Electrochemical reduction of surface metal oxides

The microwave process addresses the challenge of converting metal oxides into pure metals at low temperatures, ensuring minimal damage to adjacent materials and maintaining processing selectivity by using microwave-induced dipole rotation and eddy currents to break oxide bonds.

KR103044543B1Active Publication Date: 2026-11-06APPLIED MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020257022470
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-07
Filing Date
2023-11-27
Publication Date
2026-11-06
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

Current methods for removing surface metal oxides, such as WOx, MoOx, CoOx, and RuOx, require high temperatures and plasma processes that damage adjacent dielectric materials and affect metal deposition selectivity, necessitating a low-temperature, non-damaging process for converting metal oxides into pure metals.

Method used

A microwave process is used to reduce surface metal oxides at low temperatures by exposing the metal oxide layer to microwave radiation, utilizing microwave-induced dipole rotation and eddy currents to break oxide bonds without affecting neighboring materials.

Benefits of technology

The method effectively reduces metal oxides to pure metals at low temperatures, preserving surrounding materials and maintaining deposition selectivity, without the use of plasma, thus minimizing damage and improving processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025075517725-PCT00005_ABST
    Figure 112025075517725-PCT00005_ABST
Patent Text Reader

Abstract

The embodiments of the present disclosure relate to methods for reducing a metal oxide layer to a pure metal using microwave radiation. Certain embodiments provide methods for reducing a natural metal oxide on a metal interconnect within a substrate feature including dielectric sidewalls. In some embodiments, surrounding dielectric materials are not damaged by the disclosed processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The embodiments of the present disclosure generally relate to methods for converting surface metal oxides into pure metal. In particular, the embodiments of the present disclosure relate to methods for reducing metal oxides by a microwave process. Background Technology

[0002] Exposure of pure metal materials to air can result in the formation of a thin metal oxide layer on the surface of the metal. This surface metal oxide layer can impede the selectivity of subsequent processing steps and increase the resistance of interconnects. Accordingly, there is a need for a method to prevent metal oxides on the surface of metal materials and / or to clean them.

[0003] Although integrated processing units and the transport of wafers under vacuum have reduced the need for removing these metal oxide layers, current pre-cleaning methods typically require hydrogen plasma, high processing temperatures (above 300 °C), and / or high-energy argon (Ar) sputtering. However, these processes often damage adjacent dielectric materials (e.g., feature sidewalls) and can adversely affect the selectivity of many metal deposition processes (e.g., selective tungsten deposition).

[0004] In addition, current pre-cleaning methods need to be developed and / or adapted for different metal oxide materials (e.g., WOx, MoOx, CoOx, RuOx, CuOx, etc.). Each different material may require a different plasma source, different reactant gas mixtures or chemical immersions, and / or different treatment conditions (e.g., temperature, pressure).

[0005] Accordingly, there is a need for general-purpose methods to convert surface metal oxides into pure metals. Additionally, there is a specific need for processes that are performed at relatively low temperatures without damaging surrounding materials.

[0006] One or more embodiments of the present disclosure relate to a method for reducing a surface metal oxide layer. The method comprises the step of exposing a metal oxide layer on a metal material to microwave radiation.

[0007] Additional embodiments of the present disclosure relate to a method for reducing molybdenum oxide. The method comprises the step of exposing a substrate surface having at least one feature to microwave radiation to reduce a layer of molybdenum oxide on a molybdenum metal material. The at least one feature has two sidewalls having a low-dielectric constant (low-k) dielectric that extend in depth from the substrate surface to a lower portion containing the molybdenum oxide layer. Brief explanation of the drawing

[0008] In a manner that the features of the above-mentioned disclosure can be understood in detail, a more specific description of the disclosure briefly summarized above may be made with reference to embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the accompanying drawings are merely illustrative of typical embodiments of the disclosure and should not be construed as limiting the scope of the disclosure, as the disclosure may allow for other equally valid embodiments. FIG. 1 illustrates a schematic diagram of a microwave processing tool comprising a microwave source according to one or more embodiments of the present disclosure. FIG. 2 is a schematic diagram of a semiconductor processing tool having a modular microwave source according to one or more embodiments of the present disclosure. FIG. 3 is an example perspective view of a source array for a modular microwave source according to one or more embodiments of the present disclosure. FIG. 4 is a cross-sectional example of a treatment chamber for reducing surface metal oxides according to one or more embodiments of the present disclosure. FIGS. 5A and 5B illustrate exemplary substrates during processing according to one or more embodiments of the present disclosure. FIG. 5c illustrates a cross-sectional view of an exemplary substrate according to one or more embodiments of the present disclosure. For ease of understanding, the same reference numbers have been used where possible to designate identical elements common to the drawings. The elements and features of one embodiment are considered to be beneficially incorporated into other embodiments without further mention. Specific details for implementing the invention

