Manufacturing Method of Anode Slurry, Manufacturing Method of Anode, and Anode Slurry Composition
The use of an aqueous polyamic acid solution in manufacturing cathode slurries addresses environmental and stability issues, achieving performance comparable to organic solvent-based methods with improved stability and lifespan.
Patent Information
- Application Number
- KR1020240025404
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-02-22
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2044-02-22
AI Technical Summary
The use of organic solvents in manufacturing cathode slurries for lithium-ion batteries leads to environmental issues, low productivity, and poor storage stability due to moisture vulnerability, while silicon anode materials face challenges with volume expansion affecting charge-discharge stability.
A method using an aqueous polyamic acid solution as a solvent to prepare a cathode slurry, incorporating a two-dimensional silicon material and a polyimide binder precursor, which forms polyimide through high-temperature heat treatment, enhancing stability and cycle characteristics.
The aqueous-based cathode slurry provides environmental friendliness, improved storage stability, and equivalent performance to conventional organic solvent-based slurries, with enhanced charge-discharge stability and extended battery life.
Smart Images

Figure 112024020385301-PAT00007_ABST
Abstract
Description
Technology Field
[0001] The present application relates to a method for manufacturing a cathode slurry, a method for manufacturing a cathode, and a cathode slurry composition. Background Technology
[0002] Lithium-ion batteries are lightweight, have a small volume, and high energy density. They are widely used in mobile devices, digital cameras, laptops, etc. While graphite (~372 mAh / g) is widely used as the anode for these lithium-ion batteries, silicon anode materials are promising as next-generation anode materials due to their high theoretical capacity of 4200 mAh / g (see Korean Patent No. 10-2006-0061064, etc.).
[0003] However, there is a problem in that the volume expansion of silicon during lithium storage is very severe, making it difficult to induce charge-discharge stability of the electrode.
[0004] Recently, there have been attempts to use polyimide-based binders to improve the lifespan and cycle characteristics of the anode by increasing the charge-discharge stability of silicon anode materials.
[0005] A specific method for manufacturing a cathode was known in which a silicon cathode material and polyamic acid were mixed in an organic solvent to prepare a cathode slurry, the prepared cathode slurry was coated (or cast) onto a current collector, and the cathode was manufactured through a firing process.
[0006] During the calcination process, polyamic acid was imidized into polyimide and acted as a binder that bonded with the silicon anode material. However, in the case of anode slurries prepared using such organic solvents, there were environmental issues associated with the organic solvents, low productivity due to the high cost and complexity of the process for handling the organic solvents, and also disadvantages such as poor storage stability due to vulnerability to moisture. The problem to be solved
[0007] The present application aims to solve the problem of providing a method for manufacturing a cathode slurry using an aqueous polyamic acid solution in order to achieve an equivalent level of effect while compensating for the disadvantages of cathode slurries manufactured using conventional organic solvents. means of solving the problem
[0008] The present application relates to a method for manufacturing a cathode slurry using water as a solvent. The cathode slurry can be applied to a cathode for a lithium-ion battery.
[0009] Since the cathode slurry according to the present application is manufactured in an aqueous environment, it is environmentally friendly compared to cathode slurries manufactured in an oily environment, and has excellent storage stability due to improved moisture vulnerability, and can also exhibit an effect equivalent to that of conventional cathode slurries manufactured in an oily environment when manufacturing a cathode.
[0010] Specifically, the method for manufacturing the cathode slurry comprises the steps of: preparing an aqueous polyamic acid salt solution; and preparing a cathode slurry by mixing the aqueous polyamic acid salt solution, a conductive material, and a two-dimensional silicon material (2DSi).
[0011] The above polyamic acid salt can form a salt with a water-based catalyst or an organic base.
[0012] The above polyamic acid salt may be a polyimide binder precursor that is imidized into polyimide through a calcination step involving high-temperature heat treatment during cathode manufacturing and combined with a two-dimensional silicon material (2DSi).
[0013] Polyimide binders can ensure battery life stability by minimizing damage to the negative electrode even if the volume expands while lithium is stored during the charging and discharging process of lithium-ion batteries.
[0014] In addition, the polyimide binder can improve the lifespan and cycle characteristics of the cathode by increasing contact between materials through the sintering effect caused by high-temperature sintering.
[0015] The above two-dimensional silicon material (2DSi) may be a two-dimensional siloxene (2D-Siloxene). The two-dimensional siloxene may have Si6H3(OH)3 as a repeating unit. When manufacturing the cathode, the carboxyl group (COO-) of the polyamic acid salt and the hydroxyl group (OH) of the siloxene may be combined through a condensation reaction after undergoing a calcination step.
[0016] In addition, the conductive material may include one or more selected materials such as SUPER P, SUPER C, Ketjen Black, Acethylene Black, Carbon Black, and Conducting Graphite, and preferably may be SUPER P.
[0017] FIGS. 1 to 3 are drawings for explaining the structure of a polyamic acid salt, the structure of a two-dimensional silicon material, and the bonding structure of the polyamic acid salt and the two-dimensional silicon material, respectively.
[0018] The structures illustrated in FIGS. 1 to 3 are merely examples to aid in understanding the present invention, and the present invention is not limited by them.
