Method for manufacturing a treated wafer using double-sided pressure-sensitive adhesive
A double-sided pressure-sensitive adhesive with balanced peel strengths between glass and Si-based wafers facilitates stable mechanical peeling, addressing separation challenges and enhancing semiconductor processing efficiency.
Patent Information
- Application Number
- KR1020247025090
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-28
- Filing Date
- 2022-12-01
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-12-01
AI Technical Summary
Existing wafer support systems face challenges in stably separating wafers from laminates during mechanical peeling, often leading to unintended delamination or damage due to imbalanced adhesive strengths at different interfaces.
A double-sided pressure-sensitive adhesive with specific ratios of peel strengths between a glass substrate and a Si-based wafer, ensuring stable separation through mechanical peeling by maintaining a 10° peel strength ratio of 1.1 or greater between the adhesive layers.
The adhesive enables stable separation of wafers from laminates without damaging electronic components, enhancing handling and processing stability while reducing costs and improving productivity in semiconductor manufacturing.
Smart Images

Figure 112024080708889-PCT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a double-sided pressure-sensitive adhesive for use in a wafer processing method (wafer support system) in which the wafer is processed while being temporarily fixed to a support. More specifically, the invention relates to a double-sided pressure-sensitive adhesive in which the handling properties of the wafer are improved by temporarily fixing the support and the wafer, and which can be used in various processing processes, while allowing the support and the wafer to be stably separated by a relatively simple method such as mechanical peeling. Background Technology
[0002] In semiconductor manufacturing processes, temporary fixation is often considered necessary or desirable during wafer processing due to reasons such as the thinness of the wafer or its susceptibility to breakage. For example, due to the high integration of semiconductor devices, thin grinding of wafers with functional layers formed thereon is widely performed. However, when grinding to an extreme thinness, the wafer cannot be supported by tape alone, so it has been proposed to perform post-thin grinding processing by temporarily fixing it to a hard carrier (support) using a pressure-sensitive adhesive. A semiconductor manufacturing process utilizing such a support is called a wafer support system.
[0003] As methods for peeling off a support after processing, methods utilizing gas generation from a pressure-sensitive adhesive (e.g., see Patent Document 1), peeling using a laser, peeling by melting the resin of the pressure-sensitive adhesive to slide off the carrier, and peeling by lifting the carrier from one end (mechanical peeling) have been proposed.
[0004] Mechanical peeling is a method with excellent cost advantages due to the relatively simple equipment. However, because the principle of mechanical peeling applies peeling force at least to the wafer / pressure adhesive interface and the pressure adhesive / support interface, it has not always been easy to achieve stable peeling at the desired interface. If peeling occurs at an unintended interface (e.g., the wafer / pressure adhesive interface), problems such as damage to the support or electronic components may arise during support peeling.
[0005] On the other hand, while the adhesion strength of the unintended interface can be increased to prevent unintended delamination from the interface during mechanical peeling, if the adhesion strength is increased too much, for example, peeling of the pressure-sensitive adhesive from the wafer becomes difficult. Prior art literature
[0006] Patent Document 1 International Publication No. 2014 / 024861 A1 Pamphlet The problem to be solved
[0007] In light of the above technical background, the objective of the present invention is to provide a double-sided pressure-sensitive adhesive for use in a wafer support system, which can stably separate a wafer from a laminate through a relatively simple process such as mechanical peeling. means of solving the problem
[0008] The inventors have discovered, as a result of careful consideration, that when the ratio between the peel strength between a specific glass substrate and a specific adhesive and the peel strength between the adhesive and a specific Si-based wafer, measured under specific conditions, satisfies specific conditions, the wafer can be stably separated from the laminate by a relatively simple process such as mechanical peeling, and thus have completed the present invention.
[0009] That is, the present invention is,
[0010] [1]
[0011] A double-sided pressure-sensitive adhesive for use in a wafer support system, having A for one pressure-sensitive adhesive and B for the other pressure-sensitive adhesive,
[0012] The present invention relates to a double-sided pressure-sensitive adhesive in which the ratio of the 10° peel strength P1 between a borosilicate glass silicon backside grinding support substrate / pressure-sensitive adhesive surface A and the 10° peel strength P2 between a Si mirror wafer / pressure-sensitive adhesive surface B, measured by maintaining the angle between the peeled layers at 10°, is 1.1 or greater.
[0013] The following [2] to [6] are all preferred forms or embodiments of the present invention.
[0014] [2]
[0015] The double-sided adhesive described in [1], having a 10° peel strength P1 of 12N / 25mm or less.
[0016] [3]
[0017] A double-sided adhesive as described in [1] or [2], comprising an adhesive layer A1 having the adhesive surface A and an adhesive layer B1 having the adhesive surface B, wherein the adhesive layer A1 and the adhesive layer B1 have different compositions.
[0018] [4]
[0019] A double-sided adhesive described in any one of [1] to [3], wherein at least one of the adhesive layer A1 or the adhesive layer B1 contains a curable adhesive component.
[0020] [5]
[0021] A double-sided adhesive having a substrate film between the adhesive layer A1 and the adhesive layer B1, as described in any one of [1] to [4].
[0022] [6]
[0023] A double-sided adhesive described in any one of [1] to [5], wherein at least one of the above adhesive layer A1 or above adhesive layer B1 contains a release agent. Effects of the invention
[0024] According to the double-sided adhesive of the present invention, the handling performance of thin or easily damaged wafers is improved, allowing the wafer to be processed stably in various processing processes, while effectively suppressing unintended delamination at the interface, and allowing the wafer to be stably separated and removed after processing through a relatively simple and low-cost process such as mechanical delamination. As a result, it is possible to perform multiple and / or multi-faceted processes on the wafer with high productivity and yield without damaging electronic components such as functional layers formed on the wafer, thereby contributing significantly to the improvement of productivity of electronic components such as electronic devices. Brief explanation of the drawing
[0025] [Fig. 1] This is a schematic diagram illustrating mechanical peeling in a laminate formed using the double-sided pressure-sensitive adhesive of the present invention. [Fig. 2] A schematic diagram illustrating the separation of a support from a laminate, where (a) represents a preferred separation form and (b) to (c) represents undesirable separation forms. [Fig. 3] This is a schematic diagram illustrating a method for measuring 10° peel strength specified in the present invention, wherein (a) shows a case where a measurement is performed using a sample for measuring 10° peel strength P1 in which a pressure adhesive layer A1 on the side in contact with a support is laminated on a substrate film, (b) shows a case where a measurement is performed using a sample for measuring 10° peel strength P2 in which a pressure adhesive layer B1 on the side in contact with a wafer is laminated on a substrate film, (c) shows a case where a measurement sample with a polyimide film laminated is prepared for a double-sided pressure adhesive without a substrate film and a measurement of 10° peel strength P1 is performed, and (d) shows a case where a measurement sample with a polyimide film laminated is prepared for a double-sided pressure adhesive without a substrate film and a measurement of 10° peel strength P2 is performed. [Fig. 4] This is a schematic diagram showing a method for evaluating the removeability from a wafer in the double-sided pressure adhesive of the present invention. [Fig. 5] This is a schematic diagram showing a laminate formed using a double-sided adhesive having a substrate film, which is an embodiment of the present invention. [Fig. 6] This is a schematic diagram showing a laminate formed using the double-sided adhesive of the present invention. Specific details for implementing the invention
[0026] The present invention is,
[0027] A double-sided pressure-sensitive adhesive for use in a wafer support system, having A for one pressure-sensitive adhesive and B for the other pressure-sensitive adhesive,
[0028] The above double-sided adhesive is a borosilicate glass silicon backside grinding support substrate / point adhesive surface A measured by maintaining the angle between the peeled layers at 10°, wherein the ratio of the 10° peel strength P1 between the Si mirror wafer / point adhesive surface B and the 10° peel strength P2 between the Si mirror wafer / point adhesive surface B is 1.1 or greater.
[0029] That is, the double-sided adhesive of the present invention has different 10° peel strengths between A and between B of a specific glass substrate / adhesive and a specific Si-based wafer / adhesive.
[0030] Double-sided adhesive
[0031] Since the double-sided pressure-sensitive adhesive of the present invention is used to temporarily fix a wafer to a support, it is desirable that it can be easily peeled off from the support and the wafer. Accordingly, the double-sided pressure-sensitive adhesive of the present invention has sufficient adhesive strength to fix the wafer to the support, but has sufficiently low adhesive strength to allow for peeling.
[0032] Specifically, when peeling from a laminate by a mechanical peeling method, it is preferable that the ratio of the peel strength (referred to as "10° peel strength" in this specification) measured by maintaining the angle between each peeled layer at 10° is P2 / P1 1.1 or higher.
[0033] Here, P1 is a 10° peel strength between A if it is a specific glass substrate / point bond, more specifically between A if it is a borosilicate glass silicon or a grinding support substrate / point bond, and P2 is a 10° peel strength between B if it is a specific Si-based wafer / point bond, more specifically between B if it is a Si mirror wafer / point bond.
[0034] The double-sided pressure-sensitive adhesive of the present invention may be a single layer or a laminate of multiple layers.
[0035] In the case of a laminate of multiple layers, the double-sided adhesive of the present invention comprises an adhesive layer A1 having an adhesive surface A and an adhesive layer B1 having an adhesive surface B, wherein the adhesive layer A1 and the adhesive layer B1 may have different compositions. In this case, one adhesive surface A may be configured to have a predetermined peel strength between it and a specific glass substrate, and the other adhesive surface B may be configured to have a predetermined peel strength between it and a specific Si-based wafer. In this case, it is preferable that the adhesive layer A1 and the adhesive layer B1 have different compositions. In this case, the adhesive layer A1 and the adhesive layer B1 may be configured as layers in the general sense in which the composition changes discontinuously at the interface, but they may also be configured as so-called gradient compositions in which the composition changes continuously.
