Cathode active materials, preparing method thereof, cathode and electrochemical devices comprising the same

The positive electrode active material comprising an overlithiated layered oxide with a coating layer enhances the stability and efficiency of lithium ion diffusion, thereby improving the stability and efficiency of lithium-ion batteries, particularly under high voltage conditions, and extending the lifespan of lithium-ion batteries.

KR103047858B1Active Publication Date: 2026-11-11KOREA RES INST OF CHEM TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020250051010
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-04-18
Publication Date
2026-11-11
Estimated Expiration
2045-04-18

AI Technical Summary

Technical Problem

Lithium cobalt composite oxides, such as LiCoO2, used in lithium-ion batteries, face limitations due to poor thermal stability and high cost, making them unsuitable for widespread use in applications like electric vehicles, and require improvements in stability and efficiency under high voltage conditions.

Method used

A positive electrode active material comprising an overlithiated layered oxide with a coating layer, where the cobalt content is higher in a specific region, is manufactured through a process involving a mixture of lithium-overlayered oxide and cobalt precursor, followed by calcination, to enhance stability and efficiency.

Benefits of technology

The solution provides a positive electrode active material that improves stability under high voltage, increases capacity and charge/discharge efficiency, and enhances lithium ion diffusion, thereby improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025044368679-PAT00011_ABST
    Figure 112025044368679-PAT00011_ABST
Patent Text Reader

Abstract

A positive electrode active material for improving the performance of an electrochemical device is disclosed. According to one aspect, a positive electrode active material is provided comprising: an overlithiated layered oxide (OLO); and a coating layer on the overlithiated layered oxide; wherein the positive electrode active material comprises, with respect to the center of the positive electrode active material, a first region in which the ratio of the radius to the total radius is greater than 0 and less than or equal to 1 / 2, and a second region in which the ratio of the radius to the total radius is greater than 1 / 2 and less than or equal to 2 / 2, and wherein the content of cobalt in the second region is higher than the content of cobalt in the first region.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a positive electrode active material, and more specifically, to a positive electrode active material, a method for manufacturing the same, a positive electrode, and an electrochemical device including the same. Background Technology

[0002] With the increasing technological development and demand for mobile devices, the demand for rechargeable batteries as an energy source is rapidly rising. Among these rechargeable batteries, lithium-ion batteries, which possess high energy density and voltage, long cycle life, and low self-discharge rates, have been commercialized and are widely used.

[0003] Lithium transition metal composite oxides are used as cathode active materials for lithium-ion batteries. Among these, lithium cobalt composite metal oxides, such as LiCoO2, which exhibit high operating voltage and excellent capacity characteristics, are primarily used. However, LiCoO2 has limitations in mass use as a power source in fields such as electric vehicles because its thermal properties are very poor due to the instability of its crystal structure caused by lithium ion desorption, and it is also expensive. Prior art literature

[0004] Korean Patent Publication No. 10-1794097 (Published Nov. 06, 2017) The problem to be solved

[0005] According to one aspect of the present invention, a positive electrode active material with improved stability under high voltage conditions is provided.

[0006] According to another aspect of the present invention, a positive electrode active material is provided that has high capacity and high charge / discharge efficiency even under high rate conditions.

[0007] According to another aspect of the present invention, a positive electrode active material is provided that increases the lithium ion diffusion coefficient and extends the lifespan of an electrochemical device.

[0008] According to another aspect of the present invention, a method for manufacturing the positive electrode active material is provided.

[0009] According to another aspect of the present invention, a positive electrode comprising the positive electrode active material is provided.

[0010] According to another aspect of the present invention, an electrochemical device comprising the anode is provided.

[0011] The objects of the present invention are not limited to those mentioned above, and other unmentioned objects and advantages of the present invention may be understood from the following description and will be more clearly understood by the embodiments of the present invention. Furthermore, it will be readily apparent that the objects and advantages of the present invention can be realized by the means and combinations thereof described in the specification. means of solving the problem

[0012] To solve the above problem, the present invention provides a positive electrode active material comprising: an overlithiated layered oxide (OLO); and a coating layer on the overlithiated layered oxide; wherein the positive electrode active material comprises, based on the center of the positive electrode active material: a first region in which the ratio of the radius to the total radius is greater than 0 and less than or equal to 1 / 2; and a second region in which the ratio of the radius to the total radius is greater than 1 / 2 and less than or equal to 2 / 2, and the content of cobalt in the second region is higher than the content of cobalt in the first region.

[0013] In one embodiment of the present invention, the overlithium layered oxide may include a compound represented by the following general formula 1.

[0014] [General Formula 1]

[0015] xLi2MnO 3 · (1-x)Li[Mn a M1 b M2 c ]O2

[0016] In the above general formula 1:

[0017] 0 <x<1이고 a+b+c=1이고, 0<a<1, 0≤b<1 및 0≤c<1이고, M1 및 M2는 서로 상이한 전이금속으로서 Ni 또는 Co이다.

[0018] In one embodiment of the present invention, the overlithium layered oxide may include a compound represented by the following general formula 2.

[0019] [General Formula 2]

[0020] y[LiMn p Ni (1-p-q-r) Co q M3 r O2]·(1-y)[Li2Mn s M4 (1-s) O3]

[0021] In the above general formula 2:

[0022] M3 and M4 are each independently selected from the group consisting of Zr, Al, Re, V, Cr, Fe, Ga, Si, B, Ru, Ti, Nb, Mo, Mg, W, Na and Pt, and

[0023] 0.500 <y<0.800, 0.450<p<0.650, 0≤q≤0.025, 0≤r≤0.100, 0.900≤s≤1.000이다.

[0024] In one embodiment of the present invention, the content of cobalt in the coating layer may be higher than the content of cobalt in the overlithium layered oxide.