[0019] Referring to the drawings, in the case of a polyamic acid salt, it has a polymerization unit derived from a dianhydride monomer and a diamine monomer, and the polymerization unit may include a first polymerization unit that combines with a two-dimensional silicone material through a calcination step and a second polymerization unit that is imidized into a polyimide.
[0020] In addition, during the manufacturing of the cathode, after undergoing a calcination step, some of the hydroxyl groups (OH) of the siloxene are covalently bonded with the carboxyl groups (COO-) of the polyamic acid salt through a condensation reaction, and other hydroxyl groups (OH) of the siloxene can be covalently bonded to a current collector (e.g., a copper current collector).
[0021] The cathode slurry according to the present invention may have a polyamic acid salt, a two-dimensional silicon material, and a conductive material dispersed in water.
[0022] The cathode slurry according to the present invention has excellent storage stability even when exposed to moisture because each component exists in a form dispersed in water. Additionally, when manufacturing the cathode, the two-dimensional silicon material and the polyamic acid salt are combined during the calcination step, thereby improving the charge / discharge stability of the lithium-ion battery and the lifespan and cycle characteristics of the cathode.
[0023] In one example, an aqueous solution of a polyamic acid salt according to the present invention can be prepared by an aqueous polymerization method or a water-soluble method.
[0024] Water-based polymerization methods and water-soluble methods are distinguished by the difference in the polymerization reaction environment of polyamic acids. For example, in water-based polymerization, polyamic acids undergo polymerization in an aqueous environment, whereas in water-soluble polymerization, polyamic acids can undergo polymerization in an oily environment.
[0025] The aqueous polymerization method proceeds in one step, and the polymerization reaction of the polyamic acid and chlorination can occur simultaneously in water. The water-soluble method proceeds in two steps, and after the polyamic acid is polymerized in an organic solvent, chlorination can occur in water.
[0026] Specifically, the above-described aqueous polymerization method may include the steps of preparing an aqueous solution containing water and an aqueous catalyst, and polymerizing a diamine monomer and a dianhydride monomer in the aqueous solution to prepare an aqueous polyamic acid salt solution. The above-described aqueous catalyst may be an aqueous catalyst for polyamic acid polymerization and may be an organic base that forms a salt with the polyamic acid.
[0027] The above polymerization reaction can be carried out for 10 to 40 hours at a temperature of 30 to 100°C.
[0028] Additionally, the above water-soluble method may include the step of preparing a polyamic acid by polymerizing a diamine monomer and a dianhydride monomer in an organic solvent; and the step of preparing an aqueous polyamic acid salt solution by mixing the polyamic acid, water, and an organic base.
[0029] The cathode slurry according to the present invention comprises a polyamic acid salt produced from an aqueous polymerization method or a water-soluble method, and thus is environmentally friendly, has excellent storage stability, and can expect an equivalent level of effect compared to cathode slurries produced using conventional organic solvents.
[0030] Meanwhile, in the case of polyamic acid salts, in order to achieve an effect equivalent to that of conventional cathode slurries, water-based catalysts, organic bases, dianhydride monomers, and diamine monomers can be selectively used.
[0031] For example, the above-mentioned aqueous catalyst may include a pyridine-based compound or an imidazole-based compound.
[0032] In addition, organic bases may include pyridine-based compounds, imidazole-based compounds, alcoholamine-based compounds, or alkylamine-based compounds.
[0033] Water-based catalysts and organic bases, pyridine-based compounds and imidazole-based compounds, can overlap with each other.
[0034] The above pyridine-based compound or imidazole-based compound may be an aqueous catalyst for polyamic acid polymerization and an organic base that forms a salt with the polyamic acid, and accordingly, the types of aqueous catalyst and organic catalyst may overlap. Specifically, the above pyridine-based compound may have at least one electron donor group (non-covalent electron pair) and, for example, may satisfy Chemical Formula 1 below.
[0035] [Chemical Formula 1]
[0036]
[0037] In the above chemical formula 1, at least one of R1 to R3 is an alkylamine group having 1 to 4 carbon atoms, a hydroxyl group, an alkoxy group having 1 to 4 carbon atoms, a thiol group, a thiol ether group having 1 to 4 carbon atoms, an alkyl group having 1 to 4 carbon atoms, or a heterocyclic group.
[0038] Examples of pyridine compounds satisfying Chemical Formula 1 above include 4-(methylamino)pyridine, 4-(dimethylamino)pyridine, 2-(methylamino)pyridine, 2-(dimethylamino)pyridine, 3,4-dimethylpyridine, 2-hydroxypyridine, 4-hydroxypyridine, 4-methoxypyridine, 2-methoxypyridine, 2,6-dimethoxypyridine, 2-ethoxypyridine, 4-mercaptopyridine, 2-mercaptopyridine, 4-(methylthio)pyridine, 2-(methylthio)pyridine), 4-methylpyridine, 2-methylpyridine, 4-ethylpyridine, 2-ethylpyridine, 4-propylpyridine, 2,4,6-trimethylpyridine, It may be 4-piperidinopyridine, 4-mornopolinopyridine, or 4-pyrrolidinopyridine.
[0039] The above pyridine-based compound can satisfy the following chemical formula 2.
[0040] [Chemical Formula 2]
[0041]
[0042] In the above chemical formula 2, at least one of R4 and R5 is a monoalkylamino group having 1 to 4 carbon atoms, a dialkylamino group having 1 to 4 carbon atoms, a piperidino group, a morpholino group, or a pyrrolidino group.
