Cold rolled steel sheet and manufacturing method thereof

A cold-rolled steel sheet with a refractory layer formed from titanium, silicon, oxygen, and iron components, using a mixed solution and heat treatment, addresses oxidation issues, ensuring superior fire resistance under high temperatures.

KR103045687B1Active Publication Date: 2026-11-06HYUNDAE STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020240173930
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-11-28
Publication Date
2026-11-06
Estimated Expiration
2044-11-28

AI Technical Summary

Technical Problem

Cold-rolled steel sheets used in fire doors suffer from oxidation at high temperatures, leading to a decrease in fire resistance performance, as evidenced by the formation of cracks when exposed to flames above 900°C.

Method used

A cold-rolled steel sheet with a refractory layer comprising specific weight percentages of titanium, silicon, oxygen, iron, and other impurities, formed through a mixed solution of titanium oxide acetylacetonate and an organic silane solvent, followed by a heat treatment process.

Benefits of technology

The refractory layer effectively minimizes oxidation, maintaining the fire resistance of the steel sheet by preventing crack formation during high-temperature exposure, thus enhancing the fire-resistant properties of fire doors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024132013000-PAT00002_ABST
    Figure 112024132013000-PAT00002_ABST
Patent Text Reader

Abstract

The present invention provides a cold-rolled steel sheet comprising: a base material; and a refractory layer formed on at least one surface of the base material; wherein the refractory layer comprises 15 wt% or more and 25 wt% or less of titanium (Ti), 25 wt% or more and 35 wt% or less of silicon (Si), 45 wt% or more and 50 wt% or less of oxygen (O), 0.5 wt% or more and 5 wt% or less of iron (Fe), and other unavoidable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a cold-rolled steel sheet with excellent fire-resistant properties and a method for manufacturing the same. Background Technology

[0002] Fire doors are a type of firefighting facility designed to allow human passage while preventing the penetration of flames in the event of a fire, playing a crucial role in minimizing the spread of flames and securing evacuation routes.

[0003] Therefore, steel plates used in fire doors require excellent fire resistance properties.

[0004] In general, steel is widely used in fire doors due to its superior high-temperature strength compared to materials such as polymers. In particular, cold-rolled steel sheets or hard cold-rolled steel sheets are primarily used in fire doors.

[0005] Nevertheless, when cold-rolled steel sheets are exposed to high temperatures of 900°C or higher for a long period, an oxidation reaction occurs, causing loss of the cold-rolled steel sheet material and a decrease in the fire resistance performance of the fire door.

[0006] Accordingly, a test (KS F. 2257) in which a fire door is directly exposed to a flame at 945°C for 60 minutes to check for the occurrence of cracks of 6mm or more is adopted as a method for evaluating the fire resistance performance of fire doors.

[0007] For the reasons mentioned above, a method is required to improve the fire resistance performance of fire doors by suppressing the oxidation reaction at high temperatures on the surface of steel plates. The problem to be solved

[0008] The present invention is intended to solve various problems, including the problems mentioned above. According to one embodiment of the present invention, a cold-rolled steel sheet with excellent fire resistance and a method for manufacturing the same can be provided.

[0009] However, these tasks are exemplary and do not limit the scope of the invention. means of solving the problem

[0010] According to one aspect of the present invention, a cold-rolled steel sheet is provided, comprising: a base material; and a refractory layer formed on at least one surface of the base material, wherein the refractory layer comprises 15 wt% or more and 25 wt% or less of titanium (Ti), 25 wt% or more and 35 wt% or less of silicon (Si), 45 wt% or more and 50 wt% or less of oxygen (O), 0.5 wt% or more and 5 wt% or less of iron (Fe), and other unavoidable impurities.

[0011] The thickness of the above refractory layer may be 3 μm or more and 8 μm or less.

[0012] The above refractory layer may include titanium oxide.