[0009] Before describing some exemplary embodiments of the present disclosure, it should be understood that the present disclosure is not limited to the details of the configurations or process steps described in the following description. Other embodiments of the present disclosure are possible and may be implemented or carried out in various ways.

[0010] The term "approximately" as used herein means approximately or nearly, and in the context of a stated numerical value or range, means a variation of ±15% or less of the numerical value. For example, values ​​differing by ±14%, ±10%, ±5%, ±2%, ±1%, ±0.5%, or ±0.1% will satisfy the definition of approximately.

[0011] As used in this specification and the appended claims, the terms “substrate” or “wafer” refer to a surface or a portion of a surface on which a process is performed. It will also be understood by those skilled in the art that references to a substrate may refer to only a portion of the substrate unless the context clearly indicates otherwise. Additionally, references to deposition on a substrate may mean both a substrate on which one or more films or features are deposited or formed and a bare substrate.

[0012] As used herein, the term “substrate surface” refers to any substrate or a material surface formed on a substrate upon which film treatment is performed during a manufacturing process. For example, substrate surfaces upon which treatment may be performed include, depending on the application, materials such as silicon, silicon oxide, strained silicon, silicon on insulator (SOI), carbon-doped silicon oxides, amorphous silicon, doped silicon, germanium, gallium arsenide, and any other materials, such as metals, metal nitrides, metal alloys, and other conductive materials. Substrates include, without limitation, semiconductor wafers. Substrates may be exposed to a pretreatment process to polish, etch, reduce, oxidize, hydroxylate, anneale, and / or bake the substrate surface. In the present disclosure, in addition to performing film treatment directly on the surface of the substrate itself, any of the disclosed film treatment steps may also be performed on an underlying layer formed on the substrate, as disclosed in more detail below, and the term “substrate surface” is intended to include such underlying layer as indicated by the context. Accordingly, for example, where a film / layer or partial film / layer is deposited on the substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.

[0013] The substrate surface may have one or more features formed on the substrate surface, one or more layers formed on the substrate surface, and combinations thereof. The shape of the feature may be any suitable shape, including but not limited to trenches, holes, and vias (circular or polygonal). As used in this context, the term “feature” refers to any intentional surface irregularity. Suitable examples of features include, but are not limited to, trenches extending into the substrate and having a top, two sidewalls, and a bottom, and vias having one or more sidewalls extending into the substrate to the bottom.

[0014] The terms "on" or "on" indicate that direct contact exists between elements. The term "directly on" indicates that direct contact exists between elements without any intervening elements.

[0015] As used in this specification and the appended claims, terms such as "precursor," "reactant," and "reactive gas" are used interchangeably to refer to any gaseous species capable of reacting with a substrate surface.

[0016] Embodiments of the present disclosure advantageously provide methods for reducing surface metal oxides at relatively low temperatures without affecting neighboring materials. Certain embodiments advantageously provide methods for reducing metal oxides utilizing a microwave process. In some embodiments, the metal oxide layer is not exposed to plasma.

[0017] Embodiments of the present disclosure are described by drawings illustrating processes, substrates, and apparatus according to one or more embodiments of the present disclosure. The illustrated processes, diagrams, and resulting substrates are merely illustrative of the disclosed processes, and a person skilled in the art will recognize that the disclosed processes are not limited to the illustrative applications.

[0018] Referring to FIG. 1, a cross-sectional example of an exemplary processing tool (100) is illustrated. The processing tool (100) may be a processing tool suitable for any type of processing operation utilizing microwaves. Although the embodiments described in detail herein relate to microwave processing methods, it should be recognized that additional processing methods (including plasma processing methods) may also be performed on the processing tool (100). Additionally, it should also be recognized that the PEALD methods described herein may also be performed using different processing tools.