[0043] In a specific embodiment of the present application, examples of pyridine compounds satisfying Formula 2 may be 4-(dimethylamino)pyridine, 2-(dimethylamino)pyridine, 4-(methylamino)pyridine, 4-piperidinopyridine, 4-mornopolinopyridine, or 4-pyrrolidinopyridine.
[0044] In the case of a pyridine-based compound satisfying the above chemical formulas 1 and / or 2, it acts as a reaction promoter during polyamic acid polymerization, thereby enabling control of the weight-average molecular weight of the polyamic acid.
[0045] The above imidazole-based compound may include a compound with a weight-average molecular weight in the range of 50 to 200 g / mol, 60 to 180 g / mol, 80 to 150 g / mol, or 90 to 120 g / mol. For example, the above imidazole-based compound may be imidazole, N-methylimidazole, 2-methylimidazole, 4-methylimidazole, 1-ethylimidazole, 1,2-dimethylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, benzimidazole, isoquinoline, 2-ethyl-4-methyl-1H-imidazole-1-propanetrile, or 1-benzyl-2-methylimidazole, but is not limited thereto.
[0046] The above alcoholamine-based compound may include a compound with a weight-average molecular weight in the range of 50 to 200 g / mol, 60 to 180 g / mol, 70 to 150 g / mol, or 80 to 110 g / mol. For example, the above alcoholamine-based compound may be N,N-dimethylethanolamine (DMEA), N-methyldiethanolamine (MDEA), triethanolamine (TEOA), N,N-diethylethanolamine (DEEA), triisopropanolamine, 3-dimethylamino-1-propanol, diethanolamine (DEA), diethanolisopropanolamine (DEIPA), 3-diethylamino-1-propanol, N,N-diethylisopropanolamine, or 2-(dimethylamino)-2-methyl-1-propanol (DMAMP-80), but is not limited thereto.
[0047] The above alkylamine compounds may include compounds with a weight-average molecular weight in the range of 50 to 200 g / mol, 60 to 180 g / mol, 80 to 150 g / mol, or 90 to 120 g / mol. For example, the alkylamine compounds may be triethylamine (TEA), diethylamine, propylamine, dipropylamine, hexylamine, cyclohexylamine, N,N-diisopropylamine (DIPA), or N,N-dimethylethylamine, but are not limited thereto.
[0048] In one example, the dianhydride monomer may include at least one compound represented by the following chemical formula 3.
[0049] [Chemical Formula 3]
[0050]
[0051] In the above chemical formula 3, M comprises at least one from the group comprising alkylene group, alkylidene group, carbonyl group, alkylcarbonyl group, alkoxy group, and sulfonyl group, and M is substituted or unsubstituted with at least one from the group comprising fluorine and alkyl group.
[0052] The above M may be an alkylene group having at least one fluorine-substituted alkyl group as a substituent.
[0053] As an example, at least one fluorine-substituted alkyl group having 1 to 6 carbon atoms may be a perfluoroalkyl group, specifically, a perfluoromethyl group. In another example, the dianhydride monomer component may include at least one dianhydride monomer substituted with at least one fluorine.
[0054] In this specification, the term “alkyl group” may mean an alkyl group having 1 to 30 carbon atoms, 1 to 25 carbon atoms, 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, unless specifically defined otherwise. The alkyl group may have a straight-chain, branched-chain, or cyclic structure and may optionally be substituted by one or more substituents. Examples of such substituents include polar functional groups.
[0055] In this specification, the term “alkenyl group” may mean an alkenyl group having 1 to 30 carbon atoms, 1 to 25 carbon atoms, 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, unless specifically otherwise defined. The alkenyl group may have a straight-chain, branched-chain, or cyclic structure and may optionally be substituted by one or more substituents. Examples of such substituents include polar functional groups.
[0056] In this specification, the term “alkynyl group” may mean an alkynyl group having 1 to 30 carbon atoms, 1 to 25 carbon atoms, 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, unless specifically otherwise defined. The alkynyl group may have a straight-chain, branched-chain, or cyclic structure and may optionally be substituted by one or more substituents. Examples of such substituents include polar functional groups.
[0057] In this specification, the term “alkylene group” may mean an alkylene group having 2 to 30 carbon atoms, 2 to 25 carbon atoms, 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 10 carbon atoms, or 2 to 8 carbon atoms, unless specifically defined otherwise. The alkylene group may have a straight-chain, branched-chain, or cyclic structure and may optionally be substituted by one or more substituents. Examples of such substituents include polar functional groups.
[0058] In this specification, the term “alkylidene group” may mean an alkylidene group having 2 to 30 carbon atoms, 2 to 25 carbon atoms, 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 10 carbon atoms, or 2 to 8 carbon atoms, unless specifically defined otherwise. The alkylidene group may have a straight-chain, branched-chain, or cyclic structure and may optionally be substituted by one or more substituents. Examples of such substituents include polar functional groups.
[0059] The aromatic tetracarboxylic dianhydrides satisfying the above chemical formula 3 are pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), oxydiphthalic dianhydride (ODPA), diphenylsulfone-3,4,3',4'-tetracarboxylic dianhydride (DSDA), bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, and 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA). Bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, p-phenylenebis(trimellitic monoester acid anhydride), p-biphenylenebis(trimellitic monoester acid anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane Examples include dianhydride (BPADA), 2,3,6,7-naphthalene tetracarboxylic acid dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, and 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianhydride (6-FDA).
