Hot-dip coated and phosphated steel flat product for hot forming, hot-formed component and production method
The use of an aluminum-based corrosion protection coating with specific infrared reflectance properties on phosphated flat steel products addresses the incomplete phosphating issue in hot-formed components, enhancing heating rates and surface coverage for improved performance and appearance.
Patent Information
- Application Number
- PCT/EP2024/057403
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional corrosion protection coatings for hot-formed components, particularly those with aluminum and silicon, fail to achieve complete phosphating due to the formation of an aluminum oxide layer during hot forming, leading to inadequate surface coverage and impact on visual appearance, paintability, and surface roughness.
A phosphated flat steel product with an aluminum-based corrosion protection coating having a reflectance in the infrared range of <0.65, featuring an alloy layer and an Al base layer, which enhances heating rates during hot forming and ensures complete phosphating by promoting homogeneous heating and preventing the formation of a thick aluminum oxide layer.
The solution allows for increased heating rates (>40%) during hot forming, ensuring complete phosphating of the component surface, improving both the visual appearance and paintability while maintaining mechanical properties.
Smart Images

Figure EP2024057403_03102024_PF_FP_ABST
Abstract
Description
[0001] Hot-dip coated and phosphated flat steel product for hot forming, hot-formed component and manufacturing process
[0002] The invention relates to a phosphated flat steel product with an aluminum-based anti-corrosive coating and its production, as well as to a component which is produced from the flat steel product by means of hot forming and to a method for producing such a component.
[0003] When reference is made below to a "flat steel product" or a "sheet metal product," this refers to both rolled products, such as steel strips or sheets, and "sheet metal blanks" (also called blanks) that are cut from the rolled products. "Sheet metal blanks" also refer to parts of a rolled product that have undergone further processing other than hot forming, e.g., punching, etc. "Formed sheet metal parts" or "sheet metal components" of the type according to the invention are manufactured from such sheet metal blanks by hot forming, whereby the terms "formed sheet metal part" and "sheet metal component" are used synonymously here.
[0004] In this application, all information regarding steel composition is based on weight unless expressly stated otherwise. All unspecified "%" information relating to a steel alloy is therefore to be understood as "wt%."
[0005] Whenever this application refers to element contents in phases, these are determined using scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDX). The data are also given in "wt. %". The Si-rich phases are identified in the cross-section of the corrosion protection coating by determining the silicon content using point or area scans. To determine the continuity of a phase layer, at least three light microscope and / or SEM images are evaluated. The image section selected for the light microscope and / or SEM images is chosen so that at least the entire metallic coating, from the surface to the steel substrate, can be seen. For this purpose, the proportion of the phase parallel to the surface and parallel to the cross-section surface is measured on an SEM image. For this purpose, a straight line parallel to the surface is placed on the SEM image.To determine the phase continuity, the ratio of the total length of the straight line within the phase to the total length of the straight line is determined. The straight line parallel to the surface is positioned to obtain the maximum value of the ratio. This maximum value of the ratio is referred to as the phase continuity. The martensite start temperature and the AC1 and AC3 temperatures are defined below. The martensite start temperature of a steel that meets the specifications of the invention is determined according to the formula:
[0006] Ms [°C] = (490.85% - 302.6 %C - 30.6 %Mn - 16.6 %Ni - 8.9 %Cr + 2.4 %Mo - 11.3 %Cu + 8.58 %Co + 7.4 %W - 14.5 %Si) [°C / wt.%], where C% is the C content, %Mn is the Mn content, %Mo is the Mo content, %Cr is the Cr content, %Ni is the Ni content, %Cu is the Cu content, %Co is the Co content, %W is the W content and %Si is the Si content of the respective steel in wt.%.
[0007] The ACl temperature and the AC3 temperature of a steel within the scope of the invention specifications are according to the formulas:
[0008] AC1[°C] = (739% - 22*%C - 7*%Mn + 2*%Si + 14*%Cr + 13*%Mo - 13*%Ni +20*%V )[°C / wt.-%] and
[0009] AC3[°C] = (902% - 225*%C + 19*%Si - 11*%Mn - 5*%Cr + 13*%Mo - 20*%Ni +55*%V)[°C / wt.%], where %C denotes the C content, %Si denotes the Si content, %Mn denotes the Mn content, %Cr denotes the Cr content, %Mo denotes the Mo content, %Ni denotes the Ni content and +%V denotes the vanadium content of the respective steel (Brandis H 1975 TEW-Techn. Ber. 1 8- 10)
[0010] The coverage specified below is determined using a scanning electron microscope (SEM). For this purpose, an SEM image of the surface with a size of 1 x 1 mm is taken at at least 5 different positions. Areas without phosphate crystals with a diameter of > 10 μm are considered uncoated. All other areas are defined as covered. The coverage is defined as (uncoated area) / (covered area) and is given in % and is to be determined as the average value from the 5 positions. The reflectance R in the infrared range is specified below. For the purposes of this application, the infrared range is the wavenumber range from 667 - 10,000 cm 1 This corresponds to the wavelength range of 1 - 15 pm.
[0011] For the purposes of this application, the reflectance R in the infrared range is determined using a blackbody radiator as a reference. The blackbody has a temperature of T = 920°C, which corresponds to an average furnace temperature. Thus, the spectral radiant power i (T) of the blackbody radiator at temperature T is compared with the measured spectral reflectivity p Ä multiplied and integrated over the wavelength range. This integral is standardized to the spectral radiant power integrated over the same wavelength range. Therefore,
[0012] Here, i (T) results from Planck's radiation law with the speed of light c, the Planck constant h and the Boltzmann constant k B The integration is carried out over the wavelength range corresponding to the wavenumbers 667 - 10000 cm 1 corresponds, ie from = 1 pm to A2= 15 pm. The reflectance R used below is defined as Ä(920°C).
[0013] When AS surfaces are referred to below, this refers to the surface of an aluminum-based corrosion protection coating with silicon.
