 2 above, it was confirmed that the coating film formed from the repair material prepared in Examples 1 to 4 had an elasticity of 25.0 MPa or higher, an elongation of 6.0% or higher, and an elastic modulus of 73.0 MPa or higher, indicating excellent elasticity and superior shock absorption. In addition, it was confirmed that the film exhibited excellent adhesion strength to concrete and asphalt, as well as low wear rate and high freeze-thaw resistance (durability index). Furthermore, it was confirmed that the film possessed very high non-slip properties with a slip resistance of 70 BPN or higher.

[0112] In addition, Example 4, which did not use a friction enhancer, showed overall excellent physical property measurement results, but compared to Examples 1 to 3, which used a friction enhancer, it showed relatively lower slip resistance values.

[0113] In addition, in the case of Comparative Example 1, which did not use elastic beads and friction resistance agents, compared to Examples 1 and 2, there was a problem of poor slip resistance and a relatively large increase in the wear rate.

[0114] In addition, in the case of Comparative Example 2, which used an excessive amount of elastic beads and friction improvers, other physical properties were excellent, but compared to Examples 1 to 3, there was a problem with a significant decrease in adhesion strength.

[0115] In addition, within the subject components It was confirmed that the coating film formed from the repair material of Comparative Example 3, which was prepared using a main component that did not use an acrylic copolymer resin, had significantly lower tensile strength and elongation, significantly increased wear rate, and lower durability index compared to Examples 1 to 3. Through this, it was confirmed that by using an acrylic copolymer resin in the main component, not only the mechanical properties of the coating film but also its durability can be significantly increased.

[0117] Preparation Example 1: Repair and reinforcement work on deteriorated roads

[0118] The repair material prepared in Example 1 was used to repair and reinforce an actual deteriorated road pavement surface.

[0119] After checking the condition of the deteriorated road surface and proceeding with repairs and cleaning to prepare the surface, road lanes and other areas were protected with masking tape to prevent repair material from adhering to surfaces other than the construction surface.

[0120] Then, an MMA resin-based primer was applied to the construction surface and cured to form a primer layer.

[0121] After preparing a repair material by rapidly mixing the composition of Example 1 with an electric mixer, it was sufficiently applied to the surface of the undercoat layer and then flattened with a trowel to form a film of about 2.0 to 2.5 mm.

[0122] Before the coating gelled, it was applied by rolling it with a roller to make the surface non-slip.

[0123] Then, the protective coverings, such as the masking tape used for protection work, were removed.

[0124] In addition, the applied coating surface was inspected for any abnormalities (such as stickiness and coating condition), and repair and reinforcement work on the deteriorated road was completed.

[0126] The above description is merely an example of an embodiment of the present invention, and those skilled in the art may implement it in modified forms without departing from the essential characteristics of the present invention. Accordingly, the scope of the present invention should not be limited to the aforementioned embodiment but should be interpreted to include various embodiments within the scope equivalent to that described in the claims.

Claims

Claim 1 Step 1: Surface preparation by removing deteriorated areas and foreign substances from the road pavement surface to be repaired; Step 2: Protective work on the surface of the prepared area, followed by the application of a primer to form a base layer; A process comprising: Step 3, forming a coating film by applying a repair material to the surface of a primer layer and then leveling it; and Step 4, forming a non-slip pattern before the coating film of Step 3 gels; wherein the repair material comprises 2 to 5 parts by weight of elastic beads, 2 to 7 parts by weight of a friction improver, and 1 to 6 parts by weight of a curing agent, based on 100 parts by weight of a main component comprising methyl methacrylate (MMA) resin, an acrylic copolymer resin, silica sand, a dispersant, and a diluent; and wherein the acrylic copolymer resin comprises 43 to 50 wt% of hydroxylpropyl acrylate monomer, 3 to 8 wt% of an aromatic vinyl monomer represented by the following chemical formula 1, 2 to 6 wt% of 2-hydroxyethyl methacrylate, 0.5 to 4.0 wt% of methacrylic acid, 4 to 8 wt% of a chain transfer agent, and polymerization Initiator 0.01 ~ 0.A pavement surface reinforcement method using an MMA-based coating film with improved surface friction resistance and wear resistance, comprising a copolymer formed by copolymerizing a mixture containing 5 wt% of a solvent and the remaining amount of solvent out of a total of 100 wt%, wherein the chain transfer agent comprises one or more selected from CPDA (4-cyano-4-(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid), DDMAT (S-Dodecyl-S'-(α,α'-dimethyl-α"-aceticacid)trithiocarbonate), and CPDB (2-cyano-2-propyl benzodithioate), wherein the dispersant comprises a mixture of 20 to 40 wt% sodium polyacrylate-2-sodium carboxymethylcellulose sodium and 60 to 80 wt% ethylene glycol, and wherein the elastic bead is a shes-core type bead in which an elastomer coating layer is formed on all or part of the surface of a glass bead surface-modified with SiH4; [Chemical Formula 1]. R of Chemical Formula 1 1 is a hydrogen atom or a C1–C3 alkyl group, and R 2 is a C1–C3 alkylene group, and R 3 and R 4 Each is independently a hydrogen atom or a straight-chain C1-C5 alkyl group. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 A paving surface reinforcement method using an MMA-based coating with improved surface friction resistance and wear resistance according to claim 1, characterized in that the subject comprises 20 to 30 weight% of methyl methacrylate (MMA) resin, 15 to 30 weight% of acrylic copolymer resin, 10 to 15 weight% of silica sand, 4 to 8 weight% of dispersant, and the remaining amount of diluent among 100 weight%.

Citation Information

Patent Citations

  • MMA resin suture material for repairing crack of road and method for repairing crack of road

    KR101045340B1

  • The composition of concrete crack repair material, Concrete crack repair material containing the same and Repairing method of concrete structure using the same

    KR102493275B1

  • Pour concrete surface coating method using epoxy paint for concrete and inorganic composition

    KR102743867B1