[0060] In order to achieve an effect equivalent to that of a cathode slurry prepared using conventional organic solvents, it may be preferable that the compound satisfying Formula 3 comprises pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), or 4,4'-(2,2-hexafluoroisopropylidene)diphthalic dianhydride (6-FDA).
[0061] The above diamine monomer may be an aromatic diamine having at least one benzene ring.
[0062] The above diamine monomer is an aromatic diamine, and examples can be given by classifying it as follows.
[0063] 1) A diamine having one benzene nucleus in its structure, such as 1,4-diaminobenzene (or paraphenylenediamine, p-PDA), 1,3-diaminobenzene, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (or DABA), etc., a diamine having a relatively rigid structure;
[0064] 2) Diaminodiphenyl ethers such as 4,4'-diaminodiphenyl ether (or oxydianiline, ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (methylenediamine), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl)sulfide, 4,4'-diaminobenzanilide, 3,3'-dichlorobenzidine, 3,3'-Dimethylbenzidine (or o-tolidine), 2,2'-Dimethylbenzidine (or m-tolidine), 3,3'-Dimethoxybenzidine, 2,2'-Dimethoxybenzidine, 3,3'-Diaminodiphenyl ether, 3,4'-Diaminodiphenyl ether, 4,4'-Diaminodiphenyl ether, 3,3'-Diaminodiphenyl sulfide, 3,4'-Diaminodiphenyl sulfide, 4,4'-Diaminodiphenyl sulfide, 3,3'-Diaminodiphenylsulfone, 3,4'-Diaminodiphenylsulfone, 4,4'-Diaminodiphenylsulfone, 3,3'-Diaminobenzophenone, 4,4'-Diaminobenzophenone, 3,3'-Diamino-4,4'-Dichlorobenzophenone, Diamines having two benzene nuclei in their structure, such as 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenylsulfoxide, 3,4'-diaminodiphenylsulfoxide, 4,4'-diaminodiphenylsulfoxide, etc.;
[0065] 3) 1,3-Bis(3-aminophenyl)benzene, 1,3-Bis(4-aminophenyl)benzene, 1,4-Bis(3-aminophenyl)benzene, 1,4-Bis(4-aminophenyl)benzene, 1,3-Bis(4-aminophenoxy)benzene, 1,4-Bis(3-aminophenoxy)benzene (or TPE-Q), 1,4-Bis(4-aminophenoxy)benzene (or TPE-Q), 1,3-Bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-Diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-Diamino-4,4'-Di(4-phenylphenoxy)benzophenone, 1,3-Bis(3-aminophenylsulfide)benzene, 1,3-Bis(4-aminophenylsulfide)benzene, A diamine having three benzene nuclei in its structure, such as 1,4-bis(4-aminophenylsulfide)benzene, 1,3-bis(3-aminophenylsulfone)benzene, 1,3-bis(4-aminophenylsulfone)benzene, 1,4-bis(4-aminophenylsulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, etc.;
[0066] 4) 3,3'-Bis(3-aminophenoxy)biphenyl, 3,3'-Bis(4-aminophenoxy)biphenyl, 4,4'-Bis(3-aminophenoxy)biphenyl, 4,4'-Bis(4-aminophenoxy)biphenyl, Bis[3-(3-aminophenoxy)phenyl]ether, Bis[3-(4-aminophenoxy)phenyl]ether, Bis[4-(3-aminophenoxy)phenyl]ether, Bis[4-(4-aminophenoxy)phenyl]ether, Bis[3-(3-aminophenoxy)phenyl]ketone, Bis[3-(4-aminophenoxy)phenyl]ketone, Bis[4-(3-aminophenoxy)phenyl]ketone, Bis[4-(4-aminophenoxy)phenyl]ketone, Bis[3-(3-aminophenoxy)phenyl]sulfide, Bis[3-(4-aminophenoxy)phenyl]sulfide, Bis[4-(3-aminophenoxy)phenyl]sulfide, Bis[4-(4-aminophenoxy)phenyl]sulfide, Bis[3-(3-aminophenoxy)phenyl]sulfone, Bis[3-(4-aminophenoxy)phenyl]sulfone, Bis[4-(3-aminophenoxy)phenyl]sulfone, Bis[4-(4-aminophenoxy)phenyl]sulfone, Bis[3-(3-aminophenoxy)phenyl]sulfone, Bis[3-(3-aminophenoxy)phenyl]methane, Bis[3-(4-aminophenoxy)phenyl]methane, Bis[4-(3-aminophenoxy)phenyl]methane, Bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, A diamine having four benzene nuclei in its structure, such as 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, etc.
[0067] In order to achieve an effect equivalent to that of a cathode slurry prepared using conventional organic solvents, it may be preferable for the diamine monomer to include 4,4'-diaminodiphenyl ether (ODA), 1,4-diaminobenzene (PPD), or 2,2-dimethylbenzidine (m-TB).
[0068] In addition, in order to achieve an effect equivalent to that of a cathode slurry manufactured using conventional organic solvents, the content of the polyamic acid salt, the active material for the cathode, and the conductive material must be controlled to the following ranges.
