Template substrate for semiconductor growth, semiconductor substrate, method and device for manufacturing template substrate for semiconductor growth, and method and device for manufacturing semiconductor substrate
The template substrate with a modified base layer facilitates lateral growth of nitride semiconductor crystals, reducing defects and enhancing aspect ratios, addressing the limitations of conventional semiconductor growth methods.
Patent Information
- Application Number
- PCT/JP2023/012079
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional semiconductor growth methods using mask patterns lead to high defect densities in nitride semiconductor layers and restrict the aspect ratio of semiconductor parts, making it difficult to design devices with large dimensions and high-quality films.
A template substrate with a modified base layer featuring a growth suppression region and a seed region is used, where the growth suppression region is modified with higher impurity concentrations and different crystal structures, allowing lateral growth of nitride semiconductor crystals without a mask pattern, thereby reducing defects and enhancing the aspect ratio of semiconductor parts.
This approach results in high-quality nitride semiconductor layers with reduced defect density and increased aspect ratio, enabling the formation of semiconductor parts with greater design freedom and improved film quality.
Smart Images

Figure JP2023012079_03102024_PF_FP_ABST
Abstract
Description
Semiconductor growth template substrate, semiconductor substrate, method and apparatus for manufacturing a semiconductor growth template substrate, and method and apparatus for manufacturing a semiconductor substrate
[0001] The present disclosure relates to template substrates for semiconductor growth, etc.
[0002] A mask pattern that prevents the growth of a nitride semiconductor layer is formed on a base substrate including a heterogeneous substrate and a seed layer, and the nitride semiconductor layer is grown laterally on the mask portion, starting from the seed layer exposed in the opening where there is no mask portion, thereby reducing the defect density of the nitride semiconductor layer on the mask portion (Patent Document 1).
[0003] Japanese Patent Publication No. 2013-251304
[0004] The semiconductor growth template substrate according to the present disclosure comprises a main substrate and a base layer located above the main substrate and containing a base material, and the surface of the base layer includes a growth-inhibition region in which the base material is modified and a seed region in which the base material is not modified.
[0005] FIG. 1 is a plan view showing the configuration of a template substrate according to the present embodiment; FIG. 2 is a cross-sectional view showing the configuration of a template substrate according to the present embodiment; FIG. 3 is a flowchart showing a method for manufacturing a template substrate according to the present embodiment; FIG. 4 is a block diagram showing a manufacturing apparatus for a template substrate according to the present embodiment; FIG. 5 is a flowchart showing a method for manufacturing a template substrate; FIG. 6 is a cross-sectional view showing a method for manufacturing a template substrate; FIG. 7 is a cross-sectional view showing a configuration of a template substrate according to the present embodiment; FIG. 8 is a cross-sectional view showing a configuration of a template substrate according to the present embodiment; FIG. 9 is a cross-sectional view showing a configuration of a template substrate according to the present embodiment; FIG. 10 is a cross-sectional view showing a method for manufacturing a template substrate; FIG. 11 is a cross-sectional view showing a configuration of a semiconductor substrate according to the present embodiment; FIG. 12 is a cross-sectional view showing a configuration of a semiconductor substrate according to the present embodiment; FIG. 13 is a cross-sectional view showing a configuration of a semiconductor substrate according to the present embodiment; FIG. 14 is a flowchart showing a method for manufacturing a semiconductor substrate according to the present embodiment; FIG. 15 is a block diagram showing an apparatus for manufacturing a semiconductor substrate according to the present embodiment; FIG. 16 is a flow chart showing a method for manufacturing a semiconductor substrate according to the present embodiment; FIG. 17 is a cross-sectional view showing a method for manufacturing a semiconductor substrate according to the present embodiment; FIG. 18 is a cross-sectional view showing a configuration of a semiconductor substrate according to the present embodiment; FIG. 19 is a cross-sectional view showing a configuration of a semiconductor substrate according to the present embodiment; FIG. 19 is a cross-sectional view showing a configuration of a semiconductor substrate according to the present embodiment; 1 is a cross-sectional view showing an example of the configuration of an electronic device according to an embodiment of the present invention.
[0006] (Semiconductor Growth Template Substrate) A semiconductor growth template substrate according to this embodiment will be described. Hereinafter, the semiconductor growth template substrate will be simply referred to as the template substrate. FIG. 1 is a plan view showing the configuration of the template substrate according to this embodiment. FIG. 2 is a cross-sectional view showing the configuration of the template substrate according to this embodiment. As shown in FIGS. 1 and 2 , the template substrate TS includes a main substrate 1 and an underlayer 4 located above the main substrate 1 and containing an underlayer material. The surface of the underlayer 4 includes a growth-inhibiting region DA in which the underlayer material is modified and a seed region SA in which the underlayer material is not modified. The modification (surface modification) may involve changing at least one of the contained elements and the crystalline structure of the underlayer surface. The contained elements and at least one of the crystalline structure may differ between the growth-inhibiting region DA and the seed region SA. The growth-inhibiting region DA may be polycrystalline or amorphous. The growth-inhibiting region DA may have a larger amorphous or polycrystalline occupancy than the seed region SA.