[0014] In order to offer the combination of low weight, maximum strength and protective effect required in modern car body construction, components made from high-strength steel are now used in those areas of the car body that can be exposed to particularly high loads in the event of a crash. During hot forming, also known as hot press hardening, steel blanks (also known as sheet metal blanks), which are previously cut from cold or hot-rolled steel strip, are heated to a deformation temperature that is generally above the austenitizing temperature of the respective steel, and then placed in the tool of a forming press in the heated state. During the subsequent forming process, the sheet metal blank or the component formed from it undergoes rapid cooling due to contact with the cool tool. The cooling rates are set so that a hardened structure (i.e. martensitic structure) results in the component.
[0015] To protect hot-formed components from corrosion, anti-corrosive coatings made of aluminum and silicon, applied by hot-dip coating, are known. WO 2015 / 036151 A1 discloses a method for producing a steel component provided with a metallic, corrosion-protective coating and a corresponding steel component. The method according to this document comprises coating a flat steel product with an alloy of aluminum, zinc, magnesium, and optionally silicon and iron, cutting a blank from the flat steel product, heating the blank, and forming the blank to obtain the desired steel component.
[0016] Phosphating flat steel products and components is known from the state of the art. Phosphating is applied for additional corrosion protection, but also to alter surface adhesion, which can impact paintability, for example. This phosphating can be applied not only directly to the flat steel product, but also to other corrosion protection coatings. Schneider et al. (ASC Appl. Mater Interfaces 2013, pp. 4224-4232), for example, phosphated flat steel products that had previously been coated with an aluminum / silicon-containing corrosion protection coating. The phosphate crystals grow on the Si-rich phases of the corrosion protection coating. However, the conditions chosen by Schneider et al. did not achieve complete surface coverage with phosphate crystals. Furthermore, the flat steel product is not hot-formed.
[0017] Phosphate compounds on aluminum / silicon-containing corrosion protection coatings are also known from WO 2012 / 120081 Al. It was found that the phosphate compounds can lead to an increased heating rate to preforming temperature. However, a reduction in heating times for aluminum / silicon-containing corrosion protection coatings of only 30% is achieved. Typically, hot-formed components for automotive construction are also phosphated. The phosphating step takes place after hot forming. However, with conventional corrosion protection coatings made of aluminum and silicon, an aluminum oxide layer forms during hot forming. Due to the high temperatures during hot forming, a thick aluminum oxide layer is formed.During the subsequent phosphating step, the typical process parameters are insufficient to break down the oxide layer, preventing the conversion process from starting. As a result, only a small portion of the component's surface can be phosphated. This has a negative impact on the visual appearance before and after corrosion, the surface roughness, and the paintability.
[0018] The object of the present invention is therefore to provide a flat steel product for hot forming with which a complete phosphating of the surface of the component can be achieved and an increased heating rate, preferably > 40%, to the deformation temperature during hot forming can be ensured.
[0019] The problem is solved with a flat steel product that is provided with an aluminum-based anti-corrosive coating consisting of an alloy layer and an Al base layer and has a reflectance in the infrared range of < 0.65. The low reflectance leads to an increased heating rate, preferably > 40%, during hot forming, since the radiant heat inside the furnace is emitted primarily in the infrared range during the hot forming step. Furthermore, the flat steel product according to the invention can be used to produce a hot-formed component with complete phosphating. This cannot be achieved in a sole phosphating step after hot forming due to the aluminum oxide layer then formed on the surface.
[0020] The invention relates to a phosphated flat steel product comprising a steel substrate and a corrosion protection coating, wherein the steel substrate contains, in addition to iron and unavoidable impurities from
[0021] C: 0.04% - 0.45%,
[0022] Mn: 0.5% - 2.6%,
[0023] Si: 0.02% - 1.2%,
[0024] AI: 0.02 - 1.0%, P: < 0.05%,
[0025] S: < 0.02%, and optionally one or more of the following elements with the contents:
[0026] Ti: 0.01% - 0.08%,
[0027] Nb: 0.02% - 0.08%,
[0028] B: 0.001% - 0.005%,
[0029] Cr: 0.08% up to 1.0%,
[0030] Mo: < 0.5%,
[0031] Ni: < 0.5%,
[0032] Cu: < 0.2%,
[0033] V: < 0.1%, and wherein the corrosion protection coating is aluminum-based and has an alloy layer and an Al base layer, characterized in that the reflectance R in the infrared range is < 0.65, preferably < 0.55, in particular < 0.40, particularly preferably < 0.35.
[0034] The alloying elements ensure processability, coatability, and final properties. The explanations of the steel substrate, including the preferred design variants, apply to both the phosphated flat steel product and the corresponding manufacturing process, as well as to the component and its manufacturing process.
[0035] Carbon ("C") is present in the steel according to the invention at a level of at least 0.04% and contributes to the hardenability of the steel by delaying the formation of ferrite and bainite, as well as the formation of residual austenite in the microstructure. To ensure reliable utilization of the advantages of carbon, a proportion of at least 0.07%, particularly preferably at least 0.10%, has proven advantageous. Excessively high a carbon content can lead to a deterioration in the welding properties of the flat steel product; therefore, the carbon content is limited according to the invention to 0.45%, preferably to 0.4%, and particularly preferably to 0.25%.
[0036] The addition of manganese ("Mn") delays the formation of ferrite and bainite in the flat steel product. To minimize the amount of ferrite and bainite during cooling after hot forming, an addition of 0.5% has proven advantageous. In a preferred variant, a manganese content of at least 0.8%, particularly preferably at least 1.0%, can be added to the flat steel product. Excessively high manganese contents impair the workability of the steel; therefore, the manganese content is limited to 2.6%. In particular, to improve welding properties, the manganese content should be limited to preferably 1.6% and particularly preferably to 1.30%.
[0037] Silicon ("Si") leads to solid solution strengthening in the hot-formed product and thus to a further increase in hardenability. A content of at least 0.02% according to the invention has proven suitable for this purpose. A content of at least 0.06%, and particularly preferably at least 0.35%, has proven particularly advantageous for adjusting hardenability. Excessively high silicon content in the flat steel product can have a detrimental effect on coatability. Therefore, according to the invention, the silicon content is limited to 1.2%, preferably 1.1%, particularly preferably 0.9%.
[0038] Aluminum (Al) can be added to steel as a deoxidizer. For this purpose, at least 0.02% and preferably at least 0.03% aluminum is added to the steel. However, an excessively high aluminum content can increase the AC3 temperature, thus complicating hot forming. Therefore, it has been found advantageous to limit the aluminum content to 1.0%, preferably 0.5%, and especially preferably 0.1%.
