Composite, anode and electrochemical device comprising the same
A composite of garnet-type oxide particles with a copolymer coating layer addresses the dendrite formation and stability issues in lithium metal batteries by increasing ion conductivity and improving interfacial stability, thereby enhancing battery performance.
Patent Information
- Application Number
- KR1020260017235
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-01-28
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2046-01-28
AI Technical Summary
Lithium metal batteries face issues with continuous side reactions on the surface when in contact with liquid or solid electrolytes, leading to the formation of non-uniform lithium dendrites, which cause short circuits and severe lifespan degradation due to insufficient mechanical strength and ion conductivity of the solid electrolyte interphase (SEI).
A composite comprising garnet-type oxide particles with a coating layer formed by copolymerizing a monomer containing a carboxyl group and an amphoteric ion monomer is used to enhance ion conductivity and suppress dendrite formation, improving interfacial stability between the cathode and electrolyte.
The composite effectively increases ion conductivity and suppresses dendrite growth, enhancing the stability and performance of lithium metal batteries by improving the interfacial stability and removing impurities within the SEI.
Smart Images

Figure 112026012063936-PAT00009_ABST
Abstract
Description
Technology Field
[0001] The present invention (Disclosure) relates to a composite, and more specifically to a composite, a cathode, and an electrochemical device comprising the same.
[0002] This research was conducted with funding from the government (Ministry of Science and ICT) in 2025 and supported by the National Science and Technology Research Council's Global TOP Strategic Research Group Support Project (No. GTL24012-000). Background Technology
[0003] Batteries using lithium metal (Li metal) as the anode are attracting attention as next-generation high-energy secondary batteries due to their large theoretical capacity and low potential. However, lithium metal has problems such as continuous side reactions occurring on the surface when in contact with liquid or solid electrolytes, and the growth of non-uniform lithium dendrites during the charging and discharging process, which causes short circuits and severe lifespan degradation.
[0004] On the surface of lithium metal, the solid electrolyte interphase (SEI) formed by electrolyte decomposition lacks sufficient mechanical strength and ion conductivity, and cracking and delamination occur due to volume changes and localized current concentration resulting from repeated charging and discharging. Consequently, new lithium surfaces are continuously exposed and the SEI is reformed, leading to continuous lithium consumption, increased interfacial resistance, and the creation of an environment conducive to dendrite growth. Prior art literature
[0005] Korean Registered Patent Publication No. 10-2832655 (Published July 9, 2025) The problem to be solved
[0006] According to one aspect, it provides a composite that improves the performance of an electrochemical device.
[0007] According to another aspect, it provides a composite that improves the interfacial stability between the cathode and the electrolyte.
[0008] According to another aspect, the invention provides a composite that can increase the ion conductivity of an electrochemical device and effectively suppress the formation of dendrites.
[0009] According to another aspect, a cathode comprising the aforementioned complex is provided.
[0010] According to another aspect, an electrochemical device comprising the aforementioned cathode is provided.
[0011] The objects of the present invention are not limited to those mentioned above, and other unmentioned objects and advantages of the present invention may be understood from the following description and will be more clearly understood by the embodiments of the present invention. Furthermore, it will be readily apparent that the objects and advantages of the present invention can be realized by the means and combinations thereof described in the specification. means of solving the problem
[0012] According to one aspect, a composite is provided comprising garnet-type oxide particles and a coating layer on said garnet-type oxide particles, wherein the coating layer comprises a copolymer in which a monomer containing a carboxyl group and a zwitterion monomer are copolymerized.
[0013] In some embodiments, the garnet-type oxide particles may include a compound represented by the following chemical formula 1.
[0014] [Chemical Formula 1]
[0015] Li a La3M2O 12
[0016] In the above chemical formula 1, a is a real number between 6 and 8, and M is one or more selected from the group consisting of Zr, Hf, Ta, Nb, Sn, Sc, and Y.
[0017] In some embodiments, the amphoteric ionic monomer may include at least one of the compounds represented by the following general formulas 1 and 2.
[0018] [General Formula 1]
[0019]
[0020] [General Formula 2]
[0021]
[0022] In the above general formulas 1 and 2, R1 is each independently a hydrogen atom; or an alkyl group having 1 to 3 carbon atoms, and L1 is each independently an ester group (-COO-), an amide group (-CONH-), or a phenylene group, and R a and R b One of them is a positively charged atomic group and the other is a negatively charged atomic group, and in the above general formula 1, R2 and R3 are each independently directly bonded; or are alkylene groups with 1 to 5 carbon atoms.
[0023] In some alternative or additional embodiments, the positively charged atomic group comprises an ammonium ion, a sulfur ion, or a phosphorus cation, and the negatively charged atomic group comprises a carboxylate, SO3 -, or PO4 - It may include.
[0024] In some embodiments, the amphoteric ionic monomer comprises a compound represented by General Formula 1, wherein L1 is an ester group (-COO-), R2 and R3 are each independently an alkylene group having 1 to 5 carbon atoms, and R a is -N + (R a1 )2- and, here R a1 Each is independently an alkyl group having 1 to 3 carbon atoms, and R b -SO3 - It could be.
[0025] According to another aspect, a cathode is provided comprising a lithium metal (Li metal) and a protective film on at least one surface of the lithium metal, wherein the protective film comprises a composite of some embodiments.
[0026] In some embodiments, the protective film further comprises a binder, and the content of the binder may be 1 part by weight or more and 30 parts by weight or less per 100 parts by weight of the composite.
[0027] According to another aspect, an electrochemical element is provided comprising a cathode of some embodiment; an anode; and an electrolyte.
[0028] In some embodiments, the anode may include a lithium transition metal oxide; or sulfur.
[0029] In some embodiments, the electrochemical element may further include a separator.
[0030] According to another aspect, an electric vehicle including the above-mentioned electrochemical element may be provided.
[0031] The means for solving the above problem are not all of the features of the present invention and may be combined with some embodiments of this specification. Various features of the present invention and the advantages and effects derived therefrom may be understood in more detail by referring to the specific description below. Effects of the invention
[0032] According to one aspect, the interfacial stability between the cathode and the electrolyte can be improved.