[0025] In one embodiment of the present invention, the coating layer may include LiCoO2.

[0026] In one embodiment of the present invention, the average particle size (D) of the positive electrode active material 50 ) can be 6 µm or more and 12 µm.

[0027] In one embodiment of the present invention, the average thickness of the coating layer may be 500 nm or more and 2,000 nm or less.

[0028] In one embodiment of the present invention, the grain size of the positive active material may be 40 nm or more and 70 nm or less.

[0029] The present invention provides a method for manufacturing an anode active material, comprising: (S1) a step of preparing a mixture comprising a lithium-overlayered oxide precursor and a cobalt precursor; and (S2) a step of calcining the mixture to manufacture the anode active material of claim 1.

[0030] In one embodiment of the present invention, the content of the cobalt precursor may be 0.5 parts by weight or more and 10 parts by weight or less per 100 parts by weight of the lithium-overlayered oxide precursor.

[0031] In one embodiment of the present invention, the step (S2) may include a step of sintering at 550°C or higher and 950°C or lower for 2 hours or more and 15 hours.

[0032] The present invention provides a positive electrode comprising the above positive electrode active material.

[0033] The present invention provides a positive electrode active material manufactured according to a method for manufacturing a positive electrode active material.

[0034] The present invention provides an electrochemical device comprising: the anode; the cathode; the separator interposed between the anode and the cathode; and the electrolyte.

[0035] The present invention provides an electric vehicle comprising the electrochemical element.

[0036] The means for solving the above problem are not all of the features of the present invention and may be combined with some embodiments of this specification. Various features of the present invention and the advantages and effects derived therefrom may be understood in more detail by referring to the specific description below. Effects of the invention

[0037] According to one aspect of the present invention, it is possible to realize a positive electrode active material that improves the stability of an electrochemical device under high voltage conditions and increases capacity and charge / discharge efficiency even under high rate conditions.

[0038] According to another aspect of the present invention, a positive electrode active material can be provided to realize an electrochemical device with an increased lithium ion diffusion coefficient and an extended lifespan.

[0039] In addition to the effects described above, specific effects of the present invention are described together with the following explanation of specific details for implementing the invention. Furthermore, the effects of the present invention are not limited to those mentioned above and can be easily realized by means and combinations thereof described in the specification. Brief explanation of the drawing

[0040] FIG. 1 is a schematic diagram of a positive electrode active material according to one embodiment of the present invention. FIG. 2 is a schematic diagram showing a method for manufacturing a positive electrode active material according to one embodiment of the present invention. Figure 3a is a scanning electron microscope (SEM) image of a positive electrode active material according to a comparative example. Figure 3b is a scanning electron microscope image showing the process of a Mn-rich precursor according to a comparative example being converted into a positive electrode active material by calcination. Figure 4a is a scanning electron microscope image of the positive electrode active material according to Example 1. Figure 4b is a scanning electron microscope image showing the process of converting an Mn-rich precursor according to Example 1 into a positive electrode active material by calcination. FIG. 5a is a graph showing the elemental content according to distance in the cross-section of the positive electrode active material according to Example 1. FIG. 5b is a graph showing the elemental content according to point number in the cross-section of the positive electrode active material according to Example 1. FIG. 5c is a graph showing the cobalt content according to distance in the cross-section of the positive electrode active material according to Example 1. Figure 6 shows the capacity retention rate according to the number of cycles of a half-cell containing a positive active material according to the comparative example and Examples 1 to 3. FIG. 7 shows the lithium ion diffusion coefficient (D) according to the charging voltage of the half-cells according to the comparative example and Examples 1 to 3. GITT This is a graph representing ). FIG. 8 is a graph showing the capacity according to the C-rate according to the number of cycles of half-cells according to the comparative example and Examples 1 to 4. FIG. 9 is a graph showing the charge / discharge profiles of half-cells according to the comparative example and Examples 1 to 4. Specific details for implementing the invention

[0041] In this specification, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0042] In this specification, the terms “comprise” and / or “comprising” specify the presence of the mentioned features, steps, numbers, actions, parts, elements, and / or groups thereof, and do not exclude the presence or addition of one or more other features, steps, numbers, actions, parts, elements, and / or groups thereof.

[0043] In this specification, expressions such as "first," "second," "first," "second," "(S1)," "(S2)," etc. may modify various components regardless of order and / or importance, and do not limit such components. These expressions may be used to distinguish one component from another. For example, without departing from the scope of the present disclosure, the first component may be named the second component, and similarly, the second component may be renamed the first component.

[0044] In this specification, "at least one of a, b and c" is defined as one or more selected from the group consisting of a, b and c.

[0045] Where various embodiments are described in this specification, each embodiment may be combined unless specifically stated otherwise. In this case, the effects of the present invention may be defined as including effects derived from each embodiment and effects resulting from the organic combination of each embodiment. For example, even if embodiments 1 and 2 are described independently in this specification, unless the context clearly indicates otherwise, embodiments 1 and 2 may be organically combined with each other, and the effects of the present invention may include effects resulting from the combination of embodiments 1 and 2.

[0046] In this specification, a range of numerical values ​​indicated by the term 'to' represents a range of numerical values ​​that includes the values ​​listed before and after the term as the lower and upper limits, respectively. For example, if 'a to b' is described in the specification, it may be understood that 'a to b' (a to b) is described.

[0047] In the present specification, if multiple numerical values ​​are disclosed for the upper and lower limits of any numerical range, the numerical range disclosed in the present specification may be understood as a range of any numerical values ​​in which any one of the multiple lower limit values ​​and any one of the multiple upper limit values ​​are respectively the lower limit value and the upper limit value. For example, if a or greater, or b or greater; and c or less, or d or less is described, it may be understood as a or greater and c or less, a or greater and d or less, b or greater and c or less, or b or greater and d or less.