[0039] Phosphorus ("P") and sulfur ("S") are impurities in flat steel products that arise from iron ore. The goal is to keep their contents as low as possible, as excessive levels can negatively impact mechanical properties. For this purpose, the phosphorus content in the present invention is limited to 0.05%, preferably 0.03%. According to the invention, the sulfur content should be no more than 0.02%.
[0040] In addition to sulfur and phosphorus impurities, other elements may also occur as impurities in flat steel products. These additional elements are collectively referred to as "unavoidable impurities." The total content of these unavoidable impurities is preferably a maximum of 0.2%, and particularly preferably 0.1%.
[0041] For the optional alloying elements Ti, Nb, B, Cr, Mo, Ni, Cu, and V described below, for which a lower limit is specified, contents below the respective lower limit may also occur as impurities in the flat steel product. In this case, they are also considered "unavoidable impurities." The elements titanium, niobium, boron, chromium, molybdenum, nickel, copper, and vanadium can optionally be alloyed individually or in combination to the steel of the flat steel product according to the invention.
[0042] The optional addition of titanium (Ti) can improve grain refinement. An optional addition of at least 0.01% can help with this. The titanium content should be limited to 0.08%, as excessive titanium contents negatively impact cold rolling and recrystallizability.
[0043] Niobium (Nb) influences grain refinement during austenitization in the hot forming process. For this purpose, it has been found advantageous to add at least 0.02% Nb to the steel according to the invention. However, niobium leads to impaired recrystallizability. Therefore, the maximum niobium content is 0.08%, preferably 0.06%.
[0044] Boron "B" is added to improve the hardenability of the flat steel product. This effect occurs at a boron content of at least 0.001%, preferably at least 0.002%. Excessively high boron contents can lead to the formation of boron nitrides or boron carbides; therefore, the boron content is limited to a maximum of 0.005%, preferably 0.004%.
[0045] Chromium (Cr) is added to the steel to enable complete martensite formation at low cooling rates by suppressing ferrite and pearlite formation. The positive effect of chromium can be utilized at contents of at least 0.08%, preferably at least 0.18%. However, excessive chromium contents negatively affect the steel's coatability. Therefore, the maximum chromium content is limited to 1.0%, preferably 0.5%.
[0046] Molybdenum (Mo) can also be used optionally to suppress ferrite formation, as molybdenum slows the phase transformation through carbide formation at the grain boundaries and reduces the nucleation rate of ferrite by lowering the grain boundary energy. This effect is particularly evident at a content of at least 0.002%. Due to the high cost of the element molybdenum, the maximum content should be limited to 0.5%.
[0047] Nickel (Ni) can optionally be added to the steel. The optional addition of at least 0.01% nickel leads to a reduction in the Ac3 temperature and helps suppress the formation of bainite and ferrite. For economic reasons, the maximum nickel content should be limited to 0.5%, particularly 0.20%.
[0048] Copper (Cu) can optionally be added to the alloy at a content of at least 0.01% to increase hardenability. The maximum Cu content should be limited to 0.2%, preferably 0.1%, as excessively high copper contents impair hot-rolling properties.
[0049] Vanadium "V" can optionally be added to alloys with a minimum of 0.001%. For cost reasons, the maximum vanadium content is limited to 0.1%.
[0050] The flat steel product is provided with an anti-corrosive coating which is based on aluminium and has an alloy layer and an Al base layer.
[0051] Such a corrosion protection coating is preferably produced by hot-dip coating the flat steel product. The flat steel product is passed through a liquid melt consisting of at least 3%, preferably at least 7%, particularly preferably at least 12% and a maximum of 15%, preferably a maximum of 12% silicon (Si), as well as up to 4.0% iron (Fe), preferably 1-3.5% Fe, particularly preferably 2-3.5% Fe, preferably 0.2-0.7% magnesium, and optionally up to 15% zinc (Zn), preferably up to 10% Zn, and optionally further components, the total contents of which are limited to a maximum of 2.0%, with the remainder being aluminum.
[0052] The thickness of the anti-corrosive coating applied to the flat steel product is typically 10–40 μm per side. The coating weight is typically 30–100 g / m 2 , preferably 40 - 80 g / m 2 per page.
[0053] During hot-dip coating, iron diffuses from the steel substrate into the liquid coating, so that the corrosion protection coating of the flat steel product has, in particular, an alloy layer and an Al base layer upon solidification.
[0054] In a particular embodiment, the phosphated flat steel product according to the invention is characterized in that the alloy layer consists of Fe: 35% - 90%,
[0055] Si: 0.1% - 10%, optionally up to 0.5% Mg and optional further components, the total contents of which are limited to a maximum of 2.0%, and the remainder being aluminium and the Al base layer consisting of Si: 1.0 - 15%, and optionally Fe: 1 - 4%,
[0056] Mg: up to 0.7%,
[0057] Zn: up to 15% and optional further components, the total contents of which are limited to a maximum of 2.0%, and the remainder being aluminium.
[0058] The alloy layer has one boundary layer to the steel substrate and the other boundary layer to the Al base layer. Due to the diffusion of iron into the coating, iron is enriched in the alloy layer. The alloy layer preferably consists of at least 35% iron. The maximum iron content in the alloy layer is preferably 90%, particularly preferably 55%. The silicon content in the alloy layer is preferably at least 0.1% and in particular a maximum of 10%. Optionally, the alloy layer can contain magnesium. The magnesium content should be limited to 0.5%. A magnesium content of at least 0.1% has proven particularly advantageous. Furthermore, the alloy layer optionally consists of further components whose content is limited to a maximum of 2.0%, with aluminum as the remainder. The optional further components include in particular the optional components of the melt, e.g. zinc.