[0013] According to one aspect of the present invention, a method for manufacturing a cold-rolled steel sheet is provided, comprising: a mixed solution preparation step of preparing a mixed solution to be applied to a base material; a mixed solution application step of applying the mixed solution to at least one surface of the base material; and a heat treatment step of heat-treating the cold-rolled steel sheet to which the mixed solution is applied to form a refractory layer on the base material, wherein the base material comprises a steel sheet that has undergone a hot rolling process and a cold rolling process, and the refractory layer comprises titanium oxide.

[0014] In the above mixed solution preparation step, a mixed solution can be prepared by mixing titanium oxide acetylacetonate powder with an organic silane solvent.

[0015] The above mixed solution may contain at least 10 volume% and no more than 50 volume% of titanium oxide acetylacetonate based on the total volume of the above mixed solution.

[0016] The above organic silane solvent may include a silane-based sol-gel resin.

[0017] The above silane-based sol-gel resin is formed by bonding a first silane, a second silane, a third silane, and a fourth silane under an acid catalyst and a solvent, wherein the first silane is selected from the group consisting of tetraethyl orthosilicate, tetramethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane, the second silane is selected from the group consisting of tetraethyl orthosilicate, tetramethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane, but is different from the first silane, and the third silane is composed of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropylmethyldiethoxysilane. The fourth silane is selected from the group consisting of 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and the acid catalyst may comprise at least one selected from the group consisting of acetic acid, formic acid, lactic acid, nitric acid, and hydrochloric acid.

[0018] In the above mixing solution application step, the mixing solution can be applied to at least one surface of the base material with a thickness of 10 μm or more and 1,000 μm or less.

[0019] In the above heat treatment step, the cold-rolled steel sheet coated with the above mixed solution can be heat-treated at a heat treatment temperature of 150°C or higher and 200°C or lower.

[0020] In the above heat treatment step, the cold-rolled steel sheet coated with the above mixed solution can be heat-treated for a heat treatment time of 5 minutes or more and 10 minutes or less.

[0021] Other aspects, features, and advantages other than those described above will become clear from the following specific details, claims, and drawings for implementing the invention. Effects of the invention

[0022] According to one embodiment of the present invention as described above, a cold-rolled steel sheet with excellent fire-resistant properties and a method for manufacturing the same can be provided. Of course, the scope of the present invention is not limited by these effects. Brief explanation of the drawing

[0023] FIG. 1 is a cross-sectional view schematically showing a cold-rolled steel sheet according to one embodiment of the present invention. FIG. 2 is a flowchart illustrating a method for manufacturing a cold-rolled steel sheet according to one embodiment of the present invention. FIG. 3 is a drawing showing a cross-section of a cold-rolled steel sheet according to one embodiment of the present invention. Figure 4 is a graph showing the elemental content of a refractory layer of a cold-rolled steel sheet according to one embodiment of the present invention. FIG. 5 is a drawing showing the surface condition of a cold-rolled steel sheet after a fire simulation heat treatment test according to one embodiment of the present invention. Figure 6 is a drawing showing the surface condition of a cold-rolled steel sheet after a fire simulation heat treatment test according to one comparative example of the present invention. Specific details for implementing the invention

[0024] The present invention will be described in detail below. However, in describing the present invention, if it is determined that a detailed description of related known technologies or configurations may unnecessarily obscure the essence of the present invention, such detailed description will be omitted.

[0025] In the following embodiments, terms such as first, second, etc. are used not in a limiting sense, but for the purpose of distinguishing one component from another component.

[0026] In the following examples, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0027] In the following embodiments, when various components such as layers, films, regions, and plates are described as being "on" another component, this includes not only cases where they are "directly on" another component, but also cases where another component is interposed between them.

[0028] In the drawings, the size of components may be exaggerated or reduced for convenience of explanation. For example, the size and thickness of each component shown in the drawings are depicted arbitrarily for convenience of explanation, and therefore the present invention is not necessarily limited to what is illustrated.

[0029] In the following embodiments, terms such as "include" or "have" mean that the features or components described in the specification are present, and do not preclude the possibility that one or more other features or components may be added.

