Leak-proof upper tundish nozzle
The implementation of a nickel-based gas flow seal in the upper tundish nozzle addresses argon leakage issues, enhancing operational efficiency and reducing costs by maintaining pressure balance and fluid film integrity.
Patent Information
- Application Number
- KR1020247011341
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-24
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-09-24
AI Technical Summary
Existing upper tundish nozzles suffer from significant argon gas leakage, compromising the formation of a protective fluid film and disrupting the pressure balance necessary for uninterrupted casting, leading to increased costs and operational inefficiencies.
A leak-proof design incorporating a gas flow seal formed of nickel or nickel alloy between the protective can and the ceramic inner part, preventing gas leakage through the gaps between these components.
The seal effectively minimizes argon leakage, maintaining the necessary pressure balance and fluid film formation, ensuring uninterrupted casting and reducing production costs.
Smart Images

Figure 112024037587202-PCT00005_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to the casting of steel slabs, and more specifically to an upper tundish nozzle used in such casting. Most specifically, the present invention relates to a design of an argon-injected upper tundish nozzle in which argon leakage is minimized / eliminated. Background Technology
[0002] The present invention relates to an improved design of an upper tundish nozzle. The nozzle is designed to be used for continuous casting of steel into slabs. FIG. 1 illustrates a cross-section of such a continuous casting line. The line includes a ladle (1) that continuously brings fresh steel into a tundish (2). The tundish (2) controls the flow from therein into a casting mold (3).
[0003] FIG. 2 is a more detailed view of the tundish (2) and the casting mold (3), specifically illustrating the position of the upper tundish nozzle (4), which is the focus of the present invention. The upper tundish nozzle (4) collects molten steel from the tundish (2) and directs this steel into the casting mold (3) through a gate valve.
[0004] FIG. 3 is a simplified cross-section of the upper tundish nozzle (4). The upper tundish nozzle (4) consists of a ceramic inner part (6) and a protective can (5) that accommodates and protects the fragile ceramic inner part (6).
[0005] The ceramic inner part (6) of such a nozzle is often formed from a porous gas-permeable refractory material which may be a ceramic oxide of aluminum, silicon, magnesium, chromium, or zirconium, or a mixture thereof. Alternatively, the ceramic inner part (6) of the nozzle may be formed from a ceramic material having holes perforated / tunneled within the ceramic to provide gas flow paths set within the ceramic inner part (6).
[0006] Porous gas-permeable refractory materials and / or perforated / tunneled holes provide flow paths for argon gas injected into the upper tundish nozzle (4) during continuous casting to prevent clogging of the upper tundish nozzle (4) by solid inclusions. The argon flow also affects the flow pattern of the steel in the upper tundish nozzle (4), the gate valve, and subsequently in the casting mold (3).
[0007] As described above, the inner surface of the ceramic inner part (6) of the upper tundish nozzle (4) defines a bore for guiding the flow of liquid steel. The outer surface of the ceramic inner part (6) is surrounded by a protective can (5). The protective can (5) may be formed of a metal sheet material, such as steel, which can be spaced apart from the outer surface of the ceramic inner part (6) to define one or more annular gas guide spaces. Argon gas is injected into the upper tundish nozzle (4) through a gas injection port (7). FIG. 3 illustrates an argon flow path (8) in the upper tundish nozzle (4) having a porous ceramic inner part (6) as well as an argon gas injection port (7).
[0008] When the upper tundish nozzle (4) having a porous ceramic inner part (6) is operated, a pressurized inert gas (e.g., argon) penetrates through the annular space between the outer surface of the ceramic inner part (6) and the protective can (5) that can surround it while the molten metal flows through the bore of the upper tundish nozzle (4). The inert gas flows through the gas flow paths (8) within the porous ceramic inner part (6). The argon eventually exits the porous ceramic inner part (6) as argon bubbles (9). These bubbles can advantageously form a fluid film on the surface of the bore within the upper tundish nozzle (4) that prevents the molten metal from coming into direct contact with the inner surface forming the bore. By insulating the bore surface from the molten metal, the fluid film of gas prevents the small amount of alumina present in such steel from adhering to and accumulating on the surface of the nozzle bore. It is important to prevent such alumina deposits, because these deposits will ultimately obstruct the flow of molten steel until the molten steel stagnates around the walls of the bore, thereby clogging the upper tundish nozzle (4). Such clogged nozzles (4) require interruption of the casting process and replacement of the nozzles (4).