[0007] The growth-inhibiting region DA may have a higher impurity concentration than the seed region SA, and this impurity concentration may be an oxygen concentration or an argon concentration. At least one element of oxygen (O), silicon (Si), and carbon (C) incorporated near the surface of the growth-inhibiting region DA (for example, to a depth of about 0 to 5 nm) during the process of forming the growth-inhibiting region DA may enhance the growth-inhibiting function.
[0008] Because the template substrate according to this embodiment does not include a conventional mask pattern, lateral overgrowth (ELO) of a semiconductor portion (e.g., a nitride semiconductor crystal) is facilitated from above the seed region SA (the unmodified region on the surface of the underlayer 4) to above the growth inhibition region DA (the modified region on the surface of the underlayer 4), resulting in a high-quality semiconductor portion (semiconductor layer). Furthermore, depending on the deposition conditions for lateral overgrowth, it is possible to suppress the incorporation of impurities liberated from the mask pattern into the growing semiconductor portion. Excessive incorporation of impurities into the growing semiconductor portion can lead to segregation of the impurities on the surface of the laterally grown semiconductor portion, making it difficult to form an upper layer film on the laterally grown semiconductor portion and causing defects at the interface with the upper layer film. Furthermore, restricting the deposition conditions for lateral overgrowth to avoid these problems can make it difficult to form semiconductor portions with a large aspect ratio (the ratio of width to thickness), thereby reducing the degree of freedom in the shape of the semiconductor portion for device design.
[0009] In this embodiment, a laterally grown, high-quality semiconductor portion (e.g., nitride semiconductor crystal) can be obtained by reducing raw material debris generated from the growth-inhibited region by modifying the underlayer 4 without forming a mask pattern. The aspect ratio of the semiconductor portion can be, for example, 5.0 or more, 10.0 or more, or 20.0 or more.
[0010] 1, the seed region SA may include a first region (first growth initiation region) S1 and a second region (second growth initiation region) S2, and the growth inhibition region DA may be located between the first region S1 and the second region S2. The first region S1 and the second region S2 may be arranged in a stripe pattern.
[0011] The base material that is the main component of the base layer 4 may be a nitride semiconductor, and the main substrate 1 may be a heterogeneous substrate having a lattice constant different from that of the nitride semiconductor. The growth-inhibiting region DA and the seed region SA may be aligned in the a-axis direction of the nitride semiconductor. The width (length in the a-axis direction) of the growth-inhibiting region DA may be five times or more the width (length in the a-axis direction) of the first region S1.
[0012] A nitride semiconductor can be expressed as AlxGayInzN (0≦x≦1; 0≦y≦1; 0≦z≦1; x+y+z=1), for example, and specific examples include GaN-based semiconductors, AlN (aluminum nitride), InAlN (indium aluminum nitride), and InN (indium nitride). A GaN-based semiconductor is a semiconductor containing gallium atoms (Ga) and nitrogen atoms (N), and typical examples include GaN, AlGaN, AlGaInN, and InGaN.
[0013] The underlayer material may be, for example, aluminum nitride, and an aluminum layer (Al layer) may be provided between the main substrate 1 and the underlayer 4, which is an AlN layer. Examples of heterogeneous substrates include silicon substrates, silicon carbide substrates, sapphire substrates, aluminum nitride substrates, and ScAlMgO 4 Examples include a substrate.
[0014] The underlayer material may be AlScN, ScN, ZnO, CrN, or the like, containing a different material (e.g., a metal element other than Group III elements) such as Sc (scandium), Zn, or Cr. The underlayer 4 may have a single-layer structure or a multilayer structure, or may have a multilayer structure including a periodic structure.
[0015] FIG. 3 is a flowchart showing a template substrate manufacturing method according to this embodiment. As shown in FIG. 3 , the template substrate manufacturing method according to this embodiment includes a step S10 of forming an underlayer 4 containing an underlayer material (e.g., aluminum nitride) above a main substrate 1 (e.g., a silicon substrate), and a step S20 of forming, in the underlayer 4, a growth suppression region DA obtained by subjecting the surface underlayer material to a modification treatment, and a seed region SA that has not been subjected to the modification treatment. FIG. 4 is a block diagram showing a template substrate manufacturing apparatus according to this embodiment. The template substrate manufacturing apparatus 30 includes an apparatus M10 that performs step S10 of FIG. 3 , an apparatus M20 that performs step S20 of FIG. 3 , and a control device M15 that controls apparatus M10 and apparatus M20. Apparatus M20 may be a modification treatment apparatus.