[0033] According to another aspect, the ionic conductivity of the electrochemical device can be increased and the formation of dendrites can be effectively suppressed.
[0034] In addition to the effects described above, specific effects of the present invention are described together with the following explanation of specific details for implementing the invention. Furthermore, the effects of the present invention are not limited to those mentioned above and can be easily realized by means and combinations thereof described in the specification. Brief explanation of the drawing
[0035] Figure 1 shows the FT-IR (Fourier transform infrared spectroscopy) analysis results of LLZTO and the composite according to Synthesis Example 1. Figure 2 is a transmission electron microscope image of the composite according to Synthesis Example 1. Figure 3 is a schematic diagram showing the manufacturing process of a cathode according to Example 1. Figure 4 is a scanning electron microscope image showing the process of forming a protective film on the surface of lithium metal using aluminum foil as a transfer substrate. Figure 5 is a scanning electron microscope image of a vertically cut cross-sectional view of the cathode according to Example 1. FIG. 6 is a graph showing the ionic conductivity of a coin cell including a cathode according to Comparative Example 1, Comparative Example 2, and Example 1. Figure 7 shows the lithium ion transfer rate (Transference number) of the cathode according to Comparative Example 1, Comparative Example 2, and Example 1. FIG. 8 is a graph showing the cycle performance of a symmetric cell including a cathode according to Comparative Example 1, Comparative Example 2, and Example 1. Figure 9 shows a current density of 0.1 mA / cm² 2 , 0.5 mA / cm 2 , 1 mA / cm 2 , 2 mA / cm 2 , or 5 mA / cm 2 When adjusted to, This is a graph showing the cycle performance of a symmetric cell including a cathode according to Comparative Example 1, Comparative Example 2, and Example 1. FIG. 10 is a scanning electron microscope image of the surface of the cathode of the symmetric cell according to Comparative Example 1 and Example 1 after 100 cycles. FIG. 11 is a charge / discharge graph of a cell according to Comparative Example 1, Comparative Example 2 and Example 1. FIG. 12 is a graph showing the discharge capacity and Coulomb efficiency according to the number of cycles of the cell according to Comparative Example 1, Comparative Example 2 and Example 1. FIG. 13 is a charge / discharge graph of a cell according to Comparative Example 1 and Example 1. Figure 14 is a graph showing the discharge capacity and Coulomb efficiency according to the number of cycles of the cell according to Comparative Example 1 and Example 1. Specific details for implementing the invention
[0036] In this specification, singular expressions include plural expressions unless the context clearly indicates otherwise.
[0037] In the present specification, if multiple numerical values are disclosed for the upper and lower limits of any numerical range, the numerical range disclosed in the present specification may be understood as a range of any numerical values in which any one of the multiple lower limit values and any one of the multiple upper limit values are respectively the lower limit value and the upper limit value. For example, if a or greater, or b or greater; and c or less, or d or less is described, it may be understood as a or greater and c or less, a or greater and d or less, b or greater and c or less, or b or greater and d or less.
[0038] In this specification, a composite is defined as a material in which two or more different materials are combined and interact physically and / or chemically to exhibit an effective function.
[0039] According to one aspect of the present invention, a composite is provided comprising: garnet-type oxide particles; and a coating layer on said garnet-type oxide particles, wherein the coating layer comprises a copolymer formed by copolymerizing a monomer containing a carboxyl group and an amphoteric ion monomer. According to one aspect, by including the copolymer formed by copolymerizing a monomer containing a carboxyl group and an amphoteric ion monomer in the coating layer, the ion conductivity can be increased, and at the same time, impurities (e.g., lithium carbonate) within the SEI formed on the interface between the lithium metal and the cathode can be effectively removed. Specifically, the monomer containing a carboxyl group can effectively remove impurities (e.g., lithium carbonate) within the SEI, thereby improving the interfacial stability between the cathode and the electrolyte. Furthermore, the amphoteric ion monomer can contain both positive and negative charges within a single molecule, thereby capturing electrolyte anions and inducing a solvation structure around lithium ions. Accordingly, the mobility rate of lithium ions increases, which can further increase the ion conductivity of the electrochemical device.
[0040] The configuration of the present invention will be described in more detail below.
[0041] 1. Complex
[0042] Garnet-type oxide particles
[0043] In this specification, garnet-type oxide particles are defined as lithium-ion conductive ceramic particles having a garnet structure. For example, the garnet-type oxide particles may have a structure in which 8-coordinate LaO octahedra and 6-coordinate MO6 (M = Zr, Hf, Ta, Nb, Sn, Sc, or Y, etc.) octahedra form a three-dimensional framework, and lithium ions occupy and move in the tetrahedral / octahedral vacancies between them.
[0044] The garnet-type oxide particles according to the present invention serve as core particles of a composite, and can increase ion conductivity and effectively inhibit the growth of dendrites.
[0045] In some embodiments of the present invention, the garnet-type oxide particles may include a compound represented by the following chemical formula 1.
[0046] [Chemical Formula 1]
[0047] Li a La3M2O 12
[0048] In the above chemical formula 1, a is a real number between 6 and 8, and M is one or more selected from the group consisting of Zr, Hf, Ta, Nb, Sn, Sc, and Y. In some embodiments, the garnet-type oxide particles may include a compound represented by the above chemical formula 1, thereby increasing ion conductivity and effectively inhibiting the growth of dendrites.
[0049] In some embodiments of the present invention, the garnet-type oxide particles may include a compound represented by the following chemical formula 1-1.
[0050] [Chemical Formula 1-1]
[0051] Li a La3M1 b1 M2 b2 O 12
[0052] In the above chemical formula 1-1, a is a real number between 6 and 8, b1 and b2 are each independently real numbers between 0 and 2 satisfying b1+b2=2, M1 is one or more selected from the group consisting of Zr, Hf, Ta, Nb, Sn, Sc, and Y, and M2 is different from M1 and is one or more selected from the group consisting of Zr, Hf, Ta, Nb, Sn, Sc, and Y. In some embodiments, the garnet-type oxide particles include a compound represented by the above chemical formula 1-1, thereby increasing ionic conductivity and effectively inhibiting dendrite growth.