[0069] For example, the content of the polyamymcin salt may be in the range of 0.5 to 15 wt%, 1 to 15 wt%, 2 to 13 wt%, 3 to 12 wt%, or 5 to 10 wt% with respect to the total weight of the solids of the cathode slurry.
[0070] The content of the above-mentioned active material for the cathode may be in the range of 65 to 85 wt%, 68 to 82 wt%, or 70 to 80 wt% with respect to the total weight of the solids of the cathode slurry.
[0071] In addition, the content of the conductive material may be within the range of 5 to 30 wt%, 10 to 25 wt%, or 10 to 20 wt% with respect to the total weight of the solids of the cathode slurry.
[0072] Preferably, the content ratio of the active material for the cathode, the polyamic acid salt, and the conductive material may be 70:10:20.
[0073] In another example, the method for manufacturing a cathode slurry according to the present invention may further include the step of controlling the solid content of the cathode slurry to a range of 9 to 25 wt%, 9 to 23 wt%, 9 to 21 wt%, 9 to 19 wt%, 9 to 17 wt%, 9.5 to 25 wt%, 9.5 to 23 wt%, 9.5 to 21 wt%, 9.5 to 19 wt%, or 9.5 to 17 wt%. By controlling the solid content of the cathode slurry to the above range, uniform coating (or casting) on the current collector is possible during cathode manufacturing.
[0075] The present application also relates to a method for manufacturing a cathode. The cathode may be applied to a lithium-ion battery.
[0076] The method for manufacturing the above-described cathode includes the step of applying a cathode slurry manufactured by the above-described manufacturing method onto a current collector, and the step of firing the current collector on which the cathode slurry is applied.
[0077] The above current collector may be a metal current collector, for example, copper, but is not limited thereto.
[0078] In the calcination step, the polyamic acid salt can be bonded to the two-dimensional silicon material (2DSi) as it is imidized into polyimide.
[0079] The above-mentioned firing step involves high-temperature heat treatment, and for example, the temperature of the above-mentioned firing step may be greater than 120℃ and less than or equal to 500℃.
[0080] The cathode manufactured by the above method has the advantages of excellent charge / discharge performance, lifespan, and cycle characteristics.
[0082] This application also relates to a cathode slurry composition.
[0083] The above cathode slurry composition may be prepared by the method for preparing the cathode slurry described above. Accordingly, detailed descriptions that overlap with the above content will be omitted below.
[0084] For example, the above cathode slurry composition comprises water; a polyamic acid comprising diamine monomers and dianhydride monomers as polymerization units; an aqueous catalyst or an organic base; a two-dimensional silicon material; and a conductive material.
[0085] The above polyamic acid can form a polyamic acid salt with an aqueous catalyst or an organic base.
[0086] The above polyamic acid can form a polyamic acid salt with a water-based catalyst by a water-based polymerization method, or form a polyamic acid salt with an organic base by a water-soluble method. Effects of the invention
[0087] The method for manufacturing a cathode slurry according to the present application uses a polyamic acid salt prepared with water as a solvent as a binder, thereby providing a cathode slurry that is environmentally friendly, has a relatively simple process, excellent storage stability, and can exhibit an effect equivalent to that of a polyimide-based binder prepared with a conventional organic solvent. Brief explanation of the drawing
[0088] FIGS. 1 to 3 are drawings for explaining the structure of a polyamic acid salt, the structure of a two-dimensional silicon material, and the bonding structure of the polyamic acid salt and the two-dimensional silicon material. Figures 4 and 5 are graphs of the discharge capacity results of the half-cells prepared in Example 1 and Comparative Example 2. Figure 6 is a graph of the cycle test results of the half-cells prepared in Example 1 and Comparative Example 2. Specific details for implementing the invention
[0089] The present application will be described in more detail below through embodiments according to the present application, but the scope of the present application is not limited to the embodiments presented below.
[0091] Preparation Example 1 - Preparation of an aqueous solution of polyamic acid salt (PAA) using water-based polymerization
[0092] 72.68 g of distilled water (water) used as a solvent and 4.8065 g (0.05 mol) of 1,2-dimethylimidazole (DMIZ) were added to a 3-neck round-bottom flask equipped with nitrogen and a reflux device and stirred at room temperature. 2.1628 g (0.02 mol) of p-phenylenediamine (pPDA) was added to the reactor and dissolved for 1 hour. Subsequently, 6.4446 g (0.02 mol) of 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) was added, the reactor temperature was set to 70°C, and the reaction was carried out by stirring for 18 hours to synthesize polyamic acid salts.
[0094] Preparation Example 2 - Preparation of an aqueous solution of polyamic acid salt (PAA) using a water-solubilization method
[0095] 77.47 g of 1-methyl-2-pyrrolidone (NMP), used as a solvent, and 2.1628 g (0.02 mol) of p-phenylenediamine (Ppda) were added to a 3-neck round-bottom flask equipped with nitrogen and a reflux device, and stirred at room temperature for 1 hour. Then, the reactor temperature was set to 0°C, 6.4446 g (0.02 mol) of 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) was added, and the reaction was carried out by stirring for 4 hours to synthesize polyamic acid.
