Positive electrode material, and electrochemical device and electric device comprising same
By using lithium cobalt oxide cathode materials with P63mc crystal structure in lithium-ion batteries and doping with alkaline earth metal elements, the problem of insufficient cycle performance of lithium-ion batteries is solved, and structural stability and stability in a high delithiation state are achieved. Cycle performance improvements.
Patent Information
- Application Number
- PCT/CN2023/085543
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
The existing lithium-ion batteries have insufficient cycle performance, especially poor structural stability in high delithiation states, resulting in poor battery cycle performance.
Using lithium cobalt oxide cathode material with P63mc crystal structure, by regulating the characteristic peak intensity ratio in the range of 490cm-1±5cm-1 and 592cm-1±5cm-1 in the Raman spectrum, combined with alkaline earth metal element doping, A column effect is formed to support the transition metal layer and improve structural stability.
Significantly improves the structural stability and cycle performance of lithium-ion batteries in high delithiation states, and extends the service life of the battery.
Smart Images

Figure CN2023085543_03102024_PF_FP_ABST
Abstract
Description
Positive electrode material, electrochemical device containing the positive electrode material, and electric device Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a positive electrode material, an electrochemical device containing the positive electrode material, and an electrical device. Background Art
[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight, and are widely used in consumer electronics and other fields.
[0003] With the rapid development of electric vehicles and mobile electronic devices, people have increasingly higher requirements on the energy density, safety, cycle performance and other aspects of lithium-ion batteries. There is an urgent need to improve the positive electrode materials in lithium-ion batteries to improve the cycle performance of existing lithium-ion batteries.
[0004] Summary of the Invention
[0005] The purpose of this application is to provide a positive electrode material, an electrochemical device containing the positive electrode material, and an electrical device to improve the cycle performance of the electrochemical device. The specific technical solution is as follows:
[0006] The first aspect of the present application provides a positive electrode material, which includes lithium cobalt oxide having a P63mc crystal structure. In the Raman spectrum of the positive electrode material, the positive electrode material has a peak at 490 cm -1 ±5cm -1 The peak intensity of the characteristic peak in the range is I1, at 592cm -1 ±5cm -1 The peak intensity of the characteristic peak within the range is I2, satisfying 1<I2 / I1<5. The cathode material of the present application can support the transition metal layer, thereby reducing the collapse of the transition metal layer, improving the structural stability of the cathode material in a highly delithiated state, and thus improving the cycle stability of the electrochemical device.
[0007] In some embodiments of the present application, 1.2≤I2 / I1≤4.3. In this case, the positive electrode material exhibits good cycle stability, thereby improving the cycle performance of the electrochemical device.
[0008] In some embodiments of the present application, the lithium cobalt oxide contains an alkaline earth metal element M, and the Li site of the lithium cobalt oxide is doped with the M element. In this case, the M element doped into the Li site can form a pillar effect, which can support the transition metal layer in a highly delithiated state and reduce the collapse of the transition metal layer, thereby improving the structural stability of the positive electrode material in a highly delithiated state.
[0009] In some embodiments of the present application, based on the molar amount of metal elements other than Li, Na, and M in the lithium cobalt oxide, the molar percentage of the M element in the lithium cobalt oxide is 0.5% to 5%.
[0010] In some embodiments of the present application, the M element includes at least one of Ca and Mg. In this case, the M element can remain relatively stable and effectively doped into the Li site to form a pillar effect, and the positive electrode material exhibits good cycle stability.
[0011] In some embodiments of the present application, the lithium cobalt oxide further contains a Na element and a metal element Q; the Q element includes at least one of Al, Zr, Ni, Mn, Y, Nb, La, Fe, Cu, Cr, Ti, W, Lu or Yb; based on the molar amount of the metal elements other than Li, Na and M in the lithium cobalt oxide, the molar percentage of the Na element in the lithium cobalt oxide is 0.5% to 5%, and the molar percentage of the Q element in the lithium cobalt oxide is 2% to 10%.
[0012] In some embodiments of the present application, the general formula of lithium cobalt oxide is Na a Li b M y Co 1-z Q z O 2±n T n , where 0 < a ≤ 0.05, 0.65 ≤ b ≤ 1.1, 0 < y ≤ 0.05, 0 ≤ z ≤ 0.1, and 0 ≤ n ≤ 0.1; the M element is an alkaline earth metal element; the Q element includes at least one of Al, Zr, Ni, Mn, Y, Nb, La, Fe, Cu, Cr, Ti, W, Lu, or Yb; and the T element is a halogen element. In this case, the positive electrode material exhibits good cycle stability.
[0013] In some embodiments of the present application, the Dv50 of the positive electrode material is 5 μm to 25 μm. In this case, the positive electrode material has good cycle performance.
[0014] A second aspect of the present application provides an electrochemical device comprising a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode material of any of the aforementioned embodiments. The positive electrode material provided herein has good cycle stability, thereby providing the electrochemical device provided herein with good cycle performance.