[0036] The adhesive components used in the double-sided adhesive of the present invention may include, for example, rubber-based, acrylic-based, epoxy-based, urethane-based, allyl-based, silicone-based, fluorine-based, and polyimide-based adhesive components. Among these, acrylic-based or silicone-based adhesive components are preferred because they have heat resistance and allow for easy adjustment of adhesive strength.
[0037] The above adhesive component may be a curable adhesive component or a non-curable adhesive component. It is preferable that the component be a curable adhesive component, as curing it before heat treatment makes it difficult for voids to form during heat treatment in the manufacturing process, thereby suppressing adhesion sagging caused by high temperatures during heat treatment and facilitating easy peeling without leaving any adhesive residue.
[0038] Examples of the above-mentioned curable adhesive components include photocurable adhesive components that are crosslinked and cured by light irradiation, or thermocurable adhesive components that are crosslinked and cured by heating.
[0039] Examples of the above-mentioned photocurable adhesive components or thermosetting adhesive components include, for instance, monomers, oligomers, or polymers such as acrylic, epoxy, urethane acrylate, epoxy acrylate, silicone acrylate, or polyester acrylate as curing components, and photocurable adhesive components or thermosetting adhesive components containing a photopolymerization initiator or a thermal polymerization initiator.
[0040] As for the polymer of the acrylic adhesive component above, for example, it can be obtained by presynthesizing a (meth)acrylic polymer having functional groups within its molecule (hereinafter referred to as a functional group-containing (meth)acrylic polymer) and reacting it with a compound having a radical polymerizable unsaturated bond that reacts with the functional group within its molecule (hereinafter referred to as a functional group-containing unsaturated compound).
[0041] The above functional group-containing (meth)acrylic polymer is obtained by using an alkyl acrylate ester and / or an alkyl methacrylate ester, in which the number of carbon atoms of the alkyl group is typically in the range of 2 to 18, as the main monomer, and copolymerizing this with a functional group-containing monomer and, if necessary, other modifying monomers copolymerizable with them by a conventional method. The weight average molecular weight of the above functional group-containing (meth)acrylic polymer is typically about 200,000 to 2,000,000.
[0042] Examples of the above functional group-containing monomers include carboxyl group-containing monomers such as acrylic acid and methacrylic acid, hydroxyl group-containing monomers such as hydroxyethyl acrylic acid and hydroxyethyl methacrylate, epoxy group-containing monomers such as glycidyl acrylic acid and glycidyl methacrylate, isocyanate group-containing monomers such as ethyl acrylic acid and ethyl methacrylate, and amino group-containing monomers such as aminoethyl acrylic acid and aminoethyl methacrylate.
[0043] Other copolymerizable modifying monomers include, for example, various monomers used in common (meth)acrylic polymers such as vinyl acetate, acrylonitrile, and styrene.
[0044] As for the functional group-containing unsaturated compound to be reacted with the above functional group-containing (meth)acrylic polymer, the same as the functional group-containing monomer described above may be used depending on the functional group of the above functional group-containing (meth)acrylic polymer. For example, if the functional group of the above functional group-containing (meth)acrylic polymer is a carboxyl group, an epoxy group-containing monomer or an isocyanate group-containing monomer is used. If the same functional group is a hydroxyl group, an isocyanate group-containing monomer is used. If the same functional group is an epoxy group, a carboxyl group-containing monomer or an amide group-containing monomer such as acrylamide is used. If the same functional group is an amino group, an epoxy group-containing monomer is used.
[0045] The above photopolymerization initiator may be activated, for example, by irradiating with light of a wavelength of 250 to 800 nm. Examples of such photopolymerization initiators include acetophenone derivative compounds such as methoxyacetophenone, benzoin ether compounds such as benzoin propyl ether and benzoin isobutyl ether, ketal derivative compounds such as benzyl dimethyl ketal and acetophenone diethyl ketal, phosphine oxide derivative compounds, bis(η5-cyclopentadienyl)titanocene derivative compounds, benzophenone, mihiraketone, chlorothioxantone, dodecylthioxantone, dimethylthioxantone, diethylthioxantone, α-hydroxycyclohexylphenyl ketone, and photoradical polymerization initiators such as benzophenone, mihiraketone, chlorothioxantone, dodecylthioxantone, dimethylthioxantone, diethylthioxantone, α-hydroxycyclohexylphenyl ketone, and 2-hydroxymethylphenylpropane. These photopolymerization initiators may be used alone or in combination of two or more.
[0046] Examples of the above thermal polymerization initiators include those that decompose by heat to generate active radicals that initiate polymerization curing. Specifically, for example, t-butylperoxy-2-ethyl hexanoic acid, bis(4-methylbenzoyl)peroxide, benzoyl peroxide, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-bis-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarboxylic acid, t-butylperoxyacetate, 2,2-bis-(t-butylperoxy)butane, 4,4-bis-(t-butylperoxy)pentanoate n-butyl, bis-t-hexyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, bis(2-t-butylperoxyisopropyl)benzene, Examples include t-butylcumyl peroxide, di-t-butyl 2,5-dimethyl-2,5-bis(t-butylperoxy)hexine peroxide, and diisopropylbenzene hydroperoxide.
[0047] Among these thermal polymerization initiators, commercially available ones are not particularly limited, but examples include perbutyl O, Nyper BMT, Nyper BW, perhexa HC, perhexa C, pertetra A, perhexyl I, perbutyl A, perhexa 22, perhexa V, perhexyl D, perkmil D, perhexa 25B, perbutyl P, perbutyl C, perhexin 25B, perkmil P (all of which are Japanese equivalents), and Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.). These thermal polymerization initiators may be used alone or in combination of two or more types.
[0048] The oligomer or monomer used as a curing component generally has a molecular weight of 10,000 or less and has 1 to 40 radical polymerizable unsaturated bonds within the molecule. From the perspective of three-dimensional networking, it is preferable that the number of radical polymerizable unsaturated bonds be 2 or more.
[0049] Examples of the oligomers or monomers used as the curing components include trimethylolpropane triacrylate, tetramethylolmethane tetriacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol monohydroxypentaacrylate, dipentaerythritol hexaacrylate, or methacrylates of the above. Other examples include 1,4-butylene glycol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, commercially available oligoester acrylates, urethane acrylates, and methacrylates of the above. These multifunctional oligomers or monomers may be used alone or in combination of two or more.
[0050] The double-sided pressure-sensitive adhesive of the present invention may, if necessary, contain various thermal crosslinking agents such as acrylic polymers not having unsaturated double bonds, isocyanate compounds, melamine compounds, and epoxy compounds, or known additives such as release agents, plasticizers, resins, surfactants, waxes, and fine particle fillers.
[0051] In the double-sided pressure-sensitive adhesive of the present invention, it is preferable to use a release agent to adjust the peel strength between a specific glass substrate / pressure-sensitive surface A and / or between a specific Si-based wafer / pressure-sensitive surface B.
[0052] As for the release agent, it is not particularly limited as long as it exhibits a release effect. Examples include hydrocarbon compounds, silicone compounds, fluorine compounds, and polyethylene waxes, carnabar wax, montanic acid, and stearic acid, which are known as release agents for plastic materials. Among these, silicone compounds and fluorine compounds are preferred, and silicone compounds and fluorine compounds having functional groups capable of crosslinking with curable adhesives are more preferred.
[0053] In particular, since the silicone compound has excellent heat resistance, it prevents the adhesive from sticking even after treatment involving heating at 200°C or higher, and facilitates peeling by bleeding out to the interface of the substrate during peeling. Since the silicone compound has functional groups capable of crosslinking with the curable adhesive, it chemically reacts with the curable adhesive through light irradiation or heating and is introduced into the curable adhesive, so the silicone compound does not adhere to the substrate and contaminate it. In addition, by incorporating the silicone compound, the effect of preventing adhesive residue on the semiconductor chip is also exhibited.
[0054] In addition, other release agents include plasticizers. Plasticizers are generally not particularly limited as long as they reduce the adhesive strength of the adhesive to the substrate. Examples of plasticizers include trimellitic acid esters, pyromellitic acid esters, phthalic acid esters, and adipic acid esters.
[0055] The amount of release agent added is not specifically limited, but the amount is appropriately determined to obtain a release effect. Meanwhile, the amount added is controlled so as not to be excessive so as not to significantly impair the adhesive function of the double-sided adhesive of the present invention. For example, for a total of 100 parts by mass of the double-sided adhesive, it is preferable to adjust the amount according to the peel strength based on an amount of addition of typically 0.1 to 5 parts by mass, preferably 0.1 to 3 parts by mass, and more preferably 0.1 to 1 part by mass.
[0056] In addition, if a plasticizer is added, it is desirable to adjust the amount according to the peeling force based on an amount of addition of typically 5 to 50 parts by mass, preferably 10 to 50 parts by mass, and more preferably 20 to 40 parts by mass.
[0057] In this embodiment, these release agents may be used alone or in combination of multiple agents.
[0058] The thickness of the double-sided pressure-sensitive adhesive of the present invention is not particularly limited, but a preferred lower limit is 5 μm and a preferred upper limit is 250 μm, and a more preferred lower limit is 10 μm and a more preferred upper limit is 200 μm. When the thickness of the double-sided pressure-sensitive adhesive is within this range, it can absorb irregularities of the wafer and be temporarily fixed to the support with sufficient strength, and it becomes easier to adjust the peeling force to an appropriate range when peeling the double-sided pressure-sensitive adhesive.