[0009] Although such upper tundish nozzles (4) are generally described as effective in themselves in delaying the accumulation of alumina deposits blocking the bore, the inventors have observed a number of disadvantages associated with these nozzles. One specific issue concerns the leakage of argon gas, that is, the loss of argon from the system in areas other than the inner bore surface of the upper tundish nozzle (4). Such leakage can compromise the function of gas penetrating into the inner bore of the upper tundish nozzle (6). If the gas leakage is sufficiently severe, it can hinder the formation of a protective fluid film on the surface of the nozzle bore. The pressure of the inert gas must be maintained at a level high enough to overcome the significant back pressure that the molten steel exerts on the surface of the bore. Ideally, the gas pressure should be sufficient to form the desired film. If it is too high, the gas may excessively agitate the steel, creating additional defects. Therefore, control of gas pressure and flow is important and must be maintained within a narrow range. Any significant leakage can compromise the desired delicate pressure balance. Furthermore, such argon loss is an additional cost to production and should therefore be minimized if possible. The problem to be solved
[0010] Clearly, there is a need for an improved upper tundish nozzle (4) design that minimizes or eliminates the leakage mechanisms inherent in the prior art design. means of solving the problem
[0011] The present invention relates to a leak-proof gas-injected upper tundish nozzle. The nozzle comprises a protective can and a ceramic inner portion disposed within the protective can. The ceramic inner portion preferably has gas flow paths inside. The nozzle further comprises a gas injection port attached to the protective can, which allows for the injection of gas through the protective can and into the gas flow paths within the ceramic inner portion.
[0012] The nozzle also includes at least one gas flow seal formed between the protective can and the ceramic inner part. The gas flow seal blocks gas leakage from the gap between the protective can and the ceramic inner part. The gas flow seal may be formed of nickel or an alloy of nickel.
[0013] A gas flow seal can be formed by depositing nickel or a nickel alloy within any gap between the protective can and the ceramic inner part by a method selected from the group consisting of electroplating, electroless plating, nickel / alloy foil strips, sputtering, plasma vapor deposition, and metal printing.
[0014] In one embodiment, the gas flow seal may be formed by electroplating nickel or a nickel alloy into any gaps between the protective can and the ceramic inner part. The nickel or a nickel alloy may be electroplated across the gap on the outside of the protective can and the outside of the ceramic inner part. The nickel or a nickel alloy may be electroplated across the gap on the outside of the protective can and the outside of the ceramic inner part after the protective can and the ceramic inner part are formed as a single piece.
[0015] Nickel or a nickel alloy may be deposited on one or both of the inner surface of the protective can and the outer surface of the ceramic inner part. Preferably, nickel or a nickel alloy may be deposited on one or both of the inner surface of the protective can and the outer surface of the ceramic inner part before the protective can and the ceramic inner part are formed as a single piece.
[0016] The protective can may be formed of a metal material, preferably steel. The ceramic inner part may be formed of a porous ceramic material, and the gas flow paths may include pores within the porous ceramic material. The ceramic inner part may be formed of a gas-permeable refractory material composed of one or more ceramic oxides of aluminum, silicon, magnesium, chromium, or zirconium, or a mixture thereof.