[0016] Fig. 5 is a flowchart showing a method for manufacturing a template substrate. Fig. 6 is a cross-sectional view showing a method for manufacturing a template substrate. As shown in Figs. 5 and 6 , step S20 after step S10 of forming an underlayer 4 containing an underlayer material may include step S22 of forming a resist RZ on the underlayer 4, step S24 of patterning the resist RZ, step S26 of performing a plasma treatment on the exposed underlayer material, and step S28 of removing the resist RZ. The underlayer 4 may be formed by a sputtering method.
[0017] In the plasma treatment, for example, argon plasma is irradiated onto the exposed surface 4D of the underlayer 4 to modify the surface of the irradiated region, thereby forming a growth-inhibited region DA. By introducing not only argon gas but also oxygen gas, nitrogen gas, hydrogen gas, or the like into the chamber, the plasma treatment can also use oxygen plasma, nitrogen plasma, hydrogen plasma, or a mixture of these plasmas in addition to argon plasma. As a result, the growth-inhibited region DA may contain argon, oxygen, nitrogen, or the like as impurities. In such a case, the underlayer material may be aluminum nitride, and the growth-inhibited region DA may be aluminum oxynitride. Alternatively, the underlayer material may be AlScN (aluminum scandium nitride), and the growth-inhibited region DA may be AlScON (aluminum scandium oxynitride).
[0018] FIG. 7 is a cross-sectional view illustrating a method for manufacturing a template substrate. As shown in FIG. 7 , the following steps may be performed: patterning a resist RZ on an underlayer 4 (e.g., an AlN layer); forming a coating CM (e.g., a silicon nitride film of approximately 10 nm) covering the underlayer 4 and the resist RZ; removing the resist RZ (lift-off patterning the coating CM); annealing the coating CM and the underlayer 4 (e.g., heat treatment at 1000°C); and removing the coating CM (e.g., removing the silicon nitride film using BHF). In this way, interdiffusion between the coating CM and the underlayer 4 during annealing can form a growth suppression region DA located below the coating CM on the surface of the underlayer 4. Note that by forming the coating CM by sputtering, surface modification below the coating CM can be performed without annealing. The underlayer material may be AlScN, ScN, ZnO, CrN, or the like, containing a different material (e.g., a metal element other than Group III elements) such as Sc (scandium), Zn, or Cr. The underlayer 4 may have a single-layer structure or a multilayer structure, or may have a multilayer structure including a periodic structure.
[0019] FIG. 8 is a cross-sectional view illustrating a method for manufacturing a template substrate. As shown in FIG. 8 , the process may include patterning a resist RZ on an underlayer 4 (e.g., an AlN layer), implanting impurity ions into the exposed underlayer material, and removing the resist RZ. Examples of impurities include silicon (Si), iron (Fe), and magnesium (Mg). The implantation process involves implanting impurity ions into the exposed surface 4D of the underlayer 4 to modify the surface and form a growth suppression region DA. The underlayer material may be AlScN, ScN, ZnO, CrN, or the like, containing a heterogeneous material (e.g., a metal element other than Group III) such as Sc (scandium), Zn, or Cr. The underlayer 4 may have a single-layer structure or a multilayer structure. It may also have a multilayer structure including a periodic structure.
[0020] 9 and 10 are cross-sectional views showing the configuration of the template substrate according to this embodiment. As shown in FIG. 2, the growth inhibition region DA and the seed region SA may be flush with each other. Alternatively, as shown in FIGS. 9 and 10, the seed region SA (first and second regions S1 and S2) may be located above the growth inhibition region DA (planar region). This facilitates lateral growth of semiconductor from the seed region SA to above the growth inhibition region DA, compared to conventional cases in which the seed surface is located below the upper surface of the mask pattern. For example, as shown in FIG. 9, the base layer 4 may be configured such that the portion including the first region S1 is thicker than the portion including the growth inhibition region DA, i.e., the portion directly below the first region S1 (the portion overlapping the first region S1 in plan view) is thicker than the portion directly below the growth inhibition region DA (the portion overlapping the growth inhibition region DA in plan view). Furthermore, as shown in FIG. 10, the main substrate 1 may have a protrusion Q protruding upward, and the first region S1 may be located on the protrusion Q.
[0021] The underlayer material may be AlScN, ScN, ZnO, CrN, or the like, containing a different material (e.g., a metal element other than Group III elements) such as Sc (scandium), Zn, or Cr. The underlayer 4 may have a single-layer structure or a multilayer structure, or may have a multilayer structure including a periodic structure.
[0022] The growth-inhibited region DA formed by the surface modification process may have a thickness (t) that satisfies 0 < thickness (t) ≦ 100 nm or 0 < thickness (t) ≦ 20 nm. In this case, the surface closer to the main substrate 1 (lower surface) may have a higher impurity concentration than the surface farther from the main substrate 1 (upper surface).