[0059] The Al base layer directly borders the alloy layer. The composition of the Al base layer preferably corresponds to the composition of the melt. However, diffusion processes can lead to different contents. In a particular embodiment, the silicon content in the Al base layer is at least 1.0%, preferably 7.0%, particularly preferably 9.0%, and the maximum silicon content is 15%, preferably 12%, particularly preferably 10%. Optionally, the proportion of iron in the Al base layer can be 1%, preferably 2%. The maximum proportion of iron should be limited to 4%, particularly preferably 3.5%. Furthermore, magnesium can be present in the Al base layer in proportions of up to 0.7%, preferably 0.4%. In a particular embodiment, the minimum proportion of magnesium in the Al base layer is 0.2%.In addition, the Al base layer may contain zinc with a maximum content of 15%, optionally other components whose total contents are limited to a maximum of 2.0% and the remainder being aluminum.
[0060] To solve this problem, the flat steel product is phosphated. Commercial phosphating solutions such as Gardobond 26 T with the additive H7255 are used. These solutions typically contain zinc, nickel, manganese, phosphoric acid, and fluorides.
[0061] In a particular embodiment, the phosphated flat steel product is characterized in that the degree of coverage with metal phosphates on the surface of the flat steel product is at least 10%, preferably 25%, particularly preferably 30%. In a further particular embodiment, if the flat steel product is a sheet metal blank during the application of the phosphating solution, the degree of coverage is at least 72%, preferably 80%, particularly preferably 85%. In another embodiment, for process-related reasons, the degree of coverage can be limited to a maximum of 90%, preferably 79%, particularly preferably 72%, if the flat steel product is a rolled product during the application of the phosphating solution.
[0062] The high coverage promotes homogeneous heating of the flat steel product to the forming temperature. At a lower coverage, local temperature differences may occur briefly during heating, as the local reflectivity in areas not covered with metal phosphates is lower than in those covered with metal phosphates. Furthermore, a high coverage on the flat steel product ensures that the hot-formed component is fully phosphated.
[0063] The pH of the phosphating solution is at least 2.0, preferably 2.5, more preferably 2.8, and at most 3.5, preferably 3.4, more preferably 3.3, especially 3.2. If the pH is too low, a continuous phosphating layer cannot be formed because the pH change on the surface is insufficient for crystallization. If the pH is too high, the solution is unstable, and metal phosphates precipitate, and no continuous layer is formed. This can lead to pickling attack on the surface. The zinc concentration in the phosphating solution is at least 1 g / l. The maximum zinc concentration is 15 g / l. The nickel concentration in the phosphating solution is at least 0.5 g / l and at most 10 g / l.
[0064] In a particular embodiment, the zinc concentration and / or the nickel concentration can be increased by adding water-soluble salts, so that the sum of the zinc concentration and the nickel concentration in the phosphating solution is at least 2.4 g / l, preferably at least 7.5 g / l, particularly preferably at least 7.8 g / l. The nickel concentration in the phosphating solution after the optional addition is at least 4 g / l, preferably 5 g / l, particularly preferably at least 6 g / l. The increased zinc concentration and / or nickel concentration results in the zinc phosphate coating weight (or nickel phosphate coating weight) increasing by at least 100% for the same phosphating time. Conversely, shorter phosphating times are required to obtain a continuous phosphating layer, thus enabling a higher throughput during phosphating.
[0065] Fluorides are present in the phosphating solution at a concentration of at least 0.5 g / l F-. In a particular embodiment, the fluoride concentration is at least 1.25 g / l F-, preferably 1.66 g / l F-, which leads to an increase in the layer weight of at least 100% compared to phosphating with lower fluoride concentrations. The fluoride content in the present invention is a maximum of 3.8 g / l F-, preferably 3 g / l F-, particularly preferably 2.7 g / l F-.
[0066] In particular, the phosphating solution may contain oxidizing agents such as dimethyl sulfoxide or nitrates. In a particular embodiment, the nitrate concentration is at least 3 g / l, preferably at least 10 g / l, particularly preferably at least 12 g / l. Increasing the nitrate concentration reduces hydrogen evolution during the phosphating step, allowing a more homogeneous phosphating layer to form.
[0067] In a particular embodiment, polyethylene glycol can be added to the phosphating solution as an additive. If the concentration is increased to at least 0.05 g / l, especially 0.1 g / l, the layer weight also increases for the same phosphating time. The concentration should be limited to 5 g / l, especially 1 g / l, since excessively high concentrations have negative effects on the phosphating quality. Optionally, copper can be added to the phosphating solution. The copper can be added in the form of water-soluble copper salts, especially copper carbonate and / or copper nitrate. The copper concentration in the phosphating solution is then at least 0.01 g / l, preferably 0.05 g / l. It is known from the prior art that AS surfaces contain regions that exhibit near-surface Si-rich phases.In these areas, the Si-rich phases act as crystallization sites, as they function as so-called microcathodes. The addition of copper also allows the copper particles to act as additional microcathodes. These additional microcathodes are now also located between the areas with the Si-rich phases on the surface. This leads to the formation of a more homogeneous phosphating layer and shorter phosphating times are sufficient for complete phosphating. The copper addition should be limited to a maximum concentration of 0.5 g / l, since at higher concentrations, Cu deposition prevents effective phosphate deposition. In particular, the copper addition should be limited to a maximum of 0.1 g / l for resource reasons.
[0068] The flat steel product according to the invention has a reflectance R in the infrared range of < 0.65, preferably < 0.55, in particular < 0.40, preferably < 0.35. The lower the reflectance of the surface, the less strongly the surface reflects. This means that more heat can be absorbed into the flat steel product. Therefore, a low reflectance has a positive effect on the heating rate.
[0069] The degree of reflection is adjusted during the production of the flat steel product.
[0070] The method for producing a phosphated flat steel product comprises the following steps: a) Providing a previously described steel substrate b) Hot-dip coating the steel substrate with an aluminum-based corrosion protection coating, wherein the corrosion protection coating comprises an alloy layer and an Al base layer c) Temper rolling the flat steel product d) Optionally cleaning the flat steel product e) Optionally activating the flat steel product f) Phosphating the flat steel product with a phosphating solution g) Optionally alkaline cleaning the flat steel product h) Optionally oiling the flat steel product
[0071] In step a), a steel substrate according to the invention with the specified alloy is provided. The steel substrate is manufactured using conventional methods. One possible embodiment is the following:
[0072] First, a slab or thin slab is provided, which can be produced by continuous slab casting or thin slab casting. This slab or thin slab is soaked, optionally pre-rolled, hot-rolled, and optionally coiled. The steel substrate is then descaled, optionally cold-rolled, and optionally annealed.