[0053] In some non-limiting examples, the above garnet-type oxide particles are Li7La3Zr2O 12 , Li 6.5 La3Zr 1.5Ta 0.5 O 12 , Li 6.5 La3Zr 1.5 Nb 0.5 O 12 , and Li 6.4 La3Zr 1.4 Ta 0.6 O 12 It may include one or more types selected from the group consisting of
[0054] In this specification, the average particle size (D 50 ) refers to the particle size at the 50% reference of the volume-cumulative particle size distribution of the powder to be measured. The above D 50 The particle size can be measured by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) to obtain a volume-cumulative particle size distribution graph, and then determining the particle size corresponding to 50% of the volume-cumulative amount.
[0055] In some embodiments of the present invention, the average particle size (D) of the garnet-type oxide particles 50 The value may be 10 nm or more and 50 μm or less. In some embodiments, the average particle size of the garnet-type oxide particles is controlled to the above range, thereby further improving the interfacial stability between the cathode and the electrolyte while simultaneously increasing the ion conductivity.
[0056] coating layer
[0057] In this specification, a “layer” or “film” may include cases where, when observing the region in which the layer or film exists, it is formed over the entire region, or cases where it is formed only in a part of the region. For example, the surface of the layer or film may be defined as having a flat shape, a non-flat shape, and combinations thereof; or a continuous shape, a discontinuous shape, and combinations thereof. For example, when another member is composed of a layer or film directly on a member, the coverage of the other member on the surface of the member may be defined as 1% or more, 5% or more, 10% or more, 20% or more, 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 80% or more, 85% or more, 90% or more, 95% or more, or 99% or more. For example, it may also be defined as a “layer” or “film” when a plurality of particles form a clustered structure.
[0058] The coating layer according to the present invention can inhibit the growth of lithium dendrites while simultaneously effectively removing impurities (e.g., lithium carbonate) within the SEI formed on the interface between the lithium metal and the cathode. In addition, the coating layer can capture electrolyte anions and induce a solvation structure around lithium ions. Accordingly, the mobility rate of lithium ions increases, thereby further enhancing ion conductivity.
[0059] The coating layer according to the present invention comprises a copolymer in which a monomer containing a carboxyl group and an amphoteric ion monomer are copolymerized. Specifically, the monomer containing a carboxyl group can effectively remove impurities within the SEI, thereby improving the interfacial stability between the cathode and the electrolyte. Furthermore, the amphoteric ion monomer contains both positive and negative charges within a single molecule, which can capture electrolyte anions and induce a solvation structure around lithium ions. Accordingly, the mobility rate of lithium ions increases, thereby further enhancing ionic conductivity.
[0060] In some embodiments of the present invention, the monomer containing the carboxyl group may further include an intramolecular reactive functional group. Specifically, the reactive functional group may include one or more selected from the group consisting of vinyl groups, methacrylic groups, acrylic groups, methacrylate groups, and acrylate groups. In some embodiments, the reactive functional group may be a functional group that forms a copolymerization reaction with an amphoteric ionic monomer.
[0061] In this specification, a zwitterion monomer is defined as a compound having both a positive and a negative charge within a single molecule, which reacts with the reactive functional group of a monomer containing the carboxyl group to form a copolymer.
[0062] In some embodiments of the present invention, the amphoteric ionic monomer may include at least one of the compounds represented by the following general formulas 1 and 2.
[0063] [General Formula 1]
[0064]
[0065] [General Formula 2]
[0066]
[0067] In the above general formulas 1 and 2, R1 may each independently be a hydrogen atom; or an alkyl group having 1 to 3 carbon atoms, and L1 may each independently be an ester group (-COO-), an amide group (-CONH-), or a phenylene group, and R a and R b One of them is a positively charged atomic group, and the other is a negatively charged atomic group.
[0068] In the above general formula 1, R2 and R3 may each be independently directly bonded; or may be alkylene groups with 1 to 5 carbon atoms.
[0069] In some embodiments, the amphoteric ionic monomer may include at least one of the compounds represented by General Formulas 1 and 2, thereby capturing electrolyte anions and inducing a solvation structure around lithium ions. Accordingly, the mobility rate of lithium ions increases, which can further increase ionic conductivity.
[0070] In some embodiments of the present invention, the positively charged atomic group may include an ammonium ion, a sulfur ion, or a phosphorus cation, specifically, an ammonium ion. In some examples, the ammonium ion may include a pyridinium ion or a quaternary ammonium ion. In some alternative or additional examples, the sulfur ion is S + It may include (R)3 (where R is an organic group with 1 or more carbon atoms). In some alternative or additional examples, the above phosphorus cation is P + It may include (R)4 (where R is an organic group with 1 or more carbon atoms). In some embodiments, the ionic conductivity of the electrochemical element may be further increased by including an ammonium ion in the positively charged atomic group.
[0071] In some embodiments of the present invention, the negatively charged atomic group is a carboxylate (COO) - ), SO3 -, or PO4 - It may include, specifically SO3- It may include. In some embodiments, the negatively charged atomic group is SO3 - By including it, the ionic conductivity of the electrochemical device can be further increased.
[0072] In some embodiments of the present invention, the amphoteric ionic monomer may comprise a compound represented by General Formula 1. In this case, L1 in General Formula 1 is an ester group (-COO-), R2 and R3 are each independently an alkylene group having 1 to 5 carbon atoms, and R a is -N + (R a1 )2- and, here R a1 Each is independently an alkyl group having 1 to 3 carbon atoms, and R b -SO3 - It may be. In some embodiments, the above L1, R2, R3, R a , R b By controlling it with the above structure, the ionic conductivity of the electrochemical device can be further increased.
[0073] In some embodiments of the present invention, the molar ratio of the monomer containing the carboxyl group to the amphoteric ionic monomer may be 1:9 to 9:1, specifically 2:8 to 8:2, or 3:7 to 7:3. In some embodiments, by adjusting the molar ratio to the above range, the ionic conductivity can be increased and the interfacial stability between the cathode and the electrolyte can be further improved.