[0023] 11 is a cross-sectional view showing the configuration of the template substrate according to this embodiment. As shown in FIG. 11, the base layer 4 may include a buffer layer 4B located on the main substrate 1 side and a seed layer 4S located on the surface side. For example, a silicon substrate may be used as the main substrate 1, an Al layer as the buffer layer 4B, and an AlN layer as the seed layer 4S. Alternatively, a silicon substrate may be used as the main substrate 1, an AlN layer as the buffer layer 4B, and a GaN-based semiconductor layer as the seed layer 4S.
[0024] 12 is a cross-sectional view showing the configuration of a template substrate according to this embodiment. As shown in FIG. 12 , the template substrate TS includes a main substrate 1 and an underlayer 4 located on the main substrate 1, and includes a seed region SA located on the surface of the underlayer and a growth inhibition region DA located on the surface of the main substrate and formed by modifying the main substrate material. The main substrate 1 may be a silicon substrate or a silicon carbide substrate. The growth inhibition region may include a silicon thermal oxide film. The main substrate 1 may be an AlN substrate or a sapphire substrate.
[0025] 13 is a cross-sectional view showing a method for manufacturing a template substrate. As shown in FIG. 13 , a step of patterning an underlayer 4 (e.g., an AlN layer) using, for example, resist RZ on a main substrate 1 (e.g., a silicon substrate or a silicon carbide substrate) and a step of performing a thermal oxidation treatment on the exposed main substrate surface may be performed. The underlayer 4 may be covered with resist RZ during the thermal oxidation treatment. In the thermal oxidation treatment, the exposed surface of the main substrate 1 is modified (oxidized) to form a thermal oxide film, thereby forming a growth inhibition region DA. The growth inhibition region DA may also be formed by nitriding treatment instead of thermal oxidation treatment.
[0026] 14 is a cross-sectional view showing a method for manufacturing a template substrate. As shown in FIG. 14, a step of patterning an underlayer 4 (e.g., an AlN layer or a GaN-based semiconductor layer) on a main substrate 1 (e.g., a silicon carbide substrate, a sapphire substrate, or an AlN substrate) and a step of subjecting the exposed surface of the main substrate to plasma treatment may be performed. In the plasma treatment, the exposed surface of the main substrate 1 is modified to form a growth inhibition region DA. The growth inhibition region DA may also be formed by implanting impurity ions instead of the plasma treatment.
[0027] (Semiconductor Substrate) FIG. 15 is a plan view showing the configuration of a semiconductor substrate according to this embodiment. FIG. 16 is a cross-sectional view showing the configuration of a semiconductor substrate according to this embodiment. FIG. 17 is a plan view showing the configuration of a semiconductor substrate according to this embodiment. As shown in FIGS. 15 to 17, the semiconductor substrate 10 includes a template substrate TS having a growth inhibition region DA and a seed region SA (including first and second regions S1 and S2) aligned in a first direction X1, and a first semiconductor portion 8A located above the template substrate TS and including a nitride semiconductor. The first semiconductor portion 8A includes a first raised portion R1 extending from the first region S1 to a position above the growth inhibition region DA (planar region), a first base portion B1 located above the first raised portion R1, and a first wing portion F1 connected to the first base portion B1, separated from the growth inhibition region DA, and located above the gap JD. The semiconductor substrate 10 may include a growth inhibition film 7 in contact with the first raised portion R1.
[0028] The template substrate TS includes a main substrate 1 and an underlayer 4 located on the main substrate 1. The underlayer 4 contains argon or oxygen as an impurity at a concentration of 2×10 18 / cm 3 The base layer 4 may be made of a nitride semiconductor containing the above. For example, it is possible to form the base layer 4 by a sputtering method using argon gas. The direction from the main substrate 1 to the first semiconductor portion 8A is referred to as "upward." Viewing an object with a line of sight parallel to the normal direction of the semiconductor substrate 10 (including perspective views) is sometimes referred to as "planar view."
[0029] The first region S1, the first protrusion R1, and the first base B1 may overlap in a planar view, and the growth inhibition region DA and the first wing F1 may overlap in a planar view. The first wing F1 does not need to be in contact with the side surface of the first protrusion R1.
[0030] The first semiconductor portion 8A contains a nitride semiconductor as a main component. The first semiconductor portion 8A may be doped (e.g., n-type containing donors) or non-doped. The term "semiconductor substrate" refers to a substrate containing a semiconductor, and the main substrate 1 of the template substrate TS may or may not contain a semiconductor (e.g., silicon or silicon carbide).
[0031] The first direction X1 may be the a-axis direction (<11-20> direction) of the first semiconductor portion 8A. The second direction X2 may be the m-axis direction (<1-100> direction) of the first semiconductor portion 8A (nitride semiconductor such as GaN). The thickness direction of the first semiconductor portion 8A may be the c-axis direction (<0001> direction) of the first semiconductor portion 8A. The first semiconductor portion 8A may have two paired first wing portions F1 extending from the first base portion B1 in the first direction X1 and the opposite direction.