[0059] In one embodiment, the double-sided pressure-sensitive adhesive of the present invention is preferably a so-called double-sided pressure-sensitive adhesive tape having a substrate film between the pressure-sensitive adhesive layer A1 and the pressure-sensitive adhesive layer B1. In this embodiment, the pressure-sensitive adhesive layer A1 and the pressure-sensitive adhesive layer B1 can be designed with the viewpoint of optimizing the peel strength between the pressure-sensitive adhesive surface A or the pressure-sensitive adhesive surface B and a specific glass substrate or a specific Si-based wafer. Since the substrate film can be designed with the viewpoint of the mechanical strength or handling properties of the entire double-sided pressure-sensitive adhesive of the present invention or the entire laminate, it is particularly advantageous with the viewpoint of optimizing the performance of the double-sided pressure-sensitive adhesive.
[0060] Figure 5 shows an example of a laminate using a double-sided adhesive having a substrate film between the above-mentioned adhesive layer A1 and the above-mentioned adhesive layer B1. In the figure, 11 represents a support, 20 represents the adhesive layer A1, 19 represents the substrate film, 18 represents the adhesive layer B1, and 13 represents a wafer.
[0061] There are no particular limitations on the material of the base film, but it is preferable to use a plastic film. Examples of plastic films include films, sheets, sheets having a network structure, and perforated sheets made of acrylic, olefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), nylon, urethane, polyetheretherketone (PEEK), liquid crystal polymer (LCP), and polyimide. From the perspective of handling, PET, PEN, or polyimide films are preferred.
[0062] Support
[0063] It is desirable for the support to have sufficient strength and rigidity, as well as excellent heat resistance and chemical resistance. By using such a support, it becomes possible to handle the wafer stably even when the wafer has been ground, and to provide the wafer to a large number of and / or various processes without causing bending or the like. For example, a wafer with an electronic circuit formed thereon can be provided to various processes required for manufacturing electronic devices having a stacked structure of semiconductor chips, such as TSV connections.
[0064] Materials preferably used for the support include silicon, sapphire, quartz, metals (e.g., aluminum, copper, steel), and various glasses and ceramics. The support may be composed of a single material, but may be composed of multiple materials and may include other materials deposited on a substrate. The support may have a deposited layer, such as silicon nitride, on a silicon wafer, for example. The support may be surface-treated, such as by forming a silicon layer.
[0065] Depending on the temperature of the process in which the laminate is provided, the support may be composed of plastic. For example, sheets made of plastics such as polyimide, acrylic, polyolefin, polycarbonate, vinyl chloride, ABS, polyethylene terephthalate (PET), nylon, and urethane can be preferably used as the support. Polyimide can be used because it possesses a certain degree of heat resistance.
[0066] A specific glass substrate is preferred as the support when using the double-sided pressure adhesive of the present invention. In particular, when measuring the 10° peel strength P1 of the double-sided pressure adhesive of the present invention, a silicon back-side grinding support substrate made of borosilicate glass is used as the support. More specifically, a silicon back-side grinding support substrate made of heat-resistant borosilicate glass is preferred.
[0067] In order to obtain uniformity of thickness after grinding the wafer, it is desirable for the thickness of the support to be uniform. For example, in order to thin the silicon wafer to 50 μm or less and to achieve uniformity of ±10% or less, the deviation in the thickness of the support must be suppressed to ±2 μm or less.
[0068] There are no specific limitations on the thickness of the support, but from the perspective of effectively preventing wafer curvature, it is preferable that it be 300 μm or more, and particularly preferable that it be 500 μm or more. From the perspective of suppressing the total weight during handling or reducing the stress required for mechanical peeling, it is preferable that it be 1500 μm or less, and particularly preferable that it be 1000 μm or less.
[0069] wafer
[0070] There are no particular restrictions on the wafers processed by being temporarily fixed to a support using the double-sided pressure-sensitive adhesive of the present invention, and any wafer generally used in semiconductor manufacturing processes can be used. Among these, wafers requiring temporary fixation are preferably used because careful handling is required during processing due to reasons such as thinness or susceptibility to breakage. Here, thinness or susceptibility to breakage of the wafer implies, for example, cases where the thickness is temporarily reduced during processing, causing difficulties in handling, and the double-sided pressure-sensitive adhesive of the present invention is used for the temporary fixation of such wafers to a support. Cases of temporary reduction include processing starting from a thin point, reducing a somewhat thick wafer during the process, or further processing a thinned wafer. The thickness of the wafer that is temporarily reduced is typically 1 to 200 μm.
[0071] For example, in the case where a semiconductor wafer with a functional layer processed is temporarily fixed to a support so that the functional layer is on the support side, the opposite side (back side) of the functional layer is ground, ion implantation, annealing, and electrode formation are performed on the back side, and the wafer is separated from the support, the semiconductor wafer in the process corresponds to a wafer.
[0072] A wafer temporarily fixed using the double-sided pressure adhesive of the present invention includes, as described above, a change in state occurring during the process.
[0073] As described above, there are no particular limitations on the wafers that are temporarily fixed using the double-sided adhesive of the present invention, but more specific examples include, for semiconductor wafers, silicon wafers, SiC, AlSb, AlAs, AlN, AlP, BN, BP, BAs, GaSb, GaAs, GaN, GaP, InSb, InAs, InN, or InP, compound semiconductor wafers, quartz wafers, sapphire, glass, mold wafers, etc.
[0074] Silicon wafers or compound semiconductor wafers may be doped.
[0075] A specific Si-based wafer is preferred as the wafer when using the double-sided pressure-sensitive adhesive of the present invention. In particular, a Si mirror wafer is used as the wafer for measuring the 10° peel strength P2 of the double-sided pressure-sensitive adhesive of the present invention.
[0076] An electrical / electronic functional layer may be formed on or within a wafer. Examples of suitable functional layers include electronic circuits, capacitors, transistors, resistors, electrodes, optical elements, MEMS, etc., but may be other microdevices.
[0077] The surface of these functional layers may have a structure, typically an electrode, formed from one or more of the following materials. Examples of materials for the functional layer include silicon, polysilicon, silicon dioxide, (oxy)nitride, metals (e.g., copper, aluminum, gold, tungsten, tantalum), low k dielectrics, polymer dielectrics, and various metal nitrides and metal silicides. The side of the wafer on which the functional layer is formed (functional layer surface) may have a lifted structure such as a solder rise, a metal post, and a filler.
[0078] In addition, the wafer surface may be covered with an oxide film or a nitride film for the formation of a functional layer or for the protection of a functional layer. In addition, the wafer surface may be covered with a passivation film for wafer protection. The 10° peel strength P2 between the Si mirror wafer / point bond B may change due to the presence of such a functional layer or film on the wafer surface, but it does not exceed the range of the preferred 10° peel strength P2 described below and does not significantly affect the peel strength ratio P2 / P1.
[0079] laminate
[0080] According to the double-sided adhesive of the present invention, for example, by fixing a support to one adhesive surface A and fixing a wafer to another adhesive surface B, a laminate consisting of a support / double-sided adhesive / wafer can be obtained. The laminate has sufficient strength and rigidity and can provide the wafer to various semiconductor manufacturing processes while preventing bending or breakage.
[0081] As a method for forming a laminate, a support, a double-sided adhesive, and a wafer can be stacked sequentially. The order of stacking is not particularly limited, and these layers may be stacked at once or sequentially.
[0082] When a pressure-sensitive adhesive is supplied as a liquid curable pressure-sensitive adhesive, etc., the liquid curable pressure-sensitive adhesive, etc. can be applied by spin coating, etc., onto either or both of a wafer or a support to form a pressure-sensitive adhesive or a precursor of a pressure-sensitive adhesive, and then an additional laminate can be formed.
[0083] When a pressure-sensitive adhesive or a pressure-sensitive adhesive precursor is supplied as a solid film, the adhesion strength to the support is typically set lower than that to the wafer side; therefore, to prevent delamination during handling, it is preferable to first attach the film to the wafer and then laminate the support.
[0084] In addition, in cases where the film attachment is performed at atmospheric pressure and only the lamination is formed under reduced pressure, it is preferable to first attach the film to a support and then attach it to the wafer, from the perspective of ensuring good absorption of the wafer's irregularities.
[0085] In the case where a pressure-sensitive adhesive or a precursor of a pressure-sensitive adhesive contains a curable pressure-sensitive adhesive component, it may also be used as a pressure-sensitive adhesive by performing pressure-sensitive adhesive curing in which the curable pressure-sensitive adhesive component is cross-linked and cured by irradiating light or heating the curable pressure-sensitive adhesive component during the formation of a laminate.
[0086] Cured adhesive components that are crosslinked and cured by light irradiation or heating exhibit a dramatic improvement in chemical resistance. Consequently, even when chemical treatment is applied to the back side of a wafer during the processing stage, the dissolution of the adhesive into the chemical solution can be suppressed. Furthermore, because the elastic modulus of the crosslinked and cured adhesive components increases, adhesion becomes difficult to deteriorate even at high temperatures, making peeling relatively easy.
[0087] In this embodiment, even though the wafer is heat-treated, mechanically processed, and / or wet-treated during the wafer processing process, sufficient adhesion is maintained during wafer processing, and furthermore, in the process of peeling the wafer from the laminate after the wafer processing process is completed, the wafer can be peeled off from the adhesive without damaging the wafer or leaving any residue.
[0088] For example, when using a photocurable adhesive component that crosslinks and cures by the above light irradiation, the adhesive component containing a polymer having unsaturated double bonds such as vinyl groups in a side chain and a photopolymerization initiator activated at a wavelength of 250 to 800 nm is used, it is preferable to irradiate the photocurable adhesive component with an illuminance of 5 mW or more, more preferable to irradiate with an illuminance of 10 mW or more, even more preferable to irradiate with an illuminance of 20 mW or more, and particularly preferable to irradiate with an illuminance of 50 mW or more. In addition, it is preferable to irradiate with an integrated illuminance of 300 mJ or more, more preferable to irradiate with an integrated illuminance of 500 mJ or more and 10,000 mJ or less, even more preferable to irradiate with an integrated illuminance of 500 mJ or more and 7,500 mJ or less, and particularly preferable to irradiate with an integrated illuminance of 1,000 mJ or more and 5,000 mJ or less.