[0048] In this specification, terms such as “about” or “substantially” refer to a reasonable amount of variation of a term modified so as not to significantly alter the final result. Such terms may be interpreted to include a variation of at least ±5% or at least ±10% to the extent that the variation does not alter or invalidate the meaning of the word.

[0049] In this specification, the cobalt (Co) content by region can be measured using SEM-EDS (Scanning Electron Microscopy-Energy Dispersive X-ray Spectroscopy).

[0050] According to one aspect of the present invention, an anode active material is provided comprising an overlithiated layered oxide (OLO); and a coating layer on the overlithiated layered oxide, wherein the anode active material comprises, with respect to the center of the anode active material, a first region in which the ratio of the radius to the total radius is greater than 0 and less than or equal to 1 / 2, and a second region in which the ratio of the radius to the total radius is greater than 1 / 2 and less than or equal to 2 / 2, and the content of cobalt in the second region is higher than the content of cobalt in the first region.

[0051] According to one aspect of the present invention, by controlling the cobalt content in the second region to be higher than the cobalt content in the first region, it is possible to provide a positive electrode active material that improves the stability of the electrochemical device under high voltage conditions, increases the capacity and charge / discharge efficiency even under high rate conditions, increases the lithium ion diffusion coefficient, and extends the lifespan of the electrochemical device.

[0053] Hereinafter, the configuration of the present invention will be described in more detail with reference to the drawings.

[0055] 1. Cathode active material

[0056] FIG. 1 is a schematic diagram of a positive electrode active material according to one embodiment of the present invention.

[0057] The positive active material (100) according to the present invention includes an overlithiated layered oxide (OLO) (10).

[0058] In this specification, the overlithium layered oxide (10) is defined as a compound in which the molar ratio of lithium to the total transition metal (Li / Metal molar ratio) is greater than 1. For example, the overlithium layered oxide may include one or more phases.

[0059] In some embodiments of the present invention, the overlithium layered oxide may include a compound represented by the following general formula 1.

[0060] [General Formula 1]

[0061] xLi2MnO 3 · (1-x)Li[Mn a M1 b M2 c ]O2

[0062] In the above general formula 1, 0 <x<1이고 a+b+c=1이고, 0<a<1, 0≤b<1 및 0≤c<1이고, M1 및 M2는 서로 상이한 전이금속으로서 Ni 또는 Co이다. 상기 일반식 1로 표시되는 화합물에서 x는 두 상(Phase)의 혼합비율을 결정할 수 있다. 상기 일반식 1로 표시되는 화합물은 도핑이 되지 않은 과리튬 층상계 산화물로서 리튬 과잉 상태를 나타내는 xLi2MnO3를 통해 발현 용량을 높이는 효과와, (1-x)Li[Mn a M1 b M2 c Through O2, the effect of improving the structural stability and thermal stability of the cathode active material can be achieved simultaneously.

[0063] In some other embodiments of the present invention, the overlithium layered oxide may include a compound represented by the following general formula 2.

[0064] [General Formula 2]

[0065] y[LiMn p Ni (1-p-q-r) Co q M3 r O2]·(1-y)[Li2Mn s M4 (1-s) O3]

[0066] In the above general formula 2, M3 and M4 are each independently selected from the group consisting of Zr, Al, Re, V, Cr, Fe, Ga, Si, B, Ru, Ti, Nb, Mo, Mg, W, Na, and Pt, and 0.500 <y<0.800, 0.450<p<0.650, 0≤q≤0.025, 0≤r≤0.100, 0.900≤s≤1.000이다. 구체적으로 상기 일반식 2로 표시되는 화합물에서 y는 두 상(Phase)의 혼합 비율을 결정할 수 있다. 상기 일반식 2로 표시되는 화합물은 상기 일반식 1의 화합물과 달리, M3 및 M4로 도핑된 과리튬 층상계 산화물일 수 있다. 구체적으로 상기 일반식 2로 표시되는 화합물은 M3 및 M4로 도핑되기 때문에 리튬 과량 구조의 안정성을 강화하고 장시간 사이클 성능을 향상시킬 수 있다.

[0067] In this specification, a “layer” or “film” may include cases where, when observing the region in which the layer or film exists, it is formed over the entire region, or cases where it is formed only in a part of the region. For example, the surface of the layer or film may be defined as having a flat shape, a non-flat shape, and combinations thereof; or a continuous shape, a discontinuous shape, and combinations thereof. For example, when another member is composed of a layer or film directly on a member, the coverage of the other member on the surface of the member may be defined as 1% or more, 5% or more, 10% or more, 20% or more, 30% or more, 40% or more, 50% or more, 60% or more, 70% or more, 80% or more, 85% or more, 90% or more, 95% or more, or 99% or more. For example, it may also be defined as a “layer” or “film” when a plurality of particles form a clustered structure.

[0068] The positive electrode active material (100) according to the present invention comprises a coating layer (20) on the over-lithium layered oxide (10). Specifically, the coating layer (20) may be coated on some or all of the surface of the over-lithium layered oxide (10). In some embodiments of the present invention, by forming the coating layer on the over-lithium layered oxide, the stability of the electrochemical device under high voltage conditions is improved, and the capacity and charge / discharge efficiency are increased even under high rate conditions, and the lithium ion diffusion coefficient is increased and the lifespan of the electrochemical device is extended, thereby providing a positive electrode active material that realizes an electrochemical device.

[0069] In some embodiments of the present invention, the positive electrode active material comprises, based on the center of the positive electrode active material, a first region in which the ratio of the radius to the total radius is greater than 0 and less than or equal to 1 / 2, and a second region in which the ratio of the radius to the total radius is greater than 1 / 2 and less than or equal to 2 / 2, wherein the content of cobalt in the second region may be higher than the content of cobalt in the first region. In some embodiments of the present invention, by controlling the content of cobalt in the second region to be higher than the content of cobalt in the first region, the stability of the electrochemical device under high voltage conditions is improved, and even under high rate conditions, the capacity is high and the charge / discharge efficiency is increased, and the lithium ion diffusion coefficient is increased and the lifespan of the electrochemical device is extended, thereby providing a positive electrode active material that realizes an electrochemical device.