[0030] In this specification, "A and / or B" indicates the case where it is A, B, or both A and B. Additionally, in this specification, "at least one of A and B" indicates the case where it is A, B, or both A and B.

[0031] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0032] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0033] FIG. 1 is a cross-sectional view schematically showing a cold-rolled steel sheet according to one embodiment of the present invention.

[0034] Referring to FIG. 1, a cold-rolled steel sheet according to one embodiment of the present invention may include a base material (100) and a refractory layer (200) formed on at least one surface of the base material (100).

[0035] The base material (100) may include a steel plate that has undergone a hot rolling process and a cold rolling process.

[0036] The refractory layer (200) is an oxide layer formed on the base material (100), which blocks contact between the surface of the base material (100) and oxygen, thereby improving the refractory properties of the cold-rolled steel sheet.

[0037] In one embodiment, the refractory layer (200) may include titanium oxide.

[0038] In one embodiment, the refractory layer (200) may contain 15 wt% or more and 25 wt% or less of titanium (Ti), 25 wt% or more and 35 wt% or less of silicon (Si), 45 wt% or more and 50 wt% or less of oxygen (O), 0.5 wt% or more and 5 wt% or less of iron (Fe), and other unavoidable impurities.

[0039] Preferably, the refractory layer (200) may contain 19 weight% or more and 22 weight% or less of titanium (Ti), 30 weight% or more and 32 weight% or less of silicon (Si), 46 weight% or more and 49 weight% or less of oxygen (O), 1 weight% or more and 2 weight% or less of iron (Fe), and other unavoidable impurities.

[0040] When the refractory layer (200) has the aforementioned elemental content, the reaction between the surface of the base material (100) and oxygen is minimized, thereby maximizing the refractory properties of the cold-rolled steel sheet.

[0041] In one embodiment, the thickness of the refractory layer (200) may be 3 μm or more and 8 μm or less. In one embodiment, the thickness of the refractory layer (200) may be 6 μm or more and 7 μm or less.

[0042] If the thickness of the refractory layer (200) is too thin, the refractory properties of the cold-rolled steel sheet cannot be sufficiently secured, and if the thickness of the refractory layer (200) is too thick, the manufacturing cost may increase excessively.

[0043] Hereinafter, a method for manufacturing a cold-rolled steel sheet according to one embodiment of the present invention is described.

[0044] FIG. 2 is a flowchart illustrating a method for manufacturing a cold-rolled steel sheet according to one embodiment of the present invention.

[0045] Referring to FIG. 2, a method for manufacturing a cold-rolled steel sheet according to one embodiment of the present invention may include a mixed solution preparation step (S100), a mixed solution application step (S200), and a heat treatment step (S300).

[0046] In the mixed solution preparation step (S100), a mixed solution to be applied to the base material can be prepared.

[0047] Specifically, in the mixed solution preparation step (S100), a mixed solution can be prepared by mixing titanium oxide acetylacetonate (TiO(acac)2) powder with an organic silane solvent.

[0048] In one embodiment, the organic silane solvent may include a silane-based sol-gel resin formed by combining four or more types of silane compounds.

[0049] In one embodiment, the silane-based sol-gel resin may be formed by combining a first silane, a second silane, a third silane, and a fourth silane under an acid catalyst and a solvent.

[0050] The first silane may be selected from the group consisting of tetraethyl orthosilicate, tetramethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane.

[0051] The second silane is selected from the group consisting of tetraethyl orthosilicate, tetramethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane, and may be different from the first silane.

[0052] The tertiary silane may be selected from the group consisting of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropylmethyldiethoxysilane.

[0053] The 4th silane may be selected from the group consisting of 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropyltriethoxysilane.

[0054] The acid catalyst may include at least one selected from the group consisting of acetic acid, formic acid, lactic acid, nitric acid, and hydrochloric acid.

[0055] In one embodiment, the mixed solution may contain 10 volume% or more and 50 volume% or less of titanium oxide acetylacetonate based on the total volume of the mixed solution.