[0074] In this specification, "weight-average molecular weight" or "number-average molecular weight" refers to the standard polystyrene equivalent molecular weight and can be analyzed using a Gel Permeation Chromatography (GPC) device. For example, in the case of the GPC analysis method, the developing solvent may be set to tetrahydrofuran (THF), the column to be PL Olexis from Polymer Laboratories, the sample concentration to be 5 mg / mL, the sample injection volume to be 100 µl, the flow rate to be 1 mL / min, the detector to be an Agilent High Temperature RI detector, and the column temperature to be 40 ℃.
[0075] In some embodiments of the present invention, the weight-average molecular weight of the copolymer formed by copolymerizing the monomer containing the carboxyl group and the zwitterion monomer may be 145,000 Da or more and 260,000 Da or less. In some embodiments, by controlling the weight-average molecular weight of the copolymer to the above range, the ionic conductivity can be increased and the interfacial stability between the cathode and the electrolyte can be further improved.
[0076] In some embodiments of the present invention, the average thickness of the coating layer may be 10 nm or more and 100 μm or less. Specifically, the average thickness of the coating layer may be 15 nm or more, or 18 nm or more, and 20 nm or less, 30 nm or less, or 35 nm or less. In some embodiments, by controlling the average thickness of the coating layer to the above range, the ion conductivity can be increased and the interfacial stability between the cathode and the electrolyte can be further improved.
[0077] 2. Cathode
[0078] According to another aspect of the present invention, a cathode is provided comprising a lithium metal (Li metal) and a protective film on at least one surface of the lithium metal, wherein the protective film comprises a composite of some embodiments. According to another aspect, by the protective film comprising a composite of some embodiments, impurities (e.g., lithium carbonate) in the SEI formed on the interface between the lithium metal and the cathode can be effectively removed. Additionally, the protective film can further improve the interfacial stability between the electrolyte and the cathode and increase ion conductivity.
[0079] In some embodiments of the present invention, the content of the composite may be 50 parts by weight or more, 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, or 90 parts by weight or more, and 85 parts by weight or less, 95 parts by weight or less, or 99 parts by weight or less, based on 100 parts by weight of the protective film. In some embodiments, by controlling the content of the composite to the above range, impurities (e.g., lithium carbonate) in the SEI formed on the interface between the lithium metal and the cathode can be effectively removed. In addition, the interface stability between the electrolyte and the cathode can be further improved and the ion conductivity can be increased.
[0080] In some embodiments of the present invention, the protective film may further include a binder. Specifically, the binder may bind the composites within the protective film together to further improve the durability of the protective film.
[0081] In some embodiments of the present invention, the content of the binder (based on solid content) may be 1 part by weight or more and 30 parts by weight or less per 100 parts by weight of the composite, specifically 5 parts by weight or more, or 10 parts by weight or more, and 13 parts by weight or less, 17 parts by weight or less, or 25 parts by weight or less. In some embodiments, by controlling the content of the binder to the above range, the durability of the protective film may be further improved, and at the same time, the interfacial stability between the electrolyte and the cathode may be further improved.
[0082] In some non-limiting examples, the binder is polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, poly(ethylene-co-vinyl acetate), polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, It may include one or more selected from the group consisting of cyanoethylpolyvinyl alcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxyl methylcellulose, acrylonitrile-styrene butadiene copolymer, polyimide, and styrene-butadiene rubber.
[0083] In some embodiments of the present invention, the protective film may be formed by a transfer method using a transfer substrate (e.g., aluminum foil). In some embodiments, by forming the protective film by the transfer method, the effect of making the surface of the protective film dense and having a uniform thickness can be achieved. Accordingly, the interface stability between the electrolyte and the cathode can be further improved.
[0084] In some embodiments of the present invention, the average thickness of the protective film may be 10 nm or more and 100 μm or less. Specifically, the average thickness of the protective film may be 7 μm or more, or 8 μm or more, and 10 μm or less, 20 μm or less, or 25 μm or less. In some embodiments, by adjusting the average thickness of the protective film to the above range, the durability of the protective film and the interfacial stability between the electrolyte and the cathode may be further improved.
[0085] 3. Electrochemical devices
[0086] In this specification, the term electrochemical device is defined as a lithium metal battery (Li metal battery), a lithium-sulfur battery (Li-sulfur battery), or an all-solid-state battery.
[0087] According to another aspect of the present invention, an electrochemical device is provided comprising a cathode of some embodiment; an anode; and an electrolyte. According to another aspect, by including a cathode of some embodiment, the electrochemical device can increase the capacity and Coulomb efficiency of the electrochemical device and increase long-term cycle performance. In addition, electrochemical performance can be maintained consistently even under high current density conditions.
[0088] anode
[0089] In some embodiments of the present invention, the positive electrode may have a form in which a positive active material is laminated on a positive current collector.
[0090] For example, the above positive current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used.
[0091] In some embodiments, the cathode active material may include a lithium transition metal oxide. The lithium transition metal oxide is, for example, Li x1 CoO2(0.5 <x1<1.3), Li x2 NiO2(0.5 <x2<1.3), Li x3 MnO2(0.5 <x3<1.3), Li x4 Mn2O4(0.5 <x4<1.3), Li x5 (Ni a1 Co b1 Mn c1 )O2(0.5 <x5<1.3, 0<a1<1, 0<b1<1, 0<c1<1, a1+b1+c1=1), Li x6 Ni 1-y1 Co y1 O2(0.5 <x6<1.3, 0<y1<1), Li x7 Co 1-y2 Mn y2 O2(0.5 <x7<1.3, 0≤y2<1), Li x8 Ni 1-y3 Mn y3 O2(0.5 <x8<1.3, 0≤y3<1), Li x9 (Ni a2 Co b2 Mn c2 )O4(0.5 <x9<1.3, 0<a2<2, 0<b2<2, 0<c2<2, a2+b2+c2=2), Li x10 Mn 2-z1 Ni z1 O4(0.5 <x10<1.3, 0<z1<2), Li x11 Mn 2-z2 Co z2 O4(0.5 <x11<1.3, 0<z2<2), Li x12CoPO4(0.5 <x12<1.3) 및 Li x13 FePO4(0.5 <x13<1.3)로 이루어진 군에서 선택되는 하나 이상일 수 있다.