[0015] In some embodiments of the present application, the charge cut-off voltage of the electrochemical device is not less than 4.50 V. In this case, the electrochemical device has a higher reversible capacity and good cycle performance.
[0016] The third aspect of the present application provides an electrical device, which includes the electrochemical device according to any of the aforementioned embodiments. The electrochemical device provided in the present application has good cycle performance, and thus the electrical device provided in the present application has a long service life.
[0017] Beneficial effects of the present application: The present application provides a positive electrode material, an electrochemical device comprising the positive electrode material, and an electrical device, wherein the positive electrode material comprises lithium cobalt oxide having a P63mc crystal structure, and the Raman spectrum of the positive electrode material at 490 cm -1 ±5cm -1 The peak intensity of the characteristic peak in the range is I1, at 592cm -1 ±5cm -1 The peak intensity of the characteristic peak within the range is I2, and satisfies 1<I2 / I1<5. The positive electrode material of the present application can support the transition metal layer in a highly delithiated state, thereby reducing the collapse of the transition metal layer and improving the structural stability of the positive electrode material in a highly delithiated state, thereby improving the cycle performance of the electrochemical device.
[0018] Of course, it is not necessary to achieve all the advantages described above at the same time when implementing any product or method of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings described herein are used to provide further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0020] FIG1 is a Raman spectrum diagram of Examples 1 to 3 and Comparative Examples 1 to 2 of the present application. DETAILED DESCRIPTION
[0021] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described below with reference to the accompanying drawings and examples. It is apparent that the described examples are only a portion of the embodiments of this application, and not all of them. All other embodiments derived by persons of ordinary skill in the art based on the examples in this application are intended to fall within the scope of protection of this application.
[0022] It should be noted that, in the specific embodiments of the present application, a lithium-ion battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium-ion battery.
[0023] The first aspect of the present application provides a positive electrode material, which includes lithium cobalt oxide having a P63mc crystal structure. In the Raman spectrum of the positive electrode material, the positive electrode material has a peak at 490 cm -1 ±5cm -1 The peak intensity of the characteristic peak in the range is I1, at 592cm-1 ±5cm -1 The peak intensity of the characteristic peak within the range is I2, satisfying 1<I2 / I1<5. In one embodiment, 1.2≤I2 / I1≤4.3. By regulating the ratio of I2 to I1 within the above range, the positive electrode material of the present application can support the transition metal layer in a highly delithiated state, thereby reducing the collapse of the transition metal layer, improving the structural stability of the positive electrode material in a highly delithiated state, and thus improving the cycling stability of the lithium-ion battery.
[0024] The high delithiation state in this application means that when the charge cut-off voltage is ≥4.55V, the positive electrode material is in a high delithiation state. Compared with the material in the initial full discharge state, the amount of lithium removed from the positive electrode material at this time is generally ≥0.7mol. For example, the composition of the material in the initial full discharge state is Li 0.9 CoO2, the positive electrode material composition becomes Li when the lithium removal amount is 0.7 mol 0.2 CoO2.
[0025] In some embodiments of the present application, the lithium cobalt oxide contains an alkaline earth metal element M, and the Li site of the lithium cobalt oxide is doped with the M element. The doping of the M element into the Li site can form a pillar effect, which can support the transition metal layer in a highly delithiated state, reduce the collapse of the transition metal layer, and improve the structural stability of the positive electrode material in a highly delithiated state, thereby improving the cycle performance of the lithium-ion battery.
[0026] In some embodiments of the present application, based on the molar amount of metal elements other than Li, Na, and M in the lithium cobalt oxide, the molar percentage of the M element in the lithium cobalt oxide is 0.5% to 5%.
[0027] In some embodiments of the present application, the M element includes at least one of Ca and Mg. In this case, the M element can remain relatively stable and effectively doped into the Li site to form a pillar effect, and the lithium-ion battery exhibits good cycle stability.
[0028] In some embodiments of the present application, the lithium cobalt oxide further contains a Na element and a metal element Q; the Q element includes at least one of Al, Zr, Ni, Mn, Y, Nb, La, Fe, Cu, Cr, Ti, W, Lu or Yb; based on the molar amount of the metal elements other than Li, Na and M in the lithium cobalt oxide, the molar percentage of the Na element in the lithium cobalt oxide is 0.5% to 5%, and the molar percentage of the Q element in the lithium cobalt oxide is 2% to 10%. The lithium-ion battery containing the positive electrode material exhibits good cycle performance.
[0029] In some embodiments of the present application, the general formula of lithium cobalt oxide is Na a Li b M y Co1-z Q z O 2±n T n , wherein 0 < a ≤ 0.05, 0.65 ≤ b ≤ 1.1, 0 < y ≤ 0.05, 0 ≤ z ≤ 0.1, 0 ≤ n ≤ 0.1, the M element is an alkaline earth metal element, the Q element includes at least one of Al, Zr, Ni, Mn, Y, Nb, La, Fe, Cu, Cr, Ti, W, Lu, or Yb, and the T element is a halogen element, including at least one of F, Cl, Br, or I. By selecting a positive electrode material having the above general formula, the lithium-ion battery exhibits good cycle stability.