[0070] In some non-limiting examples, the total radius relative to the center of the positive active material may be about 2 µm or more, 3 µm or more, or 4 µm or more, or 5 µm or less, 6 µm or less, or 7 µm or less, and specifically may be 4 µm or more and 6 µm or less. For example, the total radius relative to the center of the positive active material may be the average value of any 50 values ​​for the total radius of the positive active material.

[0071] In some embodiments of the present invention, the content of cobalt in the coating layer (20) may be higher than the content of cobalt in the over-lithium layered oxide (10). In some embodiments of the present invention, by controlling the content of cobalt in the coating layer (20) to be higher than the content of cobalt in the over-lithium layered oxide (10), the stability of the electrochemical device under high voltage conditions is improved, and even under high rate conditions, the capacity is high and the charge / discharge efficiency is increased, and the lithium ion diffusion coefficient is increased and the lifespan of the electrochemical device is extended, thereby providing a positive electrode active material that realizes an electrochemical device.

[0072] In some embodiments of the present invention, the coating layer (20) may include LiCoO2. For example, the coating layer may be formed by calcining a mixture comprising the cobalt precursor and the above-described over-lithium layered oxide precursor. In some embodiments of the present invention, by including LiCoO2 in the coating layer, the electrochemical device may be provided with a positive electrode active material that improves the stability of the electrochemical device under high voltage conditions, increases capacity and charge / discharge efficiency even under high rate conditions, increases the lithium ion diffusion coefficient, and extends the lifespan of the electrochemical device.

[0073] In some embodiments of the present invention, the average thickness of the coating layer (20) may be 500 nm or more and 2,000 nm or less. Specifically, by controlling the average thickness of the coating layer (20) to the above numerical range, the stability of the electrochemical device under high voltage conditions is improved, and even under high rate conditions, the capacity is high and the charge / discharge efficiency is increased, and the lithium ion diffusion coefficient is increased and the lifespan of the electrochemical device is extended, thereby providing a positive electrode active material that realizes an electrochemical device.

[0074] In this specification, the average particle size of a particle is the particle size (D) at which the cumulative percentage in the volume-based particle size distribution curve reaches 50% when measured by a laser diffraction particle size distribution measuring device. 50 It can be defined as ). For example, the average particle size of the above particles can be calculated by dispersing the particles to be measured in a dispersion medium, introducing them into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and measuring the difference in diffraction patterns according to particle size as the particles pass through a laser beam.

[0075] In some embodiments of the present invention, the average particle size (D) of the positive electrode active material 50 ) may be 6 μm or more and 12 μm or less. Specifically, the average particle size (D) of the positive electrode active material. 50) may be 6 μm or more, 7 μm or more, or 8 μm or more; and 9 μm or less, 10 μm or less, 11 μm or less, or 12 μm or less. In some embodiments of the present invention, the lifespan and thermal stability of the electrochemical device may be further improved by controlling the average particle size of the positive electrode active material to the above numerical range.

[0076] In some embodiments of the present invention, the grain size of the positive electrode active material may be 40 nm or more and 70 nm or less. Specifically, the grain size of the positive electrode active material may be 46 nm or more, 50 nm or more, 56 nm or more, or 60 nm or more, or 47 nm or less, 58 nm or less, 62 nm or less, 65 nm or less, or 70 nm or less. For example, the grain size of the positive electrode active material may be calculated using X-ray diffraction (XRD) analysis and the Scherrer equation.

[0078] 2. Method for manufacturing positive electrode active material

[0079] FIG. 2 is a schematic diagram showing a method for manufacturing a positive electrode active material according to one embodiment of the present invention.

[0080] Referring to FIG. 2, according to another aspect of the present invention, a method for manufacturing a positive electrode active material is provided, comprising the steps of: (S1) preparing a mixture comprising a lithium-overlayered oxide precursor and a cobalt precursor; and (S2) calcining the mixture to produce a positive electrode active material of some embodiment. According to another aspect of the present invention, by calcining a mixture comprising a lithium-overlayered oxide precursor and a cobalt precursor, a positive electrode active material can be provided that enables an electrochemical device with improved stability under high voltage conditions, high capacity and increased charge / discharge efficiency even under high rate conditions, increased lithium ion diffusion coefficient, and extended lifespan of the electrochemical device.

[0081] In this specification, a precursor is defined as a compound that participates in a chemical reaction to produce another compound in chemistry.

[0082] The lithium-overlayered oxide precursor according to the present invention is defined as a precursor of a lithium-overlayered oxide. In some non-limiting examples, the lithium-overlayered oxide precursor is (Ni 0.35 Mn 0.65 )(OH)2 can be.

[0083] The cobalt precursor according to the present invention may be a raw material for forming a coating layer on the surface of a calcined overlithium layered oxide. In some non-limiting examples, the cobalt precursor may include cobalt hydroxide, and more specifically, may include Co(OH)2.