[0092] In some alternative or additional embodiments, the positive electrode active material may comprise sulfur, specifically elemental sulfur (S8), sulfur-based compounds, or mixtures thereof, and since sulfur materials alone are not electrically conductive, they may be applied in combination with a conductive material. Specifically, the sulfur-based compounds include Li2Sn (n≥1), organic sulfur compounds, or carbon-sulfur polymers (C2S x ) n : x=2.5 to 50, n≥2) etc.
[0093] For example, the above conductive material is used to further improve the conductivity of the electrode active material. Such conductive material is not particularly limited as long as it possesses conductivity without causing chemical changes in the battery, and examples may be used, such as graphite, such as natural graphite or artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as carbon fluoride, aluminum, or nickel powder; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; or polyphenylene derivatives.
[0094] In some embodiments of the present invention, the anode may further include an electrode binder for bonding the anode active material and the conductive material and bonding to the current collector. For example, the electrode binder may include a thermoplastic resin or a thermosetting resin, and specifically, may include one or more selected from the group consisting of polyethylene, polypropylene, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), styrene-butadiene rubber, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymer, propylene-tetrafluoroethylene copolymer, ethylene-chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethylvinyl ether-tetrafluoroethylene copolymer, and ethylene-acrylic acid copolymer.
[0095] For example, the above-mentioned anode can be manufactured according to a conventional method. Specifically, a composition for forming an anode active material layer, prepared by mixing an anode active material, a conductive material, and a binder in an organic solvent, can be applied and dried onto a current collector, and optionally, compression molded onto the current collector to improve electrode density. At this time, it is preferable to use an organic solvent that can uniformly disperse the anode active material, binder, and conductive material and evaporates easily. Specifically, examples include acetonitrile, methanol, ethanol, tetrahydrofuran, water, isopropyl alcohol, etc.
[0096] electrolytes
[0097] In some embodiments of the present invention, the electrolyte may be a lithium salt-containing electrolyte, and may be an aqueous or non-aqueous electrolyte.
[0098] In some non-limiting examples, non-aqueous organic solvents are N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethylmethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydroxyfranc, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxene, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate Aprotic organic solvents such as derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate may be used.
[0099] In some non-limiting examples, the lithium salt is a substance that is easily soluble in the non-aqueous electrolyte and may include LiCl, LiNO3, LiTFSI, LiLiBr, LiI, LiClO4, LiBF4, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, LiSCN, LiC(CF3SO2)3, (CF3SO2)2NLi, (FSO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate, lithium imide, etc.
[0100] In some alternative or additional embodiments, the electrolyte may include a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a polymeric solid electrolyte.
[0101] Separator
[0102] The separation membrane according to the present invention may be composed of a porous substrate or may include a porous substrate and a coating layer.
[0103] The porous substrate according to the present invention can be a porous structure with high resistance to electrolytes and fine pore diameters, capable of electrically insulating the cathode and anode to prevent short circuits while providing a pathway for the movement of lithium ions.
[0104] In some examples, the constituent material of the porous substrate may be an organic or inorganic material having electrical insulating properties, without being particularly limited. The porous substrate may include, for example, at least one selected from the group consisting of polyolefin, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenyleneoxide, polyphenylenesulfide, and polyethylenenaphthalate, and specifically may include polyolefin. Polyolefins not only have excellent coating properties but also allow for a thinner separator, thereby increasing the proportion of the electrode active material layer within the battery and raising the capacity per unit volume.
[0105] In some examples, the weight-average molecular weight (Mw) of the polyolefin may be 100,000 to 500,000 g / mol. If the weight-average molecular weight of the polyolefin is below the above numerical range, it may be difficult to secure sufficient mechanical properties, and if it exceeds the above numerical range, the shutdown function may not be implemented or molding may be difficult. The shutdown function refers to the function of preventing thermal runaway of the battery by blocking the movement of ions through the melting of the thermoplastic resin and closing the pores of the porous substrate when the temperature of the secondary battery rises.
[0106] In some examples, the thickness of the porous substrate may be, for example, 3 to 50 μm or 4 to 30 μm. If the thickness of the porous substrate is less than the numerical range, the function of the conductive barrier may not be sufficient, and if it exceeds the numerical range, the resistance of the separator may increase excessively.
[0107] In some examples, the average diameter of the pores included in the porous substrate may be, for example, 10 to 100 nm. The pores included in the porous substrate have a structure in which they are interconnected, so that gas or liquid can pass from one side of the porous substrate to another.
[0108] A separator according to another embodiment of the present invention may include a coating layer disposed on at least one surface of the porous substrate, which can improve the mechanical strength and heat resistance of the separator for a secondary battery and increase the ion conductivity within the secondary battery.
[0109] The coating layer according to the present invention may include a binder polymer and inorganic particles.
[0110] The binder polymer according to the present invention can connect inorganic particles and stably fix them. The above binder polymer is, for example, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, poly(ethylene-co-vinyl acetate), polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, One or more selected from the group consisting of cyanoethylpolyvinyl alcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxymethylcellulose, acrylonitrile-styrene butadiene copolymer, polyimide, and styrene-butadiene rubber may be used in combination.
[0111] According to another embodiment of the present invention, the weight ratio of the inorganic particles to the binder polymer (inorganic particles:binder polymer) may be 50:50 to 99:1, and specifically 70:30 to 95:5. If the content ratio of inorganic particles to the binder polymer is less than the above numerical range, the content of the binder polymer increases, which may reduce the performance of improving the thermal safety of the separator, and the pore size and porosity decrease due to the reduction of empty spaces formed between the inorganic particles, which may cause a decrease in the performance of the final battery, and if it exceeds the above numerical range, the content of the binder polymer is too low, which may weaken the peel resistance of the coating layer.