[0017] The ceramic interior may not be porous or gas permeable, and gas flow paths may be formed directly into the body of the ceramic interior. The gas flow paths may include gas distribution manifolds and gas distribution channels. The gas distribution channels may have gas outlets for releasing gas into the steel flowing within the upper tundish nozzle. Brief explanation of the drawing
[0018] FIG. 1 illustrates a cross-section of a continuous casting line in which the upper tundish nozzle of the present invention is preferably used. FIG. 2 is a more detailed view of the tundish and casting mold, specifically illustrating the position of the upper tundish nozzle. Figure 3 is a simplified cross-section of the upper tundish nozzle. FIG. 4 illustrates a typical cross-sectional view of an upper tundish nozzle, specifically showing a gap through which gas may leak. FIG. 5 illustrates a cross-sectional view of an upper tundish nozzle containing the gap seal solution of the present invention. Specific details for implementing the invention
[0019] The present invention is an improved argon-injected upper tundish nozzle (4) that minimizes / eliminates unwanted leakage of inert gas (such as argon).
[0020] FIG. 4 illustrates a typical cross-sectional view of an upper tundish nozzle (4). The drawing illustrates key components such as a protective can (5), a ceramic inner part (6), an argon injection port (7), and an argon gas flow path (8) within the ceramic inner part (6). In this type of upper tundish nozzle (4), the ceramic inner part (6) may or may not be porous, but the argon flow path (8) (including a gas distribution manifold and gas distribution channels containing gas outlets to release gas into the bore of the nozzle) is formed into the ceramic inner part (6) during manufacturing. As previously mentioned, the ceramic inner part (6) may alternatively be formed of porous ceramic without the pre-fabricated gas flow paths (8).
[0021] FIG. 4 also illustrates a problem that is solved by the present invention. That is, there may be significant leakage of argon gas from the gap between the protective can (5) and the ceramic inner part (6). The leakage path (10) may be in the upper gap and the lower gap. During manufacturing, the inner ceramic part (6) is press-molded into the protective can (5) to form a single piece. Due to the difference in thermal expansion between the metal protective can (5) and the ceramic inner part (6), a gas-tight seal between them is very difficult, if not impossible. Although these gaps may appear small and insignificant, it should be noted that for a typical upper tundish nozzle (4), a gap of 0.04318 mm between the protective can (5) and the ceramic inner part (6) has the same flow area as a 3.175 mm pipe. This can result in a significant loss of argon volume and pressure.
[0022] FIG. 5 illustrates a solution of the present invention devised by the inventors. The inventors discovered that a seal (11, 11') between a protective can (5) and a ceramic inner part (6) can prevent argon leakage. Specifically, the seal (11, 11') is formed of nickel or a nickel alloy. The temperature at the interface between the protective can (5) and the ceramic inner part (6) is lower than the melting point of the nickel / alloy seal (11, 11'). This seal (11, 11') is believed to remain ductile at the elevated temperature within the gap and to expand without cracking during the expansion of the protective can (5) and the ceramic inner part. This helps prevent leakage in the gap.
[0023] The inventors pressure-tested a commercial upper tundish nozzle (4) as accepted to determine whether there was leakage in the gaps between the protective can (5) and its ceramic inner part (6). The nozzle was pressurized and a soapy water solution was applied to the gaps. Bubbles formed, indicating significant leakage of gas.
[0024] The inventors electroplated nickel onto the upper tundish nozzle (4) in an area that completely overlapped with the gap between the protective can (5) and the ceramic inner part (6). After electroplating the seal (11, 11'), the nozzle was pressure-tested again and it was found that the leak was blocked. This was, of course, at room temperature and not at steel casting temperature.
[0025] Next, a thermal test was performed by pouring liquid steel into a nozzle using a 100 lb open air furnace on a can having an electroplated nickel seal (11, 11'). The pour proceeded from the ladle through the upper tundish nozzle (4) to the ingot mold below the nozzle. After the steel solidified, the nozzle was inspected and it was found that the electroplated nickel seal (11, 11') was not completely damaged and survived the direct metal splashing phenomenon.
[0026] The inventors conceive of two different types of nickel seals. A first type of nickel seal (11) has been described above. It is applied externally to cover the gaps between the protective can (5) and the ceramic inner part (6). This type of seal (11) is generally applied after the upper tundish nozzle (4) is formed.
[0027] Alternatively, nickel material may be applied to one or both of the protective can (5) and the ceramic inner part (6) before the upper tundish nozzle (4) is formed. Nickel is strategically deposited on the protective can (5) and / or the ceramic inner part (6) to form a nickel seal (11') between them.