[0032] The first semiconductor portion 8A can be formed by an epitaxial lateral overgrowth (ELO) method, starting from a first protrusion R1 grown from the first region S1. Of the first semiconductor portion 8A, a base portion B1 located above the first region S1 becomes a dislocation inheritance portion with many threading dislocations, and a first wing portion F1 located above the growth inhibition region DA becomes a low-defect portion with a lower threading dislocation density than the dislocation inheritance portion.
[0033] In this manner, by forming the first protrusion R1 and forming the first wing portion F1 extending laterally (parallel to the first direction X1) from the first base portion B1 on the first protrusion R1 and positioned above the gap JD, the first wing portion F1 can be formed with a low defect density and high flatness. The entire first wing portion F1 may be separated from the growth inhibition region DA. This allows the formation of a wide first wing portion F1 with a low defect density and high flatness. Furthermore, when the first wing portion F1 is separated from the growth inhibition region DA and subjected to ELO (lateral overgrowth), fewer conditions are required for the growth inhibition region DA. That is, the conditions for the growth inhibition region DA, such as the shape, selective growth function, adhesion to the semiconductor portion 8, and stress characteristics, are relaxed, which has the advantage of increasing the degree of freedom for the growth inhibition region DA.
[0034] The semiconductor substrate 10 may include a second semiconductor portion 8C located above the template substrate TS. The template substrate TS may have a second region S2 adjacent to the first region S1 with a growth inhibition region DA interposed therebetween, and the second semiconductor portion 8C may have a second raised portion R2 extending from the second region S2 to a position above the growth inhibition region DA (flat region), a second base portion B2 located above the second raised portion R2, and a second wing portion F2 connected to the second base portion B2, separated from the growth inhibition region DA, and located above the gap JD. The first wing portion F1 and the second wing portion F2 may be aligned in the first direction X1 with a gap GP interposed therebetween.
[0035] In the following, the first raised portion R1 and the second raised portion R2 may be collectively referred to as raised portion R, the first semiconductor portion 8A and the second semiconductor portion 8C may be collectively referred to as semiconductor portion 8, the first wing portion F1 and the second wing portion F2 may be collectively referred to as wing portion F, and the first base portion B1 and the second base portion B2 may be collectively referred to as base portion B.
[0036] The growth inhibiting film 7 may be in contact with the side surface RS of the first protrusion R1. This inhibits the growth of the semiconductor portion 8 from the side surface RS, making it easier for the void JD to form. To achieve the effects of this embodiment, the growth inhibiting film 7 only needs to be formed on at least a portion of the side surface RS of the first protrusion R1, and may include a first film portion 7j in contact with the side surface RS of the first protrusion R1 and a second film portion 7i in contact with the top surface RT of the first protrusion R1. The growth inhibiting film 7 does not need to be a complete film; it may be a film including one or more minute openings (a film with an imperfect shape). Forming the second film portion 7i suppresses threading dislocations and the like propagated from the seed portion 3 to the first protrusion R1, thereby achieving a new effect of improving the surface flatness and crystallinity of the first base portion B1.
[0037] The side surface RS of the first protrusion R1 may be a tapered surface that narrows downward, thereby making it possible to widen the width of the gap JD facing the back surface of the first wing portion F1 relative to the width of the gap JD facing the growth suppression area DA, thereby forming a wide first wing portion F1 with low defects.
[0038] The tapered side surface RS may intersect with the growth inhibition region DA. The growth inhibition film 7 may be in contact with the upper surface RT of the first protrusion R1. Of the growth inhibition film 7 in contact with the first protrusion R1, a second film portion 7i (a portion in contact with the upper surface RT of the first protrusion R1) located on the upper surface RT of the first protrusion R1 may be included in the first semiconductor portion 8A. This reduces stress from the template substrate TS.
[0039] 18 is a cross-sectional view showing the configuration of a semiconductor substrate according to this embodiment. As shown in FIG. 18, a growth inhibiting film 7 may be formed on a growth inhibiting area DA.
[0040] Fig. 19 is a flowchart showing a method for manufacturing a semiconductor substrate according to this embodiment. As shown in Fig. 19, the method for manufacturing a semiconductor substrate according to this embodiment includes a step S60 of preparing a semiconductor growth template substrate and a step S70 of forming a first semiconductor portion located above the template substrate. Fig. 20 is a block diagram showing an apparatus for manufacturing a semiconductor substrate according to this embodiment. A semiconductor substrate manufacturing apparatus 80 includes an apparatus M60 that performs step S60 of Fig. 19, an apparatus M70 that performs step S70 of Fig. 20, and a control device M65 that controls apparatus M60 and apparatus M70.