[0112] The inorganic particles according to the present invention can contribute to improving the mechanical strength and heat resistance of a separator for a secondary battery. Specifically, the inorganic particles are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in the present invention are applicable within the operating voltage range of the secondary battery (e.g., Li / Li). + There are no particular limitations as long as oxidation and / or reduction reactions do not occur at a standard voltage of 0 to 5V. As an example, if inorganic particles with a high dielectric constant are used as inorganic particles, it can contribute to increasing the degree of dissociation of electrolyte salts, such as lithium salts, in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte.
[0113] For the reasons stated above, the inorganic particles may be inorganic particles having a dielectric constant of 5 or more, inorganic particles having lithium ion transport capability, or a mixture thereof. In some examples, the inorganic particles having a dielectric constant of 5 or more are Al2O3, SiO2, ZrO2, AlO(OH), Al(OH)3, Mg(OH)2, BaSO4, TiO2, BaTiO3, Pb(Zr x Ti 1-x )O3(PZT, where 0 <x<1), Pb 1-x La x Zr 1-y Ti yO3(PLZT, where, 0 < x < 1, 0 < y < 1), (1-x)Pb(Mg 1 / 3 Nb 2 / 3 )O 3-x It may be one or more mixtures selected from the group consisting of PbTiO3 (PMN-PT, where 0 < x < 1), HfO2, SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, and SiC. In some examples, the inorganic particles having lithium ion transfer capability are lithium phosphate (Li3PO4) and lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y Series glass (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride(Li x N y , 0 < x < 4, 0 < y < 2), SiS2 series glass(Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4) and P2S5 series glass (Li x P y S zIt may be one or more mixtures selected from the group consisting of , 0 < x < 3, 0 < y < 3, 0 < z < 7). In some examples, the average particle size (D) of the inorganic particles. 50 ) may be 1 nm to 10 µm for the formation of a coating layer of uniform thickness and appropriate porosity, specifically 10 nm to 2 µm, and more specifically 50 nm to 1 µm. The above "average particle size (D 50 "" refers to the particle size at the 50% point of the cumulative distribution of particle numbers according to particle size. The above average particle size can be measured using the laser diffraction method. Specifically, after dispersing the powder to be measured in a dispersion medium, the powder is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) to measure the difference in diffraction patterns according to particle size as the particles pass through the laser beam, thereby calculating the particle size distribution.
[0114] In some alternative or additional examples, the thickness of the coating layer may be 0.1 to 10 μm, specifically 1 to 3 μm, and more specifically 1.4 to 1.6 μm. When the thickness of the coating layer satisfies the above numerical range, the insulation and thermal stability of the separator can be increased, and at the same time, the energy density of the battery can be improved.
[0115] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the present invention; however, this is merely an example, and the scope of the present invention is not limited by the following.
[0116] [Synthesization Example 1: Synthesis of a Complex]
[0117] In 2,2,2-trifluoroethanol (TFE), garnet-type oxide particles (Li 6.4 La3Zr 1.4 Ta 0.6 O12 A mixture was prepared with a total solid content of 2-3 wt% by mixing poly(acrylic acid-co-sulfobetaine methacrylate), copolymerized of acrylic acid and sulfobetaine methacrylate in a molar ratio of 45:55 (hereinafter referred to as 'Poly(AA-co-SBMA)'), in a weight ratio of 90:10. At this time, the weight-average molecular weight of the poly(acrylic acid-co-sulfobetaine methacrylate) was controlled to approximately 260,000 Da. Alternatively, sulfobetaine methacrylate is ([2-(Methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide).
[0118] The above mixture was mixed overnight at about 300 rpm at room temperature, and then the solid was obtained by centrifugation. The solid was dried overnight in a vacuum oven at about 25 ℃ to prepare a composite.
[0119] [Experimental Example 1: FT-IR Analysis of the Complex]
[0120] Figure 1 shows the FT-IR (Fourier transform infrared spectroscopy) analysis results of LLZTO and the composite according to Synthesis Example 1.
[0121] Referring to FIG. 1, unlike LLZTO, the composite according to Synthesis Example 1 is approximately 2,923 cm⁻¹ -1 , approximately 2,853 cm -1 Stretching peaks of -CH3 and -CH2- were observed. In addition, the composite according to Synthesis Example 1 showed CO3 relative to LLZTO. 2- The result showed that the peak became smaller. Through this, it was confirmed that a coating layer containing Poly(AA-co-SBMA) was formed on the surface of LLZTO.
[0122] [Experimental Example 2: Confirmation of the presence of a coating layer in the composite]
[0123] Figure 2 is a transmission electron microscope image of the composite according to Synthesis Example 1.
[0124] Referring to Fig. 2, a composite with a coating layer formed on the surface of LLZTO was confirmed. At this time, the average thickness of the coating layer is approximately 18 nm.
[0126] [Preparation Example 1: Preparation of Cathode]
[0127] <Example 1>
[0128] Figure 3 is a schematic diagram showing the manufacturing process of a cathode according to Example 1.
[0129] Referring to FIG. 3, after grinding the composite of Synthesis Example 1 with a hand mixer, PVDF (Poly vinylidene fluoride), M w A slurry was prepared by adding a binder solution in which approximately 10 wt% of the composite (=88,000 g / mol) was dissolved in N,N-dimethylformamide. At this time, the weight ratio of the composite and the solid content in the binder solution was adjusted to 90:10. The slurry was mixed using a Thinky mixer for approximately 10 minutes. After coating the mixed slurry onto the surface of a transfer substrate (aluminum foil), it was dried in a vacuum oven at approximately 60°C for approximately 4 hours to form a preliminary protective film (pre-transfer state). Using the transfer substrate with the preliminary protective film formed thereon, the preliminary protective film was transferred onto the surface of lithium metal (Li metal) with a thickness of approximately 300 μm to finally manufacture a cathode coated with a protective film of approximately 9 μm.
[0130] <Comparative Example 1: Bare Li>
[0131] A lithium metal (Li metal) with a thickness of about 300 μm was prepared as the negative electrode.
[0132] <Comparative Example 2: LLZTO / Li>
[0133] A cathode was prepared in the same manner as in Example 1, except that LLZTO was used instead of the composite of Synthesis Example 1.