[0028] The inventors used electroplating to deposit the nickel seals (11, 11'). Other feasible techniques include electroless plating, nickel foil strips, sputtering, plasma deposition, metal printing, etc. The important thing is to form the nickel seals (11, 11') between the protective can (5) and the ceramic inner part rather than how the nickel went into place.
Claims
Claim 1 As a gas-injected upper tundish nozzle (4), a protective can (5), as a ceramic inner part (6) disposed within the protective can (5), wherein the ceramic inner part (6) has gas flow paths inside, as a gas injection port (7) attached to the protective can (5), wherein the gas injection port (7) allows the injection of gas through the protective can (5) and into the gas flow paths (8) within the ceramic inner part (6), as a gas flow seal (11, 11') formed between the protective can (5) and the ceramic inner part (6), wherein the gas flow seal (11, 11') blocks gas leakage from the gap between the protective can (5) and the ceramic inner part (6), and wherein the gas flow seal (11, 11') is formed of nickel or an alloy of nickel A gas-injected upper tundish nozzle (4), comprising, wherein the gas flow seal (11, 11') is formed by depositing nickel or a nickel alloy within any gap between the protective can (5) and the ceramic inner part (6) by a method selected from the group consisting of electroplating, electroless plating, nickel / alloy foil strips, sputtering, plasma vapor deposition, and metal printing. Claim 2 delete Claim 3 In claim 1, the gas flow seal (11, 11') is formed by electroplating nickel or a nickel alloy into any gaps between the protective can (5) and the ceramic inner part (6), in a gas-injected upper tundish nozzle (4). Claim 4 In claim 3, the nickel or nickel alloy is electroplated across the gap on the outer surface of the ceramic inner part (6) and the protective can (5), in a gas-injected upper tundish nozzle (4). Claim 5 In claim 4, the nickel or nickel alloy is electroplated across the gap on the outside of the ceramic inner part (6) and the protective can (5) after the protective can (5) and the ceramic inner part (6) are formed as a single piece, in a gas-injected upper tundish nozzle (4). Claim 6 In claim 1, the nickel or nickel alloy is deposited on one or both of the inner surface of the protective can (5) and the outer surface of the ceramic inner part (6), a gas-injected upper tundish nozzle (4). Claim 7 In claim 6, the nickel or nickel alloy is deposited on one or both of the inner surface of the protective can (5) and the outer surface of the ceramic inner part (6) before the protective can (5) and the ceramic inner part (6) are formed as a single piece, in a gas-injected upper tundish nozzle (4). Claim 8 In claim 1, the protective can (5) is a gas-injected upper tundish nozzle (4) formed of a metal material. Claim 9 In claim 8, the protective can (5) is a gas-injected upper tundish nozzle (4) formed of steel material. Claim 10 In claim 1, the ceramic inner portion (6) is formed of a porous ceramic material, and the gas flow paths include pores within the porous ceramic material, in a gas-injected upper tundish nozzle (4). Claim 11 In claim 10, the ceramic inner part (6) is formed of a gas-permeable refractory material comprising one or more ceramic oxides of aluminum, silicon, magnesium, chromium, or zirconium, or a mixture thereof, in a gas-injected upper tundish nozzle (4). Claim 12 In claim 1, the ceramic inner part (6) is not porous or gas permeable, and the gas flow paths are formed directly within the body of the ceramic inner part, gas-injected upper tundish nozzle (4). Claim 13 In claim 12, the gas flow paths include a gas distribution manifold and gas distribution channels, a gas-injected upper tundish nozzle (4). Claim 14 In claim 13, the gas distribution channels have gas outlets for releasing the gas into the steel flowing within the upper tundish nozzle, a gas-injected upper tundish nozzle (4).
Citation Information
Patent Citations
Composite hydrogen separating element and module
JP1996215547A
Upper nozzle for gas blowing of tundish
JP2004306050A
Integrated solid oxide fuel cell system with interchangeable stack and packet modules
JP2009531830A
Tundish upper nozzle