[0030] In some embodiments of the present application, the Dv50 of the positive electrode material is 5 μm to 25 μm. By regulating the Dv50 of the positive electrode material within the above range, the lithium-ion battery has good cycle performance.
[0031] In this application, Dv50 refers to the particle size of 50% of the particles in the volume distribution of the positive electrode material.
[0032] The present application has no particular restrictions on the preparation method of the positive electrode material, as long as the purpose of the present application can be achieved. For example, the preparation method of the positive electrode material may include but is not limited to the following steps:
[0033] Step 1: adding a soluble cobalt salt and a metal salt containing a doping element Q to a solvent in proportion to form a uniform mixed solution, then adding a precipitant and a complexing agent, adjusting the pH to 5 to 9, forming a homogeneous precipitate, and then sintering, crushing, and screening the precipitate to obtain a metal oxide material;
[0034] Step 2: Weigh and mix the metal oxide material, the sodium-containing compound, and the compound containing the doping element M in proportion, and heat them at a temperature of 750° C. to 1050° C. for 24 to 72 hours to obtain a sodium cobalt oxide with a P63mc structure;
[0035] Step 3: Using sodium cobalt oxide with a P63mc structure as a precursor material, uniformly mix it with a lithium-containing compound, place it in a corundum crucible, and react it in a solid phase at a temperature of 220° C. to 280° C. for 2 to 8 hours. After cooling, a mixture containing a lithium cobalt oxide positive electrode material is obtained;
[0036] Step 4: crush the mixture material in step 3, wash it with deionized water multiple times to remove the soluble sodium salt and lithium salt in the mixture, and then filter, dry and sieve the residual powder to obtain a lithium cobalt oxide positive electrode material.
[0037] In step 1, the soluble cobalt salt and the metal salt containing the doping element are at least one of chloride, acetate, sulfate, or nitrate. For example, the soluble cobalt salt includes cobalt chloride, cobalt acetate, cobalt nitrate, and cobalt sulfate. The metal salt containing the doping element includes nickel nitrate, manganese nitrate, and yttrium nitrate. The sodium-containing compound is at least one of Na2O, Na2O2, Na2CO3, or NaOH, preferably Na2O and Na2CO3. The compound containing the doping element M is preferably a chloride or carbonate of element M, such as calcium chloride, calcium carbonate, or magnesium carbonate. The present application does not specifically limit the mixing ratio of the soluble cobalt salt and the metal salt containing the doping element Q; as long as the objectives of the present application are achieved, they can be mixed in a designed ratio. For example, the soluble cobalt salt and the metal salt containing the doping element Q are mixed in a ratio of 1:1 (0.02 to 0.11). The present application does not specifically limit the precipitant and complexing agent; as long as the objectives of the present application are achieved, they can be mixed in a designed ratio. For example, precipitants include ammonium carbonate and ammonium bicarbonate, and complexing agents include ammonia water and sodium hydroxide. The amounts of the precipitant and complexing agent added are not particularly limited, as long as the objectives of this application are achieved. For example, based on the molar number of Co, the amount of the precipitant added is 1 to 2.5 times, and the amount of the complexing agent added is 1 to 1.5 times. This application does not particularly limit the sintering temperature; for example, the sintering temperature can be 450°C to 700°C. This application can use a jet mill for crushing and a vibrating screen for particle size screening to adjust the particle size of the metal oxide material.
[0038] In step 2, the present application has no particular limitation on the mixing ratio of the metal oxide material, the sodium-containing compound, and the compound containing the doping element M, and they can be added according to the designed ratio.
[0039] In step 3, the present application has no particular limitation on the lithium-containing compound, as long as it can achieve the purpose of the present application. For example, the lithium-containing compound includes but is not limited to lithium sulfate, lithium carbonate, lithium nitrate, lithium halide, lithium carboxylate, lithium squarate, lithium alkoxide, etc.
[0040] The present application does not particularly limit the method for regulating the peak intensities I1 and I2. For example, I2 generally increases with the intensity of the Co-O bending vibration, and I1 generally increases with the intensity of the Co-O stretching vibration. Based on this, the bending and stretching vibration intensities of the Co-O bond can be controlled by adjusting the sintering process and doping, thereby adjusting the ratio range of I1 to I2.
[0041] A second aspect of the present application provides an electrochemical device comprising a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode material of any of the aforementioned embodiments. The positive electrode material provided herein has good cycle stability, thereby providing the electrochemical device provided herein with good cycle performance.
[0042] In some embodiments of the present application, the charge cut-off voltage of the electrochemical device is not less than 4.50 V. In this case, the electrochemical device has a higher reversible capacity and good cycle performance.