[0041] FIG. 21 is a flowchart showing a method for manufacturing a semiconductor substrate according to this embodiment. FIG. 22 is a cross-sectional view showing the method for manufacturing a semiconductor substrate according to this embodiment. As shown in FIGS. 21 and 22 , the method for manufacturing a semiconductor substrate according to this embodiment includes the steps of: preparing a template substrate TS including a seed region (first and second regions S1 and S2) and a growth inhibition region DA; forming a first protrusion R1 above the template substrate TS, the first protrusion R1 extending from the first region S1 to a position above the growth inhibition region DA; forming a growth inhibition film 7 in contact with the first protrusion R1; and forming a first base B1 located above the first protrusion R1 and a first wing F1 connected to the first base B1, separated from the growth inhibition region DA, and located above the gap JD.
[0042] 22 , the first base B1 and the first wing F1 may be formed using a corner RC where the top surface RT and side surface RS of the first protrusion R1 intersect as a growth starting point PG. In this manner, the corner RC may be used as the growth starting point PG, but this is not limitative. A defect (e.g., a minute opening) may be formed in the growth inhibiting film 7 on the first protrusion R1, and the defect in the growth inhibiting film 7 may be used as a growth starting point for the first base B1 and the first wing F1.
[0043] The first protrusion R1, the growth suppression film 7, the first base B1, and the first wing F1 may be successively formed using an MOCVD apparatus. The first protrusion R1 includes a GaN-based semiconductor, the growth suppression film 7 is silicon nitride, and a gallium source material (organic material such as trimethylgallium (TMG) or triethylgallium (TEG)) and a nitrogen source material (ammonia gas (NH 3 )) to form the first protrusion R1, and while maintaining the supply of the nitrogen source material, the supply of the gallium source material is stopped to supply a silicon-based material (e.g., SiH 4 The growth suppression film 7 may be formed by supplying a silicon-based material to the first base portion B1 and the first wing portion F1. The first base portion B1 and the first wing portion F1 may contain a GaN-based semiconductor, and the supply of the silicon-based material may be stopped and a gallium-based material may be supplied while maintaining the supply of the nitrogen-based material. Alternatively, the supply of a small amount of silicon-based material may be continued at a doping level.
[0044] By forming the growth suppression film 7 in this manner, continuous film formation can be performed without removing the substrate from the MOCVD apparatus while forming the void DJ below the wing portion F, thereby reducing the manufacturing time and manufacturing costs. By forming the void DJ and forming the wing portion F so that it does not come into contact with the underlayer 4 (growth suppression region DA), stresses and the like applied to the semiconductor portion 8 from the main substrate 1 and the underlayer 4 can be effectively alleviated.
[0045] When a mask pattern is formed as in the past, forming a void under the wing portion can deteriorate the flatness of the underside of the wing portion (the surface facing the mask portion). For example, when forming a mask portion by patterning a mask layer using a lift-off method or the like, burrs (protrusions) can remain on both ends of the mask portion, and when overcoming these, the flatness of the underside of the semiconductor layer deteriorates. In this embodiment, the growth suppression region DA, which is an undercoat modification layer, is formed, making it difficult for such protrusions to occur, and making it easier to flatten the underside of the wing portion F. The underside of the wing portion F can be used as a light extraction surface, for example, when forming a light-emitting device on the wing portion F, so it is desirable for it to be flat.
[0046] The growth of the first wing portion F1 and the second wing portion F2 may be stopped before the first wing portion F1 and the second wing portion F2 growing in a direction toward the first wing portion F1 meet.
[0047] 23 to 25 are cross-sectional views showing the configuration of a semiconductor substrate according to this embodiment. In the semiconductor substrates of FIGS. 16 and 18 , raised portions R are formed to lift the wing portions F (F1 and F2) above the growth inhibition region DA, but this is not limiting. As shown in FIG. 23 , in the template substrate TS, the base layer 4 may be formed so that the portion including the first region S1 (the portion directly below the first region) is thicker than the portion including the growth inhibition region DA (the portion directly below the growth inhibition region). As shown in FIG. 24 , in the template substrate TS, the main substrate 1 may have a protrusion Q that protrudes upward, and the first region S1 may be formed on the protrusion Q. Furthermore, as shown in FIG. 25 , the first wing portion F1 of the first semiconductor portion 8A and the second wing portion F2 of the second semiconductor portion 8C may be in contact with the growth inhibition region DA.
[0048] FIG. 26 is a plan view showing a method for manufacturing a semiconductor substrate according to this embodiment. FIGS. 27 and 28 are plan views showing a method for manufacturing a semiconductor substrate and a semiconductor device according to this embodiment. FIG. 29 is a cross-sectional view showing a method for manufacturing a semiconductor substrate and a semiconductor device according to this embodiment. As shown in FIGS. 26 and 29 , a functional layer (device layer) 9 may be formed on the first semiconductor portion 8A. For example, the functional layer 9 for an LED, laser, photodiode, power device, or the like is formed using MOCVD, MBE, sputtering, or the like. The active region (e.g., light-emitting region ES) of the functional layer 9 may be formed above the first wing portion F1 (device region), which is a low-defect portion (low-dislocation portion) (so as to overlap the first wing portion F1 in a plan view).