[0089] In addition, for example, when a pressure adhesive or a precursor of a pressure adhesive is used as a thermosetting pressure adhesive component that is crosslinked and cured by heating, the pressure adhesive contains a polymer having unsaturated double bonds such as vinyl groups in the side chain and a polymerization initiator that is activated by heating at a temperature of about 50 to 200°C, the thermosetting pressure adhesive component can be crosslinked and cured by heating at a temperature of about 50 to 200°C for 10 to 60 minutes.
[0090] When forming a pressure-sensitive adhesive by curing a precursor as described above, the adhesive may be laminated with a support or wafer after curing, cured after lamination, or finally cured after lamination in a semi-cured state.
[0091] Wafer processing
[0092] A laminate formed using the double-sided pressure-sensitive adhesive of the present invention may be provided for processing at least one wafer selected from heat treatment (including treatment involving heat generation; hereinafter the same), mechanical processing, wet processing, and laser processing. In addition, a laminate formed using the double-sided pressure-sensitive adhesive of the present invention may be provided for processing required for TSV processing or for forming a structure in which semiconductor chips processed via TSV are stacked.
[0093] The above heat treatment may include, for example, sputtering, deposition, etching, chemical vapor deposition (CVD), physical vapor deposition (PVD), resist coating and patterning, heat lamination of a resin composition film, heat curing of a resin composition, heat drying of a resin composition, baking of a resin composition, reflow, resin sealing, plasma treatment, chip bonding, wire bonding, flip-chip bonding, surface-activated direct bonding, etc., but is not limited to these.
[0094] The above-mentioned machining processes are typically polishing, grinding, punching, and cutting of the wafer, but are not limited thereto and also include reshaping, etc.
[0095] When a wafer having electrodes formed on a surface is ground or polished, the non-electrode surface (back side) is ground or polished. The thickness of the wafer after grinding or polishing the back side varies depending on the electronic device used with the obtained electronic device, but is typically set to 1 μm or more and 200 μm or less, preferably 5 μm or more and 100 μm or less, and more preferably 5 μm or more and 50 μm or less. By doing so, the obtained electronic device is thinned, and the electronic device using such electronic device is miniaturized.
[0096] In this embodiment, when grinding or polishing a wafer, the wafer can be ground with superior processing precision by laminating it with a rigid support through a double-sided adhesive. At the same time, after grinding, the wafer can be provided to an additional processing process without damaging the wafer, or easily separated from the support and the double-sided adhesive.
[0097] The above wet treatment is a coating treatment such as spin coating, inkjet, or screen printing, a polishing treatment such as CMP, or a treatment using an acid, alkali, or organic solvent. Examples include plating treatments such as electroplating or electroless plating, wet etching treatments using hydrofluoric acid or an aqueous solution of tetramethylammonium hydroxide (TMAH), resist stripping processes using N-methyl-2-pyrrolidone, monoethanolamine, DMSO, etc., or cleaning processes using concentrated sulfuric acid, ammonia water, hydrogen peroxide water, etc., but are not limited to these.
[0098] The above laser processing may include annealing, via processing, circuit formation processing by direct drawing, and pre-processing for separation from a support, but is not limited to these.
[0099] In addition, in a laminate formed using the double-sided pressure-sensitive adhesive of the present invention, a dicing tape may be attached to the processed surface (preferably the ground surface) of the wafer after the above processing. By attaching the dicing tape in advance, dicing can be performed quickly after peeling off the support and the double-sided pressure-sensitive adhesive.
[0100] In a semiconductor manufacturing process, after the above treatment, the support is separated from the double-sided adhesive, but a treatment before peeling may be performed in advance. Specifically, methods such as laser treatment, swelling or dissolution of the double-sided adhesive with a solvent may be appropriately employed before mechanical peeling, but it is preferable not to perform such treatment, as it is superior in terms of cost due to the ability to simplify the equipment.
[0101] 10° peel strength
[0102] In evaluating the adhesive strength of the double-sided adhesive of the present invention, when a borosilicate glass silicon back-side grinding support substrate is used as a support, the 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate and the adhesive surface A is measured. In addition, when a Si mirror wafer is used as a wafer, the 10° peel strength P2 between the Si mirror wafer and the adhesive surface B is measured.
[0103] The 10° peel strength P1 between the borosilicate glass silicon backside grinding support substrate / point adhesive side A and the 10° peel strength P2 between the Si mirror wafer / point adhesive side B is the force per width of the peel portion (N / mm) required to proceed with peeling while maintaining the angle between the peeled layers (support and double-sided point adhesive, or double-sided point adhesive and wafer) at 10°.
[0104] That is, the 10° peel strength P1 between the borosilicate glass silicon backside grinding support substrate / point adhesive surface A and the 10° peel strength P2 between the Si mirror wafer / point adhesive surface B can be determined by proceeding with peeling between the 11 borosilicate glass silicon backside grinding support substrate / 12 double-sided point adhesive or between the 12 double-sided point adhesive / 13 Si mirror wafer in the state shown in FIG. 3 or a state equivalent thereto, measuring the force required for peeling, and dividing this by the width of the peeled portion, and more specifically, by the following method.
[0105] Since supports or wafers are typically rigid or brittle, it is generally difficult to maintain the angle formed by the peeled layers at 10° in the laminate in which the support / double-sided adhesive / wafer is stacked. Therefore, when measuring the 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate / adhesive side A, a sample for measuring the 10° peel strength P1 without a wafer is used (Fig. 3(a), (c)), and when measuring the 10° peel strength P2 between the Si mirror wafer / adhesive side B, a sample for measuring the 10° peel strength P2 without a support can be used for measurement (Fig. 3(b), (d)).
[0106] In the former case, when the double-sided pressure adhesive has a substrate film, a sample for measuring 10° peel strength P1 is formed using a double-sided pressure adhesive having a borosilicate glass silicon back-side grinding support substrate and a substrate film, and the measurement is performed (Fig. 3(a)). When the double-sided pressure adhesive has no substrate film and only has a pressure adhesive layer, a sample for measuring 10° peel strength P1 is formed by lining the pressure adhesive layer with a polyimide film, etc., and the measurement is performed (Fig. 3(c)).
[0107] In the latter case, when the double-sided pressure adhesive has a substrate film, a sample for measuring 10° peel strength P2 is formed using the double-sided pressure adhesive having a substrate film and a Si mirror wafer, and the measurement is performed (Fig. 3(b)). When the double-sided pressure adhesive has no substrate film and only has a pressure adhesive layer, a sample for measuring 10° peel strength P2 is formed by lining the pressure adhesive layer with a polyimide film, etc., and the measurement is performed (Fig. 3(d)).
[0108] The above peel strength ratio P2 / P1 is preferably 1.1 or higher, and particularly preferably 1.3 or higher.
[0109] Although there is no specific upper limit for the above peel strength ratio P2 / P1, from the perspective of properly peeling the wafer from the double-sided adhesive, it is desirable that the peel strength P2 between B is not excessive in the case of a Si mirror wafer / point adhesive. In addition, from the perspective of stably performing wafer processing, particularly machining processing, it is desirable that the 10° peel strength P1 between A is not insufficient in the case of a borosilicate glass silicon back-side grinding support substrate / point adhesive. For this reason, it is desirable that the above peel strength ratio P2 / P1 be 30 or less, more desirable that it be 15 or less, and particularly desirable that it be 7 or less.
[0110] It is preferable that the 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate / point adhesive surface A is 12 N / 25 mm or less. It is more preferable that the 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate / point adhesive surface A is 10 N / 25 mm or less, and particularly preferable that it is 7 N / 25 mm or less.
[0111] The 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate / point adhesive back-side A is preferably 0.5N / 25mm or more, and more preferably 1N / 25mm or more.
[0112] Since the 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate / point adhesive surface A is 12N / 25mm or less, the support can be stably peeled from the double-sided point adhesive and across the entire front surface of the laminate without applying excessive stress to the wafer through a relatively simple process such as mechanical peeling. In addition, since the 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate / point adhesive surface A is 0.5N / 25mm or more, wafer processing, especially mechanical processing, can be performed stably.
[0113] For Si mirror wafer / point bonding, the 10° peel strength P2 between B is preferably 35N / 25mm or less, and more preferably 30N / 25mm or less.
[0114] For Si mirror wafer / point bonding, the 10° peel strength P2 between B is preferably 2N / 25mm or more, and more preferably 3N / 25mm or more.
[0115] Since the 10° peel strength P2 between the Si mirror wafer / point adhesive surfaces B is 35N / 25mm or less, separation of the double-sided adhesive and the wafer can be achieved by separating the support from the laminate and removing the double-sided adhesive remaining on the wafer. Since the 10° peel strength P2 between the Si mirror wafer / point adhesive surfaces B is 2N / 25mm or more, wafer processing, especially machining processing, can be performed stably.
[0116] By using the double-sided pressure-sensitive adhesive of the present invention, the wafer can be easily separated from the laminate after wafer processing.
[0117] It is preferable that the separation of the wafer from the laminate be achieved by separating the support from the laminate and then removing the double-sided adhesive remaining on the wafer. In this embodiment, when removing the double-sided adhesive remaining on the wafer, the rigid support is already separated from the laminate, so the wafer can be separated from the double-sided adhesive without applying excessive stress to the wafer, thereby limiting the risk of damage to the functional layer formed on the wafer.
[0118] There are no particular restrictions on the method of separating the support from the double-sided adhesive, but mechanical peeling is preferred.