[0043] The electrochemical device of the present application includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer. The present application has no special restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector, etc. In the present application, there is no special restriction on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm, preferably 6μm to 18μm. The thickness of the single-sided positive electrode active material layer is 30μm to 120μm. In the present application, the positive electrode active material layer can be arranged on one surface in the thickness direction of the positive electrode current collector, or on both surfaces in the thickness direction of the positive electrode current collector. Optionally, the positive electrode active material layer may also include a conductive agent and a binder. The present application does not particularly limit the type of binder in the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the binder may include but is not limited to at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The present application does not particularly limit the type of conductive agent in the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, Ketjen black, graphene, metal materials or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powder and / or metal fibers. Specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The conductive polymer may include, but is not limited to, at least one of a polyphenylene derivative, polyaniline, polythiophene, polyacetylene, or polypyrrole. The present application does not particularly limit the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer. Those skilled in the art may select the ratio based on actual needs, as long as the objectives of the present application are achieved.
[0044] This application places no particular restrictions on the negative electrode sheet, as long as the object of this application can be achieved. For example, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer. This application places no particular restrictions on the negative electrode current collector, as long as the object of this application can be achieved. For example, the negative electrode current collector can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam or copper foam, etc. The negative electrode active material layer of this application includes a negative electrode active material. This application places no particular restrictions on the type of the negative electrode active material, as long as the object of this application can be achieved. For example, the negative electrode active material can include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x (0 < x < 2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, lithium titanate with a spinel structure Li4Ti5O 12 , Li-Al alloy or at least one of metallic lithium. In this application, there are no particular restrictions on the thickness of the negative electrode current collector and the negative electrode active material layer, as long as the object of this application can be achieved. For example, the thickness of the negative electrode current collector is 6 μm to 10 μm, and the thickness of the negative electrode active material layer is 30 μm to 130 μm. Optionally, the negative electrode active material layer may further include at least one of a conductive agent, a stabilizer, and a binder. This application places no particular restrictions on the types of the conductive agent, the stabilizer, and the binder in the negative electrode active material layer, as long as the object of this application can be achieved. This application places no particular restrictions on the mass ratio of the negative electrode active material, the conductive agent, the stabilizer, and the binder in the negative electrode active material layer, as long as the object of this application can be achieved.
[0045] The electrochemical device of this application further includes a separator. This application places no particular restrictions on the separator, as long as the object of this application can be achieved. For example, it can include, but is not limited to, at least one of polyethylene (PE), polypropylene (PP), polyolefin (PO) membranes mainly composed of polytetrafluoroethylene, polyester membranes (such as polyethylene terephthalate (PET) membranes), cellulose membranes, polyimide membranes (PI), polyamide membranes (PA), spandex, aramid membranes, woven membranes, non-woven membranes (non-woven fabrics), microporous membranes, composite membranes, separator papers, calendared membranes or spun membranes, and PP is preferred. The separator of this application can have a porous structure, and there are no particular restrictions on the size of the pore diameter, as long as the object of this application can be achieved. For example, the size of the pore diameter can be 0.01 μm to 1 μm. In this application, there are no particular restrictions on the thickness of the separator, as long as the object of this application can be achieved. For example, the thickness can be 5 μm to 500 μm. <T <T
[0046] For example, the diaphragm may include a substrate layer and a surface treatment layer. The substrate layer may be a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer may include but is not limited to at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance.
[0047] The inorganic layer may include, but is not limited to, inorganic particles and inorganic layer binders. The present application has no particular restrictions on the inorganic particles, as long as the purpose of the present application can be achieved. For example, it may include, but is not limited to, at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. The present application has no particular restrictions on the inorganic layer binder. For example, it may include, but is not limited to, at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, or polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer may include, but is not limited to, at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinyl pyrrolidone, polyvinyl ether, polyvinylidene fluoride, or polyvinylidene fluoride-hexafluoropropylene.
[0048] In the present application, the electrochemical device also includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include at least one of LiPF6, LiBF4, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalatoborate) (LiBOB) or lithium difluoroborate. The present application does not particularly limit the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt in the electrolyte is 0.9mol / L to 1.5mol / L. Exemplarily, the concentration of the lithium salt in the electrolyte can be 0.9mol / L, 1.0mol / L, 1.1mol / L, 1.3mol / L, 1.5mol / L or a range consisting of any two of the above values. The application has no particular restrictions on non-aqueous solvents, as long as the purpose of the application can be achieved, for example, can include but not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. Above-mentioned carbonate compounds can include but not limited to at least one of linear carbonate compounds, cyclic carbonate compounds or fluorinated carbonate compounds. Above-mentioned linear carbonate compounds can include but not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or methyl ethyl carbonate (MEC). Above-mentioned cyclic carbonate can include but not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include, but is not limited to, at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, or caprolactone. The ether compound may include, but is not limited to, at least one of dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran, or tetrahydrofuran. The other organic solvent may include, but is not limited to, at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, or trioctyl phosphate.