[0049] 27 and 29 , electrodes EA and EC (e.g., anode and cathode) are formed on the functional layer 9, and predetermined portions of the first semiconductor portion 8A and the functional layer 9 are removed to perform element division. Specifically, a separation groove BM parallel to the first direction X1 is formed in the first semiconductor portion 8A and the functional layer 9, and the first semiconductor portion 8A and the functional layer 9 located on the first region S1 are removed except for two paired tether portions TZ, thereby forming an element region PA. The two tether portions TZ are portions of both ends of the element region PA facing each other in the second direction X2 that are connected to the first region S1.
[0050] As shown in Figures 28 and 29, the element region PA (including the wing portion F, functional layer 9, and electrodes EA and EC) is separated from the template substrate TS to form a semiconductor device 25. Because there is a gap JD below the wing portion F, by applying downward pressure to the element region PA with a pressure-sensitive or adhesive pressing body YS (such as an adhesive plate, adhesive sheet, or adhesive substrate), the two tether portions TZ easily crack and the semiconductor device 25 is separated from the template substrate TS. Specifically, the semiconductor device 25 is peeled off from the template substrate TS while being held by the pressing body YS. In this way, the gap JD also functions effectively in element isolation, allowing the semiconductor device 25 to be peeled off from the template substrate TS without damaging it.
[0051] Specific examples of the semiconductor device 25 include a light-emitting diode (LED), a semiconductor laser, a Schottky diode, a photodiode, and a transistor (including a power transistor and a high electron mobility transistor).
[0052] FIG. 30 is a schematic diagram showing the configuration of an electronic device according to this embodiment. The electronic device 55 in FIG. 30 includes a semiconductor device 25 including a semiconductor portion 8, a drive substrate 23 on which the semiconductor device 25 is mounted, and a control circuit 27 that controls the drive substrate 23. FIG. 31 is a schematic diagram showing another configuration of the electronic device according to this embodiment. The element region (element portion) PA does not need to be peeled off from the template substrate TS. The electronic device 55 in FIG. 31 includes a semiconductor substrate 10 including the template substrate TS and the element region PA, a drive substrate 23 on which the semiconductor substrate 10 is mounted, and a control circuit 27 that controls the drive substrate 23. In this case, the main substrate included in the template substrate TS may be a light-transmitting substrate (e.g., a sapphire substrate). Examples of the electronic device 55 include a light-emitting device, a display device, a laser emitting device (including a Fabry-Perot type and a surface-emitting type), a measuring device, a lighting device, a communication device, an information processing device, and a power control device.
[0053] (Note) The above disclosure is intended to be illustrative and explanatory, and is not intended to be limiting. Based on these examples and explanations, many variations will be obvious to those skilled in the art, and it should be noted that these variations are also included in the embodiments.
[0054] REFERENCE SIGNS LIST 1 Main substrate 4 Underlayer 7 Growth suppression film 8A First semiconductor portion 8C Second semiconductor portion 10 Semiconductor substrate 25 Semiconductor device 30 Template substrate manufacturing apparatus 55 Electronic device R1 First raised portion R2 Second raised portion B1 First base portion B2 Second base portion F1 First wing portion F2 Second wing portion JD Void SA Seed region S1 First region S2 Second region DA Growth suppression region TS Template substrate (template substrate for semiconductor growth)
Claims
1. A template substrate for semiconductor growth comprising: a main substrate; and an underlayer located above the main substrate and containing an underlayer material, the surface of the underlayer including a growth inhibition region in which the underlayer material has been modified, and a seed region in which the underlayer material has not been modified.
2. The semiconductor growth template substrate of claim 1, wherein the seed region includes a first region and a second region, and the growth inhibition region is located between the first region and the second region.
3. The template substrate for semiconductor growth according to claim 2, wherein the first region and the second region are arranged in a stripe pattern.
4. The semiconductor growth template substrate according to any one of claims 1 to 3, wherein the base material is a nitride semiconductor, and the main substrate is a heterogeneous substrate having a lattice constant different from that of the nitride semiconductor.
5. The template substrate for semiconductor growth according to any one of claims 1 to 4, wherein the growth inhibition region and the seed region differ from each other in at least one of contained elements and crystal structure.
6. The semiconductor growth template substrate according to any one of claims 1 to 5, wherein the growth inhibition region is polycrystalline or amorphous.
7. The template substrate for semiconductor growth according to claim 1, wherein the growth inhibition region and the seed region are flush with each other.