[0019] Generally, the processing tool (100) includes a chamber (178). In the processing tools (100) used for processing a substrate, the chamber (178) may be a vacuum chamber. The vacuum chamber may include a pump (not shown) for removing gases from the chamber to provide the desired vacuum. Additional embodiments may include a chamber (178) which includes one or more gas lines (170) for providing processing gases into the chamber (178) and exhaust lines (172) for removing byproducts from the chamber (178). It should be recognized that, although not shown, the processing tool may include a showerhead or other gas distribution assembly for evenly distributing processing gases over a substrate (174).

[0020] In some embodiments, the substrate (174) may be supported on a chuck (176). For example, the chuck (176) may be any suitable chuck, such as an electrostatic chuck. The chuck may also include cooling lines and / or a heater to provide temperature control to the substrate (174) during processing.

[0021] The processing tool (100) includes one or more microwave sources (104). The microwave sources (104) may include a solid-state microwave amplification circuit (130) and an applicator (142). In some embodiments, a voltage control circuit (110) provides an input voltage to a voltage-controlled oscillator (120) to generate microwave radiation of a desired frequency that is transmitted to the solid-state microwave amplification circuit (130) of each microwave source (104). After processing by the microwave amplification circuit (130), the microwave radiation is transmitted to the applicator (142). In some embodiments, an array (140) of applicators (142) is coupled to a chamber (178), and each functions as an antenna for coupling microwave radiation to a substrate (174) within the chamber (178).

[0022] Now, referring to FIGS. 2 through 4, a series of examples illustrating a microwave processing tool (100) according to an embodiment are shown. The microwave processing tool (100) generates microwaves useful for low-temperature reduction of metal oxides.

[0023] Now, referring to FIG. 2, a cross-sectional example of a microwave processing tool (100) (referred to as processing tool (100) for short) according to an embodiment is illustrated. The processing tool may emit high-frequency electromagnetic radiation. As used herein, “high-frequency” electromagnetic radiation includes radio frequency radiation, very-high-frequency radiation, ultra-high-frequency radiation, and microwave radiation. “High frequency” may refer to frequencies from 0.1 MHz to 300 GHz.

[0024] Generally, embodiments include a processing tool (100) comprising a chamber (178). In the processing tool (100), the chamber (178) may be a vacuum chamber. The vacuum chamber may include a pump (not shown) for removing gases from the chamber to provide the desired vacuum. Additional embodiments may include a chamber (178) which includes one or more gas lines (170) for providing processing gases into the chamber (178) and exhaust lines (172) for removing byproducts from the chamber (178). Although not shown, it should be recognized that gases may also be injected into the chamber (178) through a source array (150) (e.g., as a showerhead) to distribute the processing gases evenly over the substrate (174).

[0025] In an embodiment, the substrate (174) may be supported on a chuck (176). For example, the chuck (176) may be any suitable chuck, such as an electrostatic chuck. The chuck (176) may also include cooling lines and / or a heater to provide temperature control to the substrate (174) during processing. Due to the modular configuration of the high-frequency emission modules described herein, the embodiments allow the processing tool (100) to accommodate a substrate (174) of any size. For example, the substrate (174) may be a semiconductor wafer (e.g., 200 mm, 300 mm, 450 mm, or larger). Alternative embodiments also include substrates (174) other than semiconductor wafers. For example, the embodiments may include a processing tool (100) configured to process glass substrates (e.g., for display technologies).

[0026] According to an embodiment, the processing tool (100) includes a modular high-frequency emission source (104). The modular high-frequency emission source (104) may include an array of high-frequency emission modules (105). In an embodiment, each high-frequency emission module (105) may include an oscillator module (106), an amplification module (130), and an applicator (142). As illustrated, the applicators (142) are schematically depicted as being integrated into the source array (150).

[0027] In an embodiment, the oscillator module (106) and the amplifier module (130) may include electrical components that are solid-state electrical components. In an embodiment, each of the plurality of oscillator modules (106) may be communicably coupled to different amplifier modules (130). For example, each oscillator module (106) may be electrically coupled to a single amplifier module (130). In an embodiment, the plurality of oscillator modules (106) may generate non-coherent electromagnetic radiation. Accordingly, the electromagnetic radiation induced within the chamber (178) will not interact in a manner that results in an undesirable interference pattern.