[0056] If titanium oxide acetylacetonate is included in an amount of less than 10 volume%, a refractory layer containing titanium oxide is not sufficiently formed, and the refractory properties of the cold-rolled steel sheet may not be excellent. If titanium oxide acetylacetonate is included in an amount of more than 50 volume%, problems such as the mixed solution not being properly applied to the base material may occur, making it difficult to form a high-quality refractory layer.

[0057] In the mixed solution application step (S200), the mixed solution prepared in the mixed solution preparation step (S100) can be applied to the base material.

[0058] In the mixed solution application step (S200), the prepared mixed solution can be applied to at least one surface of the base material with a thickness of 10 μm or more and 1,000 μm or less.

[0059] If the thickness of the applied mixed solution is too small, a refractory layer containing titanium oxide is not sufficiently formed, which may result in poor refractory properties of the cold-rolled steel sheet; if the thickness of the applied mixed solution is too large, problems such as increased process costs and increased process time may occur.

[0060] A heat treatment step (S300) can be performed after the mixed solution application step (S200).

[0061] In the heat treatment step (S300), the silane solvent can be vaporized, and the titanium oxide acetylacetonate in the mixed solution can react with oxygen in the atmosphere to form a refractory layer on the base material.

[0062] In the heat treatment step (S300), the cold-rolled steel sheet coated with the mixed solution can be heat-treated at a heat treatment temperature of 150°C or higher and 200°C or lower.

[0063] If the heat treatment temperature is too low, the solvent may vaporize incompletely, and residual solvent may remain on the steel plate surface even after the heat treatment step, degrading surface properties. Conversely, if the heat treatment temperature is too high, thermal shock may occur when the steel plate cools after heat treatment, causing cracks in the refractory layer formed on the surface of the cold-rolled steel plate.

[0064] In the heat treatment step (S300), the cold-rolled steel sheet coated with the mixed solution can be heat-treated for a heat treatment time of 5 minutes or more and 10 minutes or less.

[0065] If the heat treatment time is too short, the solvent may vaporize incompletely, and residual solvent may remain on the steel plate surface even after the heat treatment step, degrading surface properties. On the other hand, if the heat treatment time is too long, thermal shock may occur when the steel plate cools after treatment, causing cracks in the refractory layer formed on the surface of the cold-rolled steel plate.

[0066] In the heat treatment step (S300), as the mixed solution is heated, the solvent is vaporized, and titanium oxide acetylacetonate can react with oxygen through a reaction as shown in Chemical Formula 1 to form titanium oxide (TiO2).

[0067] <Chemical Formula 1>

[0068] TiO(C5H7O2)2+ 12O2→ TiO2+ 10CO2+ 7H2O

[0069] Therefore, the refractory layer formed on the cold-rolled steel sheet may contain titanium oxide (TiO2).

[0070] Specifically, the refractory layer formed on the cold-rolled steel sheet that has undergone the heat treatment step (S300) may contain 15 wt% or more and 25 wt% or less of titanium (Ti), 25 wt% or more and 35 wt% or less of silicon (Si), 45 wt% or more and 50 wt% or less of oxygen (O), 0.5 wt% or more and 5 wt% or less of iron (Fe), and other unavoidable impurities.

[0071] Preferably, the refractory layer may contain 19 wt% or more and 22 wt% or less of titanium (Ti), 30 wt% or more and 32 wt% or less of silicon (Si), 46 wt% or more and 49 wt% or less of oxygen (O), 1 wt% or more and 2 wt% or less of iron (Fe), and other unavoidable impurities.

[0072] Hereinafter, the structure and operation of the present invention will be explained in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be interpreted in any way as limiting the present invention.

[0073] Experimental Example

[0074] The present invention will be explained in more detail below through experimental examples. However, the following experimental examples are intended to explain the present invention more specifically, and the scope of the present invention is not limited by the following experimental examples. The following experimental examples may be appropriately modified or changed by those skilled in the art within the scope of the present invention.

[0075]

[0076] The table above indicates the titanium oxide acetylacetonate (TiO(acac)2) content (based on the total volume of the mixed solution), whether an organic silane solvent was used as the solvent, and whether oxide scale formed on the steel plate surface after a fire simulation heat treatment test, according to the examples and comparative examples.