[0135] [Experimental Example 3: SEM image of the protective film formed on the cathode surface]
[0136] Figure 4 is a scanning electron microscope image showing the process of forming a protective film on the surface of lithium metal using aluminum foil as a transfer substrate.
[0137] Referring to Fig. 4, it was confirmed that after a preliminary protective film containing the composite of Synthesis Example 1 is coated on the surface of an aluminum foil (transfer substrate), the preliminary protective film is transferred to the surface of a lithium metal through a transfer process to form a protective film.
[0138] Figure 5 is a scanning electron microscope image of a vertically cut cross-sectional view of the cathode according to Example 1.
[0139] Referring to FIG. 5, it was confirmed that the cathode according to Example 1 comprises lithium metal and a protective film (average thickness: about 8 to 9 μm) coated on the surface of the lithium metal.
[0141] [Experimental Example 4: Measurement of Ionic Conductivity and Lithium Ion Transfer Rate of Coin Cells]
[0142] FIG. 6 is a graph showing the ionic conductivity of a coin cell containing a cathode according to Comparative Example 1, Comparative Example 2, and Example 1. Specifically, for the analysis of the ionic conductivity, a 2032 coin cell containing the cathode of Preparation Example 1 was prepared. Polyethylene was used as the separator, and a solution (approx. 85 μl) of 1 M LiPF6 dissolved in a mixed solvent in which EC and DEC were mixed in a 1:1 volume ratio was used as the electrolyte. The ionic conductivity of the coin cell was calculated using the resistance value from the Nyquist plot obtained through Electrochemical Impedance Spectroscopy (EIS) at a frequency range of approximately 1.0 MHz to 1.0 Hz and at approximately 25 ℃, and the following Equation 1.
[0143] [Mathematical Formula 1]
[0144] Ionic conductivity (mS / cm) = L / (RXS)
[0145] In the above mathematical formula 1, R is the resistance value (Ω) obtained through Nyquist plot analysis, S is the effective contact area between the cathode and the electrolyte, and is the thickness of the cathode. At this time, the thickness of Comparative Example 1 was adjusted to approximately 16 μm (polyethylene separator), the thickness of Comparative Example 2 to approximately 27 μm, and the thickness of Example 1 to approximately 28 μm.
[0146] Referring to Fig. 6, it was confirmed that the coin cell according to Example 1 exhibits an ionic conductivity of approximately 1.21 mS / cm or higher compared to Comparative Examples 1 and 2.
[0147] FIG. 7 shows the lithium ion transfer rate (Transference number) of the cathode according to Comparative Example 1, Comparative Example 2, and Example 1. Specifically, the lithium ion transfer rate was measured under conditions of a voltage of about 10 mV, a measurement time of about 1,000 seconds, and a temperature of about 25 ℃.
[0148] Referring to Fig. 7, it was confirmed that the lithium ion transfer rate of the coin cell according to Example 1 is approximately 0.73 or higher than that of Comparative Examples 1 and 2. Through this, it can be inferred that the inclusion of the composite of Synthetic Example 1 in the protective film of the negative electrode allows lithium ions to move selectively, thereby further improving rapid charging and the lifespan of the electrochemical device.
[0150] [Experimental Example 5: Evaluation of Electrochemical Performance of the Cell]
[0151] FIG. 8 is a graph showing the cycle performance of a symmetric cell comprising a cathode according to Comparative Example 1, Comparative Example 2, and Example 1. Specifically, the symmetric cell comprises a lithium metal / polyethylene separator / a cathode according to Comparative Example 1, Comparative Example 2, and Example 1; and an electrolyte (approx. 95 μL) in which 1M LiPF6 is dissolved in a mixed solvent in which EC and DEC are mixed in a 1:1 volume ratio. At this time, the thickness of each lithium metal was adjusted to approximately 12 mm. Approx. 0.5 mA / cm² for the symmetric cell 2Apply a constant current of 1mAh / cm 2 Charge stage that terminates upon arrival; stage of stabilizing voltage through a resting process of approximately 10 minutes; approximately 0.5 mA / cm 2 A cycle consisting of a discharge step of applying a constant current and terminating; and a resting step of about 10 minutes was carried out for 500 hours.
[0152] Referring to FIG. 8, the symmetric cell according to Example 1 showed a result with a lower and more constant voltage amplitude compared to Comparative Examples 1 and 2. Through this, it was confirmed that excellent interfacial stability between the cathode and the electrolyte is achieved by coating the surface of the lithium metal with a protective film containing the composite of Synthetic Example 1.
[0153] Figure 9 shows a current density of 0.1 mA / cm² 2 , 0.5 mA / cm 2 , 1 mA / cm 2 , 2 mA / cm 2 , or 5 mA / cm 2 When adjusted to, This is a graph showing the cycle performance of a symmetric cell including a cathode according to Comparative Example 1, Comparative Example 2, and Example 1.
[0154] Referring to FIG. 9, the symmetric cell according to Example 1 exhibited the effect of maintaining superior electrochemical performance compared to Comparative Examples 1 and 2 under high current density conditions. This is because the ion conductivity is increased by coating the surface of the lithium metal with a protective film containing the composite of Synthetic Example 1.
[0156] [Experimental Example 6: SEM image of the cathode surface of the symmetric cell after 100 cycles]
[0157] FIG. 10 is a scanning electron microscope image of the surface of the cathode of the symmetric cell according to Comparative Example 1 and Example 1 after 100 cycles.
[0158] Referring to FIG. 10, the cathode of the symmetric cell according to Example 1 exhibited the effect of maintaining a very slippery and dense surface, unlike Comparative Example 1. On the other hand, in Comparative Example 1, dendrites were formed on the surface of the cathode, and it was confirmed that the performance and lifespan of the electrochemical device were degraded.
[0160] [Experimental Example 7: Electrochemical Performance of NCM 811-Containing Cell]
[0161] FIG. 11 is a charge / discharge graph of a cell according to Comparative Example 1, Comparative Example 2 and Example 1. Specifically, the cell comprises NCM811 (anode) / polyethylene separator / cathode according to Comparative Example 1, Comparative Example 2 and Example 1; and an electrolyte (about 85 μl) in which 1M LiPF6 is dissolved in a mixed solvent in which EC and DEC are mixed in a volume ratio of 1:1.