[0119] In the case of a support / point adhesive, separation between A and separation between B in the case of a wafer / point adhesive may both be performed by mechanical peeling, or on the other hand, a method other than mechanical peeling may be adopted.
[0120] The double-sided pressure-sensitive adhesive of the present invention has a peel strength ratio P2 / P1 of 1.1 or higher, and peeling between the borosilicate glass silicon backside grinding support substrate and the pressure-sensitive adhesive surface A is relatively easy. Therefore, the support can be stably peeled from the laminate and across the entire surface of the laminate by a relatively simple process such as mechanical peeling. At this time, since unintended peeling at the interface, i.e., between the wafer and the double-sided pressure-sensitive adhesive, is effectively suppressed, the risk of damaging the functional layer formed on the wafer is limited.
[0121] In a laminate composed of a borosilicate glass silicon back-side grinding support substrate, a spot adhesive, and a Si mirror wafer that are separated in the measurement of 10° peel strength, the ratio P2 / P1 between the borosilicate glass silicon back-side grinding support substrate and spot adhesive surface A and the 10° peel strength P2 between the Si mirror wafer and spot adhesive surface B, measured by maintaining the angle between each peeled layer at 10°, is 1.1 or greater. In addition, the 10° peel strength P1 between the borosilicate glass silicon back-side grinding support substrate and spot adhesive surface A and the 10° peel strength P2 between the Si mirror wafer and spot adhesive surface B are measured values after undergoing a history equivalent to that of the wafer processing. For example, if a thermal history of 150 to 200° is applied during wafer processing, the value is the value after the said thermal history is applied. This thermal history can be appropriately carried out at temperatures and times typically used in the processing of wafers in semiconductor manufacturing processes.
[0122] The double-sided pressure-sensitive adhesive of the present invention has a peel strength ratio P2 / P1 of 1.1 or higher, and can stably peel off a support from the pressure-sensitive adhesive and across the entire surface of the laminate through a relatively simple process such as mechanical peeling.
[0123] At this time, since delamination at the unintended interface, i.e., between the wafer and the double-sided adhesive, is effectively suppressed, the risk of damaging the functional layer formed on the wafer is limited.
[0124] In addition, since phenomena such as partial residue of adhesive on the support or partial defects of adhesive on the wafer are effectively suppressed, the risk of damage to the wafer or support caused by uneven stress is also limited.
[0125] There are no particular limitations on the means for adjusting the above 10° peel strength P1, 10° peel strength P2, and peel strength ratio P2 / P1, but they can be appropriately increased or decreased by means conventionally used in the industry, for example. More specifically, they can be appropriately increased or decreased by the composition of each layer, the manufacturing process, the manufacturing process of the laminate, etc. For example, the 10° peel strength P1 or 10° peel strength P2 can be increased by increasing the amount of adhesive components, such as adhesive or pressure-sensitive adhesive used in the double-sided pressure-sensitive adhesive, and the 10° peel strength P1 and 10° peel strength P2 can be decreased by adding a release agent to the double-sided pressure-sensitive adhesive.
[0126] There are no particular limitations on the method of mechanically peeling off a support and / or wafer from a laminate formed using the double-sided pressure-sensitive adhesive of the present invention, and peeling can be performed using commercially available devices appropriately. For example, it is preferable to perform peeling by the method shown in FIG. 1.
[0127] In this method, the 13 wafer side of the laminate is fixed on a chuck table (not shown) through a 14 dicing tape, and then the 11 support is held by a holding mechanism (not shown).
[0128] 16. Slide the remover on the interface between the 11 support and the 12 double-sided adhesive, apply an upward force to the end of the 11 support, and form a peel interface between the 11 support and the 12 double-sided adhesive that serves as a peeling mechanism (Fig. 1(b)).
[0129] Pressure is applied by a retaining mechanism to bend the 11 support, widening the peel interface and promoting peeling (Fig. 1(c)).
[0130] When the release interface widens and a release interface is formed on the entire surface between the 11 support and the 12 double-sided adhesive, the 11 support is released from the 12 double-sided adhesive.
[0131] Examples of commercially available devices such as the above include SUSS’s XBC Gen2, EVG’s EVG805, and Tatsumo Corporation’s TWH-SR series.
[0132] At this time, according to the present invention, since delamination at the interface between the 12 double-sided adhesive and the 13 wafer, which is not intended to be delaminated at this stage, is effectively suppressed, the functional layer formed on the 13 wafer is effectively protected by the 12 double-sided adhesive, and the risk of damage to the functional layer can be limited (Fig. 2(a)).
[0133] In the prior art, there were cases where delamination occurred at the interface between the double-sided adhesive and the wafer, 12, before delamination between the 11 support and the 12 double-sided adhesive, where delamination at this stage was not intended (Fig. 2(b)). As a result, there was a risk that electronic circuits formed on the 13 wafer would be damaged during delamination or damaged during subsequent processes that still require protection by the 12 double-sided adhesive.
[0134] In addition, in the prior art, there were cases where the support was not completely peeled off because some of the double-sided adhesive remained on the support or some of the double-sided adhesive on the wafer was missing (Fig. 2 (c)). As a result, uneven stress was applied to the wafer or the support, and there was a risk that they might be damaged. In cases where some of the double-sided adhesive remained on the wafer, it was sometimes necessary to dissolve the adhesive with a solvent to remove it.
[0135] According to the double-sided pressure-sensitive adhesive of the present invention, the problems of the prior art are solved, and unintended delamination at the interface or non-uniform delamination is prevented, or at least the frequency of such occurrence is significantly reduced, thereby making it possible to provide the wafer to a number of and / or various processes without damaging the functional layer formed on the wafer.
[0136] A wafer processed using the double-sided pressure-sensitive adhesive of the present invention can be provided to an additional subsequent process to manufacture a final product. When a functional layer is formed on the wafer, the final product can be manufactured by performing processes such as dicing, bonding, packaging, and sealing, which are commonly used in the manufacture of electronic devices such as semiconductor devices.
[0137] [Example]
[0138] The present invention will be described in detail below. Furthermore, the present invention is not limited in any way by the following embodiments.
[0139] The physical properties and characteristics in the examples / comparative examples were evaluated using the following methods.
[0140] (1) Mechanical peelability from the support
[0141] After applying a predetermined thermal history as shown in Table 1 to the prepared laminate, it was fixed at room temperature with the 13 Si mirror wafer side facing down 15 onto a 14 dicing tape attached to a ring frame, and the 14 dicing tape was fixed by a vacuum chuck (Fig. 1(a)). Intended to delaminate the interface between the 11 borosilicate glass silicon back-side grinding support substrate and the 12 double-sided adhesive, as shown in Fig. 1, a 16 remover was slid across the interface between the 11 support and the 12 double-sided adhesive, and by applying an upward force, typically up to about 120 N, to the end of the 11 borosilicate glass silicon back-side grinding support substrate, a delamination interface was formed between the 11 borosilicate glass silicon back-side grinding support substrate and the 12 double-sided adhesive, which serves as a delamination catalyst (Fig. 1(b)).
[0142] Next, the peeling of the borosilicate glass silicon backside grinding support substrate was performed by applying pressure to the formed peeling interface and widening the peeling interface (Fig. 1(c)). The peelability was evaluated according to the following criteria.
[0143] ○: The intended borosilicate glass silicon back-side grinding support substrate / double-sided adhesive interface could be peeled off across the entire front surface, and no damage occurred to the wafer.
[0144] ×: Unintended delamination at the double-sided adhesive / wafer interface.
[0145] (2) Removability of double-sided adhesive from wafer
[0146] For the 13 Si mirror wafer / 12 double-sided adhesive laminate fixed to the 14 dicing tape attached to the 15 ring frame after the mechanical peelability evaluation described above, an adhesive tape 17 was attached to the front surface of the 12 double-sided adhesive. The 14 dicing tape was fixed with a vacuum chuck, and the 12 double-sided adhesive was peeled at a peeling angle of 90° and a peeling speed of 5 mm / s. The peelability was evaluated according to the following criteria.
[0147] ○: The double-sided adhesive could be completely peeled off from the Si mirror wafer, and no damage occurred to the Si mirror wafer.
[0148] ×: Could not peel off the double-sided adhesive from the Si mirror wafer.
[0149] (3) 10° peel strength P1 (10° peel strength between borosilicate glass silicon back-side grinding support substrate / point adhesive side A)
[0150] (3-1) When using a base film in a double-sided pressure adhesive
[0151] A sample for P1 measurement was prepared by laminating a 20 point adhesive layer A1 onto a 19 substrate film.
[0152] (3-2) Cases where a base film is not used in double-sided pressure adhesive
[0153] 21 A polyimide film (bilateral plasma treated, thickness 38 μm, manufactured by Toray DuPont, Inc., trade name: Kapton (registered trademark) 150 EN-A) was prepared, and a sample for P1 measurement was fabricated by laminating a material identical to 12 double-sided pressure adhesive onto it.
[0154] (3-3) Measurement
[0155] The sample for measuring P1 prepared in (3-1) or (3-2) above was cut to 2.5 cm × 5 cm, and the side of the P1 measurement sample that is the same material as the 20 adhesive layer A1 or 12 double-sided adhesive layer was attached to the attachment side of the 11 support cut to 3 cm × 6 cm using a 2 kg roller. Subsequently, the prepared borosilicate glass silicon back-side grinding support substrate / P1 measurement sample laminate was heated at 140°C for 30 minutes under conditions simulating the pretreatment in the laminate formation process in each example and comparative example. In addition, after applying a predetermined thermal history as shown in Table 1 under conditions simulating the actual wafer processing process, the measurement sample was cooled by leaving it at 22.5±1℃ and relative humidity 50±10% for one week, and then the 10° peel strength P1 was measured at a tensile speed of 300 mm / min and a peel angle of 10° using VPA-S (manufactured by Kyowa Interface Science Co., Ltd.) under these temperature and humidity conditions (Fig. 3 (a) or (c)).