[0077] Examples 1 to 5 involved applying a mixed solution containing titanium oxide acetylacetonate as shown in Table 1 to a thickness of 10 μm onto a substrate and heat treating it at a heat treatment temperature of 170 °C for 7 minutes.

[0078] FIG. 3 is a cross-sectional view of a cold-rolled steel sheet according to one embodiment of the present invention (e.g., Example 1), and FIG. 4 is a graph showing the elemental content of the refractory layer of a cold-rolled steel sheet according to one embodiment of the present invention. Specifically, FIG. 4 is a graph showing the results of analyzing the refractory layer of Example 1 using Energy Dispersive X-ray Spectroscopy (EDS).

[0079] Referring to FIGS. 3 and 4, in Example 1, a refractory layer is well formed on a base material, and the refractory layer contains 15 wt% or more and 25 wt% or less of titanium (Ti), 25 wt% or more and 35 wt% or less of silicon (Si), 45 wt% or more and 50 wt% or less of oxygen (O), and 0.5 wt% or more and 5 wt% or less of iron (Fe).

[0080] Comparative Examples 1 and 4 were prepared in the same manner as the Examples, except that no organic silane solvent was used, purified water was used as the solvent, and a mixed solution containing titanium oxide acetylacetonate as shown in Table 1 was used.

[0081] Comparative Examples 2, 3, and 5 were prepared in the same manner as the Examples, except that a mixed solution containing titanium oxide acetylacetonate as shown in Table 1 was used.

[0082] In the present invention, the fire simulation heat treatment test was performed by heat-treating a cold-rolled steel sheet with a refractory layer formed according to the examples and comparative examples at a temperature of 950°C for at least 10 minutes in an atmospheric environment, and then observing whether an oxide scale formed on the surface.

[0083] FIG. 5 is a drawing showing the surface condition of a cold-rolled steel sheet after a fire simulation heat treatment test according to one embodiment of the present invention, and FIG. 6 is a drawing showing the surface condition of a cold-rolled steel sheet after a fire simulation heat treatment test according to one comparative example of the present invention. Specifically, FIG. 5 is a drawing showing the surface condition of a cold-rolled steel sheet after a fire simulation heat treatment test according to Example 1, and FIG. 6 is a drawing showing the surface condition of a cold-rolled steel sheet after a fire simulation heat treatment test according to Comparative Example 2.

[0084] The examples contained 10 volume% or more and 50 volume% or less of titanium oxide acetylacetonate mixed in an organic silane solvent. Therefore, even when heat-treated in a fire-simulated atmosphere, no oxide scale formed on the surface as shown in Fig. 5, exhibiting excellent fire-resistant properties.

[0085] On the other hand, Comparative Example 1 had a titanium oxide acetylacetonate content of less than 10 volume% and did not use an organic silane solvent, so an oxide scale formed on the surface after a fire simulation heat treatment test.

[0086] Comparative Examples 2 and 3 used an organic silane solvent, but since the titanium oxide acetylacetonate content was less than 10 volume%, an oxide scale formed on the surface after the fire simulation heat treatment test as shown in Fig. 6.

[0087] Comparative Example 4 satisfies the titanium oxide acetylacetonate content of 10 volume% or more and 50 volume% or less, but does not use an organic silane solvent, so an oxide scale formed on the surface after a fire simulation heat treatment test.

[0088] Comparative Example 5 had a titanium oxide acetylacetonate content of more than 50 volume%, so oxide scale formed on the surface after the fire simulation heat treatment test.

[0089] In other words, unlike the embodiments, the comparative examples exhibit inferior fire resistance properties.

[0090] Therefore, it can be seen that the cold-rolled steel sheet produced by the cold-rolled steel sheet manufacturing method described above was able to obtain excellent fire-resistant properties.