[0028] In an embodiment, each oscillator module (106) generates high-frequency electromagnetic radiation that is transmitted to an amplification module (130). After processing by the amplification module (130), the electromagnetic radiation is transmitted to an applicator (142). In an embodiment, each applicator (142) emits electromagnetic radiation into a chamber (178). In some embodiments, the applicators (142) combine the electromagnetic radiation with a substrate (174) inside the chamber (178).

[0029] Now, referring to FIG. 3, an example perspective view of a source array (150) according to an embodiment is shown. In the embodiment, the source array (150) includes a dielectric plate (160). A plurality of cavities (167) are disposed within a first surface (161) of the dielectric plate (160). The cavities (167) do not pass through a second surface (162) of the dielectric plate (160). The source array (150) may further include a plurality of dielectric resonators (166). Each of the dielectric resonators (166) may be in a different cavity among the cavities (167). Each of the dielectric resonators (166) may include a hole (165) located at the axial center of the dielectric resonator (166).

[0030] In an embodiment, the dielectric resonators (166) may have a first width (W1), and the cavities (167) may have a second width (W2). The first width (W1) of the dielectric resonator (166) is smaller than the second width (W2) of the cavities (167). The difference in widths provides a gap (G) between the sidewalls of the dielectric resonators (166) and the sidewalls of the cavities (167). In the illustrated embodiment, each dielectric resonator (166) is shown to have a uniform width (W1). However, it should be recognized that not all dielectric resonators (166) of the source array (150) need to have the same dimensions.

[0031] Now, referring to FIG. 4, a cross-sectional example of a processing tool (100) including an assembly (190) according to an embodiment is shown. In an embodiment, the processing tool includes a chamber (178) sealed by the assembly (190). For example, the assembly (190) may be positioned to abut one or more O-rings (181) to provide a vacuum seal to the internal volume (183) of the chamber (178). In other embodiments, the assembly (190) may interface with the chamber (178). That is, the assembly (190) may be part of a cover that seals the chamber (178). In an embodiment, the processing tool (100) may include a plurality of processing volumes (which may be fluidically coupled together), each processing volume having a different assembly (190). In an embodiment, a chuck (179), etc., may support a substrate (174) (e.g., a wafer, a workpiece, etc.). The substrate (174) may be at a distance (D) from the assembly (190). That is, the chamber (178) may be a vacuum chamber. In an embodiment, the assembly (190) includes a source array (150) and a housing (182). The source array (150) may include a dielectric plate (160) and a plurality of dielectric resonators (166) extending upward from the dielectric plate (160). Cavities (167) into the dielectric plate (160) may surround each of the dielectric resonators (166). The sidewalls of the cavity (167) are separated from the sidewalls of the dielectric resonators (166) by a gap (G). The dielectric plate (160) and dielectric resonators (166) of the source array (150) may be a monolithic structure (as shown in FIG. 3d), or the dielectric plate (160) and dielectric resonators (166) may be separate components.

[0032] The housing (182) includes rings (131) that fit into the gaps (G). In an embodiment, the rings (131) and the conductive body (173) of the housing (182) may be a monolithic structure (as shown in FIG. 3d), or the conductive body (173) and the rings (131) may be separate components. The housing (182) may have openings sized to accommodate dielectric resonators (166). In an embodiment, monopolar antennas (188) may extend into the holes of the dielectric resonators (166). Each monopolar antenna (188) is electrically coupled to a power source (e.g., high-frequency emission modules (105)).

[0033] The embodiments of the present disclosure utilize a microwave process. Without being bound by theory, the microwave process described herein is believed to weaken the bonds of metal oxide materials with the aid of the oscillatory-rotational motion of metal oxide dipoles at microwave frequencies. The disclosed methods utilize an E-field for dipole rotation and a B-field for eddy currents, which leads to the heating of the metal oxide material without affecting other substrate materials. The energy of the microwaves can be tuned sufficiently low so as not to substantially damage the dielectric materials (e.g., no plasma, low temperature). Additionally, the disclosed methods are self-limiting by affecting only the metal oxides and not the metal materials.