[0096] The synthesized polyamic acid was precipitated in distilled water, washed, and dried in a vacuum oven to obtain polyamic acid powder. 3 g of the obtained polyamic acid powder, 25.45 g of distilled water, and 1.55 g of a water-soluble agent (organic base) 2-dimethylethanolamine (DMEA) (2.5 times mol relative to the polyamic acid carboxyl group) were added to a reactor and stirred to completely dissolve the mixture to prepare a polyamic acid salt solution.
[0098] Preparation Example 3 - Preparation of Polyamic Acid (PA) in an Organic Solvent
[0099] 77.47 g of 1-methyl-2-pyrrolidone (NMP), used as a solvent, and 2.1628 g (0.02 mol) of p-phenylenediamine (pPDA) were added to a 3-neck round-bottom flask equipped with nitrogen and a reflux device, and stirred at room temperature for 1 hour. Then, the reactor temperature was set to 0°C, 6.4446 g (0.02 mol) of 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) was added, and the reaction was carried out by stirring for 4 hours to synthesize polyamic acid.
[0101] Example 1
[0102] Synthesis of 2D Silicon Material (2DSi)
[0103] CaSi2 (20 g) was added to 37 wt.% hydrochloric acid (67 ml) and reacted for more than 12 hours to remove Ca ions. The remaining material (2DSi) after the removal of Ca ions was recovered by vacuum filtration, washed thoroughly with acetone, and then dried in a vacuum oven at 100°C for 12 hours before being recovered.
[0105] Cathode slurry synthesis
[0106] A cathode slurry was prepared by mixing the above-described 2DSi, the polyamic acid salt prepared in Preparation Example 1-1, and Super P. At this time, the polyamic acid salt was dissolved in a water solvent at a concentration of 5 wt.%, and 2DSi (140 mg), polyamic acid salt (400 mg), and Super P (40 mg) were dissolved in 0.5 ml of water, and the mass ratio of 2DSi:PAA:Super P was 70:10:20, respectively.
[0107] The solid content of the manufactured cathode slurry was 16 wt%.
[0109] 2DSi cathode fabrication
[0110] The above-described slurry was applied onto a copper foil (15 cm x 20 cm x 9 μm) using the doctor blade method. The copper foil (2DSi-PAA-Cu) with the cathode slurry uniformly applied was dried in a vacuum oven at 70°C for more than 12 hours, and the 2DSi-PAA-Cu foil was prepared by cutting it to a diameter of 14 mm to fit the specifications of a coin cell.
[0112] Manufacturing of half-batteries (working electrode, negative electrode)
[0113] The working electrode was prepared by calcining the above-prepared 2DSi-PAA-Cu at 350°C for 4 hours in a nitrogen atmosphere (100 cc / min) to imide the PAA into PI and using it as a cathode.
[0114] The other cell components were used as follows: 1) cell case (CR-2032, MTI KOREA Co.), 2) Li-metal (counter electrode, diameter: 10 mm, thickness: 0.75 mm, Alfa Aesar Co.), 3) separator (GF / C, diameter 19 mm, thickness: 0.26 mm, Whatman Co.), 4) electrolyte (1M LiPF6 dissolved in EC:DMC 1:1 vol.%, Sigma Aldrich Co.).
[0116] Below, various half-cells were manufactured according to the types and compositions of the manufacturing examples shown in Table 1 using the same method as Example 1.
[0117] Manufacturing Pre-classification dianhydride diamine menstruum Water-based catalyst organic bases Polyimide binder content (wt%) 2DSi content (wt%) Conductive material content (wt%) Cathode slurry solids (wt%) Example 1 Preparation Example 1 BTDA pPDA water DMIZ - 10 70 20 16 Example 2 Preparation Example 1 BPDA pPDA water DMAP - 10 70 20 16 Example 3 Preparation Example 1 6FDA pPDA water DMAP - 10 70 20 16 Example 4 Preparation Example 1 BPDA m-TB water DMAP - 10 70 20 16 Example 5 Preparation Example 1 BTDA m-TB water DMAP - 10 70 20 16 Example 6 Preparation Example 1 6FDA m-TB water DMAP - 10 70 20 16 Example 7 Preparation Example 1 BTDA pPDA water DMIZ - 5 75 20 16 Example 8 Preparation Example 1 BTDA pPDA water DMIZ - 3 77 20 16 Example 9 Preparation Example 1 BTDA pPDA water DMIZ - 1 79 20 16 Example 10 Preparation Example 1 BTDA pPDA water DMIZ - 10 80 10 16 Example 11 Preparation Example 2 BTDA pPDA water - DMEA 10 70 20 16 Example 12 Preparation Example 2 BTDA pPDA water - DMEA 10 70 20 16 Example 13 Preparation Example 1 BTDA pPDA water DMIZ - 10 70 20 11.1 Example 14 Preparation Example 1 BTDA pPDA water DMIZ - 10 70 20 9.6 Comparative Example 1 Preparation Example 3 BTDA pPDA NMP - - 10 70 20 8.0 Comparative Example 2 Preparation Example 3 PMDA ODA NMP - - 10 70 20 8.0 Comparative Example 3 Preparation Example 3 BTDA pPDA water - - 10 70 20 - Comparative Example 4 Preparation Example 1 BTDA pPDA water DMIZ - 10 70 20 8.0
[0119] In Table 1 above, "polyimide binder content" refers to the content of polyamic acid salts or polyamic acids included in the cathode slurry that have been calcined and imidized.