8. The semiconductor growth template substrate according to any one of claims 1 to 7, wherein the underlying material is an aluminum nitride.
9. The semiconductor growth template substrate of claim 8, further comprising an aluminum layer between said main substrate and said underlayer.
10. The semiconductor growth template substrate according to any one of claims 1 to 6, wherein the seed region is located above the growth inhibition region.
11. The semiconductor growth template substrate according to claim 2, wherein the portion of the underlayer directly below the first region is thicker than the portion directly below the growth inhibition region.
12. The semiconductor growth template substrate according to claim 2, wherein the main substrate has a protruding portion protruding upward, and the first region is located on the protruding portion.
13. The semiconductor growth template substrate according to claim 1, wherein the growth inhibition region has a higher impurity concentration than the seed region.
14. The template substrate for semiconductor growth according to claim 13, wherein the impurity concentration is an oxygen concentration.
15. The semiconductor growth template substrate according to claim 13, wherein the impurity concentration is an argon concentration.
16. The semiconductor growth template substrate according to any one of claims 1 to 15, wherein the growth inhibition region does not contain silicon.
17. The semiconductor growth template substrate according to claim 3, wherein the width of the growth inhibition region is at least five times the width of the first region.
18. The semiconductor growth template substrate according to claim 4, wherein the growth inhibition region and the seed region are aligned in the a-axis direction of the nitride semiconductor.
19. The semiconductor growth template substrate of claim 4, wherein the main substrate is a silicon substrate, a sapphire substrate, a silicon carbide substrate, or an aluminum nitride substrate.
20. The semiconductor growth template substrate according to any one of claims 1 to 19, wherein the growth inhibition region includes an oxide of the underlying material.
21. A semiconductor substrate comprising: a template substrate for semiconductor growth according to any one of claims 1 to 20; and a first semiconductor portion located above the template substrate for semiconductor growth.
22. The semiconductor substrate of claim 21, wherein the seed region includes a first region and a second region, and the first semiconductor portion includes a first base portion located above the first region and a first wing portion located above the growth inhibition region and connected to the first base portion.
23. The semiconductor wafer according to claim 22, wherein the first wing portion has a lower threading dislocation density than the first base portion.
24. The semiconductor substrate of claim 22 or 23, wherein the first wing portion is not in contact with the growth inhibition region.
25. The semiconductor substrate of claim 22 or 23, wherein the first wing portion contacts the growth inhibition region.
26. The semiconductor substrate according to any one of claims 22 to 24, wherein the first semiconductor portion includes a raised portion that rises from the first region and is connected to the first base portion.
27. The semiconductor substrate according to claim 26, further comprising a growth inhibiting film in contact with said protuberance.
28. A semiconductor substrate as claimed in any one of claims 22 to 27, comprising a second semiconductor portion located above the semiconductor growth template substrate, the growth inhibition region being located between the first region and the second region, the second semiconductor portion including a second base portion located above the second region and a second wing portion located above the growth inhibition region and connected to the second base, and a gap being present between the first wing portion and the second wing portion.
29. The semiconductor substrate according to any one of claims 22 to 28, further comprising a functional layer located on the first semiconductor portion and including an active layer.
30. The semiconductor substrate according to claim 29, wherein the active layer includes a light emitting region that overlaps with the first wing portion in a plan view.
31. The semiconductor substrate according to any one of claims 21 to 30, wherein the base material contains a metal element not contained in the first semiconductor portion.
32. A method for manufacturing a template substrate for semiconductor growth, comprising: forming an underlayer containing an underlayer material above a main substrate; and forming, on a surface of the underlayer, a growth inhibition region in which the underlayer material is modified and a growth region seed region in which the underlayer material is not modified.
33. An apparatus for manufacturing a template substrate for semiconductor growth, which performs each of the steps recited in claim 32.
34. A method for manufacturing a semiconductor substrate, comprising: preparing a semiconductor growth template substrate according to any one of claims 1 to 21; and forming a first semiconductor portion located above the semiconductor growth template substrate.
35. The method for manufacturing a semiconductor substrate according to claim 34, wherein the first semiconductor portion is formed using an ELO method.
36. A method for manufacturing a semiconductor substrate as described in claim 34 or 35, wherein the seed region includes a first region and a second region, the first semiconductor portion includes a first base portion located above the first region and a first wing portion located above the growth inhibition region and connected to the first base, and the first wing portion is grown laterally while being spaced apart from the growth inhibition region.
37. A semiconductor substrate manufacturing apparatus which performs each of the steps recited in claim 34.
Citation Information
Patent Citations
Substrate for semiconductor growth, manufacture thereof, and semiconductor device
JP2000077336A
Method for growing nitride semiconductor
JP2000357843A
Nitride semiconductor substrate and its producing method
JP2002100579A
Group iii nitride compound semiconductor
JP2003252700A
Heteroepitaxial growth method and crystal thin film
JP2005276951A