[0034] Referring to FIGS. 5a and 5b, the method (200) begins with a metal oxide layer (260) having a metal material (250). In operation (210), the metal oxide layer (260) is exposed to microwave radiation. As used in this context, exposing a substrate to "microwave radiation" should be understood to include activating a microwave source and exposing the metal oxide layer (260) to the generated microwave radiation. In some embodiments, the microwave process does not generate a reactive plasma. In other words, in some embodiments, the metal oxide layer is not exposed to plasma.

[0035] The metal material (250) may include any suitable metal. In some embodiments, the metal material (250) and the metal oxide layer (260) include the same metal or metals. In some embodiments, the metal material is essentially composed of or includes one or more of molybdenum, tungsten, ruthenium, copper, cobalt, tantalum, or titanium.

[0036] In some embodiments, the metal oxide layer (260) has a thickness in the range of about 20 Å to about 30 Å. In some embodiments, the method (200) reduces the thickness of the metal oxide layer (260) to a range of about 10 Å to about 30 Å, or a range of about 20 Å to about 30 Å, or a range of about 15 Å to about 25 Å. In some embodiments, the method (200) reduces the entire metal oxide layer to pure metal.

[0037] In some embodiments, the microwave process in operation (210) involves exposing the metal oxide layer (260) to a gas flow. In some embodiments, the gas flow is continuous and the microwave exposure is continuous. In other words, in some embodiments, neither the gas flow nor the microwave sources are pulsed during the microwave process.

[0038] In some embodiments, the gas flow comprises an inert gas. Without being bound by theory, exposure to an inert gas flow is believed to help facilitate the removal of volatile reaction byproducts. In some embodiments, the inert gas is essentially composed of or comprises helium (He) or argon (Ar). In some embodiments, the inert gas is essentially composed of or comprises hydrocarbons (e.g., CH4, C2H6, C2H4, C2H2). In some embodiments, the inert gas is essentially composed of or comprises CO2.

[0039] In some embodiments, the gas flow contains reactants. Without being bound by theory, exposure to the reactant gas flow is believed to react with activated oxygen atoms from the metal oxide layer (260) to form volatile species that are more easily purged from the processing chamber. In some embodiments, the reactants consist of or include one or more of hydrogen gas (H2) or carbon monoxide (CO).

[0040] In some embodiments, the method (200) is performed at relatively low temperatures. Relatively low temperatures advantageously result in reduced damage to surrounding materials (e.g., dielectrics). In some embodiments, the metal material is maintained at a temperature within the range of about 300 °C to about 400 °C. In some embodiments, the metal material is maintained at a temperature of about 300 °C or lower. In some embodiments, the metal material is maintained at a temperature within the range of about 20 °C to about 50 °C or about 20 °C to about 100 °C.

[0041] In some embodiments, the exposure period is controlled to reduce the predetermined depth of the metal oxide layer (260). In some embodiments, the period is in the range of about 60 seconds to about 600 seconds, in the range of about 60 seconds to about 300 seconds, or in the range of about 30 seconds to about 120 seconds.

[0042] In some embodiments, the power of the microwave array (140) is in the range of about 800 W to about 8000 W, or about 900 W to about 5000 W, or about 1000 W to about 3000 W.

[0043] In some embodiments, the pressure of the chamber (178) can be controlled. In some embodiments, the pressure is maintained within the range of about 1 mTorr to about 10 Torr, or about 10 mTorr to about 1 Torr, or about 10 mTorr to about 100 mTorr, or about 50 mTorr to about 75 mTorr.

[0044] As illustrated in FIG. 5c, in some embodiments, a metallic material (250) is located at the bottom (218) of the substrate feature (215). The feature (215) has sidewalls (214, 216). In some embodiments, at least a portion of the sidewalls (214, 216) comprises a low-dielectric constant material (270). In some embodiments, the top surface (212) of the feature comprises a high-dielectric constant (high-k) dielectric (280). In some embodiments, the high-dielectric constant dielectric (280) comprises silicon nitride.

[0045] In some embodiments, the low-dielectric constant material comprises SiOC. In some embodiments, the low-dielectric constant material of the sidewalls (214, 216) is not substantially damaged by the method (200). As used in this context, when the normalized loss of carbon / silicon is about 30% or less, the dielectric is "substantially not damaged".