[0049] The electrochemical device of the present application is not particularly limited and may include any device that undergoes an electrochemical reaction. In one embodiment of the present application, the electrochemical device may include, but is not limited to, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery. In one embodiment, the structure of the electrode assembly includes a wound structure or a laminated structure.
[0050] The preparation process of the electrochemical device of the present application is well known to those skilled in the art and is not particularly limited herein. For example, it may include, but is not limited to, the following steps: stacking the positive electrode sheet, separator, and negative electrode sheet in sequence, and winding, folding, and other operations as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag, and sealing the bag to obtain the electrochemical device; or stacking the positive electrode sheet, separator, and negative electrode sheet in sequence, and then securing the four corners of the entire stack with tape to obtain a stacked electrode assembly; placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag, and sealing the bag to obtain the electrochemical device. Furthermore, overcurrent protection elements, guide plates, and the like may be placed in the packaging bag as needed to prevent pressure buildup and overcharging and discharging within the electrochemical device. The present application does not limit the packaging bag, and those skilled in the art may select a suitable packaging bag based on actual needs, as long as it achieves the objectives of the present application. For example, an aluminum-plastic film packaging bag may be used.
[0051] The third aspect of the present application provides an electrical device, which includes the electrochemical device according to any of the aforementioned embodiments. The electrochemical device provided in the present application has good cycle performance, and thus the electrical device provided in the present application has a long service life.
[0052] The present application does not particularly limit the electrical device, and the electrical device may be any electrical device known in the art. For example, the electrical device may include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a power-assisted bicycle, a bicycle, lighting fixtures, toys, a game console, a clock, a power tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.
[0053] Example
[0054] The following examples and comparative examples are provided to more specifically illustrate the embodiments of the present invention. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0055] Test methods and equipment:
[0056] Raman testing:
[0057] The positive electrode materials prepared in each embodiment and comparative example were tested using a spectrometer (Jobin Yvon LabRAM HR) with a light source of 532 nm and a test range of 200 cm -1 Up to 4000cm -1 .
[0058] Cathode material particle size test:
[0059] The positive electrode materials prepared in each example and comparative example were tested using a Malvern particle size analyzer (Master Sizer 2000). In the volume-based particle size distribution of the positive electrode active material, the particle size at which the cumulative volume reaches 50% is defined as Dv50, starting from the smallest particle size.
[0060] XRD test:
[0061] The cathode material was tested using an X-ray powder diffractometer (Bruker D8ADVANCE) with a Cu Kα target, a test voltage of 40 kV, a test current of 35 mA, a scan angle range of 10° to 90°, and a scan rate of 0.02° / s. The intensity of the strongest diffraction peak was required to be greater than 10,000 counts. The collected XRD spectra were refined using Fullprof software to determine the phase structure and dopant element occupancy.
[0062] Cathode material element composition test:
[0063] The lithium and metal element content in the cathode material was measured using an inductively coupled plasma spectrometer (ICP, PE Optima 7000DV). An appropriate amount of powder sample was weighed, and approximately 10 mL of aqua regia was added. The sample was heated on a flat-plate heating device at approximately 185°C for 30 to 50 minutes to fully dissolve the sample before testing.
[0064] Cyclic performance test:
[0065] After aging the button battery at 25°C for 24 hours, the prepared button battery was subjected to charge and discharge tests in the voltage range of 3V to 4.6V. The first two cycles were activated at a charge and discharge rate of 0.1C, and the subsequent cycle tests were performed at a charge and discharge rate of 0.5C. The battery capacity retention rate was calculated based on the battery capacity of the third cycle, 1C = 273mA / g.
[0066] Cycle capacity retention rate = discharge capacity at the nth cycle / discharge capacity at the third cycle × 100%.
[0067] Example 1
[0068] <Preparation of positive electrode material>
[0069] 13.35 kg of cobalt sulfate heptahydrate (CoSO4·7H2O) and 0.66 kg of nickel sulfate hexahydrate (NiSO4·6H2O) were weighed respectively, and deionized water was added and quickly stirred to dissolve. Then, ammonium carbonate and ammonia water were added to adjust the pH of the solution to 8. After the reaction was complete, a homogeneous carbonate precipitate was formed. The precipitate was sintered at 650 ° C for 12 h, crushed and sieved to obtain the metal oxide (Co 0.95 Ni 0.05 )3O4;
[0070] Sodium carbonate (Na2CO3), calcium carbonate (CaCO3) and the prepared metal oxide are mixed uniformly according to the metal element molar ratio of Na:Ca:(Co+Ni)=0.8:0.01:1, and then placed in an environment of 830°C for 48 hours. After crushing and screening, a sodium cobalt oxide material with a P63mmc crystal structure is obtained;
[0071] The prepared sodium cobalt oxide material, lithium nitrate (LiNO3) and lithium chloride (LiCl) were mixed uniformly in a molar ratio of 1:4:1 and placed in a corundum crucible. The mixture was first reacted at 235°C for 4 hours and then at 250°C for 4 hours. After cooling, a mixture containing a lithium cobalt oxide positive electrode material was obtained.