[0162] At 28 ℃, constant current charging was performed on the cell at a rate of approximately 0.1 C-rate during the first and second cycles, and then constant voltage charging was performed while maintaining a constant voltage of 4.2 V until the cutoff current reached 4.2 V. After a rest period of 10 minutes, constant current discharge was performed at a rate of 0.1 C-rate until the voltage reached 3.0 V. Subsequently, charging and discharging were performed from the 3rd to the 50th cycles by changing the rate to 0.5 C-rate.
[0163] FIG. 12 is a graph showing the discharge capacity and Coulomb efficiency according to the number of cycles of the cell according to Comparative Example 1, Comparative Example 2 and Example 1.
[0164] Meanwhile, Table 1 below shows the values calculated based on the first cycle of the initial formation process.
[0165] Sample Loading amount (mg cm²) -2 ) Capacity (mAh) Discharge capacity (mAh g) -1 ) Coulomb efficiency (%) Comparative Example 1 (Bare) 7.05 3.94 184.12 88.55 Comparative Example 2 (LLZTO / Li) 7.03 3.93 189.00 88.84 Example 1 (LLZTO@PAcS) 7.02 3.93 193.75 89.14
[0166] Referring to Figures 11 and 12, the cell according to Example 1 showed a higher discharge capacity and Coulomb efficiency compared to Comparative Examples 1 and 2.
[0168] [Experimental Example 8: Electrochemical Performance of Lithium-Sulfur Battery]
[0169] FIG. 13 is a charge / discharge graph of a cell according to Comparative Example 1 and Example 1. Specifically, the cell comprises a sulfur anode / polyethylene separator / cathode according to Comparative Example 1 and Example 1; and an electrolyte (approx. 66.7 μL) in which 1 M LiTFSI and 0.2 M LiNO3 are dissolved in a mixed solvent in which DOL and DME are mixed in a volume ratio of 1:1. During the first and second cycles at 28°C, constant current charging was performed on the cell at a rate of approximately 0.1 C-rate until the cut-off voltage reached 2.6 V. After a rest period of 10 minutes, constant current discharge was performed at a rate of 0.1 C-rate until the voltage reached 1.8 V. Subsequently, from the 3rd to the 200th cycle, charge / discharge was performed by changing the rate to 0.5 C-rate.
[0170] Figure 14 is a graph showing the discharge capacity and Coulomb efficiency according to the number of cycles of the cell according to Comparative Example 1 and Example 1.
[0171] Meanwhile, Table 2 below shows the values calculated based on the first cycle in the initial formation process.
[0172] Sample Loading amount (mg cm²) -2 ) Capacity (mAh) E / S ratio(μL mg -1 ) Discharge capacity (mAh g) -1 ) Coulomb efficiency (%) Discharge capacity after 200 cycles (mAh g) -1 ) Comparative Example 1 (Bare) 2.16 4.00 20 1119.17 98.82 411.93 Example 1 (LLZTO@PAcS) 2.16 4.00 20 1112.85 97.23 664.5
[0173] Referring to Table 2 above, Example 1 showed a discharge capacity and Coulomb efficiency equivalent to Comparative Example 1, while showing the effect of increasing the discharge capacity after 200 cycles.
[0174] The features described in the above-described embodiment may be combined with other embodiments unless explicitly stated otherwise. Furthermore, although preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the following claims also fall within the scope of the present invention.
Claims
Claim 1 A complex comprising: garnet-type oxide particles; and a coating layer on the garnet-type oxide particles; wherein the coating layer comprises: a copolymer formed by copolymerizing a monomer containing a carboxyl group and a zwitterion monomer. Claim 2 In claim 1, the garnet-type oxide particles comprise a complex comprising a compound represented by the following chemical formula 1: [Chemical Formula 1]Li a La3M2O 12 In the above chemical formula 1: a is a real number between 6 and 8, and M is one or more selected from the group consisting of Zr, Hf, Ta, Nb, Sn, Sc, and Y. Claim 3 In claim 1, the amphoteric ionic monomer comprises: at least one of the compounds represented by the following general formulas 1 and 2, a complex: [General Formula 1] [General Formula 2] In the above general formulas 1 and 2: R1 is each independently a hydrogen atom; or an alkyl group having 1 to 3 carbon atoms, L1 is each independently an ester group (-COO-), an amide group (-CONH-), or a phenylene group, and R a and R b One of them is a positively charged atomic group and the other is a negatively charged atomic group, and in the above general formula 1: R2 and R3 are each independently directly bonded; or are alkylene groups with 1 to 5 carbon atoms. Claim 4 In paragraph 3, the positively charged atomic group comprises: ammonium ions, sulfur ions, or phosphorus cations, and the negatively charged atomic group comprises: carboxylates, SO3 -, or PO4 - A complex containing Claim 5 In paragraph 3, the amphoteric ionic monomer comprises a compound represented by General Formula 1, wherein in General Formula 1: L1 is an ester group (-COO-), R2 and R3 are each independently an alkylene group having 1 to 5 carbon atoms, and R a is -N + (R a1 )2- and, here R a1 Each is independently an alkyl group having 1 to 3 carbon atoms, and R b -SO3 - Phosphorus complex. Claim 6 A cathode comprising lithium metal (Li metal) and a protective film on at least one surface of the lithium metal; wherein the protective film comprises a composite according to claim 1. Claim 7 In claim 6, the protective film further comprises a binder, and the content of the binder is 1 part by weight or more and 30 parts by weight or less per 100 parts by weight of the composite, a cathode. Claim 8 An electrochemical device comprising a cathode according to claim 6; an anode; and an electrolyte. Claim 9 In claim 8, the anode comprises: a lithium transition metal oxide; or an electrochemical element comprising sulfur. Claim 10 In claim 8, an electrochemical device further comprising a separator. Claim 11 An electric vehicle comprising the electrochemical element of claim 10.
Citation Information
Patent Citations
Mechanical response elastic binder based on supramolecular zwitterionic network toughening, and preparation method and application thereof
CN120865812A
Lithium secondary battery cell structure
KR1020140084519A