[0120] Referring to Table 1, Examples 1 to 10 are examples in which a polyamic acid salt was synthesized by the "water-based polymerization method" according to Preparation Example 1, and then a cathode slurry was prepared by mixing 2DSi and a conductive material in water. Examples 11 and 12 are examples in which a polyamic acid salt was synthesized by the "water-soluble method" according to Preparation Example 2, and then a cathode slurry was prepared by mixing 2DSi and a conductive material in water. Comparative Examples 1 and 2 are examples in which a polyamic acid was synthesized in an organic solvent according to Preparation Example 3, and then a cathode slurry was prepared by mixing 2DSi and a conductive material in an organic solvent.
[0121] Meanwhile, Comparative Example 3 attempted to prepare a cathode slurry by synthesizing polyamic acid in an organic solvent according to Preparation Example 3 and then mixing 2DSi and a conductive material in water without an organic base, but the polyamic acid precipitated as powder the moment it was added to water, making it impossible to prepare the cathode slurry.
[0122] Examples 13, 14 and Comparative Example 4 are examples in which a cathode slurry was prepared in the same manner as Example 1, except that the solid content of the cathode slurry was adjusted differently, and these examples are intended to demonstrate the coating test effect according to the solid content of Experimental Example 3 described later.
[0123] In particular, the cathode slurry prepared in Comparative Example 4 was prepared in an aqueous environment using water as a solvent, just like in Example 1, and its solid content was adjusted to 8 wt%, the same as in Comparative Examples 1 and 2, in which the cathode slurry was prepared in an organic solvent.
[0124] The cathode slurry prepared in Comparative Example 4 could not be uniformly coated and coated on the current collector, making it impossible to manufacture the electrode.
[0126] Experimental Example 1: Electrochemical Performance Evaluation
[0127] An automatic battery cycler (WonAtech Co., WBCS 3000 model) was used to evaluate electrochemical performance. The experiment was operated with a voltage range of 0.05 to 2.0 V vs. Li / Li+ and a current density of 250 mA / g. After designing the experimental conditions to repeat the discharge-charge cycle after a sufficient rest period of 6 hours to reduce contact resistance between the electrodes, the specific capacity and capacity retention at the 50th cycle were measured, and the results are shown in Table 2.
[0128] For the discharge capacity, the current (mA) applied when lithium is inserted into the active material was multiplied by the time (h) during which the insertion reaction occurs, and then divided by the total weight (g) of the active material.
[0129] In addition, regarding the discharge capacity retention rate, the discharge capacity retention rate at the 50th cycle was calculated relative to the discharge capacity at the 2nd cycle, excluding the discharge capacity of the irreversible initial cycle (1st cycle). For reference, a higher discharge capacity retention rate can be interpreted as indicating higher electrochemical stability.
[0130] As explained above, in the case of Comparative Example 3, it was impossible to manufacture the cathode slurry, and in the case of Comparative Example 4, it was impossible to manufacture the electrode, so an electrochemical performance evaluation was not performed.
[0131] Discharge capacity (mAh / g) Discharge capacity retention rate (%) Example 1 354.8 78.6 Example 2 316.1 32.9 Example 3 77.7 6.5 Example 4 286.4 28.1 Example 5 245.4 37.0 Example 6 179.2 41.0 Example 7 293.8 28.1 Example 8 231.1 27.3 Example 9 75.6 8.6 Example 10 120.7 17.1 Example 11 351.2 78.0 Example 12 317.2 33.1 Example 13 333.7 66.3 Example 14 341.7 63.7 Comparative Example 1 250.7 20.3 Comparative Example 2 365.5 65.1 Comparative Example 3 - - Comparative Example 4 - -
[0133] Referring to Table 2, the discharge capacity of the (lithium-ion) half-cell prepared using Example 1 at the 50th cycle was 354.8 mAh / g, which was the highest among the examples, and the discharge capacity retention rate during cycles 2-50 was 78.6%, which was the highest. When utilizing the configuration of Example 1, mechanical and electrochemical stability resulting from chemical bonding with the 2DSi negative electrode active material was optimized, making it possible to secure the optimized discharge capacity and cycle stability of the (lithium-ion) battery.
[0135] Meanwhile, Figures 4 and 5 are graphs of the discharge capacity results of the half-cells prepared in Example 1 and Comparative Example 2.
[0136] Figure 4 is a graph of the discharge capacity results of the half-cell manufactured in Example 1, and Figure 5 is a graph of the discharge capacity results of the half-cell manufactured in Comparative Example 2.
[0137] Referring to Figures 4 and 5, when a charge and discharge test was conducted at a current density of 3: 250 mA / g, the batteries of Example 1 and Comparative Example 2 both formed a plateau at 0.2 V vs. Li / Li+ or lower and generated a discharge capacity.
[0138] The charge and discharge test results of the cathode slurry prepared using water (Example 1) and the cathode slurry prepared using an organic solvent (Comparative Example 2) were found to be at similar levels and were at the same position as the lithiation potential of a typical silicon material, which is 0.1-0.2 V vs. Li / Li+, indicating that 2DSi is acting as the active material in both Example 1 and Comparative Example 2.
[0139] Figure 6 is a graph of the cycle test results of the half-cells prepared in Example 1 and Comparative Example 2.