[0072] The obtained mixture material containing lithium cobalt oxide positive electrode material was crushed and washed multiple times with deionized water to remove soluble sodium salts and lithium salts in the mixture until the conductivity of the supernatant was less than 200 μS / cm. The residual powder was then filtered, dried and sieved to obtain a lithium cobalt oxide material with a Dv50 of 9.3 μm.
[0073] <Preparation of positive electrode sheet>
[0074] The lithium cobalt oxide obtained above was used as the positive electrode active material, along with conductive carbon black (SP) as the conductive agent and polyvinylidene fluoride (PVDF) as the binder, in a mass ratio of 80:10:10. N-methyl-2-pyrrolidone (NMP) was added as the solvent and stirred evenly in a vacuum mixer to obtain a positive electrode slurry with a solid content of 60 wt%. A 12 μm aluminum foil was used as the positive electrode current collector, and a 100 μm thick coating was applied to the current collector aluminum foil. The coating was first baked in a 90°C forced air drying oven for 4 hours, and then in a 110°C vacuum drying oven for 24 hours. The fully dried electrode was then cold pressed, punched, and weighed to obtain a disc-shaped positive electrode with a diameter of 1.4 cm.
[0075] <Preparation of negative electrode sheet>
[0076] A lithium metal sheet is used as the counter electrode.
[0077] <Preparation of Electrolyte>
[0078] In a dry argon atmosphere glove box, fluoroethylene carbonate (FEC), ethylene carbonate (EC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:8 to obtain an organic solvent. LiPF6 was then added to the organic solvent, dissolved, and mixed thoroughly to obtain an electrolyte solution. The LiPF6 concentration was 1 mol / L.
[0079] <Preparation of Separator>
[0080] A porous PE film with a thickness of 7 μm is used.
[0081] <Preparation of lithium-ion batteries>
[0082] In a dry argon atmosphere, the positive electrode sheet is assembled with a separator, a negative electrode sheet and an electrolyte to form a button battery.
[0083] Example 2
[0084] The only difference compared with Example 1 is the following aspects of the preparation steps of the positive electrode material: the molar ratio of the metal elements of Na2CO3, CaCO3 and the prepared metal oxide is Na:Ca:(Co+Ni)=0.8:0.03:1.
[0085] Example 3
[0086] The only difference compared with Example 1 is the following aspects of the preparation steps of the positive electrode material: the molar ratio of the metal elements of Na2CO3, CaCO3 and the prepared metal oxide is Na:Ca:(Co+Ni)=0.8:0.05:1.
[0087] Example 4
[0088] The only difference compared with Example 1 is the following aspects of the preparation steps of the positive electrode material:
[0089] 13.49 kg of raw materials of cobalt sulfate heptahydrate (CoSO4·7H2O) and 0.34 kg of manganese sulfate monohydrate (MnSO4·H2O) were weighed respectively, and deionized water was added and quickly stirred to dissolve. Then, ammonium carbonate was added to adjust the pH of the solution to 8. After the reaction was complete, a homogeneous carbonate precipitate was formed. The precipitate was sintered at 650 ° C for 12 h, crushed and sieved to obtain the metal oxide (Co 0.96 Mn 0.04 )3O4;
[0090] Sodium carbonate (Na2CO3), magnesium oxide (MgO) and the prepared metal oxide are mixed uniformly according to the metal element molar ratio of Na:Mg:(Co+Mn)=0.8:0.01:1, and then placed in an environment of 850°C for 48 hours. After crushing and screening, a sodium cobalt manganese oxide material with a P63mmc crystal structure is obtained;
[0091] The prepared sodium cobalt oxide material, lithium nitrate (LiNO3) and lithium hydroxide (LiOH) were mixed uniformly in a molar ratio of 1:4:1 and placed in a corundum crucible. The mixture was reacted at 250°C for 8 hours and cooled to obtain a mixture containing a lithium cobalt manganese oxide positive electrode material.
[0092] The obtained mixture material was crushed and washed multiple times with deionized water to remove soluble sodium and lithium salts in the mixture until the conductivity of the supernatant was less than 200 μS / cm. The residual powder was then filtered, dried, and sieved to obtain a lithium cobalt manganese oxide material having a Dv50 of 10.2 μm.
[0093] Example 5
[0094] The only difference compared with Example 4 is the following aspects of the preparation steps of the positive electrode material: the molar ratio of the metal elements of Na2CO3, MgO and the prepared metal oxide is Na:Mg:(Co+Mn)=0.8:0.03:1.
[0095] Example 6
[0096] The only difference compared with Example 4 is the following aspects of the preparation steps of the positive electrode material: the metal element molar ratio of Na2CO3, MgO and the prepared metal oxide is Na:Mg:(Co+Mn)=0.8:0.05:1.