[0073] In step b), the steel substrate is hot-dip coated with a corrosion protection coating. Hot-dip coating is preferably carried out in a continuous process.
[0074] In step c), the flat steel product is skin-passed to improve the surface roughness. According to the invention, skin-pass degrees of up to 3%, preferably up to 2%, are achieved.
[0075] In step d), the steel flat product is optionally cleaned. Whether this step is necessary depends on the strip cleanliness and the skin-passing agents used. In a special embodiment, cleaning can be performed with a solution containing sodium hydroxide and water as its main components.
[0076] In step e), the flat steel product can optionally be activated. The activation solution results in more nucleation nuclei being present on the surface for subsequent phosphating. The activation solution preferably consists of zinc phosphates, as this allows a higher zinc phosphate coating to be achieved after the subsequent phosphating compared to activations using other phosphate compounds, such as titanyl phosphates. Commercially available activation solutions can be used, such as the activation agents ZL 6 or V6513, in particular V6559 from Chemetall. The activation concentration used is at least 1 g / l, in particular at least 3 g / l, in order to apply sufficient nucleation nuclei to the surface. No significant improvement was observed above a concentration of 10 g / l; therefore, the activation concentration is limited to 10 g / l.To further conserve resources, the activation bath concentration is, in particular, a maximum of 5 g / l. In step f), the flat steel product is phosphated with a phosphating solution, in particular with one of the phosphating solutions previously discussed as advantageous.
[0077] In step g), the steel flat product is optionally cleaned with alkali. Alternatively, the steel flat product can also be rinsed. This cleaning step can serve to reduce the fluoride content on the surface. This reduction may be desired to prevent the formation of a toxic HF atmosphere during hot forming.
[0078] In step h) the flat steel product is optionally oiled.
[0079] A hot-formed component can be produced from the phosphated flat steel product. The following process steps are necessary: a) Provision of a previously described flat steel product; b) Optionally, cutting a sheet blank from the flat steel product and optionally further processing; c) Heating the sheet blank such that the AC3 temperature of the blank is at least partially exceeded and the temperature T Einig the blank when placed in a forming tool intended for hot press forming (working step d)) at least partially has a temperature above Ms+100 °C, where Ms is the martensite start temperature; d) placing the heated sheet metal blank in a forming tool, wherein the transfer time t required for removing the blank from the heating device and placing it in the forming tool Trans is at most 20 s, preferably at most 15 s; e) hot-press forming the sheet metal blank to form the sheet metal part, wherein the blank is subjected to a heat treatment during the hot-press forming process for a period t wz of more than 1 s with a cooling rate r of at least partially more than 30 K / s w to the target temperature T Ziei cooled and optionally held there; f) removing the sheet metal part cooled to the target temperature from the tool.
[0080] To produce the hot-formed component according to the invention, the previously described flat steel product is provided in step a). If the flat steel product is a rolled product, it can optionally be divided into sheet blanks in step b) and optionally undergo further processing that does not involve hot forming, e.g., punching, etc. If the flat steel product in step a) already consists of sheet blanks, step b) is omitted.
[0081] To produce the hot-formed component according to the invention, the flat steel product prepared in step a) is heated at least partially to AC3 temperature in step c). In addition, the temperature T Einigof the blank when placed in a forming tool intended for hot press forming (working step d)) must at least partially have a temperature above Ms+100 °C. For the purposes of this application, partially exceeding a temperature (here AC3 or Ms+100 °C) means that at least 30%, in particular at least 60%, of the volume of the blank exceeds a corresponding temperature. When placed in the forming tool, at least 30% of the blank therefore has an austenitic structure, i.e. the transformation from the ferritic to the austenitic structure does not have to be complete when placed in the forming tool. Rather, up to 70% of the volume of the blank when placed in the forming tool can consist of other structural components, such as tempered bainite, tempered martensite and / or non- or partially recrystallized ferrite.For this purpose, certain areas of the blank can be kept at a lower temperature than others during heating. To do this, the heat can be specifically directed only at certain sections of the blank, or the parts that are to be heated less can be shielded from the heat supply. In the part of the blank material whose temperature remains lower, no or only significantly less martensite is formed during forming in the tool, so that the microstructure there is significantly softer than in the other parts that have a martensitic microstructure. In this way, a softer area can be specifically set in the formed sheet metal part, for example by ensuring optimal toughness for the respective intended use, while the other areas of the sheet metal part have maximized strength.
[0082] Maximum strength properties of the resulting sheet metal part can be achieved by ensuring that the temperature reached at least partially in the sheet metal blank is between AC3 and 1000 °C, preferably between 850 °C and 950 °C.
[0083] An optimally uniform distribution of properties can be achieved by heating the blank thoroughly in step c). In a preferred embodiment, the average heating rate is r O f e n of the sheet metal blank during heating in step c) is at least 5 K / s, preferably at least 11 K / s, in particular at least 15 K / s. The average heating rate r O f e n is to be understood as the average heating rate from 30 °C to 700 °C.
[0084] The heating rate depends particularly on the sheet thickness. Therefore, in a preferred embodiment, the product of heating rate and sheet thickness in the temperature range from 30 °C to 700 °C is greater than or equal to 12 (K*mm) / s, preferably greater than or equal to 15 (K*mm) / s, particularly preferably greater than or equal to 18 (K*mm) / s.
[0085] In a particular embodiment, the average heating rate in the temperature range 500 °C to 750 °C is lower than the average heating rate in the temperature range 30 °C to 700 °C. In particular, the average heating rate in the range 500 °C to 750 °C is >7 K / s, preferably >9 K / s, particularly preferably >10 K / s.
[0086] Phosphating the steel substrate increases the product of average heating rate and sheet thickness compared to a non-phosphated steel substrate. The metal phosphate layer changes the surface reflectivity. The improvement in the heating rate compared to a non-phosphated steel sheet is at least 40%, preferably 60%, particularly preferably 70%, especially 80%. The improvement in the heating rate is defined as (heating rate phosphated - heating rate unphosphated) / heating rate unphosphated, with all other parameters remaining unchanged. This makes it possible to perform hot forming with lower energy consumption.