[0084] In some embodiments of the present invention, the content of the cobalt precursor may be 0.5 parts by weight or more and 10 parts by weight or less per 100 parts by weight of the overlithium layered oxide precursor. Specifically, the content of the cobalt precursor may be 0.5 parts by weight or more, 1.0 parts by weight or more, 2.0 parts by weight or more, 2.5 parts by weight or more, 3.0 parts by weight or more, 4 parts by weight or more, 5 parts by weight or more, 6 parts by weight or more, 7 parts by weight or more, 8 parts by weight or more, or 9 parts by weight or more per 100 parts by weight of the overlithium layered oxide precursor, or 1.0 parts by weight or less, 2.0 parts by weight or less, 2.5 parts by weight or less, 3.0 parts by weight or less, 4 parts by weight or less, 5 parts by weight or less, 6 parts by weight or less, 7 parts by weight or less, 8 parts by weight or less, 9 parts by weight or less, or 10 parts by weight or less. In some embodiments of the present invention, by controlling the content of the cobalt precursor to the above numerical range, a positive electrode active material can be provided that enables an electrochemical device having high capacity and increased charge / discharge efficiency even under high rate conditions, increased lithium ion diffusion coefficient, and extended lifespan of the electrochemical device.

[0085] In some embodiments of the present invention, the step (S2) may include a step of sintering at a temperature of 550°C or higher and 950°C or lower for 2 hours or more and 15 hours or less. Specifically, by controlling the sintering temperature and sintering time of the step (S2) to the above numerical range, the crystal structure and particle size of the anode active material can be controlled to an appropriate level, thereby further improving electrochemical performance.

[0086] In some embodiments of the present invention, the step (S2) may include: a step of primary sintering at a temperature of 550°C or higher and 650°C or lower for 3 hours or more and 5 hours or less; and a step of secondary sintering at a temperature of 800°C or higher and 950°C or lower for 10 hours or more and 14 hours or less by increasing the temperature of the primary sintered product at a rate of 1°C / min to 3°C / min. In some embodiments of the present invention, by controlling the sintering temperature and sintering time of the step (S2) to the above numerical range, the crystal structure and particle size of the anode active material can be controlled to an appropriate level, thereby further improving electrochemical performance.

[0088] 3. Anode

[0089] According to another aspect of the present invention, a positive electrode comprising a positive electrode active material of several embodiments is provided.

[0090] The anode according to the present invention may include an anode current collector and an anode active material layer disposed on at least one surface of the anode current collector. The anode active material layer may include an anode active material, a conductive material, and an anode binder.

[0091] For example, the positive current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. Specifically, the positive current collector may be copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy. The positive current collector may typically have a thickness of 6 to 20 μm.

[0092] The conductive material can improve conductivity between active material particles or with a metal current collector at the electrode and prevent the binder from acting as an insulator. The conductive material may be, for example, a mixture of one or more conductive materials selected from the group consisting of graphite, carbon black, carbon fiber, metal fiber, metal powder, conductive whiskers, conductive metal oxide, activated carbon, and polyphenylene derivatives; more specifically, it may be a mixture of one or more conductive materials selected from the group consisting of natural graphite, artificial graphite, Super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermo black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide.

[0093] For example, the anode binder is poly(vinylidene fluoride-hexafluoropropylene(poly(vinylidene fluoride) co -hexafluoropropylene)), polyvinylidene fluoride-trichloroethylene(poly(vinylidene fluoride- co-trichloroethylene)), poly(methylmethacrylate)), poly(ethylhexylacrylate)), poly(butylacrylate)), poly(acrylonitrile)), poly(vinylpyrrolidone)), poly(vinyl acetate)), poly(ethylene-co-vinyl acetate)), poly(ethylene oxide)), polyacrylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl poly(vinylalcohol)), cyanoethylcellulose, It may be one or more selected from the group consisting of cyano ethylsucrose, pullulan, and carboxyl methyl cellulose, but is not limited thereto.

[0095] 4. Electrochemical devices

[0096] In this specification, the term "electrochemical device" is defined as any device that performs an electrochemical reaction. For example, the electrochemical device may be a secondary battery or a supercapacitor, and specifically may be a lithium metal battery or a lithium-ion secondary battery.

[0097] cathode

[0098] The cathode according to the present invention may comprise a cathode current collector and a cathode active material layer disposed on at least one surface of the cathode current collector, or may be lithium metal (Li metal).

[0099] For example, the cathode active material layer may include the cathode active material, the conductive material, and the cathode binder.

[0100] The above-mentioned negative current collector can serve as a channel to transfer electrons from the outside to cause an electrochemical reaction to occur in the negative active material, or to receive electrons from the negative active material and send them to the outside. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., may be used as the negative current collector, and specifically, transition metals that adsorb carbon well, such as copper and nickel, may be used as the current collector. For example, the thickness of the above-mentioned negative current collector may be 6㎛ to 20㎛, but the thickness of the above-mentioned negative current collector is not limited thereto.

[0101] The conductive material included in the above cathode may be the same as or different from the conductive material included in the above anode.

[0102] If necessary, the cathode active material layer may further include an additive. The additive may be, for example, at least one selected from the group consisting of dispersants, plasticizers, antioxidants, lubricants, stabilizers, and antistatic agents.

[0103] Separator

[0104] The separator according to the present invention includes a porous substrate to electrically insulate the cathode and the anode to prevent a short circuit.

[0105] As long as the constituent material of the above porous substrate is an organic or inorganic material having electrical insulating properties, it may be used without particular limitation. The above porous substrate may include, for example, at least one selected from the group consisting of polyolefin, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalene, and specifically may include polyolefin. Polyolefin not only has excellent coating properties but also allows for a thinner separator thickness, thereby increasing the proportion of the electrode active material layer within the battery and increasing the capacity per volume. Specifically, the weight-average molecular weight (M) of the above polyolefin w The weight-average molecular weight of the polyolefin may be 100,000 to 500,000 g / mol. If the weight-average molecular weight of the polyolefin is below the above numerical range, it may be difficult to secure sufficient mechanical properties, and if it exceeds the above numerical range, the shutdown function may not be implemented or molding may be difficult. The shutdown function refers to a function in which, when the temperature of the secondary battery rises, the thermoplastic resin melts to close the pores of the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery.