[0097] Example 7 to Example 11
[0098] The only difference compared with Example 1 is the following aspects of the preparation steps of the positive electrode material: Y(NO3)3, Nb(NO3)5, La(NO3)3, Fe(NO3)3, and Cu(NO3)2 are used to replace NiSO4·6H2O, thereby adjusting the type of Q element as shown in Table 1, and changing the amount of CaCO3 added to adjust the content of the Ca element as shown in Table 1.
[0099] Example 12 to Example 16
[0100] The only difference compared with Example 4 is the following aspects of the preparation steps of the positive electrode material: replacing MnSO4·H2O with Cr(NO3)3, TiCl4, W(NO3)3, Lu(NO3)3, and Yb(NO3)2, respectively, thereby adjusting the type of Q element as shown in Table 1, and changing the amount of MgO added to adjust the content of Mg element as shown in Table 1.
[0101] Example 17
[0102] The only difference compared with Example 4 is the following aspects of the preparation steps of the positive electrode material: 2 wt% NH4F is added during the sintering process of mixing sodium carbonate (Na2CO3) and magnesium oxide (MgO) with the prepared metal oxide.
[0103] Example 18
[0104] The only difference compared with Example 4 is the following aspects of the preparation steps of the positive electrode material: 5 wt% NH4F is added during the sintering process of mixing sodium carbonate (Na2CO3) and magnesium oxide (MgO) with the prepared metal oxide.
[0105] Comparative Example 1
[0106] The only difference compared with Example 1 is the following aspects of the preparation steps of the positive electrode material: no CaCO3 is added, and the metal element molar ratio of Na2CO3 to the prepared metal oxide is Na:(Co+Ni)=0.8:1.
[0107] Comparative Example 2
[0108] The only difference compared with Example 1 is the following aspects of the preparation steps of the positive electrode material: the molar ratio of the metal elements of Na2CO3, CaCO3 and the prepared metal oxide is Na:Ca:(Co+Ni)=0.8:0.07:1.
[0109] Comparative Example 3
[0110] The only difference compared with Example 2 is the following aspects of the preparation steps of the positive electrode material: Ca is introduced in the form of Ca(NO3)2 during the precursor co-precipitation stage.
[0111] Comparative Example 4
[0112] The only difference compared with Example 5 is the following aspects of the preparation steps of the positive electrode material: Mg is introduced in the form of Mg(NO3)2 during the precursor co-precipitation stage.
[0113] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Table 1.
[0114] Referring to Table 1, it can be seen from Examples 1 to 18 and Comparative Examples 1 to 4 that the capacity retention rate of the button battery after 100 cycles is significantly improved, indicating that by regulating the relationship between the peak intensity I1 and the peak intensity I2 of the positive electrode material within the scope of this application, it is beneficial to improve the cycle performance of the lithium-ion battery.
[0115] FIG1 shows the Raman spectra of the materials of Examples 1 to 3 and Comparative Examples 1 to 2. Two Raman characteristic peaks can be seen in FIG1 , with peak positions at 490±5 cm -1 and 592±5cm -1 , the former represents the bending vibration mode of O-Co-O, and the latter represents the stretching vibration mode of Co-O.
[0116] From Examples 1 to 3 and Comparative Examples 1 to 2, it can be seen that the higher the relative content of the M element, the greater the peak intensity ratio I2 / I1, and when I2 / I1 is within the scope of this application, the button battery exhibits excellent cycle performance. This indicates that by regulating the relationship between the peak intensity I1 and the peak intensity I2 of the positive electrode material within the scope of this application, it is beneficial to improve the cycle performance of the lithium-ion battery. From Example 2 and Comparative Example 3, as well as Example 5 and Comparative Example 4, it can be seen that under the same M element doping amount, when the M element is introduced in the coprecipitation precursor stage, the I2 / I1 of the obtained material is relatively small, while when the M element is introduced in the sodium cobalt oxide sintering stage, the I2 / I1 of the obtained material is relatively large. A possible explanation for this is that M is introduced by co-precipitation in the precursor stage, and M tends to be uniformly doped and distributed in the bulk phase of the target material. However, when introduced in the sodium cobalt oxide sintering stage, the M element is likely to be distributed in a gradient in the target material, and the doping concentration of the surface layer is higher than that of the bulk phase. Therefore, the I2 / I1 ratio is relatively high, and the actual improvement effect on the material structure stability, especially the surface interface stability, is more significant.