[0156] (4) 10° peel strength P2 (10° peel strength between B on Si mirror wafer / point bonding surface)
[0157] (4-1) When using a base film in a double-sided pressure adhesive
[0158] A sample for P2 measurement was prepared by laminating an 18 point adhesive layer B1 onto a 19 substrate film.
[0159] (4-2) Cases where a base film is not used in double-sided pressure adhesive
[0160] 21 A polyimide film (bilateral plasma treated, thickness 38 μm, manufactured by Toray DuPont, Inc., trade name: Kapton (registered trademark) 150 EN-A) was prepared, and a sample for P2 measurement was prepared by laminating a material identical to 12 double-sided pressure adhesive onto it.
[0161] (4-3) Measurement
[0162] The P2 measurement sample prepared in (4-1) or (4-2) above was cut to 2.5 cm × 5 cm, and the side of the P2 measurement sample that is made of the same material as the 18th adhesive layer B1 or 12th double-sided adhesive of the P2 measurement sample was attached to the attachment side of a Si mirror wafer cut to 3 cm × 6 cm using a 2 kg roller once. Subsequently, the prepared Si mirror wafer / P2 measurement sample laminate was heated at 140°C for 30 minutes under conditions simulating the pretreatment in the laminate formation process in each example and comparative example. In addition, after applying a predetermined thermal history as shown in Table 1 under conditions simulating an actual wafer processing process, the sample for measurement was cooled by leaving it at 22.5±1℃ and relative humidity 50±10% for one week, and then, under these temperature and humidity conditions, the 10° peel strength P2 was measured at a tensile speed of 300 mm / min and a peel angle of 10 degrees using VPA-S (manufactured by Kyowa Interface Science Co., Ltd.) (Fig. 3(b) or (d)).
[0163] The details of the materials and materials used in the examples / comparative examples are as follows.
[0164] Support, and wafer
[0165] The following glass, Si, or PBO film-attached wafer was used as either a support or a wafer.
[0166] Glass
[0167] A borosilicate heat-resistant glass silicon backside grinding support substrate with an outer diameter of 300 or 200 mm × thickness of 700 μm was used.
[0168] ㆍSi
[0169] Si mirror wafers with an outer diameter of 300 or 200 mm × thickness of 750 μm were used.
[0170] ㆍWafer with PBO film attached
[0171] A wafer with a 6 μm PBO film installed on a Si mirror wafer with an outer diameter of 300 or 200 mm × a thickness of 730 μm was used.
[0172] Resin for forming double-sided pressure-sensitive adhesives
[0173] ㆍ(Meta)acrylic resin solution N
[0174] 49 parts by mass of ethyl acrylate, 20 parts by mass of 2-ethylhexyl acrylate, 21 parts by mass of methyl acrylate, 10 parts by mass of glycidyl methacrylate, and 0.5 parts by mass of a benzoyl peroxide-based polymerization initiator as a polymerization initiator were reacted at 80°C for 10 hours in a solvent consisting of 65 parts by mass of toluene and 50 parts by mass of ethyl acetate. After the reaction was completed, the obtained solution was cooled, and 25 parts by mass of xylene, 5 parts by mass of acrylic acid, and 0.5 parts by mass of tetradecyldimethylbenzylammonium chloride were added to the cooled solution and reacted at 85°C for 32 hours while blowing air to obtain a (meth)acrylic resin solution N.
[0175] ㆍSilicone-modified (meth)acrylic resin solution NS
[0176] To 270 parts by mass of the above-described (meth)acrylic resin solution N, 0.3 parts by mass of carboxy-modified organopolysiloxane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name: X-22-3710) was added and reacted at 60°C for 7 days to obtain a silicone-modified (meth)acrylic resin solution NS.
[0177] ㆍ(Meta)acrylic resin solution L
[0178] A (meth)acrylic adhesive (Mitsui Chemicals Co., Ltd., Bind Serum SA591) was used.
[0179] ㆍ(Meta)acrylic resin emulsion H
[0180] 0.5 parts by mass of ammonium persulfate was used as a polymerization initiator, and 63 parts by mass of 2-ethylhexyl acrylate, 21 parts by mass of n-butyl acrylate, 9 parts by mass of methyl methacrylate, 3 parts by mass of 2-hydroxyethyl methacrylate, 2 parts by mass of methacrylic acid, 1 part by mass of acrylamide, 1 part by mass of polytetramethylene glycol diacrylate (manufactured by Nippon Oil & Fat Co., Ltd., trade name: ADT-250), and 2 parts by mass of an aqueous solution of ammonium polyoxyethylene nonylpropenylphenyl ether sulfate (manufactured by Daiichi Kogyo Pharmaceutical Co., Ltd., trade name: Aquaron HS-1025) were emulsion polymerized in deionized water at 70°C. After the polymerization was completed, (meth)acrylic resin emulsion H with a solid content of 56.5% by mass was obtained by adjusting the pH to 7.0 using ammonia water.
[0181] ㆍ(Meta)acrylic resin emulsion B
[0182] 0.5 parts by mass of 4,4'-azobis-4-cyanovaleric acid (manufactured by Otsuka Chemical Co., Ltd., trade name: ACVA) was used as a polymerization initiator, and 74 parts by mass of n-butyl acrylate, 14 parts by mass of methyl methacrylate, 9 parts by mass of 2-hydroxyethyl methacrylate, 2 parts by mass of methacrylic acid, 1 part by mass of acrylamide, and 3 parts by mass of HS-1025 were emulsion polymerized in deionized water at 70°C. After the polymerization was completed, the pH was adjusted to 7.0 using ammonia water to obtain (meth)acrylic resin emulsion B with a solid content of 42.5% by mass.
[0183] ㆍ(Meta)acrylic resin emulsion A
[0184] 0.65 parts by mass of ACVA was used as a polymerization initiator, and 63 parts by mass of 2-ethylhexyl acrylate, 18 parts by mass of n-butyl acrylate, 12 parts by mass of methyl methacrylate, 3 parts by mass of 2-hydroxyethyl methacrylate, 2 parts by mass of methacrylic acid, 1 part by mass of acrylamide, 1 part by mass of ADT-250, and 2 parts by mass of Aquaron HS-1025 were emulsion polymerized in deionized water at 70°C. After the polymerization was completed, (meth)acrylic resin emulsion A with a solid content of 42.5 mass% was obtained by adjusting the pH to 7.0 using ammonia water.
[0185] ㆍ(Meta)acrylic resin emulsion S
[0186] 0.5 parts by mass of ACVA was used as a polymerization initiator, and 47 parts by mass of acrylate-n-butyl, 22 parts by mass of methyl methacrylate, 9 parts by mass of methacrylate-2-hydroxyethyl, 15 parts by mass of methacrylic acid, 8 parts by mass of acrylamide, and 0.2 parts by mass of Aquaron HS-1025 were emulsion polymerized in deionized water at 70°C to obtain a (meth)acrylic resin emulsion S with a solid content of 40% by mass.
[0187] base film
[0188] ㆍPEN film
[0189] A polyethylene naphthalate film (double-sided corona treated, thickness: 50μm, manufactured by Dongyangbang Film Solution Co., Ltd., Teonex Q83) was used.
[0190] PET film
[0191] A biaxially extended polyethylene terephthalate film (double-sided corona treated, thickness 38 μm, manufactured by Toray Corporation, Lumirror S10) was used.
[0192] Polyimide film
[0193] A polyimide film (bilateral plasma treated, thickness 38 μm, manufactured by Toray DuPont, Inc., trade name: Kapton (registered trademark) 150 EN-A) was used.
[0194] To 250 parts by mass of a (meth)acrylic resin solution L, 2.84 parts by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 50 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronics M-402), 2.0 parts by mass of silicon diacrylate (manufactured by Daicel Allnex Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of Parkadox 12XL25 manufactured by Hwayak Nurion Co., Ltd. were added to obtain coating solution 1-1 for a pressure-sensitive adhesive layer on the support side. Coating solution 1-1 was applied to a base film (PET film) and dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer 1-1 with a thickness of 25 μm as a pressure-sensitive adhesive layer on the support side. Next, by bonding a silicone-release treated polyethylene terephthalate film (separator), a laminate consisting of a separator-attached adhesive layer 1-1 / substrate film was obtained.
[0195] Next, 100 parts by weight of (meth)acrylic resin emulsion A, 0.7 parts by weight of (meth)acrylic resin emulsion S, 0.3 parts by weight of dimethyl ethanolamine, 5 parts by weight of an epoxy compound (manufactured by Nagase Chemtex Co., Ltd., trade name: Ex-614), 9 parts by weight of butyl carbinol, and 12 parts by weight of pure water were mixed to prepare coating solution 1-2 for the adhesive layer on the wafer side. Coating solution 1-2 was applied to a silicone-release treated polyethylene terephthalate film (separator) and dried at 120°C for 3 minutes to form an adhesive layer 1-2 with a thickness of 20 μm as the adhesive layer on the wafer side.
[0196] Next, by bonding the adhesive layer 1-2 to the substrate film side of the laminate composed of the adhesive layer 1-1 / substrate film described above, a double-sided adhesive precursor before heat treatment was produced, consisting of three layers of adhesive layer 1-1 / substrate film / adhesive layer 1-2 with a separator attached. The separators used on both sides of the said three-layer composition were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, heated at 140°C for 30 minutes, and a laminate consisting of a support / double-sided adhesive / wafer was produced. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0197] Separately, a laminate consisting of a pressure-sensitive adhesive layer 1-1 / substrate film and a laminate consisting of a substrate film / pressure-sensitive adhesive layer 1-2 were each fabricated individually (with the same coating conditions), and the 10° peel strengths P1 and P2 were measured using the method described above. The measurement results are shown in Table 1.