[0046] Throughout this specification, references to “one embodiment,” “specific embodiments,” “one or more embodiments,” or “exemplars” mean that a specific feature, structure, material, or property described in relation to an embodiment is included in at least one embodiment of this disclosure. Accordingly, the appearance of phrases such as “in one or more embodiments,” “in specific embodiments,” “in one embodiment,” or “in an embodiment” at various locations throughout this specification does not necessarily refer to the same embodiment of this disclosure. Furthermore, specific features, structures, materials, or properties may be combined in any suitable manner in one or more embodiments.

[0047] Although the disclosure herein has been described with reference to specific embodiments, those skilled in the art will understand that the described embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations may be made to the methods and apparatus of the disclosure without departing from the spirit and scope of the disclosure. Accordingly, the disclosure may include modifications and variations within the scope of the appended claims and their equivalents.

Claims

Claim 1 A method for processing a semiconductor substrate, comprising the step of exposing a surface of a semiconductor substrate to microwave radiation—the surface of the semiconductor substrate having at least one feature formed on the surface, said at least one feature having two sidewalls and extending to a depth of the lowest part, said lowest part comprising a metal oxide layer on a metal material—and said microwave radiation reducing the metal oxide layer to the metal material. Claim 2 The method according to claim 1, wherein the metal material comprises one or more of molybdenum, tungsten, ruthenium, cobalt, copper, tantalum, or titanium. Claim 3 A method according to claim 1, wherein the metal oxide layer is not exposed to plasma. Claim 4 A method according to claim 1, further comprising the step of exposing the metal oxide layer to a gas flow while exposing the metal oxide layer to microwave radiation. Claim 5 In paragraph 4, the method wherein both the gas flow and the microwave radiation are continuous. Claim 6 In paragraph 4, the method wherein the gas flow comprises an inert gas. Claim 7 In paragraph 6, the method wherein the inert gas comprises helium (He). Claim 8 In paragraph 4, the method wherein the gas flow comprises a reactant. Claim 9 A method according to claim 8, wherein the reactant is supplied at a flow rate within the range of about 1 sccm to about 50 sccm. Claim 10 In claim 8, the method comprises the reactant containing hydrogen gas (H2). Claim 11 In claim 8, the method comprises the reactant containing carbon monoxide (CO). Claim 12 A method according to claim 1, wherein the metal material is maintained at a temperature within the range of about 300 ℃ to about 400 ℃. Claim 13 A method according to claim 1, wherein the metal material is maintained at a temperature of about 300°C or lower. Claim 14 A method according to claim 1, wherein the metal material is maintained at a temperature within the range of about 20 ℃ to about 100 ℃. Claim 15 A method according to claim 1, wherein the duration of the exposure is within the range of about 60 seconds to about 600 seconds. Claim 16 A method according to claim 1, wherein the sidewalls comprise a low-dielectric constant (low-k) dielectric material. Claim 17 In paragraph 16, the method wherein the low-dielectric constant dielectric material is not substantially damaged by the exposure step. Claim 18 A method according to claim 1, wherein the exposing step reduces the thickness of the metal oxide layer within the range of about 15 Å to about 25 Å. Claim 19 A method for processing a semiconductor substrate, comprising the step of exposing a surface of a semiconductor substrate having at least one feature to microwave radiation to reduce a molybdenum oxide layer on a molybdenum metal material, wherein the at least one feature has two sidewalls having a low dielectric constant dielectric material, the depth extending from the surface of the substrate to a lower portion including the molybdenum oxide layer. Claim 20 In claim 19, the method wherein the low-dielectric constant dielectric material is not substantially damaged by the exposure step.

Citation Information

Patent Citations

  • Conductive-pattern formation method and composition for forming conductive pattern via light exposure or microwave heating

    KR1020140082810A

  • Methods for Removing Metal Oxides

    US20190273019A1

  • Method and apparatus for reacting thin films on low-temperature substrates at high speeds

    KR1020110082575A

  • Methods for reducing metal oxide surfaces to modified metal surfaces using a gaseous reducing environment

    US20140256127A1

  • Pre-treatment method for metal-oxide reduction and device formed

    US20150001728A1