[0087] Preferably, the dew point in the furnace during the hot forming step is at least -20 °C, preferably at least -15 °C, in particular at least -5 °C, particularly preferably at least 0 °C, in particular at least 5 °C and a maximum of +25 °C, preferably a maximum of +20 °C, in particular a maximum of +15 °C. In a particular embodiment, the atmosphere in the furnace consists of air, ie 19-22 vol.% oxygen and 77-79 vol.% nitrogen and unavoidable air components (e.g. noble gases).
[0088] In a special embodiment, the heating in step c) takes place stepwise in areas with different temperatures. In particular, the heating takes place in a roller hearth furnace with different heating zones. Here, the heating takes place in a first heating zone at a temperature (so-called furnace inlet temperature) of at least 650 °C, preferably at least 680 °C, in particular at least 720 °C. The maximum temperature in the first heating zone is preferably 900 °C, in particular a maximum of 850 °C. Furthermore, the maximum temperature of all heating zones in the furnace is preferably a maximum of 1200 °C, in particular a maximum of 1000 °C, preferably a maximum of 950 °C, particularly preferably a maximum of 930 °C.
[0089] The total time in the oven t OThe furnace time, which consists of a heating time and a holding time, is preferably at least 2 minutes, in particular at least 3 minutes, and preferably at least 4 minutes for both variants (constant furnace temperature, stepwise heating). Furthermore, the total time in the furnace for both variants is preferably a maximum of 20 minutes, in particular a maximum of 15 minutes, preferably a maximum of 12 minutes, and in particular a maximum of 8 minutes. Longer total times in the furnace have the advantage of ensuring uniform austenitization of the sheet metal blank. On the other hand, holding for too long above AC3 leads to grain coarsening, which has a negative effect on the mechanical properties.
[0090] The blank heated in this way is removed from the respective heating device, which can be, for example, a conventional heating furnace, an equally known induction heating device or a conventional device for keeping steel components hot, and transported into the forming tool so quickly that its temperature upon arrival in the tool is at least partially above Ms+100 °C, preferably above 600 °C, in particular above 650 °C, particularly preferably above 700 °C. Here, Ms denotes the martensite start temperature. In a particularly preferred variant, the temperature is at least partially above the ACl temperature. In all of these variants, the temperature is in particular a maximum of 900 °C. These temperature ranges ensure good formability of the material overall.
[0091] In step d), the transfer of the austenitized blank from the heating device used to the forming tool is completed within preferably a maximum of 20 seconds, in particular within a maximum of 15 seconds. Such rapid transport is necessary to avoid excessive cooling prior to forming.
[0092] In step e), the sheet metal blank is hot-pressed into a sheet metal part. When the blank is inserted, the tool typically has a temperature between room temperature (RT) and 200 °C, preferably between 20 °C and 180 °C, in particular between 50 °C and 150 °C. Optionally, in a special embodiment, the tool can be tempered at least in some areas to a temperature Twz of at least 200 °C, in particular at least 300 °C, in order to only partially harden the component. Furthermore, the tool temperature T Wz preferably a maximum of 600 °C, especially a maximum of 550 °C. It is only necessary to ensure that the tool temperature T W z below the desired target temperature T Z iei. In step d), the sheet metal blank is partially subjected to a cooling rate r of more than 30 K / s wz to the target temperature T Ziei cooled and optionally held there. The residence time in the tool t wz is more than 1 s, preferably at least 2 s, in particular at least 3 s, particularly preferably at least 5 s. The maximum residence time in the tool is preferably 25 s, in particular a maximum of 20 s.
[0093] The target temperature T Ziei of the sheet metal part is at least partially below 400 °C, preferably below 300 °C, in particular below 250 °C, preferably below 200 °C, particularly preferably below 180 °C, in particular below 150 °C. Alternatively, the target temperature T Zieiof the sheet metal part is particularly preferably below Ms-50 °C, where Ms denotes the martensite start temperature. Furthermore, the target temperature of the sheet metal part is preferably at least 20 °C, particularly preferably at least 50 °C.
[0094] The phosphating layer on the flat steel product acts as a forming aid during hot press forming. The phosphate crystals serve as an additional slip surface.
[0095] In step f) the sheet metal part is removed from the tool and cooled to the target temperature.
[0096] In a particular embodiment, the resulting component can be further phosphated using conventional methods. Optionally, activation can take place before the phosphating step. This step may be necessary if a continuous phosphating layer, i.e., a coverage of >99%, is required for the technical application. In the further optional phosphating step of the component, the zinc phosphates can also serve as additional crystallization nuclei. This makes it possible to achieve a denser phosphate layer on the AS surface compared to a non-inventive component without a phosphated flat steel product. A non-phosphated flat steel product forms a dense, continuous oxide layer on the surface after hot forming, so that subsequent large-area phosphating is hardly possible.In the subject matter of the invention, it is helpful for a good subsequent phosphating if the degree of coverage with metal phosphate crystals from the phosphating is as high as possible.
[0097] The hot-formed component obtained, comprising a flat steel substrate with the composition according to the invention and an anti-corrosive coating, wherein the anti-corrosive coating is aluminum-based and has an alloy layer and an Al base layer, is characterized in that the degree of coverage with metal phosphates on the surface is preferably at least 10%, in particular 25%, particularly preferably 30%. In a further particular embodiment, if the flat steel product is a sheet metal blank during the application of the phosphating solution, the degree of coverage is at least 72%, preferably 80%, particularly preferably 85%. In another embodiment, for process-related reasons, the degree of coverage can be limited to a maximum of 90%, preferably 79%, particularly preferably 72%, if the product is a rolled product during the application of the phosphating solution.However, 100% coverage is technically impossible to achieve. Due to the high degree of coverage after hot forming, a further phosphating step may not be necessary.