[0117] It can also be seen from Examples 1 to 3 and Comparative Examples 1 to 2 that when the relative content of Ni is 0.05 mol, as the content of Ca doped into the Li site increases, the Raman characteristic peak intensity ratio I2 / I1 of the material shows an increasing trend, and the capacity retention rate corresponding to 100 cycles of the battery shows a trend of first increasing and then decreasing. When not doped with Ca, the Raman characteristic peak intensity ratio I2 / I1 of the material provided in Comparative Example 1 is about 0.7, and the capacity retention rate of the material after 100 cycles of battery cycling is low, only 67%; with the increase of the Ca doping amount, the Raman characteristic peak intensity ratio I2 / I1 of Examples 1 to 3 is between 1 and 5, and the battery cycle capacity retention rate is significantly improved, greatly increasing to 87% to 93%; when the Ca doping amount is further increased to 0.07, the Raman characteristic peak intensity ratio I2 / I1 of the material provided in Comparative Example 2 is 5.5, and the battery cycle capacity retention rate begins to decrease, only 62%. ICP test was performed on the fully charged positive electrode sheets after 100 cycles of the materials of Examples 1 to 3. The Ca content was the same as that of the initial powder state, indicating that Ca does not undergo deintercalation during the charge and discharge process. It is speculated that the main reason for the improvement of Ca doping is that Ca forms a pillar effect at the Li position, stabilizing the structure. However, due to Ca 2+ He Li + The radius difference is large, and excessive doping will destroy the balance of the overall crystal structure and worsen the structural stability. By comparing Examples 1 to 3 and Comparative Examples 1 to 2, it can be seen that Ca 2+ The preferred doping concentration should not be higher than 5% (mol percent).
[0118] Referring to Table 1, the type of metal element Q in lithium cobalt oxide generally also affects the performance of the button battery. From Examples 7 to 16, it can be seen that by regulating the type of metal element Q within the scope of this application, it is beneficial to obtain a lithium-ion battery with high cycle performance.
[0119] Comparing Examples 17 and 18 with Example 4 shows that the inclusion of halogen elements in lithium cobalt oxide further improves the cycling stability of the material. Compared to Example 4, Examples 17 and 18, which were doped with F and Cl, respectively, showed capacity retention rates after 100 cycles, increasing from 86% in Example 4 to 94% and 89%, respectively.
[0120] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A positive electrode material, characterized in that: comprising lithium cobalt oxide having a P63mc crystal structure, In the Raman spectrum of the positive electrode material, at 490 cm -1 ±5cm -1 The peak intensity of the characteristic peak in the range is I1, at 592cm -1 ±5cm -1 The peak intensity of the characteristic peak within the range is I2, which satisfies: 1 <I2 / I1<5。 2. The positive electrode material according to claim 1, characterized in that: 1.2≤I2 / I1≤4.
3.
3. The positive electrode material according to claim 1, characterized in that: The lithium cobalt oxide contains an alkaline earth metal element M; and satisfies at least one of the following conditions: (1) The Li site of the lithium cobalt oxide is doped with the M element; (2) Based on the molar amount of the metal elements other than Li, Na and M in the lithium cobalt oxide, the molar percentage of the M element in the lithium cobalt oxide is 0.5% to 5%.
4. The positive electrode material according to claim 3, characterized in that: The M element includes at least one of Ca and Mg.
5. The positive electrode material according to claim 3, characterized in that: The lithium cobalt oxide further comprises Na element and metal element Q; The Q element includes at least one of Al, Zr, Ni, Mn, Y, Nb, La, Fe, Cu, Cr, Ti, W, Lu or Yb; Based on the molar amount of metal elements other than Li, Na and M in the lithium cobalt oxide, the molar percentage of Na element in the lithium cobalt oxide is 0.5% to 5%, and the molar percentage of Q element in the lithium cobalt oxide is 2% to 10%.
6. The positive electrode material according to claim 1, characterized in that: The general formula of the lithium cobalt oxide is Na a Li b M y Co 1-z Q z O 2±n T n , Among them, 0<a≤0.05, 0.65≤b≤1.1, 0<y≤0.05, 0≤z≤0.1, 0≤n≤0.1, The M element is an alkaline earth metal element, the Q element includes at least one of Al, Zr, Ni, Mn, Y, Nb, La, Fe, Cu, Cr, Ti, W, Lu or Yb, and the T element is a halogen element.
7. The positive electrode material according to claim 1, characterized in that: The Dv50 of the positive electrode material is 5 μm to 25 μm.
8. An electrochemical device, characterized in that: The invention comprises a positive electrode plate, wherein the positive electrode plate comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode material according to any one of claims 1 to 7.
9. The electrochemical device according to claim 8, characterized in that: The charging cut-off voltage of the electrochemical device is not less than 4.50V.
10. An electrical device comprising the electrochemical device according to claim 8 or 9.
Citation Information
Patent Citations
Positive electrode material and electrochemical device using positive electrode material
CN109994729A
Composition, methods for its production, and its use
CN112204774A
Positive electrode body, method for manufacturing positive electrode body, and nonaqueous electrolyte battery
JP2011233402A
LiCoO2 CONTAINING SPUTTERING TARGET AND LiCoO2 CONTAINING SINTERED BODY
JP2017088956A
Positive electrode material, secondary battery, electronic apparatus, and method for producing positive electrode material
JP2020071901A
Cited By
Positive electrode material, electrochemical device, and electronic device
WO2026207672A1