[0106] The thickness of the porous substrate may be, for example, 3 to 12 μm or 5 to 12 μm. If the thickness of the porous substrate is less than the numerical range, the function of the conductive barrier may not be sufficient, and if it exceeds the numerical range, the resistance of the separator may increase excessively.

[0107] The average diameter of the pores included in the porous substrate may be, for example, 10 to 100 nm. The pores included in the porous substrate have a structure in which they are interconnected, so that gas or liquid can pass from one side of the porous substrate to another side.

[0108] According to some embodiments of the present invention, a coating layer may be disposed on at least one surface of the porous substrate. Specifically, the coating layer can improve the mechanical strength and heat resistance of the separator and increase the ion conductivity in the secondary battery.

[0109] The coating layer according to the present invention may include a binder polymer and inorganic particles.

[0110] The binder polymer according to the present invention can connect inorganic particles and stably fix them. The above binder polymer is, for example, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, poly(ethylene-co-vinyl acetate), polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethylpullulan, One or more selected from the group consisting of cyanoethylpolyvinyl alcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxymethylcellulose, acrylonitrile-styrene butadiene copolymer, polyimide, and styrene-butadiene rubber may be used in combination.

[0111] According to another embodiment of the present invention, the weight ratio of the inorganic particles to the binder polymer (inorganic particles:binder polymer) may be 50:50 to 99:1, and specifically 70:30 to 95:5. If the content ratio of inorganic particles to the binder polymer is less than the above numerical range, the content of the binder polymer increases, which may reduce the performance of improving the thermal safety of the separator, and the pore size and porosity decrease due to the reduction of empty spaces formed between the inorganic particles, which may cause a decrease in the performance of the final battery, and if it exceeds the above numerical range, the content of the binder polymer is too low, which may weaken the peel resistance of the coating layer.

[0112] The inorganic particles according to the present invention can contribute to improving the mechanical strength and heat resistance of a separator for a secondary battery. Specifically, the inorganic particles are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in the present invention are applicable within the operating voltage range of the secondary battery (e.g., Li / Li). + It is not specifically limited as long as oxidation and / or reduction reactions do not occur at a standard of 0~5V.

[0113] As an example, when using inorganic particles with a high dielectric constant, the ionic conductivity of the electrolyte can be improved by contributing to an increase in the degree of dissociation of electrolyte salts, such as lithium salts, within the liquid electrolyte. For the reasons mentioned above, the inorganic particles may be inorganic particles having a dielectric constant of 5 or more, inorganic particles having lithium ion transport capability, or a mixture thereof.

[0114] The above inorganic particles having a dielectric constant of 5 or greater are Al2O3, SiO2, ZrO2, AlO(OH), Al(OH)3, Mg(OH)2, BaSO4, TiO2, BaTiO3, Pb(Zr x Ti 1-x )O3(PZT, where 0 < x < 1), Pb 1-x La x Zr 1-y Tiy O3(PLZT, where, 0 < x < 1, 0 < y < 1), (1-x)Pb(Mg 1 / 3 Nb 2 / 3 )O 3-x It may be one or more selected from the group consisting of PbTiO3 (PMN-PT, where 0 < x < 1), HfO2, SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO and SiC.

[0115] The inorganic particles having the above lithium ion transfer capability are lithium phosphate (Li3PO4) and lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y Series glass (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride(Li x N y , 0 < x < 4, 0 < y < 2), SiS2 series glass(Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4) and P2S5 series glass (Li x P y S z It may be one or more types selected from the group consisting of , 0 < x < 3, 0 < y < 3, 0 < z < 7).

[0116] For example, the average particle size (D) of the above inorganic particles 50 The particle size may be 1 nm to 10 µm for the formation of a coating layer of uniform thickness and appropriate porosity, specifically 10 nm to 2 µm, and more specifically 50 nm to 1 µm. The "average particle size (D50)" refers to the particle size at the 50% point of the cumulative distribution of the number of particles according to particle size. The average particle size can be measured using a laser diffraction method. Specifically, after dispersing the powder to be measured in a dispersion medium, the particle size distribution can be calculated by introducing it into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and measuring the difference in diffraction patterns according to particle size as the particles pass through the laser beam.

[0117] electrolytes

[0118] The electrolyte according to the present invention may include a solvent and a lithium salt.

[0119] The solvent according to the present invention is, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone, ethyl methyl carbonate (EMC), gamma-butyrolactone (GBL), fluoroethylene carbonate (FEC), methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, pentyl acetate, methyl propionate, ethyl propionate, It may be one or more mixtures selected from the group consisting of ethyl propionate and butyl propionate.

[0120] The lithium salt according to the present invention is, for example, NO3 - , F - , Cl - , Br - , I - , PF6 - It may include negative ions such as the back.

[0121] The secondary battery according to the present invention may be a cylindrical, prismatic, or pouch-type secondary battery, but is not particularly limited as long as it corresponds to a charge / discharge device.

[0122] According to another aspect of the present invention, a battery module comprising the electrochemical element as a unit cell and a battery pack comprising the same may be provided. The battery pack may be used as a power source for one or more medium-to-large devices selected from the group consisting of, for example, a power tool; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0123] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the present invention; however, this is merely an example, and the scope of the present invention is not limited by the following.

[0125] [Preparation Example 1: Preparation of Cathode Active Material]

[0126] <Comparison Example: LiCOO 2 Preparation of OLO cathode active material without a coating layer

[0127] Mn-rich precursor synthesis step:

[0128] Aqueous solutions of NiSO4 and MnSO4, each with a concentration of approximately 2.0 M, were mixed in a molar ratio of 35:65, respectively, and approximately 5.0 M aqueous NaOH solution and approximately 2.8 M aqueous NH4OH solution were added and continuously mixed in a co-precipitation apparatus. The obtained mixture was co-precipitated at pH 9.5–11.5 for a reaction time of 20 hours, a reaction temperature of 40–80℃, and a reaction rate of approximately 1000 rpm (Ni 0.35 Mn 0.65 A (OH)2 precursor was obtained. The precursor was washed with water, dried in a 120°C oven, and filtered. Then, the precursor and LiOH were mixed using a simple mixer to synthesize an Mn-rich precursor.