[0140] Referring to Fig. 6, the batteries prepared in Example 1 (2DSi-PI_aqueous system) and Comparative Example 2 (2DSi-PI organic system) at a current density of 3: 250 mA / g showed discharge capacities of 354.8 mAh / g and 365.5 mAh / g, respectively, after 50 charge-discharge cycles, and it was possible to recover almost all stored lithium ions (Coulombic efficiency ~100%) when charged to 2 V vs. Li / Li+.
[0141] In addition, during 50 charge-discharge cycles, the batteries of Example 1 and Comparative Example 2 had discharge capacity retention rates of 78.6% and 65.1%, respectively.
[0143] Experimental Example 3: Coating Test According to Solid Content
[0144] Examples 13, 14 and Comparative Example 4 each had the solid content of the cathode slurry of Example 1 changed as shown in Table 3 below, and then the cathode slurry was applied to a current collector in the same way as in Example 1 to prepare the cathode.
[0145] A coating test was performed by visually inspecting the cathode surface, and the results are shown in Table 3 below (uniform coating and coating possible: O, coating impossible: X).
[0146] Example 1 Example 13 Example 14 Comparative Example 4 Cathode slurry solids (wt%) 16 11.1 9.6 8.0 Application test O O O X
Claims
Claim 1 The method comprises the steps of: preparing an aqueous polyamic acid salt solution; and preparing a cathode slurry by mixing an active material for a cathode comprising the aqueous polyamic acid salt solution, a conductive material, and a two-dimensional silicon material (2DSi), wherein the two-dimensional silicon material (2DSi) is a two-dimensional siloxene, the aqueous polyamic acid salt solution is prepared by an aqueous polymerization method or a water-soluble method, the polyamic acid of the aqueous polyamic acid salt solution is prepared by polymerizing a dianhydride monomer and a diamine monomer, the dianhydride monomer comprises pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), or 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and the diamine monomer comprises 1,4-diaminobenzene (PPD), 4,4'-diaminodiphenyl ether (ODA), or A method for preparing a cathode slurry comprising 2,2-dimethylbenzidine (m-TB). Claim 2 delete Claim 3 A method for preparing a cathode slurry according to claim 1, wherein the aqueous polymerization method comprises the steps of: preparing an aqueous solution containing water and an aqueous catalyst; and polymerizing a diamine monomer and a dianhydride monomer in the aqueous solution to prepare an aqueous polyamic acid salt solution. Claim 4 A method for preparing a cathode slurry according to claim 1, wherein the water-soluble method comprises the steps of: preparing a polyamic acid by polymerizing a diamine monomer and a dianhydride monomer in an organic solvent; and preparing an aqueous polyamic acid salt solution by mixing the polyamic acid, water, and an organic base. Claim 5 In claim 3, the method for preparing a cathode slurry comprising a pyridine-based compound or an imidazole-based compound, wherein the aqueous catalyst comprises a pyridine-based compound or an imidazole-based compound. Claim 6 A method for preparing a cathode slurry according to claim 4, wherein the organic base comprises a pyridine-based compound, an imidazole-based compound, an alcoholamine-based compound, or an alkylamine-based compound. Claim 7 delete Claim 8 delete Claim 9 delete Claim 10 delete Claim 11 A method for preparing a cathode slurry according to claim 1, wherein the content of the polyamic acid salt is within the range of 0.5 to 15 wt% with respect to the total weight of the solids of the cathode slurry. Claim 12 A method for manufacturing a cathode slurry according to claim 1, wherein the content of the cathode active material is within the range of 65 to 85 wt% with respect to the total weight of the solids of the cathode slurry. Claim 13 A method for manufacturing a cathode slurry according to claim 1, wherein the content of the conductive material is within the range of 5 to 30 wt% with respect to the total weight of the solids of the cathode slurry. Claim 14 A method for manufacturing a cathode slurry according to claim 1, further comprising the step of adjusting the solid content of the cathode slurry to 9 to 25 wt%. Claim 15 A method for manufacturing a cathode, comprising the steps of: applying a cathode slurry manufactured by the method of claim 1 onto a current collector; and firing the current collector coated with the cathode slurry. Claim 16 A method for manufacturing a cathode according to claim 15, wherein, in the step of calcining, the polyamic acid salt is imidized with polyimide and bonded to the two-dimensional silicon material (2DSi). Claim 17 A method for manufacturing a cathode according to claim 15, wherein the temperature of the calcination step is greater than 120℃ and less than or equal to 500℃. Claim 18 A cathode slurry composition comprising water; a polyamic acid prepared by polymerizing a diamine monomer and a dianhydride monomer; an aqueous catalyst or an organic base; a two-dimensional silicon material; and a conductive material, wherein the two-dimensional silicon material (2DSi) is a two-dimensional siloxene, the polyamic acid forms a polyamic acid salt with the aqueous catalyst or organic base, the dianhydride monomer comprises pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), or 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and the diamine monomer comprises 1,4-diaminobenzene (PPD), 4,4'-diaminodiphenyl ether (ODA), or 2,2-dimethylbenzidine (m-TB). Claim 19 delete
Citation Information
Patent Citations
Binder for electrodes of secondary battery, and electrode empolyed with the binder, and manufacture of method for the same
KR1020190004941A
Aqueous polyamic acid composition
KR1020210059436A
Anode for lithium ion battery and manufacturing method for the same
KR1020220022267A