[0198] [Example 1-1]
[0199] A laminate was fabricated in the order of support / double-sided pressure adhesive / wafer, in the same manner as in Example 1, except that a Si (support) and a wafer (wafer) with a PBO film attached were used. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0200] To 270 parts by mass of a (meth)acrylic resin solution N, 2.84 parts by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 50 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronics M-402), 2.0 parts by mass of silicon diacrylate (manufactured by Daicel Allnex Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) were added to obtain coating solution 2-1 for the adhesive layer on the support side. Coating solution 2-1 was applied to a base film (PEN film) and dried at 100°C for 10 minutes to form an adhesive layer 2-1 with a thickness of 25 μm as the adhesive layer on the support side. Next, by bonding a silicone-release treated polyethylene terephthalate film (separator), a laminate consisting of a separator-attached adhesive layer 2-1 / substrate film was obtained.
[0201] To 270 parts by mass of a (meth)acrylic resin solution N, 0.1 parts by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronix M-402), 0.5 parts by mass of silicon diacrylate (manufactured by Daicel Allnex Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of Parkadox 12XL25 manufactured by Hwayak Nurion Co., Ltd. were added to obtain a coating solution 2-2 for a pressure-sensitive adhesive layer on the wafer side. The coating solution 2-2 was applied to a polyethylene terephthalate film (separator) that had been treated with a silicone release agent, and dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer (2-2) with a thickness of 40 μm as a pressure-sensitive adhesive layer on the wafer side. Next, by bonding the adhesive layer (2-2) to the substrate side of the laminate composed of the adhesive layer 2-1 / substrate film described above, a laminate composed of three layers of adhesive layer 2-1 / substrate film / adhesive layer 2-2 with a separator attached was obtained.
[0202] To 270 parts by mass of a (meth)acrylic resin solution N, 5.68 parts by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronics M-402), 0.5 parts by mass of silicon diacrylate (manufactured by Daicel Allnex Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) were added to obtain coating solution 2-3 for a pressure-sensitive adhesive layer on the wafer side. Coating solution 2-3 was applied to a polyethylene terephthalate film (separator) treated with silicone release agent, and dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer 2-3 with a thickness of 10 μm as a pressure-sensitive adhesive layer on the wafer side. Next, a double-sided adhesive precursor before heat treatment was prepared by bonding the adhesive layer 2-3 to the side of the adhesive layer 2-2 of a laminate composed of three layers: adhesive layer 2-1 / substrate film / adhesive layer 2-2, with the aforementioned separator attached, thereby forming a four-layer structure consisting of adhesive layer 2-1 / substrate film / adhesive layer 2-2 / adhesive layer 2-3 with the separator attached. The separators used on both sides of the four-layer structure were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, heated at 140°C for 30 minutes, and a laminate consisting of a support / double-sided adhesive / wafer was prepared. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0203] Separately, a laminate consisting of a pressure-sensitive adhesive layer 2-1 / substrate film and a laminate consisting of a substrate film / pressure-sensitive adhesive layer 2-2 / pressure-sensitive adhesive layer 2-3 were each fabricated individually (with the same coating conditions), and the 10° peel strengths P1 and P2 were measured using the method described above. The measurement results are shown in Table 1.
[0204] [Example 2-1]
[0205] A laminate was fabricated in the same order as in Example 2, except that a Si (support) and a wafer (wafer) with a PBO film attached were used, consisting of a support / double-sided adhesive / wafer. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0206] To 270 parts by mass of a (meth)acrylic resin solution N, 2.84 parts by mass of HDI isocyanurate (manufactured by Dongso Corporation, trade name: Colonate HX), 50 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronics M-402), 2.0 parts by mass of acrylic group-containing polyether-modified polydimethylsiloxane (manufactured by Big Chem Japan Co., Ltd., trade name: BYK-UV3500), and 2 parts by mass of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) were added to obtain a coating solution 3-1 for a pressure-sensitive adhesive layer on the support side. The coating solution 3-1 was applied to a base film (PEN film) and dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer 3-1 with a thickness of 25 μm as a pressure-sensitive adhesive layer on the support side. Next, by bonding a silicone-release treated polyethylene terephthalate film (separator), a laminate consisting of a separator-attached adhesive layer 3-1 / substrate film was obtained.
[0207] To 270 parts by mass of a (meth)acrylic resin solution N, 0.1 parts by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronics M-402) and 2 parts by mass of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) were added to obtain coating solution 3-2 for a wafer-side adhesive layer. Coating solution 3-2 was applied to a silicone-release polyethylene terephthalate film (separator) and dried at 100°C for 10 minutes to form an adhesive layer 3-2 with a thickness of 40 μm as a wafer-side adhesive layer. Next, by bonding the adhesive layer 3-2 to the substrate side of the laminate composed of the adhesive layer 3-1 / substrate film described above, a laminate having a three-layer structure of adhesive layer 3-1 / substrate film / adhesive layer 3-2 with a separator attached was obtained.
[0208] To 270 parts by mass of a (meth)acrylic resin solution N, 5.68 parts by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 30 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronics M-402) and 2 parts by mass of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) were added to obtain coating solution 3-3 for a pressure-sensitive adhesive layer on the wafer side. Coating solution 3-3 was applied to a silicone-release polyethylene terephthalate film (separator) and dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer 3-3 with a thickness of 10 μm as a pressure-sensitive adhesive layer on the wafer side. Next, by bonding the adhesive layer 3-3 to the side of the adhesive layer 3-2 of a laminate having a three-layer structure of adhesive layer 3-1 / substrate film / adhesive layer 3-2 with the aforementioned separator attached, a double-sided adhesive precursor before heat treatment was produced having a four-layer structure of adhesive layer 3-1 with a separator attached / substrate film / adhesive layer 3-2 / adhesive layer 3-3. The separators used on both sides of the said four-layer structure were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, heated at 140°C for 30 minutes, and a laminate consisting of a support / double-sided adhesive / wafer was produced. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0209] Separately, a laminate consisting of a pressure-sensitive adhesive layer 3-1 / substrate film and a laminate consisting of a substrate film / pressure-sensitive adhesive layer 3-2 / pressure-sensitive adhesive layer 3-3 were each fabricated individually (under the same coating conditions), and the 10° peel strengths P1 and P2 were measured using the method described above. The measurement results are shown in Table 1.
[0210] In Example 1, the coating solution 1-1 for the adhesive layer on the support side was applied to a silicone-release treated polyethylene terephthalate film (separator) and dried at 100°C for 10 minutes to form an adhesive layer 4-1 with a thickness of 25 μm as the adhesive layer on the support side. Subsequently, by bonding a base film (polyimide film), a laminate consisting of the adhesive layer 4-1 attached to the separator and the base film was obtained.
[0211] 42.6 parts by mass of (meth)acrylic resin emulsion H, 57.4 parts by mass of (meth)acrylic resin emulsion B, 0.4 parts by mass of dimethyl ethanolamine, 3.4 parts by mass of an epoxy compound (manufactured by Nagase Chemtex Co., Ltd., trade name: Ex-1610), 13 parts by weight of butyl carbinol, and 20 parts by weight of pure water were each mixed to prepare coating solution 4-2 for the adhesive layer on the wafer side. Coating solution 4-2 was applied to a silicone-release treated polyethylene terephthalate film (separator) and dried at 120°C for 3 minutes to form an adhesive layer 4-2 with a thickness of 13 μm as the adhesive layer on the wafer side. Next, by bonding the adhesive layer 4-2 to the substrate side of the adhesive layer 4-1 / substrate film laminate described above, a double-sided adhesive precursor before heat treatment was produced with a three-layer composition of adhesive layer 4-1 / substrate film / adhesive layer 4-2 with a separator attached. The separators used on both sides of the said three-layer composition were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, and heated at 140°C for 30 minutes to produce a laminate consisting of a support / double-sided adhesive / wafer in that order. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0212] Separately, a laminate consisting of a pressure-sensitive adhesive layer 4-1 / substrate film and a laminate consisting of a substrate film / pressure-sensitive adhesive layer 4-2 were each fabricated individually (with the same coating conditions), and the 10° peel strengths P1 and P2 were measured using the method described above. The measurement results are shown in Table 1.
[0213] [Example 4-1]
[0214] A laminate was fabricated in the order of support / double-sided adhesive / wafer, in the same manner as in Example 4, except that Si (support) and glass (wafer) were used. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0215] In Example 1, the coating solution 1-1 for the adhesive layer on the support side was applied to a silicone-release treated polyethylene terephthalate film (separator) and dried at 100°C for 10 minutes to form an adhesive layer 5-1 with a thickness of 25 μm as the adhesive layer on the support side. Subsequently, by bonding a base film (PEN film), a laminate consisting of the adhesive layer 5-1 attached to the separator and the base film was obtained.
[0216] In Example 4, the coating solution 4-2 for the adhesive layer on the wafer side was coated onto a silicone-release polyethylene terephthalate film (separator) and dried at 100°C for 10 minutes to form an adhesive layer 5-2 with a thickness of 13 μm as the adhesive layer on the wafer side. Subsequently, by bonding the adhesive layer 5-2 to the substrate side of a laminate consisting of the adhesive layer 5-1 and the substrate film described above, a double-sided adhesive precursor before heat treatment was produced having a three-layer structure of adhesive layer 5-1 with a separator attached, a substrate film, and adhesive layer 5-2. The separators used on both sides of the 3-layer structure were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, and heated at 140°C for 30 minutes to produce a laminate consisting of a support / double-sided adhesive / wafer in that order. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0217] Separately, a laminate consisting of a pressure-sensitive adhesive layer 5-1 / substrate film and a laminate consisting of a substrate film / pressure-sensitive adhesive layer 5-2 were each fabricated individually (with the same coating conditions), and the 10° peel strengths P1 and P2 were measured using the method described above. The measurement results are shown in Table 1.