[0129] Firing stage:

[0130] The above Mn-rich precursor is placed in a calcination vessel and heated at a rate of 2°C / min to a temperature of 550-650°C for approximately 4 hours, and then heated at a rate of 2°C / min to a temperature of 800-950°C for approximately 12 hours to produce the cathode active material Li 1.130 Ni 0.305 Mn 0.565 O2 was manufactured.

[0131] <Examples 1 to 4: LiCOO 2 Preparation of OLO cathode active material with a formed coating layer

[0132] Synthesized by the same method as the comparative example (Ni 0.35 Mn 0.65 A Co source (Co(OH)2) with an amount as listed in Table 1 below was added to 100 parts by weight of (OH)2, and then calcined under the calcination conditions listed in Table 1 below to prepare an OLO cathode active material coated with a LiCoO2 layer.

[0133] division Sample name chemical formula Co source (parts by weight) Coating layer thickness Grain size (nm) firing conditions Comparative example OLO Li 1.130 Ni 0.305 Mr 0.565 O2 - - 200-400nm Stage 1: 550-650℃, 4hr; Stage 2: 800-950℃, 12hr(2℃ / min) Example 1 OLO-LCO_2 Li 1.130 Ni 0.301 Co 0.009 Mr 0.560 O2 1 part by weight 0.2㎛ Example 2 OLO-LCO_3 Li 1.130 Ni 0.297 Co 0.022 Mr 0.551 O2 2.5 parts by weight 0.5nm Example 3 OLO-LCO_4 Li 1.130 Ni 0.289 Co 0.044 Mr 0.537 O2 5.0 parts by weight 1㎛ Example 4 OLO-LCO_5 Li 1.130 Ni 0.274 Co 0.087 Mr 0.509 O2 10.0 parts by weight 2㎛

[0134] [Experimental Example 1: SEM images of precursor and cathode active material]

[0135] Figure 3a is a scanning electron microscope (SEM) image of a positive electrode active material according to a comparative example. Figure 3b is a scanning electron microscope image showing the process of a Mn-rich precursor according to a comparative example being converted into a positive electrode active material by calcination.

[0136] Figure 4a is a scanning electron microscope image of the positive electrode active material according to Example 1. Figure 4b is a scanning electron microscope image showing the process of converting an Mn-rich precursor according to Example 1 into a positive electrode active material by calcination.

[0137] Referring to FIGS. 3a to 4b, it was confirmed that a coating layer is formed on the surface of the positive active material according to Example 1. In addition, it was confirmed that the diameter of the positive active material according to Example 1 is approximately 8 μm.

[0139] [Experimental Example 2: Analysis of Elemental Content According to Distance]

[0140] For cross-sectional analysis, a positive active material specimen according to Example 1 was prepared. Assuming that the coating layer was uniformly coated, measurements were taken randomly from one end to the other end of the specimen so that the center passed through (diameter: approximately 8.5 μm). Here, the point number was 200, and each point was measured by evenly distributing the distance of 8.5 μm. Then, the elemental content from one end to the other end was measured using SEM-EDS (Scanning Electron Microscopy-Energy Dispersive X-ray Spectroscopy).

[0141] Figure 5a is a graph showing the elemental content according to distance in the cross-section of the positive electrode active material according to Example 1. Figure 5b is a graph showing the elemental content according to the point number in the cross-section of the positive electrode active material according to Example 1. Figure 5c is a graph showing the cobalt content according to distance in the cross-section of the positive electrode active material according to Example 1. Here, the y-axis of Figures 5a to 5c represents X-ray intensity. Relative elemental content was compared through a comparison of X-ray intensity.

[0142] Referring to Figures 5a to 5c, it was confirmed that the cobalt content increases from the center of the positive active material to the surface.

[0144] [Experimental Example 3: Evaluation of Dose Retention Rate According to Cycle Count]

[0145] Half-cell sample manufacturing:

[0146] A mixture comprising 96.5 wt% of each positive active material according to Preparation Example 1, 2 wt% of polyvinylidene fluoride, 1.0 wt% of carbon nanotubes, and 0.5 wt% of acetylene black was dispersed in N-methyl-2-pyrrolidone to prepare a positive slurry with a total solid content of 62.5 wt%. The positive slurry was coated onto an aluminum foil with a thickness of 15 μm, rolled, and dried to produce a positive electrode. A porous polyethylene separator was interposed between the positive electrode and the negative electrode (lithium metal, Li metal), and an electrolyte was injected to fabricate a coin-type half-cell. At this time, the electrolyte used was a mixed solution of ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) in a ratio of 2:4:4 (v / v), in which 1.0% vinylene carbonate (VC) and 1.15 M concentration of LiPF6 were dissolved.

[0148] evaluation:

[0149] FIG. 6 shows the capacity retention rate according to the number of cycles of half-cells containing positive electrode active materials according to the comparative example and Examples 1 to 3. Here, the capacity retention rate is the initial capacity (1 st It is the ratio of the current capacity (n-th cycle) to the cycle. Charging and discharging were performed at 25℃, charging was done at a rate of 0.5C to 2.0~4.75V, and discharging was done at a rate of 0.5C to 2.0~4.75V for 100 cycles.

[0150] Referring to FIG. 6, it was confirmed that the half-cells according to Examples 1 to 3, compared to the comparative example, achieve a high capacity retention rate even when the number of cycles increases.