[0091] The embodiments of the present invention are merely illustrative, and those skilled in the art will understand that various modifications and equivalent alternative embodiments are possible therefrom. Accordingly, the true scope of technical protection of the present invention should be determined by the technical spirit of the appended claims. Explanation of the symbols

[0092] 100: Base material 200: Refractory layer

Claims

Claim 1 A cold-rolled steel sheet comprising: a base material; and a refractory layer formed on at least one surface of the base material; wherein the refractory layer comprises 15 wt% or more and 25 wt% or less of titanium (Ti), 25 wt% or more and 35 wt% or less of silicon (Si), 45 wt% or more and 50 wt% or less of oxygen (O), 0.5 wt% or more and 5 wt% or less of iron (Fe), and other unavoidable impurities. Claim 2 A cold-rolled steel sheet according to claim 1, wherein the thickness of the refractory layer is 3 μm or more and 8 μm or less. Claim 3 In claim 1, the refractory layer comprises titanium oxide, and the cold-rolled steel sheet. Claim 4 A method for manufacturing a cold-rolled steel sheet, comprising: a mixed solution preparation step of preparing a mixed solution to be applied to a base material; a mixed solution application step of applying the mixed solution to at least one surface of the base material; and a heat treatment step of heat-treating the cold-rolled steel sheet coated with the mixed solution to form a refractory layer on the base material comprising 15 wt% or more and 25 wt% or less of titanium (Ti), 25 wt% or more and 35 wt% or less of silicon (Si), 45 wt% or more and 50 wt% or less of oxygen (O), 0.5 wt% or more and 5 wt% or less of iron (Fe), and other unavoidable impurities; wherein the base material comprises a steel sheet that has undergone a hot rolling process and a cold rolling process, and the refractory layer comprises titanium oxide. Claim 5 A method for manufacturing a cold-rolled steel sheet according to claim 4, wherein in the step of preparing the mixed solution, titanium oxide acetylacetonate powder is mixed with an organic silane solvent to prepare a mixed solution. Claim 6 A method for manufacturing a cold-rolled steel sheet according to claim 5, wherein the mixed solution comprises 10 volume% or more and 50 volume% or less of the titanium oxide acetylacetonate based on the total volume of the mixed solution. Claim 7 A method for manufacturing cold-rolled steel sheets according to claim 5, wherein the organic silane solvent comprises a silane-based sol-gel resin. Claim 8 In claim 7, the silane-based sol-gel resin is formed by combining a first silane, a second silane, a third silane, and a fourth silane under an acid catalyst and a solvent, wherein the first silane is selected from the group consisting of tetraethyl orthosilicate, tetramethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane, the second silane is selected from the group consisting of tetraethyl orthosilicate, tetramethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane, but is different from the first silane, and the third silane is 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and A method for manufacturing a cold-rolled steel sheet, wherein the fourth silane is selected from the group consisting of 3-glycidoxypropylmethyldiethoxysilane, the fourth silane is selected from the group consisting of 3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and the acid catalyst comprises at least one selected from the group consisting of acetic acid, formic acid, lactic acid, nitric acid, and hydrochloric acid. Claim 9 A method for manufacturing a cold-rolled steel sheet according to claim 4, wherein in the step of applying the mixed solution, the mixed solution is applied to at least one surface of the base material to a thickness of 10 μm or more and 1,000 μm or less. Claim 10 A method for manufacturing a cold-rolled steel sheet according to claim 4, wherein in the heat treatment step, the cold-rolled steel sheet coated with the mixed solution is heat-treated at a heat treatment temperature of 150°C or higher and 200°C or lower. Claim 11 A method for manufacturing a cold-rolled steel sheet according to claim 10, wherein in the heat treatment step, the cold-rolled steel sheet coated with the mixed solution is heat-treated for a heat treatment time of 5 minutes or more and 10 minutes or less.

Citation Information

Patent Citations

  • Method for manufacturing silica coating film on metal matrix

    KR100287964B1

  • Metal coated with graded-ceramic and manufacturing method thereof

    KR100824275B1

  • Uncombustible color steel sheet and method of manufacturing the same

    KR1020200117658A