[0218] [Example 5-1]
[0219] A laminate was fabricated in the order of support / double-sided adhesive / wafer, in the same manner as in Example 4, except that Si (support) and glass (wafer) were used. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0220] To 270 parts by mass of a (meth)acrylic resin solution N, 0.5 parts by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 12 parts by mass of dipentaerythritol penta / hexaacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: Aronix M-400), 1.5 parts by mass of silicon diacrylate (manufactured by Daicel Allnex Co., Ltd., trade name: Ebecryl 350), and 2 parts by mass of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) were added to obtain a coating solution 6-1 for a pressure-sensitive adhesive layer on the support side. This coating solution 6-1 was coated onto a silicone-release treated polyethylene terephthalate film (separator) and dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer 6-1 with a thickness of 100 μm as a pressure-sensitive adhesive layer on the support side. Next, by bonding a base film (PET film), a laminate consisting of a separator-attached adhesive layer 6-1 / base film was obtained.
[0221] Next, the coating solution 4-2 for the wafer-side adhesive layer in Example 4 was applied to a silicone-release polyethylene terephthalate film (separator) and dried at 120°C for 3 minutes to form an adhesive layer 6-2 with a thickness of 6 μm as the wafer-side adhesive layer. By bonding the laminate consisting of the adhesive layer 6-1 and the substrate film described above to the substrate film side, a double-sided adhesive precursor before heat treatment was produced, having a three-layer structure of adhesive layer 6-1 with a separator attached, substrate film, and adhesive layer 6-2.
[0222] The separators used on both sides of the 3-layer structure were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, heated at 140°C for 30 minutes, and a laminate consisting of a support / double-sided adhesive / wafer was fabricated. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0223] Separately, a laminate consisting of a pressure-sensitive adhesive layer 6-1 / substrate film and a laminate consisting of a substrate film / pressure-sensitive adhesive layer 6-2 were each fabricated individually (under the same coating conditions), and the 10° peel strengths P1 and P2 were measured using the method described above. The measurement results are shown in Table 1.
[0224] A pressure-sensitive adhesive coating solution 7 for a double-sided pressure-sensitive adhesive was obtained by adding 1.0 part by mass of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX) and 2 parts by mass of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) to 269 parts by mass of a silicone-modified (meth)acrylic resin solution NS. Coating solution 7 was applied to a silicone-release treated polyethylene terephthalate film (separator), and then dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer 7 with a thickness of 100 μm. Subsequently, a double-sided pressure-sensitive adhesive precursor prior to heat treatment was prepared by bonding the silicone-release treated polyethylene terephthalate film (separator) (attached to a double-sided separator). The separators on both sides were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, and heated at 140°C for 30 minutes to produce a laminate consisting of a support / double-sided adhesive / wafer in that order. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0225] In addition, 10° peel strengths P1 and P2 were measured according to the above method (when a base film is not used in the double-sided pressure adhesive). The measurement results are shown in Table 1.
[0226] [Comparative Example 1]
[0227] Coating solution C1 for a double-sided pressure-sensitive adhesive was obtained by adding 0.1 parts by weight of HDI isocyanurate (manufactured by Dongso Co., Ltd., trade name: Colonate HX), 6 parts by weight of pentaerythritol tri / tetraacrylate (manufactured by Dong-A Synthetic Co., Ltd., trade name: M-450), and 2 parts by weight of Parkadox 12XL25 (manufactured by Hwayak Nurion Co., Ltd.) to 269 parts by weight of a silicone-modified (meth)acrylic resin solution N, respectively. This coating solution was applied to a silicone-release treated polyethylene terephthalate film (separator), and then dried at 100°C for 10 minutes to form a pressure-sensitive adhesive layer C1 with a thickness of 50 μm. Subsequently, a double-sided pressure-sensitive adhesive precursor prior to heat treatment was prepared by bonding the silicone-release treated polyethylene terephthalate film (separator) (attached to a double-sided separator). The separators on both sides were peeled off, glass (support) and Si (wafer) were laminated using a vacuum laminator, and heated at 140°C for 30 minutes to produce a laminate consisting of a support / double-sided adhesive / wafer in that order. The results of evaluating the mechanical peelability and removalability of the laminate are shown in Table 1.
[0228] In addition, 10° peel strengths P1 and P2 were measured according to the above method (when a base film is not used in the double-sided pressure adhesive). The measurement results are shown in Table 1.
[0229]
[0230] It has been confirmed that for a double-sided adhesive with a ratio P2 / P1 of 10° peel strength P1 between a borosilicate glass silicon backside grinding support substrate / point adhesive surface A and 10° peel strength P2 between a Si mirror wafer / point adhesive surface B of 1.1 or higher, it has good mechanical peelability and removeability from the wafer even when a support other than a borosilicate glass silicon backside grinding support substrate or a wafer other than a Si mirror wafer is used.
[0231] [Industrial Applicability]
[0232] According to the double-sided pressure adhesive of the present invention, multiple and / or multi-directional processes can be performed on a wafer with high productivity and yield without damaging electronic components, such as functional layers formed on the wafer, thereby significantly contributing to the improvement of productivity of electronic devices and having high applicability in various fields of industry, including the semiconductor process industry, electronic component industry, electrical and electronic industry using electronic components, transportation machinery industry, information and communication industry, and precision instrument industry. Explanation of the symbols
[0233] 11: Support or borosilicate glass silicon backside grinding support substrate 12: Double-sided pressure-sensitive adhesive 13: Wafer or Si mirror wafer 14: Dicing Tape 15: Ring frame 16: Remover 17: Adhesive tape 18: Pressure-sensitive adhesive layer B1 19: Record film 20: Pressure-sensitive adhesive layer A1 21: Polyimide film
Claims
Claim 1 A method for manufacturing a processed wafer using a double-sided adhesive having one adhesive surface A and another adhesive surface B, comprising: a step of forming a laminate comprising a support / double-sided adhesive / wafer by fixing a support to the adhesive surface A and fixing a wafer to the adhesive surface B; a step of processing the wafer; and a step of separating the support from the laminate and subsequently removing the double-sided adhesive remaining on the wafer. A method for manufacturing a treated wafer comprising: a double-sided pressure adhesive, wherein the ratio of the 10° peel strength P1 between a borosilicate heat-resistant glass silicon backside grinding support substrate / pressure adhesive surface A and the 10° peel strength P2 between a Si mirror wafer / pressure adhesive surface B, measured by maintaining the angle formed by the peeled layers at 10°, P2 / P1 is 1.1 or greater, the 10° peel strength P1 is 12N / 25mm or less, and the double-sided pressure adhesive contains a release agent, wherein the release agent is a silicon-based compound. Claim 2 A method for manufacturing a treated wafer according to claim 1, wherein the double-sided adhesive contains an acrylic adhesive component or a silicone adhesive component. Claim 3 A method for manufacturing a processed wafer according to claim 1 or 2, wherein the pressure adhesive comprises a pressure adhesive layer A1 having a pressure adhesive surface A and a pressure adhesive layer B1 having a pressure adhesive surface B, and the pressure adhesive layer A1 and the pressure adhesive layer B1 have different compositions. Claim 4 A method for manufacturing a treated wafer, wherein, in paragraph 3, the pressure adhesive comprises at least one of the pressure adhesive layer A1 or the pressure adhesive layer B1 containing a curable pressure adhesive component. Claim 5 In paragraph 3, the method for manufacturing a treated wafer, wherein the pressure adhesive has a substrate film between the pressure adhesive layer A1 and the pressure adhesive layer B1. Claim 6 In paragraph 3, the method for manufacturing a treated wafer wherein the pressure adhesive comprises at least one of the pressure adhesive layer A1 or the pressure adhesive layer B1 containing a release agent. Claim 7 A method for manufacturing a treated wafer according to claim 5, wherein the above-described film is a plastic film selected from PET, PEN, and polyimide. Claim 8 A method for manufacturing a treated wafer according to claim 3, wherein the pressure-sensitive adhesive layer A1 or the pressure-sensitive adhesive layer B1 contains an acrylic pressure-sensitive adhesive component or a silicone pressure-sensitive adhesive component. Claim 9 A method for manufacturing a treated wafer according to claim 1, wherein the ratio of the 10° peel strength P1 between the borosilicate heat-resistant glass silicon backside grinding support substrate / point adhesive surface A and the 10° peel strength P2 between the Si mirror wafer / point adhesive surface B, P2 / P1 is 15.0 or less. Claim 10 A method for manufacturing a processed wafer according to claim 1, wherein the 10° peel strength P1 is 0.5N / 25mm or greater. Claim 11 A method for manufacturing a treated wafer according to claim 3, wherein the adhesive layer A1 contains a release agent of a (meth)acrylic adhesive component and a silicon-based compound, or contains a silicon-modified (meth)acrylic adhesive. Claim 12 A method for manufacturing a treated wafer according to claim 1, wherein the treatment is at least one selected from heat treatment, mechanical processing, wet processing, and laser processing. Claim 13 In paragraph 12, the above-mentioned mechanical processing is the grinding of the wafer, a method for manufacturing a processed wafer.
Citation Information
Patent Citations
Laminate for wafer processing, temporary adhesive material for wafer processing and method of manufacturing thin wafer
JP2016086158A
Method of peeling electronic member and laminate
KR1020150140801A
Laminate, method for processing base, composition for temporary fixing and semiconductor device
KR1020160090819A
Tape for semiconductor processing
JP2018203973A
Thermosetting temporary-bonding-film for semiconductor wafer, laminated body comprising the same and method for debonding laminated body
KR101532756B1