[0152] [Experimental Example 4: Ion Diffusion Coefficient According to Voltage]

[0153] FIG. 7 shows the lithium ion diffusion coefficient (D) according to the charging voltage of the half-cells according to the comparative example and Examples 1 to 3. GITTThis is a graph showing ). Specifically, for the half-cells according to the above Comparative Example and Examples 1 to 3, the lithium-ion diffusion coefficient (D) according to the charging voltage was obtained using the Galvanostatic Intermittent Titration Technique (GITT). GITT ) was measured. At this time, the charging stage was set to constant current charging at 0.5C for 50 seconds, the first resting stage for about 50 seconds, the discharging stage for about 50 seconds at 0.5C, and the second resting stage for about 50 seconds.

[0154] Referring to FIG. 7, compared to the comparative example, the batteries according to Examples 1 and 2 have a higher lithium-ion diffusion coefficient, which kinetically exhibits an effect favorable for high-rate charging.

[0156] [Experimental Example 5: Measurement of Capacity by C-Rate According to Cycle Count]

[0157] FIG. 8 is a graph showing the capacity according to the C-rate according to the number of cycles of half-cells according to the comparative example and Examples 1 to 4. Specifically, to analyze the capacity, the C-rate was set to 0.1C, 0.2C, 0.5C, 1C, 2C, and 3C based on the constant current method, and the charging voltage was set to 4.75V and the discharging voltage to 2.0V.

[0158] Referring to FIG. 8, it was confirmed that under high rate conditions, the half-cells according to Examples 1 to 4, compared to the comparative example, exhibited an effect of significantly increasing the capacity of the cell even as the number of cycles increased.

[0160] [Experimental Example 6: Charge / Discharge Profile]

[0161] FIG. 9 is a graph showing the charge / discharge profiles of half-cells according to the comparative example and Examples 1 to 4. Charging and discharging were performed at 25°C; for charging, the voltage was charged at a rate of 0.5C to 2.0–4.75V, and for discharging, the voltage was discharged at a rate of 0.5C to 2.0–4.75V. In addition, the charge / discharge profiles were measured based on the first cycle.

[0162] Referring to FIG. 9, it was confirmed that the discharge capacity of the half-cells according to Examples 1 and 2 is higher than that of the comparative example. From this, it can be inferred that the electrochemical device can be used for a longer period with a single charge.

[0163] The features described in the above-described embodiment may be combined with other embodiments unless explicitly stated otherwise. Furthermore, although preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the following claims also fall within the scope of the present invention. Explanation of the symbols

[0164] 100: Positive electrode active material 10: Lithium-over-layered oxide 20: Coating layer

Claims

Claim 1 An anode active material comprising: an overlithiated layered oxide (OLO); and a coating layer on the overlithiated layered oxide; wherein the anode active material comprises, based on the center of the anode active material: a first region in which the ratio of the radius to the total radius is greater than 0 and less than or equal to 1 / 2; and a second region in which the ratio of the radius to the total radius is greater than 1 / 2 and less than or equal to 2 / 2, wherein the elemental content of cobalt in the second region is higher than the elemental content of cobalt in the first region, and the elemental content of cobalt in the coating layer is higher than the elemental content of cobalt in the overlithiated layered oxide. Claim 2 In claim 1, the positive active material comprising a compound represented by the following general formula 1, wherein the overlithium layered oxide comprises: In the above general formula 1:0 <x<1이고 a+b+c=1이고, 0<a<1, 0≤b<1 및 0≤c<1이고, M1 및 M2는 서로 상이한 전이금속으로서 Ni 또는 Co이다. Claim 3 In claim 1, the positive active material, wherein the overlithium layered oxide comprises a compound represented by the following general formula 2: In the above general formula 2: M3 and M4 are each independently selected from the group consisting of Zr, Al, Re, V, Cr, Fe, Ga, Si, B, Ru, Ti, Nb, Mo, Mg, W, Na and Pt, and 0.500 <y<0.800, 0.450<p<0.650, 0≤q≤0.025, 0≤r≤0.100, 0.900≤s≤1.000이다. Claim 4 delete Claim 5 In claim 1, the coating layer comprises a positive active material including LiCoO2. Claim 6 In claim 1, the average particle size (D of the positive active material) of the positive active material 50 ) is a positive electrode active material having a size of 6 µm or more and 12 µm. Claim 7 A positive active material according to claim 1, wherein the average thickness of the coating layer is 500 nm or more and 2,000 nm or less. Claim 8 A positive active material according to claim 1, wherein the grain size of the positive active material is 40 nm or more and 70 nm or less. Claim 9 (S1) a step of preparing a mixture comprising a precursor for manufacturing a lithium-overlayer oxide and a cobalt precursor; and (S2) a step of calcining the mixture to manufacture the positive active material of claim 1; comprising a method for manufacturing a positive active material. Claim 10 A method for manufacturing a positive electrode active material according to claim 9, wherein the content of the cobalt precursor is 0.5 parts by weight or more and 10 parts by weight or less per 100 parts by weight of the lithium-overlayered oxide precursor. Claim 11 A method for manufacturing an anode active material according to claim 9, wherein the above step (S2) comprises a step of sintering at a temperature of 550°C or higher and 950°C or lower for 2 hours or more and 15 hours or less. Claim 12 A positive electrode comprising a positive electrode active material according to any one of claims 1 to 8. Claim 13 A positive active material manufactured according to the method for manufacturing a positive active material of claim 9. Claim 14 An electrochemical device comprising: an anode according to claim 12; a cathode; a separator interposed between the anode and the cathode; and an electrolyte. Claim 15 An electric vehicle comprising an electrochemical element according to paragraph 11.

Citation Information

Patent Citations

  • Composite cathode active material, cathode and lithium battery containing the material and preparation method thereof

    KR1020140034606A

  • Composite cathode active material, cathode and lithium battery containing composite cathode active material and preparation method thereof

    KR1020170079942A