[0098] In a particular embodiment, the hot-formed component is characterized in that the alloy layer consists of
[0099] Fe: 35 - 90%,
[0100] Si: 0.1 - 10%, optionally up to 0.5% Mg, and optional further components, the total contents of which are limited to a maximum of 2.0%, and the remainder being aluminium and the Al base layer comprising silicon-poor and silicon-rich phases, whereby for the silicon contents in the phases in relation to the average value of the silicon content in the Al base layer Si ai applies:
[0101] Low S < 0.8 * Si ai
[0102] String 1<2 * Si aiIn particular, phosphating before hot forming causes a change in the Al base layer after hot forming, which lies directly beneath the oxide layer. The change in the alloy layer, in contrast, is minimal. Preferably, the alloy layer after hot forming should have the same composition as before hot forming. Only the thickness of the alloy layer has increased during hot forming. The alloy layer after hot forming preferably consists of at least 35% iron. The maximum iron content in the alloy layer is preferably 90%, particularly preferably 55%. The silicon content in the alloy layer after hot forming is preferably at least 0.1% and at most 10%. Optionally, the alloy layer can contain magnesium. The magnesium content should be limited to 0.5%. A magnesium content of at least 0.1% has proven particularly advantageous.Furthermore, after hot forming, the alloy layer optionally consists of additional components, the content of which is limited to a maximum of 2.0%, with aluminum as the remainder. The optional additional components include, in particular, the optional components of the melt, e.g., zinc.
[0103] Phosphating changes the layer structure of the Al base layer. In the case where hot forming takes place without phosphating of the flat steel product, a five-layer structure of Si-rich and Si-poor phases is known from the prior art. In the present invention, the Si-rich phase is more discrete. Discrete means that the Si-rich phases have a lower permeability. After hot forming, the Al base layer comprises silicon-poor and silicon-rich phases, with the silicon contents in the phases in relation to the average value of the silicon content in the Al base layer being ai applies:
[0104] ^poor < 0.8 * Si ai String 1<2 * Si ai
[0105] In particular, silicon-rich phases are arranged within the silicon-poor phase and / or the silicon-rich phases have a permeability of at most 90% and are in particular delimited by silicon-poor regions. In a particular embodiment, the permeability is at most 75%, particularly preferably at most 65%.
[0106] During hot forming, an oxide layer forms on the Al base layer. This oxide layer is a mixture of different oxide types. The oxides formed depend on the composition of the corrosion protection coating. The free reaction enthalpy required to form typical Al oxides, e.g., Al2O3, is lower than that of typical silicon oxides, e.g., Si2O3, at hot forming temperatures. Therefore, a large part of the outer oxide layer consists of Al oxides. These are formed by the diffusion of aluminum to the surface, where the aluminum reacts with the oxygen from the environment. The formation of this oxide layer in the present invention is disrupted by the metal phosphates on the surface during hot forming. As a result, a small proportion of aluminum from the Al base layer can diffuse to the surface, leaving a larger proportion of aluminum in the Al base layer.Due to this increased proportion of aluminum, the silicon-rich phases cannot form a continuous layer, as is known from the state of the art for hot-formed components without prior phosphating of the flat steel product.
[0107] The Si-rich phases with lower permeability ensure that more aluminum remains in the Al base layer. This leaves more free aluminum available in the Al base layer in the event of damage to the component's surface. This free aluminum diffuses to the surface and re-forms an external aluminum oxide layer, thus protecting the component against corrosion.
[0108] The invention is explained in more detail below using exemplary embodiments.
[0109] To test the invention, a flat steel product with the composition shown in Table 1 was chosen.
[0110] This flat steel product was hot-dip coated with different corrosion protection coatings (a) and (g) using standard methods (see Table 2). The melt analyses for each sample are given in weight percent. The coating thickness on one side is also indicated.
[0111] The rolled product was then phosphated directly as a coil and then cut into sheet metal blanks, or the rolled product was first cut into sheet metal blanks and then phosphated. The resulting sheet metal blanks each measured 200x300 mm. The respective procedures can be found in the "Process" column in Table 4.
[0112] For phosphating, different phosphating solutions were tested according to Table 3. For the present invention, zinc, nickel, copper, polyethylene glycol, nitrate, and fluoride concentrations proved particularly favorable with regard to coating thickness at the same contact time. Various phosphating variants with different phosphating times / contact times are shown in Table 3.
[0113] Table 4 shows the different phosphating variants in combination with the different alloy variants. Example 0 is a non-inventive example. In Example 0, the flat steel product was not phosphated. Therefore, only a reflectance of 0.68 was achieved. In Example 19, the hot forming step was not performed.
[0114] In Examples 1-18 according to the invention, lower reflectances were measured compared to the examples according to the invention. The respective coverage was determined before hot forming (WUF) and after hot forming using a scanning electron microscope. The coverage can be found in Table 4. The coverages for the rolled products are lower (Examples 2-13) than the coverages for the sheet blanks (Examples 14-18).
[0115] In order to hot-form the sheet metal blanks, they were heated to a furnace temperature T O f en heated and over a total time t O f enThe furnace temperature and total time are listed in Table 5. The heating rate in the temperature range 30 °C to 700 °C as a function of sheet thickness is listed in Table 6. Different values result depending on the phosphating solution. In addition, the heating rate was determined in the range 30 °C to 700 °C and in the range 500 °C to 100 °C. Both are shown in Table 6.
[0116] The heated sheet metal blanks were then placed into a forming tool with a maximum transfer time of 15 seconds. At least some of the sheet metal blanks had a temperature above Ms+100 °C. The forming tool was heated to room temperature. The sheet metal blanks were formed in the forming tool. The formed sheet metal blanks were then cooled to room temperature within 20 seconds and removed from the tool.
[0117] In addition, the increase in heating rate compared to a phosphated flat steel product was determined using (heating rate_phosphated - heating rate_unphosphated) / heating rate_unphosphated. The heating rate of reference example 0 was chosen as the unphosphated heating rate.
[0118] The Si phases were determined on the cross-section using scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDX). The permeability of the Si phase was determined using
[0119] Three scanning electron micrographs were used. When creating a cross-section, the samples are embedded in commercially available polymer mass as standard. To determine the patency, the patency was measured for all three images, and the average value was calculated. Variant 19 has a patency greater than 90%. The inventive variants 1-18 have patencies <75%.
[0120] Table 1 (Composition of steel substrate in wt.%)
[0121]
[0122] Table 2 (Corrosion protection coating variants)
[0123]
[0124] Table 3 (Phosphating variants)
[0125]
[0126] Table 4 (test program) (underlined variants are counterexamples)
[0127] Data partially rounded Table 5 (Hot forming parameters)
[0128]
[0129] Table 6 (heating properties) (underlined variants are counterexamples) The invention is explained in more detail below with reference to the figures.
[0130] Figure 1 shows a schematic cross-section of the hot-formed component without prior phosphating. The figure is intended as a reference. On the steel substrate (1) there is an alloy layer (2) and on the alloy layer there is the Al base layer (3) with the Si-rich phases (4). The Si-rich phases border one another and this forms a 5-layer layer consisting of Al base layer / layer of Si-rich phases / Al base layer / layer of Si-rich phases / Al base layer. An oxide layer (5) is located on the 5-layer structure. Figure 2 shows a schematic view of the hot-formed component according to the invention. The layer structure also shows the alloy layer (2) on the steel substrate (1). The Si-rich phases (4) are not bonded to one another and are embedded in the Al base layer (3). On the surface there is an oxide layer with phosphorus (6).Figure 3 shows an SEM image of the surface of the steel compartment product according to the invention at different magnifications.
Claims
Patent claims 1. Phosphated flat steel product comprising a steel substrate and a corrosion protection coating, wherein the steel substrate contains, in addition to iron and unavoidable impurities from C: 0.04% - 0.45%, Mn: 0.5% - 2.6%, Si: 0.02% - 1.2%, AI: 0.02 - 1.0%, P: < 0.05%, S: < 0.02%, and optionally one or more of the following elements with the contents: Ti: 0.01% - 0.08%, Nb: 0.02% - 0.08%, B: 0.001% - 0.005%, Cr: 0.08% up to 1.0%, Mo: < 0.5%, Ni: < 0.5%, Cu: < 0.2%, V: < 0.1%, and wherein the anti-corrosive coating is aluminum-based and has an alloy layer and an Al base layer, characterized in that the reflectance R in the infrared range is < 0.
65.
2. Phosphated flat steel product according to claim 1, characterized in that the degree of coverage with metal phosphates on the surface of the flat steel product is at least 10%.
3. Phosphated flat steel product according to claim 1 and / or claim 2, characterized in that the alloy layer consists of Fe: 35% - 90%, Si: 0.1% - 10%, optionally up to 0.5% Mg and optional further components, the total contents of which are limited to a maximum of 2.0%, and the remainder being aluminum and the Al base layer consisting of Si: 1.0% - 15%, and optionally Fe: 1% - 4%, Mg: up to 0.7%, Zn: up to 15% and optional further components, the total contents of which are limited to a maximum of 2.0%, and the remainder being aluminium.
4. A method for producing a phosphated flat steel product, comprising the following steps: a) providing a steel substrate having the composition according to claim 1, b) hot-dip coating the steel substrate with an aluminum-based corrosion protection coating, wherein the corrosion protection coating has an alloy layer and an Al base layer, c) temper rolling the flat steel product, d) optionally cleaning the flat steel product, e) optionally activating the flat steel product, f) phosphating the flat steel product with a phosphating solution, g) optionally alkaline cleaning the flat steel product, h) optionally oiling the flat steel product.
5. Process according to claim 4, characterized in that the pH of the phosphating solution is at least equal to 2 and at most 3.
5.
6. Process according to claim 4 and / or 5, characterized in that the sum of the zinc concentration and the nickel concentration in the phosphating solution is at least 2.4 g / l.
7. Process according to claims 4 to 6, characterized in that the copper concentration in the phosphating solution is at least 0.01 g / l.
8. The hot-formed component obtained comprising a flat steel substrate with the composition according to the invention and a corrosion protection coating, wherein the corrosion protection coating is aluminum-based and has an alloy layer and an Al base layer, is characterized in that the degree of coverage with metal phosphates on the surface is at least 10%.
9. Hot-formed component according to claim 8, characterized in that the alloy layer consists of Fe: 35% - 90%, Si: 0.1% - 10%, optionally up to 0.5% Mg, and optional further components, the total contents of which are limited to a maximum of 2.0%, and the remainder being aluminium and the Al base layer comprising silicon-poor and silicon-rich phases, whereby for the silicon contents in the phases in relation to the average value of the silicon content in the Al base layer Si ai applies: Low S < 0.8 * Si ai String 1<2 * Si ai 10. Hot-formed component according to one of claims 8 to 9, characterized in that the silicon-rich phases are arranged within the silicon-poor phase and / or the silicon-rich phases have a permeability of at most 90% and are delimited in particular by silicon-poor regions.
11. A method for producing a hot-formed component, comprising the following steps: a) providing a flat steel product according to one of claims 1 to 3; b) Optionally separating a sheet blank from the flat steel product and optionally further processing; c) Heating the sheet blank in such a way that the AC3 temperature of the blank is at least partially exceeded and the temperature T Einig the blank when placed in a forming tool intended for hot press forming (working step d)) at least partially has a temperature above Ms+100°C, where Ms denotes the martensite start temperature; d) placing the heated sheet metal blank in a forming tool, wherein the transfer time t required for removing the blank from the heating device and placing it in the forming tool Tr ans is at most 20 s; e) hot-press forming the sheet metal blank to form the sheet metal part, wherein the blank is subjected to a heat treatment during the hot-press forming process for a period t wz of more than 1 s with a cooling rate r of at least partially more than 30 K / s w to the target temperature T Zieicooled and optionally held there; f) removing the sheet metal part cooled to the target temperature from the tool.
12. The method according to claim 11, characterized in that in step c) in the temperature range 30 °C to 700 °C the product of the average heating rate and the sheet thickness is greater than or equal to 12 (K*mm) / s.
13. A method according to any one of claims 11 to 12, characterized in that the average heating rate in the temperature range 500 °C to 750 °C is lower than the average heating rate in the temperature range 30 °C to 700 °C.
14. Method according to one of claims 10 to 13, characterized in that the hot forming is followed by a phosphating step with an optional prior activation.
Citation Information
Patent Citations
Flat steel product and method for producing a flat steel product
WO2012120081A2
Method for producing a steel component having a metal coating protecting it against corrosion, and steel component
WO2015036151A1
Aluminum-plated steel plate with tensile strength of 1800 MPa, manufacturing method thereof and hot forming part
CN111424212A
Al-plated hot-stamped steel material
CN115443350A
Pretreatment of aluminum-based metal sheet for press forming and coating
JP1992254587A